Concrete mix design and fabrication methods in underground environments coupled with loads

By establishing a correlation system between underground environment and load coupling parameters and optimizing concrete mix design and manufacturing process, the problems of insufficient erosion resistance and fatigue resistance in underground engineering are solved, and the durability and mechanical stability of concrete are improved. It is suitable for underground engineering such as subways, tunnels, and underground utility tunnels.

CN122275158APending Publication Date: 2026-06-26CHINA UNIV OF MINING & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610769564.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-01
Publication Date
2026-06-26

AI Technical Summary

Technical Problem

Existing concrete mix design for underground engineering does not fully consider the coupling effect between the underground environment and the load, resulting in insufficient resistance to erosion, cracking, and fatigue. During service, it is prone to cracking, spalling, and steel corrosion. Furthermore, the manufacturing process is poorly adapted to the coupled environment, making it impossible to accurately assess the performance in the actual service environment.

Method used

A correlation system of "coupled environmental parameters - concrete components - performance indicators" was established. By quantifying the coupling parameters of underground environment and load, a suitable foundation mix ratio was determined. Composite admixtures and modifiers were adopted, and graded mixing, gradient curing and coupled simulation curing processes were designed to ensure that the internal structure of concrete is dense and the interface is firmly bonded.

Benefits of technology

It improves the durability and mechanical stability of concrete in coupled environments, extends the service life of underground engineering structures, and has excellent resistance to sulfate attack, chloride penetration and fatigue load. The 28-day compressive strength is ≥60MPa, the sulfate attack resistance coefficient is ≥0.9, and the chloride diffusion coefficient is ≤1.5×10-12m2/s.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122275158A_ABST
    Figure CN122275158A_ABST
Patent Text Reader

Abstract

This invention discloses a concrete mix design and manufacturing method for underground engineering concrete in a coupled environment of underground environment and load, relating to the field of underground engineering concrete technology. It aims to address the problem that traditional concrete mix design does not fully consider the coupling effect of underground environment and load. The underground environment includes groundwater erosion, wet-dry cycle, and temperature fluctuation; the load includes stress ratio. α s Dynamic load frequency and dynamic load amplitude α d This leads to technical problems such as insufficient erosion resistance, crack resistance, and mechanical stability of concrete, resulting in a short service life. This mix design is based on quantitative analysis of coupled environmental parameters. With cement, composite admixtures, recycled aggregates, modifiers, water, and additives as core components, the basic mix proportion is determined through a mapping model between "environment-load" coupled parameters and component content. The target mix proportion is then obtained through orthogonal experimental optimization. The manufacturing method includes four core steps: raw material pretreatment, graded mixing, gradient curing, and coupled environmental simulation curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of underground engineering concrete technology, specifically to concrete mix design and manufacturing methods in underground environments coupled with loads. It is a concrete mix design method and corresponding manufacturing process adapted to the coupling effect of underground environments and loads, applicable to various underground engineering concrete structures such as subways, tunnels, underground utility tunnels, deep foundation pit support, and underground parking garages. Background Technology

[0002] With the rapid development of underground engineering construction, the number of infrastructure projects such as subways, tunnels, and underground utility tunnels has surged. The underground environment is significantly complex and unique. Concrete structures are subjected to harsh environments of groundwater erosion, alternating wet and dry cycles, and temperature fluctuations for extended periods. Groundwater erosion is characterized by corrosive ions containing sulfates, chlorides, and carbonates. Simultaneously, the structures must withstand multiple loads, including their own weight, soil pressure, vehicle dynamic loads, and seismic loads, forming a coupled "environment-load" system.

[0003] Existing underground engineering concrete and its preparation technologies have many shortcomings and are difficult to adapt to the stringent requirements of coupled environments. The reasons are as follows: First, the mix design lacks specificity. Traditional concrete mix design is mostly based on a single mechanical property, such as compressive strength, without fully considering the coupling effect of the underground environment and loads. This results in insufficient resistance to erosion, cracking, and fatigue, making the concrete prone to cracking, spalling, and steel corrosion during service, significantly shortening the structural service life. Second, the selection and proportion of composite admixtures are unreasonable. Existing technologies mostly use single admixtures to improve concrete performance, which cannot simultaneously resist... The synergistic damage caused by multiple corrosive media and loads is significant. For example, while fly ash admixtures can improve impermeability, their resistance to sulfate attack is limited. Third, the manufacturing process is poorly adapted to the coupled environment. The mixing and curing processes are not optimized for the hydration characteristics of concrete under coupled conditions, resulting in high internal porosity and a weak interfacial transition zone, further reducing structural durability. Fourth, there is a lack of performance verification under coupled conditions. Traditional curing methods only simulate standard temperature and humidity environments without considering the actual underground corrosive media and loads, making it impossible to accurately assess the performance of concrete in actual service environments. Summary of the Invention

[0004] To address the problems of existing underground engineering concrete mix design not considering the coupling effect of environment and load, insufficient resistance to erosion and fatigue, poor adaptability of manufacturing process, and insufficient performance verification, this invention provides a concrete mix design and manufacturing method in underground environment coupled with load. This method achieves dynamic and precise adaptation of mix proportion and synergistic optimization of manufacturing process, improves the durability and mechanical stability of concrete in coupled environment, and extends the service life of underground engineering structures.

