A novel long-acting solid coated sustained-release acid and a preparation method thereof
By preparing a core-shell structured solid-coated slow-release acid, the problem of poor slow-release effect of existing slow-release acid systems under high temperature and high pressure was solved. This achieved delayed acid release, clean expansion of rock formation fractures, and improved the effect of oil and gas reservoir stimulation and oilfield production efficiency.
Patent Information
- Application Number
- CN202411884882.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-19
- Publication Date
- 2026-06-23
AI Technical Summary
Existing slow-release acid systems have poor slow-release effects under high temperature and high pressure, and suffer from problems such as formation environment pollution, short acid release time, poor deep penetration performance, low acid generation efficiency and complicated preparation.
Solid-coated slow-release acid with a core-shell structure was prepared by phase separation method. The shell was composed of polymer, and the core contained an acid-generating agent, such as chlorinated aromatic hydrocarbons or chlorinated esters. Stable slow-release acid particles were formed by microencapsulation. Under high temperature and pressure, the polymer shell ruptured to release the acid-generating agent and generate hydrochloric acid.
It achieves delayed acid release under high temperature and high pressure, cleans and expands rock strata fractures, reduces geological environmental pollution, has a long acid release time, excellent deep penetration performance, high acid generation efficiency, simple preparation, and is easy to store and transport.
Smart Images

Figure CN122255982A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a novel long-lasting solid-coated slow-release acid and its preparation method, belonging to the field of acid fracturing for enhanced production in carbonate reservoirs. Background Technology
[0002] Currently, given the emergence and implementation of important issues such as energy security and environmental protection, the demand for carbonate rock exploration and development in my country is becoming increasingly urgent. Relatively abundant oil and gas resources exist in the deep strata of the Tarim Basin (Shunbei and Shunnan areas) and the Yuanba area of the Sichuan Basin, which urgently need efficient extraction. Therefore, my country has a significant demand for the modification and corrosion inhibition industry of ultra-deep, high-temperature reservoirs, and there is an urgent need for the research and development of novel slow-release acid systems that are resistant to high temperatures and pressures and have moderate corrosion inhibition rates.
[0003] Slow-release acid, also known as latent acid, refers to an acid matrix that is weak or non-acidic at room temperature and generates active acid in situ under formation conditions. Using slow-release acid systems in high-temperature formations can not only avoid problems such as rapid deactivation of acid at high temperatures and shortening of the effective length of acid-etched cracks, but also prevent corrosion of pipelines and equipment.
[0004] Currently, the most widely used sustained-release acid systems are mainly divided into three categories, each with different sustained-release principles and characteristics.
[0005] One method is the emulsified acid system, which involves mixing and emulsifying a hydrochloric acid solution of a specific concentration with a hydrocarbon oil phase in a specific ratio to obtain a water-in-oil slow-release system. Because the acid solution is encapsulated in the oil phase in droplet form, the surface area of contact between the acid solution and the rock formation is directly reduced. At the same time, the oil phase can effectively block the diffusion of hydrogen ions. Therefore, compared with a single acid solution, the emulsified acid system can significantly reduce the rate of corrosion of the rock formation.
[0006] Secondly, there is the self-generating acid system, which is currently the most widely studied slow-release system. Its main principle involves mixing specific acid-generating materials and injecting them underground into the formation, where the system spontaneously generates acid under high temperature and pressure. Because it uses acid-generating materials instead of acid liquid, this system is not acidic before operation, thus overcoming some of the inherent drawbacks of emulsified acid systems.
[0007] Thirdly, there is the organic acid system, which is actually a variant of the autogenous acid system. It primarily uses organic acid esters and other raw materials for high-temperature hydrolysis and acidification, and then employs organic acids to corrode and modify rock formations. The organic acid system does not contain environmental pollutants and is relatively cleaner than ordinary autogenous acid systems. Summary of the Invention
[0008] The problem the invention aims to solve
[0009] The three major categories of sustained-release acid systems in the existing technology each have their own problems.
[0010] The essence of the emulsified acid system is still ordinary acid liquid. It only relies on the oil phase to reduce the slow release rate, resulting in poor slow release effect.
