A method for synthesizing a large single-crystal sodium-ion battery layered-oxide cathode material

By using acid treatment and high-temperature calcination, a large single-crystal layered oxide cathode material for sodium-ion batteries was formed, overcoming the limitations of traditional methods and achieving the synthesis of materials with excellent performance and low cost.

CN122257093APending Publication Date: 2026-06-23JIANGSU ZHENGXUQI NEW MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610271307.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-06
Publication Date
2026-06-23

AI Technical Summary

Technical Problem

Existing technologies struggle to prepare low-cost, high-performance large single-crystal sodium-ion battery layered oxide cathode materials, and both traditional liquid precipitation and solid-state methods have limitations.

Method used

By introducing an acid treatment process, the surface of the metal oxide is etched to form a defect structure, and then mixed with a sodium-containing alkali and calcined at high temperature to form a large single-crystal layered oxide structure.

Benefits of technology

It significantly improves the stability, specific capacity, rate performance and cycle performance of the material, simplifies the synthesis process, and reduces the complexity and cost of operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122257093A_ABST
    Figure CN122257093A_ABST
Patent Text Reader

Abstract

The application discloses a synthesis method of a large single-crystal sodium-ion battery layered oxide positive electrode material, and comprises the following steps: (1) weighing metal oxides containing transition metal elements, transferring to a device with mixing functions, uniformly mixing, and obtaining a metal oxide mixture; (2) adding acid to the metal oxide mixture, fully mixing, and completing an acid treatment process; (3) adding alkali to the mixture after acid treatment, fully mixing; (4) transferring the mixture obtained in the step (3) to a calcining furnace, high-temperature calcining, and obtaining a layered oxide. The acid treatment process is introduced, the surface of the metal oxide forms a defect structure under the action of the acid, and the defect structure is more beneficial to the formation of strong interaction between each component of the metal oxide and between the metal oxide and sodium-containing alkali, so that a larger single-crystal layered oxide structure is finally formed, and the specific capacity, rate performance and cycle performance are excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery technology, and specifically to a method for synthesizing a large single-crystal layered oxide cathode material for sodium-ion batteries. Background Technology

[0002] The cathode materials for sodium-ion batteries mainly include layered oxides, polyanionic materials, and Prussian blue (white) materials. Among them, layered oxides have the highest energy density and are considered to be materials with great commercial potential. Currently, the main processes for synthesizing layered oxide precursors are liquid precipitation and solid-state methods. The liquid precipitation method involves simultaneously allowing a precipitation reaction to occur between three solutions: transition metal salts such as nickel, iron, manganese, and copper, a precipitant, and a complexing agent. After filtration, washing, and drying, the precursor is obtained. Then, a sodium-containing alkali is introduced, followed by high-temperature calcination to obtain the sodium-ion battery layered oxide. The advantage of the liquid precipitation method is the uniform distribution of the nickel, iron, manganese, and copper components, thus it has gradually become the mainstream method. For example, patents CN202410063503.7 and CN202510065739.9 use sulfate solution, sodium hydroxide precipitant, and ammonia complexing agent to synthesize a hydroxide and carbonate composite precursor, which is then used to synthesize the layered oxide. However, the sodium-ion battery layered oxide prepared by the liquid precipitation method is generally a polycrystalline aggregate. For example, patent CN202510065739.9 synthesized layered oxide precursors via a liquid co-precipitation method. By increasing the calcination temperature (900-1200℃), ion migration was promoted, increasing the grain growth rate and gradually forming small single-crystal aggregates. The solid-state method involves directly mixing transition metal oxides such as nickel, iron, manganese, and copper with a sodium-containing alkali and calcining at high temperatures to obtain layered oxides for sodium-ion batteries, generally resulting in polycrystalline aggregates. For instance, patent CN202510340836.4 successfully prepared polycrystalline aggregate layered oxides for sodium-ion batteries using metal oxides such as NiO, Fe2O3, Mn2O3, and CuO, and Na2CO3 as raw materials, through high-temperature calcination to achieve a high-temperature solid-state reaction. The disadvantages of the traditional solid-state method are the difficulty of the solid-state reaction and the poor uniformity of elements in the material. Therefore, the performance of the synthesized layered oxides for sodium-ion batteries is inferior to that of the co-precipitation method, limiting its application. However, because the solid-state method has a simpler synthesis process and lower cost, it still has potential commercial value. Research has found that changing the particle morphology of layered oxides from spherical polycrystalline aggregates to large single-crystal structures can improve material performance. Therefore, if traditional solid-state methods can be optimized to effectively improve the solid-state reaction process, and layered oxides with large single-crystal structures for sodium-ion batteries with low cost and superior performance can be prepared, it will have significant commercial value. Summary of the Invention