[0005] The core idea of ​​this invention is to establish a correlation system of "coupled environmental parameters - concrete components - performance indicators". By quantifying the coupling parameters of the underground environment and load, a suitable basic mix proportion is determined, and then the final mix proportion is obtained through orthogonal experiments. Simultaneously, a comprehensive manufacturing process of "pretreatment - graded mixing - gradient curing - coupled simulation curing" is specifically designed to ensure a dense internal structure and strong interfacial bonding of the concrete. Performance is verified through curing processes simulating actual coupled environments. Specifically, it includes two core parts: first, a dynamic mix design method based on graded coupled environments, using composite admixtures and modifiers to adapt to different coupling levels; second, a synergistically optimized manufacturing process, using graded mixing to improve homogeneity, gradient curing to optimize the structure of hydration products, and coupled simulation curing to ensure performance matches the actual service environment.

[0006] To achieve the above-mentioned technical objectives, the present invention adopts the following technical solution: This invention protects a concrete mix design method for underground environments coupled with loads, comprising the following steps: The coupling environment parameters are quantified to determine the underground environmental parameters and load parameters, and an evaluation system for the coupling effect level is established, classifying them into three levels: weak coupling, moderate coupling, and strong coupling. The underground environmental parameters include groundwater sulfate concentration, chloride concentration, wet-dry cycle frequency, and ambient temperature; the load parameters include stress ratio. α s Dynamic load frequency and dynamic load amplitude α d .

[0007] The criteria for weak coupling are: sulfate ≤ 500 mg / L, chloride ≤ 100 mg / L, and stress ratio. α s ≤0.3, wet-dry cycle frequency ≤2 times / year, dynamic load frequency ≤1Hz, dynamic load amplitude α d ≤0.15.

[0008] The criteria for determining intermediate coupling are: 500 mg / L < sulfate ≤ 2000 mg / L, 100 mg / L < chloride ≤ 500 mg / L, and 0.3 < stress ratio. α s ≤0.6, wet-dry cycle frequency 3 times / year to 12 times / year, 1Hz < dynamic load frequency < 5Hz, 0.15 < dynamic load amplitude α d ≤0.35.

[0009] The criteria for strong coupling are: sulfate > 2000 mg / L, chloride > 500 mg / L, and stress ratio. α s >0.6, wet-dry cycle frequency >12 times / year, dynamic load frequency >5Hz, dynamic load amplitudeα d >0.35.

[0010] In the case of weak coupling, the concrete mix proportions are as follows: 320-350 parts of P·O 42.5 ordinary Portland cement, 80-110 parts of composite admixture, 1100-1300 parts of recycled aggregate, 178-198 parts of water, and 6-12 parts of admixture.

[0011] In the intermediate coupling, the concrete mix proportions are: 280-320 parts of P·O 52.5 ordinary Portland cement, 110-130 parts of composite admixture, 1100-1300 parts of recycled aggregate, 169-178 parts of water, and 6-12 parts of admixture.

[0012] Strong coupling, the concrete mix proportion is: 280-320 parts of P·O 52.5 ordinary Portland cement, 130-150 parts of composite admixture, 1100-1300 parts of recycled aggregate, 148-169 parts of water and 6-12 parts of admixture.

[0013] The composite admixture is a combination of fly ash, slag powder and silica fume; the admixture is a polycarboxylate-based high-efficiency water-reducing agent with a water reduction rate of ≥25% and an air content of 3%~5%, and the dosage of the water-reducing agent in concrete is 1.5%~2.5%.

[0014] Orthogonal optimization of the mix proportion was carried out, selecting the dosage of composite admixture, type and dosage of modifier, and water-cement ratio as optimization variables. The 28-day compressive strength, sulfate erosion resistance coefficient, chloride diffusion coefficient and fatigue strength were used as evaluation indicators. An L9 orthogonal experiment was designed, and the optimal level of each variable was determined by range analysis to obtain the final mix proportion adapted to the target coupled environment.

[0015] Preferably, based on the coupling effect level, the proportion of each component is adjusted through a mapping model between the "environment-load" coupling parameters and the component content; under weak coupling conditions, the composite admixture accounts for 20%~25% of the mass of the cementitious material; under medium coupling conditions, the composite admixture accounts for 25%~35% of the mass of the cementitious material; under strong coupling conditions, the composite admixture accounts for 35%~45% of the mass of the cementitious material; wherein, the cementitious material is composed of cement and composite admixture.

[0016] Preferably, for high-salinity groundwater strongly coupled environments with chloride concentrations >1000 mg / L, the concrete mix proportion is: 300 parts of P·O 52.5 ordinary Portland cement, 140 parts of composite admixture, 1100-1300 parts of recycled aggregate, 161 parts of water, 12.25 parts of admixture, and 17.5-28 parts of metakaolin modifier; wherein, the active alumina content in the metakaolin modifier is ≥40%.

[0017] Preferably, for strong dynamic load coupling environment with dynamic load frequency > 2Hz, the concrete mix proportion is: 310 parts of P·O52.5 ordinary Portland cement, 147 parts of composite admixture, 1100-1300 parts of recycled aggregate, 157.5 parts of water, 10.85 parts of admixture and 2.8-4.2 parts of basalt fiber modifier; wherein, the length of the basalt fiber modifier is 6mm-12mm and the tensile strength is ≥3500MPa.

[0018] Preferably, to adapt to the coupling environment dominated by sulfate corrosion, 7 to 10.5 parts of nano-silica modifier are added, with the nano-silica modifier having a particle size of 20 nm to 50 nm.