[0011] The main problem with autogenous acid systems is that the reaction between ammonium chloride and formaldehyde is too rapid at high temperatures, making the resulting system unsuitable for oil and gas extraction operations in ultra-high temperature formations (temperatures greater than 150°C). Furthermore, the reaction is difficult to control, and the formulation cannot be adjusted according to different formation environments. In addition, formaldehyde pollution of the formation operating environment is an unavoidable issue with autogenous acid systems.
[0012] Organic acid systems have three main problems: First, traditional methylacetic acid has low acidity and poor corrosion effect on rock formations at high temperatures. Although adding halogens can significantly improve the acidity of organic acids, it will lead to a large amount of organic halide residues, which will seriously affect the quality of extracted oil and gas. Second, organic acids react with carbonate rocks to easily generate a large amount of organic acid calcium precipitate, which can easily block oil and gas extraction pipelines. Third, organic acid systems are relatively expensive compared to other systems, which limits their industrial application.
[0013] In addition, the three major types of slow-release acid systems in the existing technology also have problems such as poor temperature resistance, large filtration loss, and poor flow conductivity.
[0014] Therefore, there is still an urgent need to develop a slow-release acid that has minimal impact on the formation environment, long acid release time, excellent deep penetration performance, high acid generation efficiency, is easy to store and transport, has good slow-release performance, and can be easily prepared.
[0015] Solution for solving the problem
[0016] The inventors have conducted long-term and in-depth research on the above-mentioned problems and proposed a long-acting solid-encapsulated sustained-release acid system based on microcapsule encapsulation of organic acid-generating agents using phase separation method.
[0017] Specifically, the present invention solves the problems of the present invention through the following solutions.
[0018] [1] A solid coated slow-release acid, wherein it has a core-shell structure, the shell layer contains a polymer, and the core contains an acid-generating agent; the acid-generating agent is at least one selected from chlorinated aromatic hydrocarbons, chlorinated esters and acyl chlorides, and the polymer is at least one selected from polyesters, poly(meth)acrylates, epoxy resins, polyolefins, polyacrylonitrile, polyimide and polyvinyl alcohol.
[0019] [2] According to the solid-coated slow-release acid described in [1], wherein, based on the total weight of the solid-coated slow-release acid, the content of the acid-generating agent is 60-90% by weight and the content of the polymer is 10-40% by weight.
[0020] [3] The solid-coated slow-release acid according to [1] or [2], wherein the acid-generating agent is at least one selected from vinyl chloride carbonate, methyl chloroformate, ethyl chloroformate, trichloromethyl chloroformate, and 1-chloroethyl chloroformate.
[0021] [4] The solid-coated slow-release acid according to [1] or [2], wherein the polymer is at least one selected from polyethylene, polypropylene, polybutadiene, polylactic acid, polyacrylonitrile, polyimide, epoxy resin, polyvinyl alcohol, polybutylene succinate, polystyrene, polymethyl methacrylate, and polyethylene terephthalate.
[0022] [5] The solid-coated slow-release acid according to [1] or [2], wherein the average particle size is 10 to 100 micrometers, preferably 20 to 80 micrometers.
[0023] [6] The method for preparing solid coated sustained-release acid according to any one of [1] to [5] includes the following steps:
[0024] (1) Mix the surfactant with water to obtain an aqueous phase;
[0025] (2) Dissolve the polymer and acid-generating agent in an organic solvent to obtain an oil phase;
[0026] (3) Add the oil phase to the aqueous phase, then stir and heat to evaporate the organic solvent;
[0027] (4) Perform solid-liquid separation on the system obtained in step (3).
[0028] [7] According to the preparation method described in [6], the organic solvent is at least one selected from chloroalkanes, chloroalkenes, alcohols, ketones, heterocyclic compounds, sulfones or sulfoxides; preferably at least one selected from chloroalkanes, more preferably at least one selected from dichloromethane and trichloromethane;
[0029] In the oil phase, the content of the polymer is 1-10% by weight, and the content of the acid-generating agent is 5-25% by weight.
