A high corrosion resistance amorphous alloy electroplating method
By combining organophosphonic acid complexation activation, ultrasonic field assistance, and pulse electroplating, the corrosion problem of 304 stainless steel in chloride ion-containing environments was solved, achieving high adhesion and long service life of highly corrosion-resistant amorphous alloy electroplating layers.
Patent Information
- Application Number
- CN202610301869.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-03-12
AI Technical Summary
304 stainless steel is prone to pitting corrosion and stress corrosion cracking in chloride ion-containing environments. Traditional electroplating processes suffer from poor adhesion, serious pollution, and difficulty in adapting to the optimization of stainless steel passivation characteristics.
Electrochemical activation treatment was performed using an organophosphonic acid complexation activation solution combined with an ultrasonic field and periodic commutation potential to form an organophosphonic acid adsorption layer. Subsequently, a Ni-P amorphous pre-plating layer was generated through wet transfer and chemical flash plating. Finally, a Ni-P amorphous main plating layer was deposited using pulse electroplating.
It significantly improves the adhesion and corrosion resistance of the coating, and extends the protective life of 304 stainless steel.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of electroplating technology, and in particular to a method for electroplating highly corrosion-resistant amorphous alloys. Background Technology
[0002] 304 austenitic stainless steel is widely used in chemical, marine engineering, and medical device industries due to its excellent comprehensive properties. However, in chloride-containing environments, this material is prone to pitting corrosion and stress corrosion cracking, which seriously affects its long-term service safety. To improve the material's corrosion resistance, an alloy coating is often electroplated on the surface to block corrosive media.
[0003] However, the dense chromium-rich passivation film on the surface of 304 stainless steel leads to poor coating adhesion and easy peeling. Traditional pickling processes for removing the passivation film (such as those containing highly toxic chromic anhydride and hydrofluoric acid) cause serious pollution and harm to health. Furthermore, the separation of activation and electroplating processes can cause the activated fresh surface to be re-passivated during transfer, affecting the bonding effect. In addition, existing plating solutions are mostly designed for low-carbon steel and have not been optimized for the passivation characteristics of stainless steel, making them difficult to apply directly. Summary of the Invention
[0004] This application provides a method for electroplating highly corrosion-resistant amorphous alloys to solve the technical problem of limited protective life of 304 stainless steel coatings.
[0005] In a first aspect, this application provides a method for electroplating highly corrosion-resistant amorphous alloys, comprising: S1, the clean stainless steel workpiece is immersed in a complexing activation solution containing organophosphonic acid, and electrochemical activation is performed under the assistance of an ultrasonic field and the periodic commutation potential is controlled to remove the surface purification film of the clean stainless steel workpiece and form an organophosphonic acid adsorption layer to obtain the first workpiece. S2, the first workpiece is removed from the complexing activation solution and kept moisturized by spraying until the first workpiece is immersed in the nickel-phosphorus chemical flash plating solution for chemical deposition to form a pre-plating layer on the surface of the first workpiece, thus obtaining the second workpiece; S3, the second workpiece is placed in a nickel-phosphorus electroplating solution, the second workpiece is used as the cathode and a pure nickel plate is used as the anode, and a Ni-P amorphous main plating layer is deposited on the surface of the pre-plating layer by pulse electroplating to obtain the target stainless steel workpiece.
[0006] In some embodiments, S1 includes: After heating the complexing activation solution to 35℃~45℃, a clean stainless steel workpiece is immersed in the complexing activation solution. The ultrasonic generator is turned on, and the ultrasonic frequency is controlled at 28 kHz~40 kHz with a power density of 0.3 W / cm². 2 ~0.6 W / cm 2 ; Under the action of an ultrasonic field, the clean stainless steel workpiece is activated by applying a periodic commutation potential to obtain the first workpiece. The periodic commutation potential includes 3 to 5 activation cycles. Each activation cycle includes an anodic polarization stage in which an anodic potential of +0.3 V to +0.8 V is applied and held for 10 to 30 seconds, and a cathodic polarization stage in which a cathodic potential of -0.8 V to -1.2 V is applied and held for 40 to 80 seconds.
[0007] In some embodiments, the complexing activation solution in S1 comprises the following components: hydroxyethylidene diphosphonic acid 35 g / L~55 g / L, hydroxylamine sulfate 8 g / L~12 g / L, ammonium bifluoride 3 g / L~7 g / L, and the balance being deionized water.