[0019] Preferably, the mass ratio of fly ash, slag powder, and silica fume is 5:3:2; wherein the fly ash is Class F, Grade I, with a specific surface area ≥350 m². 2 / kg; Slag powder is grade S95, with a specific surface area ≥400m². 2 / kg; Silica fume specific surface area ≥18000m² 2 / kg.

[0020] Preferably, the recycled aggregate is recycled aggregate from crushed construction waste, with a particle size of 5mm~25mm, a crushing index of ≤20%, a water absorption rate of ≤3%, and is saturated surface-drying treatment before use.

[0021] This invention also protects a concrete production method based on the above-mentioned concrete mix design method in the coupled environment of underground environment and load, comprising the following steps: Raw material pretreatment: The recycled aggregate was dried in a 60℃ oven for 12 hours, cooled to room temperature, and then subjected to saturated surface drying to obtain pretreated recycled aggregate.

[0022] Impurities were removed by passing the composite admixture through a 45μm sieve.

[0023] Preheat the cement to 20℃~30℃ in advance to avoid the hydration reaction being affected by the temperature being too low.

[0024] Staged mixing.

[0025] First, mix the pretreated recycled aggregate, cement, and composite admixture, and dry mix for 2 to 3 minutes until the mixture is uniform. Then, add 70% water and admixtures, and wet mix for 3 to 4 minutes. Then, add the remaining 30% water and continue mixing for 2 to 3 minutes at a speed of 60 to 80 r / min to ensure the homogeneity of the concrete.

[0026] After casting, let it stand for 12h~24h in an environment of 20±2℃ and relative humidity ≥90%, and then carry out gradient temperature curing: first raise the temperature from room temperature to 40℃ at a rate of 5℃ / h and keep it at a constant temperature for 12h; then raise the temperature to 60℃ at a rate of 3℃ / h and keep it at a constant temperature for 24h; finally, let it cool naturally to room temperature at a rate of ≤5℃ / h.

[0027] Coupled environment simulation curing: The gradient-cured concrete is placed in a curing box simulating the target underground coupled environment. The simulation parameters are consistent with the actual underground environment, including sulfate / chloride concentration, wet-dry cycle period, temperature and load. The curing is completed after ≥7 days. During the curing process, the cracks on the concrete surface and the changes in strength are monitored in real time.

[0028] Preferably, the mixing process of pretreated recycled aggregate, cement, composite admixture, water and additives is carried out using a twin-shaft forced mixer. During the mixing process, the concrete temperature is monitored by an infrared thermometer and the mixing temperature is controlled at 15℃~25℃.

[0029] Preferably, gradient curing adopts steam curing method, with a steam pressure of 0.1MPa~0.15MPa.

[0030] Preferred parameters for coupled environment simulation curing are: wet-dry cycle, 12 hours, specifically: 8 hours of soaking + 4 hours of air drying; temperature controlled at 10℃~30℃, with fluctuation range ≤5℃ / d; load application adopts periodic loading method, with loading frequency consistent with actual engineering, and loading amplitude of 30%~50% of concrete design strength.

[0031] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Coupling Environment Graded Adaptive Design: This invention establishes for the first time an evaluation system for the coupling effect between underground environment and load. Based on key parameters such as sulfate concentration, chloride concentration, wet-dry cycle frequency, annual average temperature and fluctuation, and load strength, the coupling level is divided to achieve dynamic and accurate adaptation of mix proportions. This solves the problem of poor adaptability caused by the traditional "one-size-fits-all" mix proportion, and ensures that the concrete performance under different coupling levels can reach the optimal level.

[0032] 2. Synergistic Optimization of Composite Admixtures: This invention innovatively adopts a ternary composite admixture system of fly ash, slag powder, and silica fume. By utilizing the complementary advantages of each admixture, fly ash improves workability, slag powder enhances erosion resistance, and silica fume strengthens interfacial strength. With the selection of targeted modifiers, the synergistic improvement of concrete's erosion resistance, crack resistance, and fatigue resistance is achieved. Compared with single admixture of fly ash or slag, the sulfate erosion resistance coefficient of concrete is increased by more than 20%.

[0033] 3. Full-process process synergistic optimization: The design of a graded mixing process improves the homogeneity of concrete and avoids the separation of aggregates and cementitious materials; the use of gradient temperature curing optimizes the structure of hydration products and reduces internal stress and porosity; the addition of a coupled environment simulation curing process exposes potential performance defects in advance, ensuring that the concrete performance matches the actual service environment and solving the problem of the disconnect between traditional curing and the actual service environment.

[0034] 4. Parametric design and strong operability: Establish an "environment-load-component" mapping model, clarify the component value range and process parameters under each coupling level, achieve precise optimization through orthogonal experiments, reduce dependence on operator experience, and facilitate large-scale engineering application.

[0035] 5. This invention aims to address the problem that traditional concrete mix design does not fully consider the coupling effect of the underground environment and load. The underground environment includes groundwater erosion, wet-dry cycles, and temperature fluctuations, while the load includes stress ratio. α s Dynamic load frequency and dynamic load amplitude α d This leads to technical problems such as insufficient erosion resistance, crack resistance, and mechanical stability of concrete, resulting in a short service life. This mix design is based on quantitative analysis of coupled environmental parameters. With cement, composite admixtures, recycled aggregates, modifiers, water, and additives as core components, the basic mix proportion is determined through a mapping model between "environment-load" coupled parameters and component content. The target mix proportion is then optimized through orthogonal experiments. The manufacturing method includes four core steps: raw material pretreatment, graded mixing, gradient curing, and coupled environment simulation curing. The mix proportion of this invention can dynamically adapt to different underground coupled environments. The resulting concrete exhibits excellent resistance to sulfate attack, chloride permeation, and fatigue load, with a 28-day compressive strength ≥60MPa, a sulfate attack resistance coefficient ≥0.9, and a chloride diffusion coefficient ≤1.5×10⁻⁶. -12 m 2 / s can significantly improve the durability and service safety of underground concrete structures. It is applicable to various underground projects such as subways, tunnels, underground utility tunnels, and deep foundation pit support, and has important engineering application value and economic and social benefits.