[0030] The surfactant is selected from at least one of the following: sorbitol fatty acid ester, sorbitan sesquioleate, alkylphenol polyoxyethylene ether, sodium hexadecyl p-toluenesulfonate, sodium dodecyl sulfonate, sodium dodecyl trimethyl bromide, and polyvinyl alcohol; preferably, it is selected from at least one of sodium hexadecyl p-toluenesulfonate and sodium dodecyl sulfonate.
[0031] The content of the surfactant in the aqueous phase is 0.01 to 0.5% by weight.
[0032] [8] According to the preparation method described in [6] or [7], the weight ratio of the oil phase to the water phase is 1:(2-5); the heating temperature in step (3) is 20-80°C.
[0033] [9] Solid coated slow-release acid obtained by any one of [6] to [8].
[0034]
[10] The use of solid coated slow-release acid according to any one of [1] to [5] and [9] in the oilfield exploitation industry and oil and gas resource extraction industry is preferred as an oilfield acidifier and corrosion inhibitor.
[0035] The effects of the invention
[0036] The solid-coated slow-release acid of the present invention has the functions of low acidity at room temperature, delayed acid generation after entering high temperature and high pressure wells, thereby cleaning and expanding rock formation fractures. It has low pollution to the formation environment, long acid release time, excellent deep penetration performance, high acid generation efficiency, easy storage and transportation, good slow release performance and can be easily prepared.
[0037] This invention is of great significance for solving the problem of excessively rapid acidification in existing oilfield acidizing agent systems and optimizing the industrial process of oilfield drilling and extraction. In addition, this invention is of great significance for improving the effect of high-temperature oil and gas reservoir stimulation and developing a new paradigm for the design and application of oilfield acidizing agents. Attached Figure Description
[0038] Figure 1 This is a graph showing the results of the acid-generating performance test of the solid-coated slow-release acid obtained in Example 1.
[0039] Figure 2 This is a transmission electron microscope image of the solid-coated slow-release acid obtained in Example 1.
[0040] Figure 3 This is a transmission electron microscope image of the solid-coated slow-release acid obtained in Example 3. Detailed Implementation
[0041] The present invention will now be described in detail. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples.
[0042] In this instruction manual, "room temperature" or "room temperature" means 20-30°C, for example, 25°C.
[0043] In this manual, "atmospheric pressure" refers to 1 standard atmosphere, or 0.1013 MPa.
[0044] In this manual, "high temperature" refers to a temperature above 80°C.
[0045] In this manual, "high pressure" refers to pressure above 1.2 standard atmospheres.
[0046] In this specification, the range of values referred to as "value A to value B" refers to the range including the endpoint values A and B.
[0047] In this specification, the numerical range indicated by "above" or "below" refers to the numerical range that includes the stated number.
[0048] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.
[0049] In this specification, the terms "optionally" or "optionally" are used to indicate the use or non-use of certain substances, components, procedures, application conditions, etc.
[0050] All unit names used in this manual are international standard unit names, and unless otherwise stated, the "%" used refers to weight or mass percentage content.
[0051] In this specification, references to "preferred embodiments," "implementation methods," etc., mean that a specific element (e.g., feature, structure, property, and / or characteristic) related to that embodiment is included in at least one of the embodiments described herein, and may or may not be present in other embodiments. Furthermore, it should be understood that the elements may be combined in any suitable manner in various embodiments.
[0052] One object of the present invention is to provide a solid coated slow-release acid having a core-shell structure, wherein the shell comprises a polymer and the core comprises an acid-generating agent; the acid-generating agent is at least one selected from chlorinated aromatic hydrocarbons, chlorinated esters and acyl chlorides, and the polymer is at least one selected from polyesters, poly(meth)acrylates, epoxy resins, polyolefins, polyacrylonitrile, polyimide and polyvinyl alcohol.
[0053] The solid-coated sustained-release acid of the present invention has a microcapsule (core-shell) structure. Under normal temperature and pressure, the acid-generating agent located in the core is protected by the polymer shell and is therefore stable. After being injected into the reservoir, the polymer shell ruptures under high temperature and high pressure conditions to release the internal acid-generating agent, which reacts with water to generate hydrochloric acid, thereby achieving the purpose of acid release.
[0054] In some embodiments, the content of the acid-generating agent is 60-90% by weight, preferably 65-88% by weight, and more preferably 70-85% by weight, based on the total weight of the solid-coated slow-release acid of the present invention.