[0008] In some embodiments, S2 includes: After the first workpiece is removed from the complexing activation solution, the moisturizing solution is continuously sprayed onto the surface of the first workpiece, and the first workpiece is transferred to the treatment tank containing the nickel-phosphorus chemical flash plating solution. The first workpiece is immersed in the nickel-phosphorus electroless flash plating solution heated to 45℃~55℃. Under no external current or with a cathode microcurrent of 0.1 A / dm²~0.5 A / dm², it is left to stand for 4min~8min to allow the nickel-phosphorus electroless flash plating solution to undergo an autocatalytic reduction reaction on the surface of the first workpiece, generating a continuous and dense Ni-P amorphous pre-plating layer with a thickness of 80nm~150nm and a phosphorus content of 9 wt%~13wt%, thus obtaining the second workpiece.
[0009] In some embodiments, the moisturizing solution is a 0.1 wt% to 1 wt% aqueous solution of dilute hydroxyethylidene diphosphonic acid.
[0010] In some embodiments, the nickel-phosphorus electroless flash plating solution comprises: 25 g / L to 45 g / L nickel salt, 18 g / L to 32 g / L sodium hypophosphite, 15 g / L to 25 g / L sodium citrate, 10 g / L to 20 g / L sodium acetate, 0.2 g / L to 1 g / L nanonucleation promoter, an appropriate amount of pH adjuster to a pH value of 4.2 to 5.2, and the balance being deionized water.
[0011] In some embodiments, the nanonucleation promoter is a silicon carbide whisker or nanodiamond particle with a particle size of 20 nm to 50 nm.
[0012] In some embodiments, S3 includes: The workpiece is immersed in the nickel-phosphorus electroplating solution heated to 50°C~60°C. The second workpiece is used as the cathode and the pure nickel plate is used as the anode. The pulse power supply is started for electroplating for 45min~75min, so that the Ni-P amorphous main coating grows homogeneously on the surface of the pre-plating layer, and the target stainless steel workpiece with a total thickness of 15μm~30μm and a phosphorus content of 9wt%~13wt% is obtained.
[0013] In some embodiments, the nickel-phosphorus electroplating solution in S3 includes: Nickel sulfamate 280 g / L~320 g / L, sodium hypophosphite 25 g / L~35 g / L, boric acid 30 g / L~40 g / L, saccharin 0.8 g / L~1.2 g / L, sodium dodecyl sulfate 0.05 g / L~0.15 g / L, pH adjuster adjusted to 1.8~2.5, balance is deionized water.
[0014] In some embodiments, the average current density of the pulse electroplating method in S3 is 3 A / dm³. 2 ~6 A / dm 2 The pulse duty cycle is 20%~40%, the pulse frequency is 800Hz~2000Hz, the forward and reverse pulse time ratio is (5~10):1, and the electroplating time is 45min~75min.
[0015] Compared with the prior art, this application has at least the following beneficial effects: S1 employs a complexing activation solution containing organophosphonic acid, combined with ultrasonic field assistance and periodic commutation potential control for electrochemical activation treatment. Organophosphonic acid has a strong complexing ability for iron and nickel ions, efficiently stripping the dense passivation film from the stainless steel surface. The cavitation effect of the ultrasonic field generates microjets, physically impacting and loosening the passivation layer while enhancing mass transfer. Periodic commutation potential electrochemically dissolves the passivation film through anodic polarization and reduces metal ions to an active metallic state through cathodic polarization, synergistically achieving complete removal of the passivation film and forming an organophosphonic acid adsorption layer on the fresh surface, effectively preventing re-oxidation. S2 uses a combination of wet transfer and chemical flash plating. After removing the workpiece, a moisturizing solution is immediately sprayed to maintain surface wettability, avoiding secondary passivation caused by air exposure. After immersion in the nickel-phosphorus chemical flash plating solution, the surface catalytic activity triggers a self-deposition reaction, generating an ultrathin Ni-P amorphous pre-plating layer in situ. S3 employs pulse electroplating to deposit a Ni-P amorphous main coating on a pre-coating layer. The pre-coating layer and the main coating layer have the same composition and matching structure, forming a homogeneous epitaxial metallurgical bond. This method achieves full-process optimization from surface activation and interface transition to the main coating layer, significantly improving coating adhesion and corrosion resistance, thereby extending the protective life of 304 stainless steel coatings. Detailed Implementation
[0016] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0017] As used herein, the terms “prepared from” and “comprising” are synonymous. The terms “comprising,” “including,” “having,” “containing,” or any other variations thereof, as used herein, are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.
[0018] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1 to 5” is disclosed, the described range should be interpreted as including the ranges “1 to 4”, “1 to 3”, “1 to 2”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.