[0036] 6. Compared with existing concrete technologies, the main difference of this invention is that the admixtures in the concrete are mostly fly ash, slag, and silica fume, and the aggregates are recycled aggregates. Although the raw materials are conventional, the performance of the concrete is different from that of ordinary concrete commonly used in engineering after the multiple components are added. The main components of ordinary concrete are cement, yellow sand, and gravel. The cement may contain fly ash or slag, and the aggregates may also contain recycled aggregates, but they do not all meet the conditions of this invention at the same time. Therefore, the concrete mix ratio is different, and the performance is also different. Attached Figure Description

[0037] Figure 1 This is a schematic diagram illustrating the method for producing concrete in underground environments and load-coupled environments without modifiers.

[0038] Figure 2 This is a schematic diagram illustrating the method for producing concrete in an underground environment coupled with loads containing modifiers. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0040] Statistics show that the annual maintenance and renovation costs for underground concrete structures due to the coupled damage caused by the environment and load exceed 10 billion yuan, and approximately 30% of underground concrete structures experience serious durability problems within 10 to 15 years of service. Therefore, this invention provides a concrete mix design and manufacturing method that can accurately adapt to the coupling characteristics of the underground environment and load, while balancing erosion resistance and mechanical stability. This method has significant practical implications for improving the quality of underground engineering projects, extending the service life of structures, and reducing engineering maintenance costs.

[0041] 1. Detailed process of mix design method: (1) Quantification and classification of coupled environmental parameters: ① Parameter Acquisition: Through on-site investigation and testing, the core environmental and load parameters of the target underground project are determined: Core environmental parameters include groundwater sulfate concentration (mg / L), chloride concentration (mg / L), wet-dry cycle frequency (times / day), annual average temperature and its fluctuation range; Load parameters include stress ratio α s Dynamic load frequency (Hz) and dynamic load amplitude α d .

[0042] ② Grading Evaluation: A weighted scoring method was used to establish a grading evaluation system for coupling effects. The weights were allocated as follows: concentration of corrosive medium 40%, frequency of wet-dry cycles 20%, and stress ratio. α s 25% for dynamic load frequency and 15% for dynamic load frequency, divided into three levels based on the scoring results: - Weak Coupling Level: Total score ≤ 30 points, corresponding to sulfate ≤ 500 mg / L, chloride ≤ 100 mg / L, and stress ratio α s ≤0.3, wet-dry cycle frequency ≤2 times / year, dynamic load frequency ≤1Hz α d≤0.15, the annual average temperature is the same as the natural temperature, and there is no artificial temperature intervention; such as shallow underground garages and small underground utility tunnels.

[0043] - Coupling level: 30 points < total score ≤ 60 points, corresponding to 500mg / L < sulfate ≤ 2000mg / L, 100mg / L < chloride ≤ 500mg / L, 0.3 < stress ratio α s ≤0.6, 1Hz < dynamic load frequency ≤5Hz, 0.15 < α d ≤0.35, 3 times / year ≤ dry and wet cycle frequency ≤12 times / year, with a temperature difference of 15℃~30℃ on both sides of the concrete or artificial temperature intervention; such as subway tunnels and medium-sized underground utility tunnels.

[0044] - Strong Coupling Level: Total score > 60 points, corresponding to sulfate > 2000 mg / L, chloride > 500 mg / L, stress ratio α s >0.6, dynamic load frequency >5Hz α d >0.35, wet-dry cycle frequency exceeds 12 times / year, and there is a temperature difference of >30℃ on both sides of the concrete; such as deep-sea concrete structures and deep foundation pit support structures.

[0045] (2) Basic formulation construction and component selection: ① Core components and their functions: For typical strongly coupled environments involving high-salinity groundwater and intense dynamic loads, specific mix proportion parameters are further clarified to ensure precise performance adaptation; at the same time, the mechanisms of action of each modifier are refined, elucidating their core principles for enhancing concrete's resistance to coupled failure. - Cement: Use P·O 42.5 or P·O 52.5 ordinary Portland cement to ensure the mechanical properties of the concrete foundation; use P·O 42.5 for weakly coupled environments, with a dosage of 320-350 parts; use P·O 52.5 for medium and strong coupled environments, with a dosage of 280-320 parts; in particular, use P·O 52.5 cement for strong coupled environments with high salinity groundwater (chloride concentration > 1000 mg / L), with a dosage of 300 parts; use P·O 52.5 cement for strong coupled environments with strong dynamic loads (dynamic load frequency > 2 Hz), with a dosage of 310 parts.

[0046] - Composite admixture: A ternary composite of Class F Grade I fly ash, S95 grade slag powder, and silica fume, in a mass ratio of 5:3:2. The total admixture dosage is adjusted according to the coupling level. The dosage of the composite admixture in concrete is as follows: weak coupling 20%~25%, medium coupling 25%~35%, and strong coupling 35%~45%, specifically: weak coupling 80~110 parts, medium coupling 110~130 parts, and strong coupling 130~150 parts. It reduces the porosity of concrete and improves its erosion resistance through pozzolanic reaction. Among them, the total admixture dosage in the high-salinity groundwater strong coupling environment is 40%, 140 parts; and the total admixture dosage in the strong dynamic load strong coupling environment is 42%, 147 parts.