[0055] In some embodiments, the polymer content is 10-40% by weight, preferably 12-35% by weight, and more preferably 15-30% by weight, based on the total weight of the solid-coated slow-release acid of the present invention.
[0056] The solid-coated slow-release acid of the present invention is in the form of granules or powder. In some embodiments, its average particle size is 10 to 100 micrometers, preferably 20 to 80 micrometers.
[0057] acidifier
[0058] The acid-generating agent used in this invention is a substance that can react with water to produce acid (e.g., hydrochloric acid).
[0059] In some embodiments, the acid-generating agent is at least one selected from chlorinated aromatic hydrocarbons, chlorinated esters, and acyl chlorides.
[0060] Examples of chlorinated aromatic hydrocarbons include, but are not limited to, chlorinated benzene, chlorinated toluene (mixture of isomers), and chlorinated cumene (mixture of isomers).
[0061] Examples of chloroesters include, but are not limited to, chloroethylene carbonate, ethyl chlorocarbonate, methyl chloroformate, ethyl chloroformate, trichloromethyl chloroformate, and 1-chloroethyl chloroformate.
[0062] Examples of acyl chlorides include, but are not limited to, acetyl chloride, oxalyl chloride, dicarboxyl chloride, thionyl chloride, chloroacetyl chloride, and benzoyl chloride.
[0063] More preferably, the acid-generating agent is at least one selected from vinyl chloride carbonate, methyl chloroformate, ethyl chloroformate, trichloromethyl chloroformate, and 1-chloroethyl chloroformate.
[0064] polymer
[0065] In some embodiments, the polymer is at least one selected from polyester, polyurethane, poly(meth)acrylate, epoxy resin, polyolefin, polyacrylonitrile, polyimide, and polyvinyl alcohol.
[0066] Examples of polyesters include, but are not limited to, polybutylene succinate, polyhexanediol adipate, polyethylene terephthalate, polylactic acid, etc.
[0067] Examples of polyurethane include, but are not limited to, polyester polyurethane, polyether polyurethane, polyurea polyurethane, polypolyol polyurethane, polyamide polyurethane, and two-component polyurethane.
[0068] Examples of poly(meth)acrylates include, but are not limited to, polymethyl methacrylate, polymethyl acrylate, polyethyl methacrylate, polyethyl acrylate, polypropyl methacrylate, polypropyl acrylate, polybutyl methacrylate, polybutyl acrylate, etc.
[0069] Examples of epoxy resins include, but are not limited to, bisphenol A epoxy resins, bisphenol F epoxy resins, glycidyl ester epoxy resins, and polyphenolic glyceryl ester epoxy resins, which are commercially available.
[0070] Examples of polyolefins include, but are not limited to, polyethylene, polypropylene, polystyrene, and polybutadiene.
[0071] Preferably, the polymer is selected from at least one of polyethylene, polybutadiene, polylactic acid, polyacrylonitrile, polyimide, epoxy resin, polyvinyl alcohol, polyethylene terephthalate, polystyrene, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polypropylene, and polybutylene succinate.
[0072] One objective of this invention is to provide a method for preparing the solid-coated sustained-release acid, which includes the following steps:
[0073] (1) Mix the surfactant with water to obtain an aqueous phase;
[0074] (2) Dissolve the polymer and acid-generating agent in an organic solvent to obtain an oil phase;
[0075] (3) The oil phase is added to the aqueous phase, and then heated under stirring to evaporate the organic solvent;
[0076] (4) Perform solid-liquid separation on the system obtained in step (3).
[0077] This invention utilizes a phase separation method to prepare solid-coated slow-release acid with a core-shell structure. The following describes each step of the preparation method of this invention.
[0078] Step (1)
[0079] In step (1), the surfactant is mixed with water to obtain an aqueous phase.
[0080] This invention does not impose any particular limitation on the surfactant, which can be any suitable surfactant in the art. In some embodiments, the surfactant is at least one selected from sorbitol fatty acid ester, sorbitan sesquioleate, alkylphenol polyoxyethylene ether, sodium hexadecyl p-toluenesulfonate, sodium dodecyl sulfonate, sodium dodecyl trimethyl bromide, and polyvinyl alcohol.