[0019] Furthermore, the indefinite articles “a” and “an” preceding the elements or components of this invention do not impose any limitation on the quantity (i.e., number of occurrences) of the elements or components. Therefore, “an” or “a” should be interpreted as including one or at least one, and the singular form of an element or component also includes the plural form, unless the quantity clearly refers to the singular form.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. Example 1
[0021] S1, Complexation and Activation Treatment: A complexing activation solution was prepared using 45 g / L hydroxyethylidene diphosphonic acid, 10 g / L hydroxylamine sulfate, 5 g / L ammonium hydrogen fluoride, and the remainder being deionized water, and then heated to 40°C. The 304 stainless steel workpiece (50mm×50mm×2mm) was successively polished with 600#, 1000# and 1500# sandpaper, degreased with alkaline solution (60℃, 10min), and cleaned with deionized water to obtain a clean stainless steel workpiece. The clean stainless steel workpiece was immersed in the complexing activation solution, and the ultrasonic generator was turned on, with the ultrasonic frequency set to 34 kHz and the power density to 0.45 W / cm². Periodic commutation potentials were applied for activation treatment, and a total of 4 activation cycles were performed. Anodic polarization phase: Apply +0.5 V (vs SCE) and hold for 20 s; Cathodic polarization phase: Apply -1.0 V (vs SCE) and hold for 60 s; After the activation treatment is completed, the first workpiece is obtained.
[0022] S2, Wet transfer and chemical flash plating: A nickel-phosphorus electroless flash plating solution was prepared using 35 g / L nickel sulfate, 25 g / L sodium hypophosphite, 20 g / L sodium citrate, 15 g / L sodium acetate, 0.6 g / L nano-SiC whiskers (35 nm particle size), and ammonia water to adjust the pH to 4.7, with the remainder being deionized water. The first workpiece was removed from the complexing activation solution and sprayed with a 0.5 wt% dilute HEDP aqueous solution immediately without water washing. While maintaining the spraying, it was transferred to the treatment tank containing nickel-phosphorus electroless flash plating solution. The flash plating solution is heated to 50°C, the first workpiece is immersed in the flash plating solution, a cathode microcurrent of 0.3 A / dm² is applied, and the workpiece is left to stand for 6 minutes to form a Ni-P amorphous pre-plating layer, thus obtaining the second workpiece.
[0023] S3, Pulse electroplating main plating layer: A nickel-phosphorus electroplating solution was prepared using 300 g / L nickel aminosulfonate, 30 g / L sodium hypophosphite, 35 g / L boric acid, 1.0 g / L saccharin, 0.1 g / L sodium dodecyl sulfate, and dilute sulfuric acid to adjust the pH to 2.2, with the remainder being deionized water. The electroplating solution was heated to 55°C. The second workpiece was used as the cathode and the pure nickel plate as the anode. A pulse power supply was used with an average current density of 4.5 A / dm², a duty cycle of 30%, a pulse frequency of 1400 Hz, a forward-reverse pulse time ratio of 8:1, and an electroplating time of 60 min. After electroplating, the workpiece is removed, rinsed with deionized water for 2 minutes, and dried with hot air at 60℃ for 10 minutes to obtain the target stainless steel workpiece. Example 2
[0024] S1, Complexation and Activation Treatment: Complexing activation solution: HEDP 35 g / L, hydroxylamine sulfate 8 g / L, ammonium bifluoride 3 g / L; The ultrasonic frequency was 28 kHz, and the power density was 0.3 W / cm². Three activation cycles: anode +0.3 V / 30s, cathode -0.8 V / 40s.
[0025] S2, Wet transfer and chemical flash plating: Moisturizing solution: 0.1 wt% dilute HEDP aqueous solution; Flash plating solution: Nickel chloride 25 g / L, sodium hypophosphite 18 g / L, sodium citrate 15 g / L, sodium acetate 10 g / L, nanodiamond particles (particle size 20nm) 0.2 g / L, pH 4.2; The flash plating temperature is 45℃, no external current is applied, and the substrate is left to stand for 8 minutes to form a pre-plating layer.
[0026] S3, Pulse electroplating main plating layer: The electroplating solution is the same as in Example 1; Pulse power supply parameters: average current density 3 A / dm², duty cycle 20%, pulse frequency 800 Hz, forward / reverse time ratio 5:1, electroplating time 75 min. Example 3
[0027] S1, Complexation and Activation Treatment: Complexing activation solution: HEDP 55 g / L, hydroxylamine sulfate 12 g / L, ammonium bifluoride 7 g / L; The ultrasonic frequency is 40 kHz, and the power density is 0.6 W / cm². Five activation cycles: anode +0.8 V / 10s, cathode -1.2 V / 80s.