[0003] This invention provides a method for synthesizing large single-crystal layered oxide cathode materials for sodium-ion batteries. The method introduces an acid treatment process, in which the surface of the metal oxide forms a defect structure under the action of acid, which is more conducive to the formation of strong interactions between the components of the metal oxide and between the metal oxide and the sodium-containing alkali. Ultimately, a larger single-crystal layered oxide structure is formed, which has excellent specific capacity, rate performance and cycle performance.

[0004] To address the aforementioned technical problems, this invention provides a method for synthesizing a large single-crystal sodium-ion battery layered oxide cathode material, comprising the following steps: (1) Weigh the metal oxide containing transition metal elements, transfer it to a device with mixing function, mix it evenly, and obtain a metal oxide mixture; (2) Add acid to the metal oxide mixture and mix thoroughly to complete the acid treatment process; (3) Add alkali to the acid-treated mixture and mix thoroughly; (4) The mixture precursor obtained in step (3) is transferred to a calcining furnace and calcined at high temperature to obtain a layered oxide with a large single crystal structure.

[0005] Further, in step (1), the transition metal element is at least one of Ni, Fe, Mn, and Cu; The device with mixing function is at least one of a mixer, a stirring vessel, a pulverizer, and a grinding mill, and the device is equipped with a heating function.

[0006] Further, the acid in step (2) is at least one of hydrochloric acid, nitric acid, phosphoric acid, hydrofluoric acid, oxalic acid, citric acid, acetic acid, and ascorbic acid; The amount of acid added is 0.1%-100% of the mass of the metal oxide mixture; the acid treatment temperature is 0-300℃, and the time is 1-100h.

[0007] Further, the alkali in step (3) is at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate; The mixing temperature is 0-750℃, and the time is 1-50h.

[0008] Furthermore, the calcination temperature in step (4) is 800-1200℃ and the time is 1-50h.

[0009] The beneficial effects of this invention are: 1. It breaks through the structural limitations of traditional polycrystalline aggregate layered oxides. The large single crystal structure avoids the problems of electrolyte penetration and stress cracking during cycling caused by interparticle porosity, and significantly improves the stability of the material; 2. It can be completed in just four steps: mixing metal oxides, acid treatment, mixing with alkali, and high-temperature calcination. Compared with the liquid precipitation method, it is simpler to operate and has a shorter cycle. Compared with the traditional solid method, it does not require complex optimization. 3. Acid treatment etches the surface of metal oxides to form defect structures, which strengthens the interaction between the components of the metal oxides and with sodium-containing bases, reduces the difficulty of solid-phase reactions, and improves the uniformity of element distribution. 4. The synthesized large single-crystal layered oxides outperform materials prepared by traditional methods in terms of specific capacity, rate performance (such as 3C high-rate discharge performance) and cycle stability (1C 150 cycles); 5. Various acids such as hydrochloric acid, nitric acid, phosphoric acid, hydrofluoric acid, oxalic acid, citric acid, and ascorbic acid can achieve defect induction effects, without the need for specific acids, resulting in high process flexibility. Attached Figure Description

[0010] Figure 1 This is a SEM image of the large single-crystal sodium-electric layered oxide C-1 of the present invention.

