Antistatic low-extraction polyethylene blow molded article and method of making

CN122253517APending Publication Date: 2026-06-23JIANGYIN LONGYUN PLASTIC IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610565718.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-27
Publication Date
2026-06-23

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application discloses an anti-static low-extraction polyethylene blow-molding product, which comprises, from outside to inside, an outer layer, an intermediate layer and an inner layer; the outer layer comprises high-density polyethylene and an anti-static agent; the intermediate layer comprises high-density polyethylene; the inner layer is fusible polytetrafluoroethylene; a transition layer is further arranged between the intermediate layer and the inner layer; the transition layer comprises high-density polyethylene and a fluorine-containing alkylated poly(ethylene-g-maleic anhydride) polymer; and the fluorine-containing alkylated poly(ethylene-g-maleic anhydride) polymer is obtained by reacting a fluorine-containing alcohol and poly(ethylene-g-maleic anhydride) under the catalysis of toluenesulfonic acid. The product has the advantages of corrosion resistance and clean protection, high compatibility and structural strength, and double-sided anti-static performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyethylene material technology, specifically to an antistatic, low-exudation polyethylene blow-molded product and its preparation method. Background Technology

[0002] Polyethylene products are used for the storage and transportation of liquids, and are characterized by their fragility, rust resistance, and lightweight. However, when commonly used polyethylene products are used for long-term storage of chemical reagents, impurities in the resin composition of the inner layer, which are in direct contact with the reagents, can leach out and seep into the contained chemical reagents, compromising their purity. This is especially true for electronic pharmaceuticals, negatively impacting their quality and performance. Furthermore, containers for chemical reagents must be protected against and controlled for static electricity to prevent hazards such as fires and explosions caused by static electricity.

[0003] Therefore, it is necessary to improve polyethylene blow-molded products. Summary of the Invention

[0004] One of the objectives of this invention is to overcome the deficiencies in the prior art and provide an antistatic, low-exudation polyethylene blow-molded product that combines corrosion resistance and cleanliness protection, high compatibility and structural strength, and double-sided antistatic properties.

[0005] To achieve the above-mentioned process effects, the technical solution of the present invention is as follows: an antistatic low-exudation polyethylene blow-molded product, comprising an outer layer, an intermediate layer and an inner layer from the outside to the inside, wherein the outer layer comprises high-density polyethylene and an antistatic agent, the intermediate layer comprises high-density polyethylene, the inner layer is fusible polytetrafluoroethylene, and a transition layer is further provided between the intermediate layer and the inner layer, wherein the transition layer comprises high-density polyethylene and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer; The fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer is obtained by reacting a fluorinated alcohol with poly(ethylene-g-maleic anhydride) under the catalysis of toluenesulfonic acid.

[0006] A preferred technical solution is that the fluorinated alcohol is a perfluoroalkyl ethyl alcohol and / or a perfluoroalkyl propyl alcohol; the alkyl carbon chain of the perfluoroalkyl ethyl alcohol is C6~12, and / or the alkyl carbon chain of the perfluoroalkyl propyl alcohol is C6~12.

[0007] The preferred technical solution is that the mass ratio of the high-density polyethylene to the fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer is (30~50):(50~70).

[0008] The preferred technical solution is that the antistatic agent is obtained by blending high-density polyethylene and ethylene-vinyl acetate copolymer as matrix materials, multi-walled carbon nanotubes as conductive fillers, and modified high-density polyethylene as compatibilizer, and then obtaining the mixture under the action of a crosslinking agent.

[0009] A preferred technical solution is that the outer layer comprises high-density polyethylene and an antistatic agent in a mass ratio of (90~95):(5~10).

[0010] A preferred technical solution is that the crosslinking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and / or triallyl isocyanurate; further, the crosslinking agent includes triallyl isocyanurate and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane in a mass ratio of 1:(2~4).

[0011] A preferred technical solution is that the modifier of the modified high-density polyethylene is vinyltrimethoxysilane and / or maleic anhydride; further, the modifier of the modified high-density polyethylene includes vinyltrimethoxysilane and maleic anhydride in a mass ratio of 1:(1~1.3).

[0012] The preferred technical solution is that the mass ratio of high-density polyethylene, ethylene-vinyl acetate copolymer, multi-walled carbon nanotubes, modified high-density polyethylene and crosslinking agent in the antistatic agent is (87~92):(5~7):(7~10):(3~6):(0.6~0.8).