[0028] S2, Wet transfer and chemical flash plating: Moisturizing solution: 1.0 wt% dilute HEDP aqueous solution; Flash plating solution: Nickel sulfamate 45 g / L, sodium hypophosphite 32 g / L, sodium citrate 25 g / L, sodium acetate 20 g / L, nano-SiC whiskers (particle size 50 nm) 1.0 g / L, pH 5.2; The flash plating temperature is 55℃, a cathode microcurrent of 0.5 A / dm² is applied, and the mixture is left to stand for 4 minutes to form a pre-plating layer.
[0029] S3, Pulse electroplating main plating layer: The electroplating solution is the same as in Example 1; Pulse power supply parameters: average current density 6 A / dm², duty cycle 40%, pulse frequency 2000 Hz, forward-reverse time ratio 10:1, electroplating time 45 min.
[0030] Comparative Example 1 The difference from Example 1 is that the ultrasonic generator is not turned on in the S1 activation treatment of Comparative Example 1.
[0031] Comparative Example 2 The difference from Example 1 is that in the S1 activation treatment of Comparative Example 2, a constant cathode potential of -1.0 V is used instead of a periodic commutation potential.
[0032] Comparative Example 3 The difference from Example 1 is that, after activation treatment in S1, Comparative Example 3 takes out the first workpiece for deionized water cleaning (1 min), allows the surface moisture to drain naturally (30 s), and then transfers it to the flash plating tank in S2.
[0033] Comparative Example 4 The difference from Example 1 is that the S2 flash plating solution of Comparative Example 4 does not contain a nano-nucleation promoter.
[0034] Comparative Example 5 The difference from Example 1 is that in Comparative Example 5, S3 uses DC electroplating (4.5 A / dm², 60 min) instead of a pulse power supply.
[0035] Table 1 Performance test results of Examples 1 to 3 and blank 304 stainless steel
[0036] Table 2 Performance test results of Comparative Examples 1 to 5
[0037] As shown in Tables 1 and 2, Examples 1-3 are significantly superior to the comparative examples in all key performance indicators. Among them, the adhesion and corrosion resistance of Comparative Example 1 are significantly reduced, indicating that the ultrasonic-assisted cavitation effect is crucial for thoroughly removing the passivation film in the micro-pits and achieving uniform activation. The weaker bonding force in Comparative Example 2 indicates that the synergistic effect of anodic dissolution and loosening by periodic commutation potential and cathodic reduction stripping is more effective than cathodic reduction alone in removing the dense passivation film while avoiding excessive corrosion. Comparative Example 3 showed a sharp deterioration in adhesion, with a salt spray time of only 180 hours and a self-corrosion current density that was an order of magnitude higher than that of Example 1. This may be because the conventional water washing step exposes the activated fresh surface to oxygenated water, causing immediate re-oxidation and the formation of a thin and loose secondary oxide film, which severely hinders the formation and adhesion of the subsequent flash coating. However, by using water washing and dilute HEDP spraying for hydration, the high activity state of the surface was successfully maintained by utilizing the adsorption and protection effect of HEDP molecules. Comparative Example 4 showed a decrease in coating density, a reduction in salt spray time from 650 h to 480 h, and a decrease in hardness from 612 HV to 541 HV. This indicates that nano-SiC whiskers provide heterogeneous nucleation centers during flash plating, significantly increasing the nucleation density of the pre-coated layer, making the pre-coated layer more uniform and dense, and providing an excellent substrate for the growth of the main coating. The decrease in corrosion resistance in Comparative Example 5 indicates that the high instantaneous current density of pulse electroplating and the leveling effect of the reverse pulse are beneficial to obtaining a completely amorphous structure and eliminating internal stress, thereby improving hardness and corrosion resistance.
[0038] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0039] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit the scope of protection of this application. In particular, it should be noted that any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application for those skilled in the art.