[0047] -Recycled aggregate: Crushed and recycled aggregate from construction waste, with a continuous gradation of 5mm~25mm particle size, crushing index ≤20%, water absorption rate ≤3%, and saturated surface drying treatment before use. It can replace 30%~50% of natural aggregate in weak coupling, medium coupling and strong coupling environments, realizing resource recycling; among them, the replacement rate in strong coupling environment with high salinity groundwater is 30%, 1150 parts; and the replacement rate in strong coupling environment with strong dynamic load is 35%, 1200 parts.

[0048] - Modifiers: Targeted selection; the mechanism of action and suitable scenario parameters for each modifier are as follows: 1) Nano silica modifier, adapted to the coupling environment dominated by sulfate attack: The particle size of the nano silica modifier is 20nm~50nm, and the dosage is 2%~3%; the corresponding strong coupling environment is 3%, that is, 10.5 parts; the mechanism of action is: the nano-sized particles can fill the tiny pores between cement hydration products, realize the densification of the internal structure of concrete, and at the same time, it reacts with the hydration product Ca(OH)2 to form a secondary pozzolanic reaction and generate CSH gel, which improves the bonding strength of the cementitious material system, reduces the sulfate ion penetration channels, and thus significantly improves the resistance to sulfate attack.

[0049] 2) Metakaolin modifier, suitable for high-salinity groundwater coupled environment dominated by chloride erosion: The active alumina content in the metakaolin modifier is ≥40%, and the dosage is 5%~8%; the corresponding high-salinity groundwater strongly coupled environment is 8%, i.e., 28 parts; the mechanism of action is: the active alumina in metakaolin reacts with Ca(OH)2 produced by cement hydration to generate calcium aluminate hydrate C3AH6. Calcium aluminate hydrate has a very strong chloride ion binding capacity, which can convert free chloride ions into stable Friedel salt 3CaO·Al2O3·CaCl2·10H2O, preventing chloride ions from diffusing into the interior of concrete and avoiding steel corrosion; at the same time, the hydration products generated by the reaction can fill the pores and further improve the impermeability.

[0050] 3) Basalt fiber modifier, suitable for dynamic load-dominated coupling environment: Basalt fiber modifier length 6mm~12mm, tensile strength ≥3500MPa, dosage 0.8%~1.2%; the corresponding strong dynamic load strong coupling environment is 1.2%, i.e. 4.2 parts; the mechanism of action is: basalt fibers are randomly distributed in the concrete to form a three-dimensional support network. When the concrete is subjected to dynamic load and microcracks are generated, the fibers can transfer stress through "bridging effect" and inhibit the expansion and penetration of microcracks; at the same time, the fibers can enhance the toughness and fatigue resistance of concrete, reduce the energy accumulation damage under repeated dynamic loads, and extend the service life of concrete under strong dynamic loads.

[0051] - Water and Admixtures: The water-cement ratio, obtained by the water / cement mass ratio, is controlled at 0.35~0.45, with 0.42~0.45 for weak coupling, 0.40~0.42 for medium coupling, and 0.35~0.40 for strong coupling; among which, the water-cement ratio in a strong coupling environment with high salinity groundwater is 0.38 (161 parts water); the water-cement ratio in a strong coupling environment with strong dynamic load is 0.36 (157.5 parts water); the admixture is a polycarboxylate-based high-efficiency water-reducing agent with a water reduction rate ≥25% and a dosage of 1.5%~2.5%; among which, the admixture dosage in a strong coupling environment with high salinity groundwater is 2.5% (12.25 parts); the admixture dosage in a strong coupling environment with strong dynamic load is 2.2% (10.85 parts); this improves the workability of concrete and reduces the water-cement ratio.

[0052] In summary, specifically: - Cement: Use P·O 42.5 or P·O 52.5 ordinary Portland cement to ensure the mechanical properties of the concrete foundation. Use P·O 42.5 for weakly coupled environments, with a dosage of 320 to 350 parts. Use P·O 52.5 for medium and strong coupled environments, with a dosage of 280 to 320 parts.

[0053] - Composite admixture: Class I fly ash (F type), S95 grade slag powder, and silica fume are mixed in a ternary ratio of 5:3:2. The total admixture amount is adjusted according to the coupling level: 80-110 parts for weak coupling, 110-130 parts for medium coupling, and 130-150 parts for strong coupling. It reduces the porosity of concrete and improves its erosion resistance through pozzolanic reaction.

[0054] -Recycled aggregate: Crushed and recycled aggregate from construction waste, with a continuous gradation of 5mm~25mm particle size, crushing index ≤20%, water absorption rate ≤3%, saturated surface dry treatment before use, replacing 30%~50% of natural aggregate, realizing resource recycling.

[0055] - Modifiers: Targeted selection. For sulfate attack, nano-silica is selected at a dosage of 2%~3% to densify the concrete structure through the filling effect; for chloride attack, metakaolin is selected at a dosage of 5%~8% to enhance chloride ion binding capacity; for dynamic load, basalt fiber is selected at a dosage of 0.8%~1.2% to inhibit crack propagation and improve fatigue resistance.