[0011] Figure 2 This is a SEM image of the small single-crystal aggregate sodium-electric layered oxide CC-1 of the present invention.

[0012] Figure 3 These are the electrochemical performance test results of the layered oxide of the present invention. Detailed Implementation

[0013] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments are not intended to limit the present invention.

[0014] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0015] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0016] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise explicitly limited. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0017] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0018] It should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only possible implementation.

[0019] Reference Figures 1 to 3 As shown, the present invention provides a method for synthesizing a large single-crystal sodium-ion battery layered oxide cathode material, comprising the following steps: (1) weighing a metal oxide containing transition metal elements, transferring it to a device with a mixing function, mixing it evenly to obtain a metal oxide mixture; (2) adding acid to the metal oxide mixture, mixing it thoroughly to complete the acid treatment process; (3) adding alkali to the acid-treated mixture, mixing it thoroughly; (4) transferring the mixture precursor obtained in step (3) to a calcining furnace, calcining it at high temperature to obtain a large single-crystal layered oxide.

[0020] In step (1), the transition metal element is at least one of Ni, Fe, Mn, and Cu; the equipment with mixing function is at least one of a mixer, a stirring vessel, a pulverizer, and a grinding mill, and the equipment is equipped with a heating function. The acid in step (2) is at least one of hydrochloric acid, nitric acid, phosphoric acid, hydrofluoric acid, oxalic acid, citric acid, acetic acid, and ascorbic acid; the amount of acid added is 0.1%-100% of the mass of the metal oxide mixture; the acid treatment temperature is 0-300℃ and the time is 1-100h; The alkali mentioned in step (3) is at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate; the mixing temperature is 0-750℃ and the time is 1-50h; The roasting temperature in step (4) is 800-1200℃ and the time is 1-50h.

[0021] The specific implementation method is as follows: (1) Weigh NiO (D50=5μm), Fe2O3 (D50=5μm) and 2 (D50=5μm), placed in a mixer, wherein the molar ratio of Ni, Fe and Mn is 1 / 3:1 / 3:1 / 3 (i.e. 1:1:1). Turn on the stirrer and stir at 200 rpm for 1 h to obtain a metal oxide mixture. (2) Weigh hydrofluoric acid solution (40wt% concentration, accounting for 2% of the total mass of oxides), add it to the metal oxide mixture, and continue stirring at 100 rpm for 5 h to obtain an acid-modified metal oxide mixture. (3) Weigh sodium hydroxide powder (D50=1mm, Na:(Ni+Fe+Mn) molar ratio is 1.0), add it to the above mixer, and continue stirring for 10 h to obtain a precursor. (4) Transfer the precursor to a calcining furnace and calcinate at 900℃ for 15 h in an air atmosphere to obtain layered oxide C1.

[0022] Example 2: (1) Weigh NiO (D50=5μm), Fe2O3 (D50=5μm) and MnO2 (D50=5μm) and place them in a stirred tank, wherein the molar ratio of Ni, Fe and Mn is 1 / 3:1 / 3:1 / 3 (i.e. 1:1:1). Turn on the stirrer and heat the stirred tank to 80℃. Stir at 100 rpm for 1 h to obtain a metal oxide mixture. (2) Weigh hydrochloric acid solution (37wt% concentration, accounting for 4% of the total mass of oxides) and add it to the metal oxide mixture. Continue stirring at 100 rpm for 10 h to obtain an acid-modified metal oxide mixture. (3) Weigh sodium carbonate powder (D50=3.5μm, Na:(Ni+Fe+Mn) molar ratio is 1.0) and add it to the stirred tank above. Continue stirring for 5 h to obtain the precursor. (4) The precursor was transferred to a calcining furnace and calcined at 950°C for 15 hours in an air atmosphere to obtain layered oxide C2.