[0081] Preferably, the surfactant is at least one selected from sodium hexadecyl p-toluenesulfonate and sodium dodecyl sulfonate.
[0082] In some embodiments, the surfactant content in the aqueous phase is 0.01 to 0.5% by weight, preferably 0.02 to 0.4% by weight.
[0083] In some embodiments, the water content in the aqueous phase is 99.5–99.99% by weight, preferably 99.6–99.98% by weight.
[0084] In some embodiments, the surfactant is mixed with water by stirring. Preferably, the stirring speed is 100-500 rpm, more preferably 200-250 rpm.
[0085] In some implementations, step (1) is performed at room temperature, for example at 20–30°C.
[0086] Step (2)
[0087] In step (2), the polymer and acid generator are dissolved in an organic solvent to obtain an oil phase.
[0088] In some embodiments, the organic solvent is at least one selected from chlorinated alkanes, chlorinated alkenes, alcohols, ketones, heterocyclic compounds, sulfones, or sulfoxides.
[0089] Examples of chlorinated alkane solvents include, but are not limited to, dichloromethane, trichloromethane, carbon tetrachloride, dichloroethane, hexachloroethane, chloroisopropane, and chlorobutane.
[0090] Examples of chlorinated olefin solvents include, but are not limited to, tetrachloroethylene, chloropropylene, and chloroprene.
[0091] Examples of alcohol solvents include, but are not limited to, methanol, ethanol, and isopropanol.
[0092] Examples of ketone solvents include, but are not limited to, acetone and methyl ethyl ketone.
[0093] Examples of heterocyclic solvents include, but are not limited to, pyrrole, furan, pyridine, furfural, furfural, tetrahydrofuran, hexahydropyridine, and bipyridine.
[0094] Examples of sulfone solvents include, but are not limited to, methyl sulfone, dimethyl sulfone, and methyl ethyl sulfone.
[0095] Examples of sulfoxide solvents include, but are not limited to, dimethyl sulfoxide, diethyl sulfoxide, butyl sulfoxide, etc.
[0096] Preferably, the organic solvent is at least one selected from chloroalkane solvents.
[0097] More preferably, the organic solvent is at least one selected from dichloromethane and trichloromethane.
[0098] In some embodiments, the polymer content in the oil phase is 1 to 10% by weight, preferably 1.5 to 6% by weight.
[0099] In some embodiments, the content of the acid-generating agent in the oil phase is 5-25% by weight, preferably 6-20% by weight.
[0100] In some embodiments, the content of organic solvent in the oil phase is 65-94% by weight, preferably 74-92.5% by weight.
[0101] In some embodiments, the polymer and acid-generating agent are dissolved in the organic solvent by stirring. Preferably, the stirring speed is 100-500 rpm.
[0102] In some implementations, step (2) is performed at room temperature, for example at 20–30°C.
[0103] Step (3)
[0104] In step (3), the oil phase is added to the aqueous phase, and then stirred and heated to evaporate the organic solvent.
[0105] In step (3), the oil phase is dispersed in the aqueous phase and the system is emulsified by stirring. The organic solvent in the oil phase is evaporated by heating. During the evaporation of the organic solvent, the system undergoes phase separation to form microcapsules with a polymer shell and an acid-generating agent core.
[0106] In some embodiments, the weight ratio of the oil phase to the water phase is 1:(2-5).
[0107] In some embodiments, in step (3), stirring is performed by magnetic stirring and / or mechanical stirring. Preferably, the stirring speed is 100 to 500 rpm, more preferably 200 to 250 rpm.
[0108] The heating temperature in step (3) can be selected according to the boiling point of the organic solvent. In some embodiments, the heating temperature in step (3) is 20 to 80°C, preferably 30 to 50°C, more preferably 40 to 45°C, for example 40 to 42°C.
[0109] In some implementations, the stirring and heating time in step (3) is 4 to 20 hours, preferably 6 to 12 hours.
[0110] Step (4)
[0111] In step (4), the system obtained in step (3) is subjected to solid-liquid separation to obtain the solid-coated slow-release acid of the present invention. The solid-liquid separation can be carried out by conventional methods in the art, such as filtration and centrifugation.