[0056] - Water and admixtures: The water-cement ratio is controlled at 0.35~0.45, weak coupling 0.42~0.45, medium coupling 0.40~0.42, and strong coupling 0.35~0.40; the admixture is a polycarboxylate-based high-efficiency water-reducing agent with a water reduction rate ≥25% and a dosage of 1.5%~2.5%, which improves the workability of concrete and reduces the water-cement ratio.

[0057] ② Basic proportion adjustment model: A component adjustment model is established based on the coupling level. The core formula is: Composite admixture dosage = 20% + k × (coupling level score - 30), where k is the adjustment coefficient with a specific value of 0.005, to ensure that the dosage is accurately matched with the coupling level.

[0058] (3) Orthogonal experiment optimization: The total amount of composite admixture (A), modifier (B), water-cement ratio (C), and additive (D) were selected as optimization variables, with each variable having three levels, as shown in Table 1. The 28-day compressive strength, 28-day sulfate resistance coefficient, chloride diffusion coefficient, and strength retention rate after 2 million fatigue loading cycles were used as evaluation indicators. The 28-day sulfate resistance coefficient was calculated as: 28-day immersion strength / 28-day standard curing strength. The chloride diffusion coefficient was obtained using the RCM method. An L9 orthogonal experiment was designed, i.e., 3... 4 Orthogonal experiments. For typical strongly coupled environments of high-salinity groundwater and intense dynamic loads, a verification group was added to the orthogonal experiments to ensure that the optimized mix proportions meet the specific performance requirements: the high-salinity groundwater environment verification group focused on assessing the chloride diffusion coefficient, with a target of ≤1.2×10⁻⁶. -12 m 2 / s, the dynamic load environment verification group focuses on assessing the strength retention rate after 2 million fatigue loading cycles, with a target of ≥88%. Range analysis is used to determine the significance of each variable's impact on performance indicators, and the parameter combination with the optimal overall performance is selected as the final ratio.

[0059] Table 1. Factor Level Table for Orthogonal Experiment

[0060] 2. Detailed steps for making the product: Methods for constructing concrete in underground environments coupled with loads, such as... Figure 2 As shown, it includes the following steps: (1) Raw material pretreatment: ① Recycled aggregate treatment: After screening, the recycled aggregate is placed in a 60℃ constant temperature oven for 12 hours to remove moisture; after cooling to room temperature, it is immersed in the corresponding erosion medium solution for 24 hours. The erosion medium solution is pure water or distilled water to achieve saturated surface drying treatment, improve the interfacial adhesion between the aggregate and the cementitious material, and obtain pretreated recycled aggregate.

[0061] ② Pretreatment of cementitious materials: Mix the composite admixture and modifier evenly according to the proportions in Table 1, put them into a mixer and dry mix for 1 minute, then pass them through a 45μm standard sieve to remove lumps and impurities, ensuring uniform mixing, and obtain the composite admixture-modifier.

[0062] ③ Cement and water pretreatment: Cement should be placed in an environment of 20℃~25℃ for 24 hours in advance to avoid slow hydration reaction due to low temperature; pure water should be used, and the water temperature should be heated to 20℃~30℃ during winter construction to ensure that the temperature of the cement entering the mold meets the standard.

[0063] (2) Staged mixing process: The mixer uses a JS500 twin-shaft forced mixer and mixes in three stages: ① Dry mixing stage: Add the pretreated recycled aggregate, cement and composite admixture-modifier mixture into the mixer, mix at a speed of 60 r / min, and dry mix for 2 min to 3 min to ensure that the aggregate surface is evenly covered with cementitious material.

[0064] ② Initial wet mixing stage: Add 70% water and the remaining admixture, increase the mixing speed to 80r / min, and wet mix for 3min~4min to form a uniform cement mortar coating layer.

[0065] ③ Secondary wet mixing stage: Add the remaining 30% of water, maintain a mixing speed of 80r / min, and continue mixing for 2min~3min until the concrete mixture has a uniform color and no obvious aggregate accumulation. The slump is tested as follows: strong coupling 120mm~160mm, weak coupling 140mm~160mm, medium-strong coupling 120mm~140mm; pour into the mold, and control the temperature of the mold at 15℃~25℃.

[0066] (3) Gradient maintenance process: Casting is done using steel or wooden molds, followed by application of a release agent. After casting and shaping, gradual temperature increase steam curing is implemented. ① Standing stage: Let the concrete stand for 12h~24h in a standard environment of 20±2℃ and relative humidity ≥90% to ensure the initial setting of the concrete and avoid surface cracking caused by early temperature rise.

[0067] ② Heating stage one: Steam heating is used to raise the temperature from room temperature to 40℃, with the heating rate controlled at 5℃ / h to avoid excessively rapid heating and the generation of temperature stress.

[0068] ③ Constant temperature stage one: 40℃ constant temperature curing for 12 hours to promote the formation of early hydration products and improve the early strength of concrete.

[0069] ④ Heating stage two: Continue heating to 60℃, reduce the heating rate to 3℃ / h, and reduce internal porosity and defects.

[0070] ⑤ Constant temperature stage two: 60℃ constant temperature curing for 24 hours, with steam pressure controlled at 0.1MPa~0.15MPa to ensure full hydration reaction.

[0071] ⑥ Cooling stage: Allow the temperature to cool naturally to room temperature at a rate of ≤5℃ / h to avoid cracks caused by excessively rapid cooling.