[0023] Example 3: (1) Weigh NiO (D50=5μm), CuO (D50=5nm), Fe2O3 (D50=5μm) and 2 (D50=5μm), placed in a stirred tank, wherein the molar ratio of Ni, Cu, Fe and Mn is 5 / 18:1 / 18:1 / 3:1 / 3 (i.e. 5:1:6:6). Turn on the stirrer and stir at 100 rpm for 1 h to obtain a metal oxide mixture. (2) Add oxalic acid (accounting for 10% of the total mass of oxides), then add hydrochloric acid solution (accounting for 20% of the total mass of oxides), add it to the mixed salt, heat the stirred tank to 100℃, and continue stirring at 200 rpm for 30 h to obtain an acid-modified metal oxide mixture. (3) Weigh sodium carbonate powder (D50=3.5μm, Na:(Ni+Fe+Mn+Cu) molar ratio is 1.0), add it to the stirred tank above, and continue stirring for 20 h to obtain the precursor. (4) Transfer the precursor to a calcining furnace and calcinate at 1000℃ for 15 h in an air atmosphere to obtain layered oxide C3.

[0024] Example 4: (1) Weigh NiO (D50=5μm), Fe2O3 (D50=5μm) and Mn3O4 (D50=5μm) and place them in a stirred tank, wherein the molar ratio of Ni, Fe and Mn is 1 / 3:1 / 3:1 / 3 (i.e. 1:1:1). Turn on the stirrer and stir at 100 rpm for 1 h to obtain a metal oxide mixture. (2) Weigh hydrochloric acid solution (37wt% concentration, accounting for 4% of the total mass of oxides) and add it to the mixed salt. Heat the stirred tank to 80℃ and continue stirring at 200 rpm for 5 h to obtain an acid-modified metal oxide mixture. (3) Weigh sodium bicarbonate powder (D50=5μm, Na:(Ni+Fe+Mn) molar ratio is 1.05) and add it to the stirred tank above. Continue stirring for 5 h to obtain the precursor. (4) The precursor was transferred to a calcining furnace and calcined at 950°C for 15 hours in an air atmosphere to obtain layered oxide C4.

[0025] Example 5: (1) Weigh NiO (D50=5μm), Fe2O3 (D50=5μm) and MnO (D50=5μm) and place them in a stirred tank, wherein the molar ratio of Ni, Fe and Mn is 1 / 3:1 / 3:1 / 3 (i.e. 1:1:1). Turn on the stirrer and stir at 100 rpm for 1 h to obtain a metal oxide mixture. (2) Weigh nitric acid solution (68wt% concentration, accounting for 5% of the total mass of oxides) and add it to the mixed salt. Heat the stirred tank to 80℃ and continue stirring at 200 rpm for 5 h to obtain an acid-modified metal oxide mixture. (3) Weigh sodium carbonate powder (D50=3.5μm, Na:(Ni+Fe+Mn) molar ratio of 1.0) and add it to the stirred tank above. Continue stirring for 5 h to obtain a precursor. (4) Transfer the precursor to a calcining furnace and calcinate at 950℃ for 15 h in an air atmosphere to obtain layered oxide C5.

[0026] Example 6: (1) Weigh NiO (D50=5μm), Fe2O3 (D50=5μm) and MnO (D50=5μm) and place them in a stirred tank, wherein the molar ratio of Ni, Fe and Mn is 1 / 3:1 / 3:1 / 3 (i.e. 1:1:1). Turn on the stirrer and stir at 100 rpm for 1 h to obtain a metal oxide mixture. (2) Weigh citric acid (accounting for 10% of the total mass of oxides) and add it to the mixed salt, then add hydrochloric acid solution (accounting for 40% of the total mass of oxides), heat the stirred tank to 100℃, and continue stirring at 100 rpm for 10 h to obtain an acid-modified metal oxide mixture. (3) Weigh sodium carbonate powder (D50=3.5μm, Na:(Ni+Fe+Mn) molar ratio is 1.0) and add it to the stirred tank above, and continue stirring for 5 h to obtain the precursor. (4) The precursor was transferred to a calcining furnace and calcined at 950°C for 15 hours in an air atmosphere to obtain layered oxide C6.