Claims
1. A method for electroplating highly corrosion-resistant amorphous alloys, characterized in that, include: S1, the clean stainless steel workpiece is immersed in a complexing activation solution containing organophosphonic acid, and electrochemical activation is performed under the assistance of an ultrasonic field and the periodic commutation potential is controlled to remove the surface purification film of the clean stainless steel workpiece and form an organophosphonic acid adsorption layer to obtain the first workpiece. S2, the first workpiece is removed from the complexing activation solution and kept moisturized by spraying until the first workpiece is immersed in the nickel-phosphorus chemical flash plating solution for chemical deposition to form a pre-plating layer on the surface of the first workpiece, thus obtaining the second workpiece; S3, the second workpiece is placed in a nickel-phosphorus electroplating solution, the second workpiece is used as the cathode and a pure nickel plate is used as the anode, and a Ni-P amorphous main plating layer is deposited on the surface of the pre-plating layer by pulse electroplating to obtain the target stainless steel workpiece. S1 includes: After heating the complexing activation solution to 35℃~45℃, a clean stainless steel workpiece is immersed in the complexing activation solution. The ultrasonic generator is turned on, and the ultrasonic frequency is controlled at 28 kHz~40 kHz with a power density of 0.3 W / cm². 2 ~0.6 W / cm 2 ; Under the action of an ultrasonic field, the clean stainless steel workpiece is activated by applying a periodic commutation potential to obtain the first workpiece. The periodic commutation potential includes 3 to 5 activation cycles. Each activation cycle includes an anodic polarization stage in which an anodic potential of +0.3 V to +0.8 V is applied and held for 10 to 30 seconds, and a cathodic polarization stage in which a cathodic potential of -0.8 V to -1.2 V is applied and held for 40 to 80 seconds. The complexing activation solution in S1 comprises the following components: hydroxyethylidene diphosphonic acid 35 g / L~55 g / L, hydroxylamine sulfate 8 g / L~12 g / L, ammonium bifluoride 3 g / L~7 g / L, and the balance being deionized water; The nickel-phosphorus electroless flash plating solution in S2 comprises: 25 g / L to 45 g / L nickel salt, 18 g / L to 32 g / L sodium hypophosphite, 15 g / L to 25 g / L sodium citrate, 10 g / L to 20 g / L sodium acetate, 0.2 g / L to 1 g / L nano-nucleation promoter, an appropriate amount of pH adjuster to a pH value of 4.2 to 5.2, and the balance being deionized water; the nano-nucleation promoter is silicon carbide whiskers or nanodiamond particles with a particle size of 20 nm to 50 nm; The average current density of the pulse electroplating method in S3 is 3 A / dm. 2 ~6 A / dm 2 The pulse duty cycle is 20%~40%, the pulse frequency is 800Hz~2000Hz, the forward and reverse pulse time ratio is (5~10):1, and the electroplating time is 45min~75min.
2. The electroplating method for high corrosion resistance amorphous alloys as described in claim 1, characterized in that, S2 includes: After the first workpiece is removed from the complexing activation solution, the moisturizing solution is continuously sprayed onto the surface of the first workpiece, and the first workpiece is transferred to the treatment tank containing the nickel-phosphorus chemical flash plating solution. The first workpiece is immersed in the nickel-phosphorus electroless flash plating solution heated to 45℃~55℃. Under no external current or with a cathode microcurrent of 0.1 A / dm²~0.5 A / dm², it is left to stand for 4min~8min to allow the nickel-phosphorus electroless flash plating solution to undergo an autocatalytic reduction reaction on the surface of the first workpiece, generating a continuous and dense Ni-P amorphous pre-plating layer with a thickness of 80nm~150nm and a phosphorus content of 9 wt%~13 wt%, thus obtaining the second workpiece.
3. The electroplating method for high corrosion resistance amorphous alloys as described in claim 2, characterized in that, The moisturizing solution is a 0.1wt%~1wt% aqueous solution of dilute hydroxyethylidene diphosphonic acid.
4. The electroplating method for high corrosion resistance amorphous alloys as described in claim 1, characterized in that, S3 includes: The workpiece is immersed in the nickel-phosphorus electroplating solution heated to 50°C~60°C. The second workpiece is used as the cathode and the pure nickel plate is used as the anode. The pulse power supply is started for electroplating for 45min~75min, so that the Ni-P amorphous main coating grows homogeneously on the surface of the pre-plating layer, and the target stainless steel workpiece with a total thickness of 15μm~30μm and a phosphorus content of 9wt%~13wt% is obtained.
5. The electroplating method for high corrosion resistance amorphous alloys as described in claim 4, characterized in that, The nickel-phosphorus electroplating solution in S3 includes: Nickel sulfamate 280 g / L~320 g / L, sodium hypophosphite 25 g / L~35 g / L, boric acid 30 g / L~40 g / L, saccharin 0.8 g / L~1.2 g / L, sodium dodecyl sulfate 0.05 g / L~0.15 g / L, pH adjuster adjusted to 1.8~2.5, balance is deionized water.
Citation Information
Patent Citations
Electroplating solution and surface treatment method for improving corrosion resistance of stainless steel by using same
CN114717614A
Pretreatment liquid for magnesium alloy coating processing and application thereof
CN119194431A
Efficient electroplating process for cotton picker spindle and electroplating liquid formula
CN120425427A
Electro-chemical deposition system and method of electroplating on substrates
US6261433B1