[0112] Optionally, step (4) may include washing and drying the solid portion after solid-liquid separation. Preferably, drying is performed at room temperature (20–30°C).
[0113] The present invention also relates to solid-coated slow-release acid obtained by the preparation method of the present invention.
[0114] One of the objectives of this invention is to provide the use of the solid-coated slow-release acid of this invention in the oilfield exploitation industry and the oil and gas resource extraction industry, preferably as an oilfield acidifier and corrosion inhibitor.
[0115] The solid-coated slow-release acid of this invention is typically a white solid. It needs to be mixed with water before use, and the acid concentration can be adjusted by changing the mixing ratio with water. After being mixed with water and injected into the formation, the solid-coated slow-release acid of this invention can be used for fracturing and fracture creation. Under high temperature and pressure, the microcapsules gradually rupture, and the internal acid-generating agent gradually reacts with water to produce hydrochloric acid, achieving the purpose of slow-release acidification of the rock formation.
[0116] Compared with traditional slow-release acid systems, the solid-coated slow-release acid of this invention has advantages such as good slow-release performance, long acid release time, high acid generation efficiency, excellent deep penetration performance, easy storage and transportation, relatively simple and convenient production process, and environmental friendliness. It is a type of high-efficiency slow-release acidizer system for oilfield drilling.
[0117] Example
[0118] The following specific embodiments further illustrate the present invention. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the contents of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by this invention.
[0119] The reagents used in the following examples were: polystyrene (molecular weight 280,000), polymethyl methacrylate (high flow type), chloroethylene carbonate, trichloromethyl chloroformate, and dichloromethane, which were purchased from Aladdin Company; sodium dodecyl sulfonate was purchased from Energie Company; and the remaining reagents were commercially available products.
[0120] Example 1
[0121] 1) Add 1 part by weight of sodium dodecyl sulfonate to 2000 parts by weight of water and stir at 200 rpm to obtain an aqueous phase.
[0122] 2) Add 15 parts by weight of polystyrene and 40 parts by weight of chloroethylene carbonate to 400 parts by weight of dichloromethane, and stir at 200 rpm for 30 minutes at room temperature to fully dissolve the solid.
[0123] 3) Add the solution obtained in 2) dropwise to the aqueous phase obtained in 1), heat to 42°C at 200 rpm, and maintain for 6 hours.
[0124] 4) After completing 3), the system is filtered to obtain solid-coated slow-release acid.
[0125] Example 2
[0126] 1) Add 1 part by weight of sodium dodecyl sulfonate to 1000 parts by weight of water and stir at 200 rpm to obtain an aqueous phase.
[0127] 2) Add 10 parts by weight of polystyrene and 40 parts by weight of chloroethylene carbonate to 400 parts by weight of dichloromethane, and stir at 200 rpm for 30 minutes at room temperature to fully dissolve the solid.
[0128] 3) Add the solution obtained in 2) dropwise to the aqueous phase obtained in 1), heat to 42°C at 200 rpm, and maintain for 6 hours.
[0129] 4) After completing 3), the system is filtered to obtain solid-coated slow-release acid.
[0130] Example 3
[0131] 1) Add 1 part by weight of sodium dodecyl sulfonate to 2000 parts by weight of water and stir at 200 rpm to obtain an aqueous phase.
[0132] 2) Add 15 parts by weight of polymethyl methacrylate and 50 parts by weight of trichloromethyl chloroformate to 400 parts by weight of dichloromethane, and stir at 200 rpm for 30 minutes at room temperature to fully dissolve the solid.
[0133] 3) Add the solution obtained in 2) dropwise to the aqueous phase obtained in 1), heat to 42°C at 200 rpm, and maintain for 8 hours.
[0134] 4) After completing 3), the system is filtered to obtain solid-coated slow-release acid.
[0135] Example 4
[0136] 1) Add 3 parts by weight of sodium dodecyl sulfonate to 2000 parts by weight of water and stir at 200 rpm to obtain an aqueous phase.
[0137] 2) Add 10 parts by weight of polystyrene and 50 parts by weight of trichloromethyl chloroformate to 400 parts by weight of dichloromethane, and stir at 200 rpm for 30 minutes at room temperature to fully dissolve the solid.