[0027] Example 7: (1) Weigh NiO (D50=5μm), 2O3 (D50=5μm) and MnO2 (D50=5μm) were placed in a stirred tank, with the molar ratio of Ni, Fe and Mn being 1 / 3:1 / 3:1 / 3. The stirrer was turned on and stirred at 100 rpm for 1 h to obtain a metal oxide mixture. (2) Ascorbic acid (5% of the total mass of oxides) was weighed and added to the mixed salt, followed by hydrochloric acid solution (2% of the total mass of oxides). The stirred tank was heated to 80℃ and stirred at 200 rpm for 15 h to obtain an acid-modified metal oxide mixture. (3) Sodium carbonate powder (D50=3.5μm, Na:(Ni+Fe+Mn) molar ratio of 1.0) was weighed and added to the stirred tank. The mixture was stirred for 5 h to obtain a precursor. (4) The precursor was transferred to a calcining furnace and calcined at 950℃ for 15 h in an air atmosphere to obtain the initial layered oxide C7.

[0028] Reference Example 1: The preparation method is basically the same as in Example 1, except that step (2) is removed to obtain layered oxide CC-1.

[0029] Reference Example 2: The preparation method is basically the same as in Example 1, using NiO (D50=5μm), Replacing 2O3 (D50=5μm) and MnO2 (D50=5μm) with NiO (D50=30nm), Fe2O3 (D50=30nm) and MnO2 (D50=30nm) yields layered oxide CC-2.

[0030] Reference Example 3: The preparation method is basically the same as in Example 2, except that step (2) is removed, and layered oxide CC-3 is obtained.

[0031] Reference Example 4: The preparation method is basically the same as in Example 3, except that step (2) is removed to obtain layered oxide CC-4.

[0032] Reference Example 5: The preparation method is basically the same as in Example 4, except that step (2) is removed, and layered oxide CC-5 is obtained.

[0033] Reference Example 6: The preparation method is basically the same as in Example 5, except that step (2) is removed to obtain layered oxide CC-6.

[0034] Reference Example 7: The preparation method is basically the same as in Example 6, except that step (2) is removed to obtain layered oxide CC-7.

[0035] Reference Example 8: The preparation method is basically the same as in Example 7, except that step (2) is removed, and layered oxide CC-8 is obtained.

[0036] Battery assembly and testing Layered oxide cathode material, conductive carbon black, PVDF, and NMP were mixed in a mass ratio of 94:3:3:100, stirred for 5 hours, coated onto aluminum foil, and dried in a vacuum drying oven at 100°C for 10 hours. The mixture was then cut into Φ12mm electrode sheets, which were used as the positive electrode. A sodium metal sheet was used as the negative electrode. The electrolyte was 1M NaPF6 DMC:EC:EMC = 1:1:1 (Vol%), and the separator was a glass fiber optic GF / D membrane. The mixture was assembled into CR2032 type button cell half-cells in an argon-filled glove box. The button cell half-cells were first allowed to stand for 12 hours, and then charge-discharge tests were performed in the voltage range of 2.0-4.0V. Specific capacity was tested sequentially at 0.1C, 1C, and 3C rates, followed by a 150-cycle test at 1C rate.

[0037] In summary, this patent proposes a technique for synthesizing large single-crystal layered oxide cathode materials for sodium-ion batteries using oxides as precursors. The synthesis process is simple and easily industrialized. Large single-crystal layered oxide cathode materials for sodium-ion batteries can be obtained through four steps: metal oxide mixing, acid treatment, addition of a sodium-containing alkali, and calcination. The mixing process ensures uniform mixing of the metal oxides. The acid treatment introduces inorganic or organic acids, which can etch the surface of the metal oxides. The addition of a sodium-containing alkali provides sufficient sodium to the system and reacts with the metal oxides to form layered oxides. The calcination process utilizes high temperature to promote the formation of stable large single-crystal layered oxides between the metal oxides and the sodium-containing alkali. Compared with the traditional oxide route, this patent introduces an acid treatment process. Under the action of acid, the surface of the metal oxide forms defect structures, which is more conducive to strong interactions between the components of the metal oxide and between the metal oxide and the sodium-containing alkali, ultimately forming a larger single-crystal layered oxide structure. The large single-crystal layered oxide synthesized by this patent exhibits excellent specific capacity, rate performance, and cycle performance.