[0013] The preferred technical solution is that the layer thickness ratio of the outer layer, middle layer, transition layer and inner layer of the blow-molded product is (4.5~5.5):(2.5~3.5):(1~1.5):(1~1.5).

[0014] The second objective of this invention is to overcome the deficiencies in the prior art and provide a method for preparing an antistatic, low-exudation polyethylene blow-molded product. Based on the above-mentioned antistatic, low-exudation polyethylene blow-molded product, the outer layer extrusion temperature of the polyethylene blow-molded product is 200~220℃, the middle layer extrusion temperature is 200~250℃, the transition layer extrusion temperature is 200~250℃, and the inner layer extrusion temperature is 300~350℃.

[0015] The advantages and beneficial effects of this invention are as follows: The inner layer, made of fusible polytetrafluoroethylene, is corrosion-resistant and ensures the cleanliness of the contents. The transition layer, which is a composite of high-density polyethylene and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer, not only improves the compatibility between the layers and thus improves the stability of the layer structure, but also ensures the flexural strength and compressive strength of the product. The outer layer, composed of high-density polyethylene and an antistatic agent, combined with the low surface energy of the inner layer, provides double-sided antistatic properties, effectively eliminating the risks associated with static electricity. Detailed Implementation

[0016] The specific embodiments of the present invention will be further described below with reference to examples. These examples are only used to more clearly illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention.

[0017] Antistatic agent The antistatic agent is obtained by blending high-density polyethylene and ethylene-vinyl acetate copolymer as matrix materials, multi-walled carbon nanotubes as conductive fillers, and modified high-density polyethylene as compatibilizer, and then applying a crosslinking agent.

[0018] Multi-walled carbon nanotubes are modified to contain hydroxyl or carboxyl groups. They have a diameter of 10–30 nm, a length of 10–30 μm, and a specific surface area ≥120 m². 2 / g, containing hydroxyl groups of 1.5 wt%~4 wt%. Beijing Deco Island Gold Technology Co., Ltd., model CNT204, can be selected.

[0019] The modified high-density polyethylene (HDPE) is prepared using vinyltrimethoxysilane as a modifier, maleic anhydride as a modifier, or a mixture of vinyltrimethoxysilane and maleic anhydride as modifiers. Preferably, the modified HDPE is a mixture of vinyltrimethoxysilane and maleic anhydride, wherein the mass ratio of vinyltrimethoxysilane to maleic anhydride is 1:(1~1.3). The vinyltrimethoxysilane and maleic anhydride compound-modified HDPE exhibits a higher grafting rate, thereby promoting the dispersion of multi-walled carbon nanotubes (MWCNTs), i.e., improving the dispersibility of MWCNTs in HDPE.

[0020] The crosslinking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and / or triallyl isocyanurate. Further, the crosslinking agent comprises triallyl isocyanurate and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane in a mass ratio of 1:(2~4). The combined use of the crosslinking agents promotes the formation of a crosslinked network between high-density polyethylene, ethylene-vinyl acetate copolymer, and modified high-density polyethylene. This interwoven structure facilitates the dispersion of multi-walled carbon nanotubes and forms a conductive network structure. Furthermore, the modified high-density polyethylene contains silanol and / or anhydride groups that react with the hydroxyl / carboxyl groups of the multi-walled carbon nanotubes, further improving the dispersibility of the multi-walled carbon nanotubes and preventing their precipitation.

[0021] The mass ratio of high-density polyethylene, ethylene-vinyl acetate copolymer, multi-walled carbon nanotubes, modified high-density polyethylene and crosslinking agent is (87~92):(5~7):(7~10):(3~6):(0.6~0.8).

[0022] Preparation of modified high-density polyethylene: The modifier and dicumyl peroxide are dissolved in acetone, then mixed into high-density polyethylene, and stirred until the acetone evaporates. Grafting reaction is then carried out at 210℃. The amount of dicumyl peroxide added is 1.1‰ of the mass of high-density polyethylene.

[0023] Preparation of antistatic agent: First, high-density polyethylene, multi-walled carbon nanotubes and one of their crosslinking agents are mixed at 85°C to obtain a first mixture. Then, high-density polyethylene, ethylene-vinyl acetate copolymer, another crosslinking agent and the first mixture are mixed at 172°C and then granulated for later use.

[0024] transition layer The transition layer comprises high-density polyethylene and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer.

[0025] Fluorinated alkylated poly(ethylene-g-maleic anhydride) polymers are obtained by reacting fluorinated alcohols and poly(ethylene-g-maleic anhydride) under the catalysis of toluenesulfonic acid.