[0072] (4) Coupled environment simulation maintenance: The HLY-600 multi-functional environmental-load coupling curing chamber was used to simulate the underground coupled environment parameters of the target: ①Simulation of erosion medium: Sulfate or chloride solution with the same concentration as actual groundwater is injected into the curing chamber to ensure that the concrete specimens are completely soaked or in a wet-dry cycle, specifically: 8h soaking + 4h air drying, cycle 12h.

[0073] ②Temperature simulation: The temperature of the curing box is controlled at 10℃~30℃, and adjusted according to the actual underground temperature fluctuation pattern, with a fluctuation range of ≤5℃ / d.

[0074] ③ Load simulation: A servo loading system is used to apply periodic loads to the concrete specimens. The loading frequency and amplitude are consistent with those of the actual project, such as 2Hz for subway tunnels.

[0075] ④ Curing period and testing: Simulate curing for 7 days. During the curing process, monitor the surface cracks of the concrete specimens daily. After curing, test the 28-day compressive strength, sulfate erosion resistance coefficient, and chloride diffusion coefficient to ensure that they meet the design requirements.

[0076] The above operations are further illustrated below with examples, as detailed below: Example 1 The method for preparing concrete in underground environments coupled with loads includes the following steps: In this embodiment, the raw materials were weighed according to the following parts by weight: 330 parts of P・O 42.5 ordinary Portland cement, 110 parts of composite admixture (composite admixture accounts for 25% of cementitious materials), 1200 parts of recycled aggregate, 198 parts of water (water-cement ratio = 0.45), 6.6 parts of polycarboxylate-based high-efficiency water-reducing agent (polycarboxylate-based high-efficiency water-reducing agent dosage is 1.5%, water reduction rate ≥ 25%), and 7.7 parts of nano-silica modifier (nano-silica modifier dosage is 2%). The mixture had a particle size of 20nm~50nm and was prepared for use.

[0077] (1) Raw material pretreatment: ① Recycled aggregate treatment: Place the recycled aggregate in a 60℃ oven to dry for 12 hours, cool it to room temperature, and then soak it in water for 24 hours to fully saturate the interior of the recycled aggregate with water. Then pour off the surface water and wipe the surface of the recycled aggregate with a damp towel until there is no free water film, thus obtaining recycled aggregate in a saturated surface-dry state.

[0078] ② Pretreatment of cementitious materials: Mix the composite admixture and nano silica modifier evenly at a ratio of 14.3:1, put them into a mixer and dry mix for 1 minute, then pass them through a 45μm standard sieve to obtain the composite admixture-modifier.

[0079] ③ Cement and water pretreatment: Cement is placed in an environment of 20℃ for 24 hours in advance, and purified water is used.

[0080] (2) Staged mixing process: The JS500 model is a twin-shaft forced mixer, which performs mixing in three stages: ① Dry mixing stage: The pretreated recycled aggregate, cement, and composite admixture-modifier mixture are put into the mixer and mixed at a speed of 60 r / min for 2.5 min to obtain the mixture.

[0081] ② Initial wet mixing stage: Add 70% water and the remaining admixture to the mixture, increase the mixing speed to 80 r / min, and wet mix for 3.5 min to form a uniform cement mortar coating layer.

[0082] ③ Secondary wet mixing stage: Add the remaining 30% of water, maintain a mixing speed of 80r / min, and continue mixing for 2.5min until the concrete mixture has a uniform color and no obvious aggregate accumulation. The slump is 150mm. Pour the mixture into the mold, and control the temperature at 20℃.

[0083] (3) Gradient maintenance process: Steel molds are used for casting, a release agent is applied, and after casting and shaping, gradient temperature steam curing is implemented. ①Stationary stage: Let stand for 18 hours in a standard environment at 20℃ and relative humidity ≥90%.

[0084] ② Heating stage one: Steam heating is used to raise the temperature from room temperature to 40℃, with the heating rate controlled at 5℃ / h.

[0085] ③ Constant temperature stage one: 40℃ constant temperature curing for 12 hours.

[0086] ④ Heating stage two: Continue heating to 60℃, and reduce the heating rate to 3℃ / h.

[0087] ⑤ Constant temperature stage two: 60℃ constant temperature curing for 24 hours, with steam pressure controlled at 0.15MPa.

[0088] ⑥ Cooling stage: Cool naturally to room temperature, with a cooling rate of ≤5℃ / h.

[0089] (4) Coupled environment simulation maintenance: The HLY-600 multi-functional environmental-load coupling curing chamber was used to simulate the underground coupled environment parameters of the target: ①Simulation of erosion medium: Sulfate or chloride solution with the same concentration as actual groundwater is injected into the curing chamber to ensure that the concrete specimens are completely soaked or in a wet-dry cycle, specifically: 8h soaking + 4h air drying, cycle 12h.

[0090] ②Temperature simulation: The temperature of the curing box is controlled according to the actual underground temperature fluctuation pattern, with a fluctuation range of ≤5℃ / d.

[0091] ③ Load simulation: A servo loading system is used to apply periodic loads to the concrete specimens, with the loading frequency and amplitude consistent with the actual project.

[0092] ④ Curing period and testing: Simulate curing for 7 days. During the curing process, monitor the surface cracks of the concrete specimens daily. After curing, test the 28-day compressive strength, sulfate erosion resistance coefficient, and chloride diffusion coefficient.

[0093] Example 2 The preparation steps are the same as in Example 1, except that the amount of composite admixture is replaced by 35% instead of 25%.

[0094] Example 3 The preparation steps are the same as in Example 1, except that the amount of composite admixture is replaced by 45% instead of 25%.