[0138] 3) Add the solution obtained in 2) dropwise to the aqueous phase obtained in 1), heat to 40°C at 200 rpm, and maintain for 12 hours.
[0139] 4) After completing 3), the system is filtered to obtain solid-coated slow-release acid.
[0140] <Tests and Evaluations>
[0141] 1. Test of acid-generating performance of acid-generating agent
[0142] A 50 mL polytetrafluoroethylene-lined hydrothermal reactor was used. Ten parts by weight of the solid-coated slow-release acid obtained in Example 1 and 50 parts by weight of water were added. The reactor was placed in a dedicated heating oven for a 6-hour hydrolysis experiment. After hydrolysis, the pH value of the hydrolysis residue was measured using a Leici PHSJ-4F laboratory pH meter, and the percentage of acid generated by the acid-generating agent was calculated. Results at different experimental temperatures are shown below. Figure 1 As shown.
[0143] Depend on Figure 1 It can be seen that when the experimental temperature is below the boiling point of water, the acid-generating agent reacts with water relatively slowly, while when the experimental temperature is above the boiling point of water, the acid-generating agent can be completely hydrolyzed to generate hydrochloric acid more quickly. It can be seen that the solid-coated slow-release acid of the present invention has good hydrolysis and acid-generating performance, and has a certain ability to delay acid generation.
[0144] 2. Morphological characterization of solid-coated slow-release acid
[0145] The surface morphology of the solid-coated sustained-release acid obtained in Examples 1 and 3 was observed using a Bruker Nano XFlash Detector transmission electron microscope. The results are as follows: Figure 2 and Figure 3 As shown. By Figure 2 and Figure 3 It can be seen that the solid-coated slow-release acid of the present invention has a good surface morphology, a smooth and uniform surface, and a relatively stable coating effect.
[0146] 3. Test on the sustained-release effect of solid-coated sustained-release acid
[0147] Test method: A 50mL polytetrafluoroethylene-lined hydrothermal reactor was used. Solid coated slow-release acid and water (weight ratio 1:1) were added. The reactor was placed in a special heating oven and hydrolysis experiments were carried out at 160℃ for 0 hours (direct measurement without oven), 2 hours, 4 hours and 6 hours respectively. After hydrolysis, the pH value of the hydrolysis residue was measured using a Leici PHSJ-4F laboratory pH meter and the hydrogen ion concentration of the hydrolysis residue was calculated.
[0148] The solid-coated slow-release acids obtained in Examples 1, 2, and 3 were tested according to the above method, and the results are shown in Table 1 (the data in the table are the hydrogen ion concentrations of the hydrolysis residue after hydrolysis, and the units are all mol / L).
[0149] Table 1
[0150] 0h 2h 4h 6h Example 1 0.3 0.7 1.6 2.5 Example 2 0.2 0.4 1.3 2.1 Example 3 0.5 0.9 1.4 1.9
[0151] The results shown in Table 1 demonstrate that the solid-coated slow-release acid of this invention exhibits excellent delayed acid-generating ability during the 6-hour hydrolysis process. This indicates that the solid-coated slow-release acid of this invention can gradually rupture and release the internal acid-generating agent under high temperature and pressure. The acid-generating agent further reacts with water to generate hydrochloric acid, resulting in a significant acid-generating effect.
[0152] 4. Tests on sustained-release effects at different temperatures
[0153] Test method: A 50mL polytetrafluoroethylene-lined hydrothermal reactor was used. Solid coated slow-release acid and water (weight ratio 1:1) were added. The reactor was placed in a special heating oven and hydrolyzed for 6 hours at 60℃, 90℃, 120℃ and 150℃ respectively. After hydrolysis, the pH value of the hydrolysis residue was measured using a Leici PHSJ-4F laboratory pH meter and the hydrogen ion concentration of the hydrolysis residue was calculated.
[0154] The solid-coated slow-release acids obtained in Examples 1, 2, and 3 were tested according to the above method, and the results are shown in Table 2 (the data in the table are the hydrogen ion concentrations of the hydrolysis residue after hydrolysis, and the units are all mol / L).