[0026] Fluorinated alkylated poly(ethylene-g-maleic anhydride) polymers are crosslinked with fluorinated alcohols via ring-opening of maleic anhydride to obtain compatibilizers. Poly(ethylene-g-maleic anhydride) has a carbon chain as the main chain and contains side branching points. The main chain improves the compatibility with high-density polyethylene, and the grafted fluorinated alkyl part improves the compatibility with the inner layer of fusible polytetrafluoroethylene, thereby improving the interlayer bonding strength and compatibility.

[0027] The fluorinated alcohols are perfluoroalkyl ethyl alcohols and / or perfluoroalkyl propyl alcohols, with the alkyl carbon chain of the perfluoroalkyl ethyl alcohol being C6-12; the alkyl carbon chain of the perfluoroalkyl propyl alcohol is C6-12. A short fluoroalkyl carbon chain in the fluorinated alcohol is detrimental to optimizing compatibility with the inner layer, while an excessively long fluoroalkyl carbon chain reduces the grafting rate with poly(ethylene-g-maleic anhydride).

[0028] Preparation of fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer: First, poly(ethylene-g-maleic anhydride) was dissolved in toluene, then a fluorinated alcohol was added and stirred until completely dissolved. Next, toluenesulfonic acid catalyst was added. The reaction was carried out under a nitrogen atmosphere at 85°C for 6 hours. After the reaction, the mixture was filtered, washed, and dried at 45°C. The mass ratio of the fluorinated alcohol to poly(ethylene-g-maleic anhydride) was (1.4~2):1, and the amount of toluenesulfonic acid added was 0.2% of the total mass of the reactants.

[0029] Example 1

[0030] The antistatic, low-emission polyethylene blow-molded product consists of an outer layer, a middle layer, and an inner layer from the outside in. The outer layer consists of high-density polyethylene (Shanghai SECCO HD5401AA) with a mass ratio of 93:7 and an antistatic agent. The middle layer consists of high-density polyethylene (Shanghai SECCO HD5401AA). The inner layer is fusible polytetrafluoroethylene (Daikin AP-231SH). A transition layer is provided between the middle layer and the inner layer. The transition layer consists of high-density polyethylene (Shanghai SECCO HD5401AA) with a mass ratio of 40:60 and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer.

[0031] The preparation of fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer: Perfluorooctylpropanol and poly(ethylene-g-maleic anhydride) (CAS:9006-26-2) were prepared in a mass ratio of 1.6:1. First, poly(ethylene-g-maleic anhydride) was dissolved in toluene, and then perfluorooctylpropanol was added and stirred until completely dissolved. Then, toluenesulfonic acid catalyst was added, with the amount of toluenesulfonic acid added being 0.2% of the total mass of the reactants. The reaction was carried out in a nitrogen protective atmosphere at a temperature of 85°C for 6 hours. After the reaction was completed, the product was filtered, washed, and dried at 45°C.

[0032] The antistatic agent contains high-density polyethylene (Dow DMDA-8920), ethylene-vinyl acetate copolymer (Mitsui EVA260), multi-walled carbon nanotubes, modified high-density polyethylene, and a crosslinking agent in a mass ratio of 90:6:9:4:0.8. The crosslinking agent comprises triallyl isocyanurate and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane in a mass ratio of 1:3.

[0033] Preparation of the antistatic agent: First, high-density polyethylene, multi-walled carbon nanotubes, and triallyl isocyanurate were mixed at 85°C to obtain a first mixture. Then, high-density polyethylene, ethylene-vinyl acetate copolymer, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and the first mixture were further mixed at 172°C. The mass ratio of triallyl isocyanurate to 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane was 1:3.

[0034] Preparation of modified high-density polyethylene: The modifier and dicumyl peroxide were dissolved in acetone, then mixed into high-density polyethylene (Shanghai Jinfei HHM5502), and stirred until the acetone evaporated. Grafting reaction was then carried out at 210℃. The amount of dicumyl peroxide added was 1.1‰ of the mass of the high-density polyethylene. The modifier was vinyltrimethoxysilane and maleic anhydride in a mass ratio of 1:1.2.

[0035] The resulting blow-molded product has a total thickness of 1.1 mm, a capacity of 4 L, and a weight of 245 g. The outer layer has a thickness of 0.53 mm, the middle layer has a thickness of 0.33 mm, the transition layer has a thickness of 0.12 mm, and the inner layer has a thickness of 0.12 mm.