[0038] A comparison of Examples 1-7 and Reference Examples 1-8 reveals that introducing an acid treatment process can alter the crystal morphology of layered oxides in sodium-ion batteries. Traditional solid-state methods synthesize polycrystalline aggregates, while acid treatment can induce the formation of large single crystals, improving the rate performance and cycle stability of layered oxides in sodium-ion batteries. Hydrochloric acid, nitric acid, phosphoric acid, hydrofluoric acid, oxalic acid, citric acid, ascorbic acid, etc., can all achieve similar effects in the acid treatment process. It is worth noting that if a solid acid is used, it is best to use it in combination with other liquid acids, because the hydrogen ions in solid acids are difficult to ionize, which would affect the effectiveness of the acid treatment. Given the volatility of some acids, this patent employs a closed stirred tank to reduce acid volatilization. A comparison of Example 1 and Reference Example 2 shows that using nanoscale metal oxides cannot yield large single crystals. This is because while small particle size facilitates the formation of a more uniform mixture, small particles are not easily grown into large single crystals due to the need to overcome excessively high energy barriers. In order to induce a melting reaction between large-particle metal oxides and between them and sodium-containing alkalis, it is necessary to first treat them with acid to create defects for induction.

[0039] The embodiments described above are merely preferred embodiments for fully illustrating the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the claims.

Claims

1. A method for synthesizing a layered oxide cathode material for large single-crystal sodium-ion batteries, characterized in that, Includes the following steps: (1) Weigh the metal oxide containing transition metal elements, transfer it to a device with mixing function, mix it evenly, and obtain a metal oxide mixture; (2) Add acid to the metal oxide mixture and mix thoroughly to complete the acid treatment process; (3) Add alkali to the acid-treated mixture and mix thoroughly; (4) The mixture precursor obtained in step (3) is transferred to a calcining furnace and calcined at high temperature to obtain a layered oxide with a large single crystal structure.

2. The method for synthesizing the large single-crystal sodium-ion battery layered oxide cathode material as described in claim 1, characterized in that, In step (1), the transition metal element is at least one of Ni, Fe, Mn, and Cu; The device with mixing function is at least one of a mixer, a stirring vessel, a pulverizer, and a grinding mill, and the device is equipped with a heating function.

3. The method for synthesizing the large single-crystal sodium-ion battery layered oxide cathode material as described in claim 1, characterized in that, The acid mentioned in step (2) is at least one of hydrochloric acid, nitric acid, phosphoric acid, hydrofluoric acid, oxalic acid, citric acid, acetic acid, and ascorbic acid; The amount of acid added is 0.1%-100% of the mass of the metal oxide mixture; the acid treatment temperature is 0-300℃, and the time is 1-100h.

4. The method for synthesizing the large single-crystal sodium-ion battery layered oxide cathode material as described in claim 1, characterized in that, The alkali mentioned in step (3) is at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate; The mixing temperature is 0-750℃, and the time is 1-50h.

5. The method for synthesizing the large single-crystal sodium-ion battery layered oxide cathode material as described in claim 1, characterized in that, The roasting temperature in step (4) is 800-1200℃ and the time is 1-50h.

Citation Information

Patent Citations

  • Copper uniform distribution type high-tap-density precursor material and preparation method thereof, positive electrode material and sodium ion battery

    CN117865239A

  • Layered positive electrode material of high-capacity sodium-ion battery and preparation method of layered positive electrode material

    CN120072923A

  • High-entropy sodium ion battery positive electrode material and preparation method thereof

    CN120208312A