[0155] Table 2
[0156] 60℃ 90℃ 120℃ 150℃ Example 1 0.5 0.8 1.7 2.4 Example 2 0.3 0.9 1.6 2.0 Example 3 0.5 1.1 1.5 1.7
[0157] As shown in Table 2, the solid-coated slow-release acids obtained in Examples 1, 2, and 3 exhibit slow acid generation at lower temperatures, gradually generating acid as the temperature increases, demonstrating a good delay effect. This meets the requirements of oilfield acidizing processes where acid generation is minimal at low temperatures and delayed under high temperatures and pressures.
[0158] Industrial availability
[0159] The solid-coated slow-release acid of this invention can be widely used in the oilfield development industry and the oil and gas resource extraction industry, and has promising prospects for promotion. It provides a new method and paradigm for delayed acidizing processes in oilfield development and drilling.
Claims
1. A solid-coated slow-release acid, characterized in that: It has a core-shell structure, with the shell containing a polymer and the core containing an acid-generating agent; the acid-generating agent is at least one selected from chlorinated aromatic hydrocarbons, chlorinated esters and acyl chlorides, and the polymer is at least one selected from polyesters, polyurethanes, poly(meth)acrylates, epoxy resins, polyolefins, polyacrylonitrile, polyimide and polyvinyl alcohol.
2. The solid-coated slow-release acid according to claim 1, characterized in that, Based on the total weight of the solid-coated slow-release acid, the content of the acid-generating agent is 60-90% by weight, and the content of the polymer is 10-40% by weight.
3. The solid-coated slow-release acid according to claim 1 or 2, characterized in that, The acid-generating agent is at least one selected from vinyl chloride carbonate, methyl chloroformate, ethyl chloroformate, trichloromethyl chloroformate, and 1-chloroethyl chloroformate.
4. The solid-coated slow-release acid according to claim 1 or 2, characterized in that, The polymer is selected from at least one of polyethylene, polypropylene, polybutadiene, polylactic acid, polyacrylonitrile, polyimide, epoxy resin, polyvinyl alcohol, polybutylene succinate, polystyrene, polymethyl methacrylate, and polyethylene terephthalate.
5. The solid-coated slow-release acid according to claim 1 or 2, characterized in that, The average particle size is 10–100 micrometers, preferably 20–80 micrometers.
6. The method for preparing solid-coated sustained-release acid according to any one of claims 1 to 5, characterized in that, Includes the following steps: (1) Mix the surfactant with water to obtain an aqueous phase; (2) Dissolve the polymer and acid-generating agent in an organic solvent to obtain an oil phase; (3) Add the oil phase to the aqueous phase, then stir and heat to evaporate the organic solvent; (4) Perform solid-liquid separation on the system obtained in step (3).
7. The preparation method according to claim 6, characterized in that, The organic solvent is at least one selected from chlorinated alkanes, chlorinated alkenes, alcohols, ketones, heterocyclic compounds, sulfones, or sulfoxides; preferably at least one selected from chlorinated alkanes, more preferably at least one selected from dichloromethane and trichloromethane; In the oil phase, the content of the polymer is 1-10% by weight, and the content of the acid-generating agent is 5-25% by weight. The surfactant is selected from at least one of the following: sorbitol fatty acid ester, sorbitan sesquioleate, alkylphenol polyoxyethylene ether, sodium hexadecyl p-toluenesulfonate, sodium dodecyl sulfonate, sodium dodecyl trimethyl bromide, and polyvinyl alcohol; preferably, it is selected from at least one of sodium hexadecyl p-toluenesulfonate and sodium dodecyl sulfonate. The content of the surfactant in the aqueous phase is 0.01 to 0.5% by weight.
8. The preparation method according to claim 6 or 7, characterized in that, The weight ratio of the oil phase to the water phase is 1:(2-5); the heating temperature in step (3) is 20-80℃.
9. The solid-coated slow-release acid obtained by the preparation method according to any one of claims 6 to 8.
10. The use of solid-coated slow-release acid according to any one of claims 1 to 5 and 9 in the oilfield exploitation industry and oil and gas resource extraction industry, preferably as an oilfield acidifying agent and corrosion inhibitor.