[0036] Based on the above-mentioned antistatic low-exudation polyethylene blow-molded product, its preparation method is as follows: the outer layer extrusion temperature of the polyethylene blow-molded product is 210℃, the middle layer extrusion temperature is 240℃, the transition layer extrusion temperature is 240℃, and the inner layer extrusion temperature is 340℃.

[0037] Example 2

[0038] Example 2 is based on Example 1, except that the high-density polyethylene used for the outer layer is Qatar HDPETR-571 with a capacity of 20L.

[0039] Example 3

[0040] Example 3 is based on Example 1, except that the transition layer includes high-density polyethylene and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer in a mass ratio of 50:50, while other components and processes remain unchanged.

[0041] Example 4

[0042] Example 4 is based on Example 1, except that the transition layer includes high-density polyethylene and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer in a mass ratio of 30:70, while other components and processes remain unchanged.

[0043] Example 5

[0044] Example 5 is based on Example 1, except that in the fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer, the mass ratio of perfluorooctylpropanol to poly(ethylene-g-maleic anhydride) is 2.2:1, while other components and processes remain unchanged.

[0045] Example 6

[0046] Example 6 is based on Example 1, except that in the fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer, the mass ratio of perfluorooctylpropanol to poly(ethylene-g-maleic anhydride) is 1:1, while other components and processes remain unchanged.

[0047] Example 7

[0048] Example 7 is based on Example 1, except that the mass ratio of high-density polyethylene, ethylene-vinyl acetate copolymer, multi-walled carbon nanotubes, modified high-density polyethylene and crosslinking agent in the antistatic agent is 90:7:9:3:0.8, while other components and processes remain unchanged.

[0049] Example 8

[0050] Example 8 is based on Example 1, except that the antistatic agent does not contain modified high-density polyethylene. The mass ratio of high-density polyethylene, ethylene-vinyl acetate copolymer, multi-walled carbon nanotubes, modified high-density polyethylene and crosslinking agent is 90:10:9:0.8, and other components and processes remain unchanged.

[0051] Example 9

[0052] Example 9 is based on Example 1, except that the mass ratio of high-density polyethylene, ethylene-vinyl acetate copolymer, multi-walled carbon nanotubes, modified high-density polyethylene and crosslinking agent in the antistatic agent is 90:6:5:4:0.8, while other components and processes remain unchanged.

[0053] Example 10

[0054] Example 10 is based on Example 1, except that the outer layer includes high-density polyethylene and an antistatic agent in a mass ratio of 97:3, while other components and processes remain unchanged.

[0055] Comparative Example 1 Comparative Example 1 is based on Example 1, except that the transition layer only includes a fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer, while the other components and processes remain unchanged.

[0056] Performance testing of the examples and comparative products: 1. Bending strength: Tested according to GB / T9341-2008 standard; 2. Impact resistance: According to GB18191-2008 standard, a drop test is conducted to determine whether the product breaks when dropped from a height of 2m (4L product) or 1.8m (20L product). 3. Stress crack resistance: The 4L product is tested according to GB18191-2008 standard. A 7% aqueous solution of 0.4L nonylphenol polyoxyethylene ether (also known as TX-10 or OP-10) as solute is injected into the 4L product. The test temperature is 65℃ and the duration is 72h. Whether cracking occurs is observed. According to GB19160-2008 standard, the 20L product is tested by injecting 2L of nonylphenol polyoxyethylene ether (also known as TX-10 or OP-10) as a solute to form a 7% aqueous solution at a temperature of 65℃ for 72 hours to see if it cracks. 4. Stacking compressive strength: The 4L product was tested according to GB18191-2008 standard, with a test temperature of 40℃, a mass of 40kg, and a duration of 28 days; The 20L product was tested according to GB19160-2008 standard, with a test temperature of 40℃, a mass of 238kg, and a duration of 28 days. 5. Surface resistivity: Tested according to GB / T1410-2006 standard.

[0057] The performance test results of the examples and comparative examples are as follows:

[0058] In Example 2, the 20L product was dropped from a height of 1.8 m without breakage; the stress cracking test showed no cracking; the compressive strength test showed no significant deformation; and the surface resistivity reached 10. 7 Ω level.

[0059] Compared to Example 1, Example 3 shows an increase in the high-density polyethylene content in the transition layer, which has a positive impact on the mechanical properties of the product. If the proportion of fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer is too low, it is easy to cause blistering on the inner surface during stress cracking tests.

[0060] Compared to Example 1, Example 4 shows a reduction in the high-density polyethylene content in the transition layer, which has a negative impact on the mechanical properties of the product.

[0061] Example 5: In the synthesis of fluoropolymers, excessive perfluorooctylpropanol content leads to a violent reaction, which in turn reduces the grafting rate of the polymer, resulting in delamination of the intermediate and inner layers during application.

[0062] In Example 6, during the synthesis of fluoropolymers, the perfluorooctylpropanol content was too low, resulting in a reduced grafting rate and delamination of the intermediate and inner layers during application.

[0063] Compared to Example 1, in Example 7, the content of ethylene-vinyl acetate copolymer was increased and the content of modified high-density polyethylene was decreased in the preparation of the antistatic agent, while the sum of the two remained unchanged. This had a negative impact on the network structure formed by the dispersion of multi-walled carbon nanotubes, and the surface resistivity showed an upward trend.

[0064] Compared to Example 1, Example 8 did not contain modified high-density polyethylene in its antistatic agent, which negatively affected the dispersibility of multi-walled carbon nanotubes.

[0065] Compared to Example 1, Comparative Example 1's transition layer only includes a fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer. The poly(ethylene-g-maleic anhydride) has a flexible main chain, which results in poor strength of the inner layer and obvious deformation in the stacking compressive strength test.

[0066] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. An antistatic, low-exudation polyethylene blow-molded product, comprising an outer layer, a middle layer, and an inner layer from the outside to the inside, characterized in that, The outer layer comprises high-density polyethylene and an antistatic agent, the intermediate layer comprises high-density polyethylene, the inner layer is fusible polytetrafluoroethylene, and a transition layer is provided between the intermediate layer and the inner layer, the transition layer comprising high-density polyethylene and fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer. The fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer is obtained by reacting a fluorinated alcohol with poly(ethylene-g-maleic anhydride) under the catalysis of toluenesulfonic acid.

2. The antistatic, low-exudation polyethylene blow-molded product according to claim 1, characterized in that, The fluorinated alcohol is a perfluoroalkyl ethyl alcohol and / or a perfluoroalkyl propyl alcohol; the alkyl carbon chain of the perfluoroalkyl ethyl alcohol is C6~12, and / or the alkyl carbon chain of the perfluoroalkyl propyl alcohol is C6~12.

3. The antistatic low-exudation polyethylene blow-molded product according to claim 1 or 2, characterized in that, The mass ratio of the high-density polyethylene to the fluorinated alkylated poly(ethylene-g-maleic anhydride) polymer is (30~50):(50~70).

4. The antistatic, low-exudation polyethylene blow-molded product according to claim 1, characterized in that, The antistatic agent is obtained by blending high-density polyethylene and ethylene-vinyl acetate copolymer as matrix materials, multi-walled carbon nanotubes as conductive fillers, and modified high-density polyethylene as compatibilizer, and then applying a crosslinking agent.

5. The antistatic, low-exudation polyethylene blow-molded product according to claim 4, characterized in that, The outer layer comprises high-density polyethylene and an antistatic agent in a mass ratio of (90~95):(5~10).

6. The antistatic, low-exudation polyethylene blow-molded product according to claim 5, characterized in that, The crosslinking agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and / or triallyl isocyanurate; further, the crosslinking agent comprises triallyl isocyanurate and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane in a mass ratio of 1:(2~4).

7. The antistatic, low-exudation polyethylene blow-molded product according to claim 5, characterized in that, The modifier of the modified high-density polyethylene is vinyltrimethoxysilane and / or maleic anhydride; further, the modifier of the modified high-density polyethylene includes vinyltrimethoxysilane and maleic anhydride in a mass ratio of 1:(1~1.3).

8. The antistatic low-exudation polyethylene blow-molded product according to claim 1 or 7, characterized in that, The mass ratio of high-density polyethylene, ethylene-vinyl acetate copolymer, multi-walled carbon nanotubes, modified high-density polyethylene and crosslinking agent in the antistatic agent is (87~92):(5~7):(7~10):(3~6):(0.6~0.8).

9. The antistatic, low-exudation polyethylene blow-molded product according to claim 1, characterized in that, The thickness ratio of the outer layer, middle layer, transition layer and inner layer of the blow-molded product is (4.5~5.5):(2.5~3.5):(1~1.5):(1~1.5).

10. A method for preparing an antistatic, low-exudation polyethylene blow-molded product, characterized in that, Based on any one of claims 1 to 9, the antistatic low-exudation polyethylene blow-molded product has an outer layer extrusion temperature of 200-220°C, an intermediate layer extrusion temperature of 200-250°C, a transition layer extrusion temperature of 200-250°C, and an inner layer extrusion temperature of 300-350°C.