[0095] Example 4 The preparation steps are the same as in Example 1, except that the amount of modifier is replaced by 2.5% instead of 2%.

[0096] Example 5 The preparation steps are the same as in Example 1, except that the amount of modifier is replaced by 3% instead of 2%.

[0097] Example 6 The preparation steps are the same as in Example 1, except that the water-cement ratio is changed from 0.45 to 0.40. After the change, the amount of cementitious material remains unchanged.

[0098] Example 7 The preparation steps are the same as in Example 1, except that the water-cement ratio is changed from 0.45 to 0.35. After the change, the amount of cementitious material remains unchanged.

[0099] Example 8 The preparation steps are the same as in Example 1, except that the amount of additive is replaced by 2.0 instead of 1.5.

[0100] Example 9 The preparation steps are the same as in Example 1, except that the amount of additive is replaced by 2.5 instead of 1.5.

[0101] 3. Performance Verification and Scope of Application: Performance metrics: The core performance indicators of the weakly coupled environment concrete of this invention are: 28-day compressive strength ≥ 60 MPa, sulfate attack resistance coefficient ≥ 0.9, and chloride diffusion coefficient ≤ 1.5 × 10⁻⁶. -12 m 2 / s, with a fatigue load retention rate of ≥85% after 2 million cycles, extending the erosion resistance life of traditional underground engineering concrete by 3 times.

[0102] Key performance indicators for concrete in medium-coupled environments: 28-day compressive strength ≥ 65 MPa, sulfate attack resistance coefficient ≥ 0.93, chloride diffusion coefficient ≤ 1.2 × 10⁻⁶. -12 m 2 / s, with a fatigue strength retention rate of ≥87% after 2 million cycles of loading, extending the erosion resistance life by 4 times compared to traditional concrete. For details on the formulation of traditional concrete, please refer to JGJ 55-2011 "Specification for Mix Proportion Design of Ordinary Concrete".

[0103] Key performance indicators for concrete in strongly coupled environments: 28-day compressive strength ≥ 68 MPa, sulfate attack resistance coefficient ≥ 0.95, chloride diffusion coefficient ≤ 1.0 × 10⁻⁶. -12 m 2 / s, with a fatigue strength retention rate of ≥88% after 2 million fatigue loading cycles, extending the erosion resistance life of traditional concrete by 5 times.

[0104] Among them, the specific indicator for the strongly coupled environment of high-salinity groundwater is: chloride diffusion coefficient ≤ 1.2 × 10⁻⁶. -12 m 2 / s, extending the service life against chloride salt corrosion by 6 to 8 times; special indicators for strong dynamic load and strong coupling environment: ≥88% strength retention rate after 2 million fatigue loading cycles, and crack resistance increased by more than 30%.

[0105] Table 2. Core Indicators of Concrete Prepared in Examples 1 to 9 of this Invention

[0106] Example 10 For concrete in highly saline groundwater environments with chloride concentrations >1000 mg / L, the preparation steps are the same as in Example 1, except for the raw material composition: by mass, 300 parts of P·O 52.5 ordinary Portland cement, 140 parts of composite admixture, 1150 parts of recycled aggregate, 161 parts of water, 12.25 parts of polycarboxylate-based high-efficiency water-reducing agent, and 28 parts of metakaolin modifier, wherein the metakaolin active alumina content is ≥40%.

[0107] Example 11 For concrete in environments with strong dynamic load coupling and dynamic load frequency > 2Hz, the preparation steps are the same as in Example 1, except for the raw material composition: by mass, 310 parts of P.O 52.5 ordinary Portland cement, 147 parts of composite admixture, of which 73.5 parts of fly ash, 44.1 parts of slag powder, 29.4 parts of silica fume, 1200 parts of recycled aggregate, 157.5 parts of water, 10.85 parts of polycarboxylate-based high-efficiency water-reducing agent, and 4.2 parts of basalt fiber modifier; wherein the basalt fiber is a mixture with a length of 6mm to 12mm and a tensile strength ≥ 3500MPa.

[0108] Example 12 Methods for constructing concrete in underground environments coupled with loads, such as... Figure 1 As shown, this embodiment is a medium-coupled concrete, and the preparation steps are the same as those in Example 1. The only difference is the raw material composition: by mass parts, 300 parts of P·O 52.5 ordinary Portland cement, 120 parts of composite admixture, 1200 parts of recycled aggregate, 175 parts of water, and 9 parts of polycarboxylate-based high-efficiency water-reducing agent.

[0109] Example 13 Methods for constructing concrete in underground environments coupled with loads, such as... Figure 1 As shown, this embodiment is a strongly coupled concrete, and the preparation steps are the same as those in Example 1. The only difference is the raw material composition: by mass parts, 300 parts of P.O 52.5 ordinary Portland cement, 140 parts of composite admixture, 1200 parts of recycled aggregate, 160 parts of water, and 9 parts of polycarboxylate-based high-efficiency water-reducing agent.

[0110] The concrete of this invention is applicable to various underground projects such as subways, tunnels, underground pipe corridors, deep foundation pit support, underground garages, and undersea tunnels. It is compatible with concrete structures of strength grades C30 to C80 and can flexibly adjust the mix proportions and manufacturing parameters according to different underground environments and load coupling levels.

[0111] The concrete operation requirements of this invention are as follows: operators must undergo professional training and be familiar with the coupled environment grading standards and mix proportion adjustment methods; raw materials must be strictly tested to ensure they meet the selection requirements; mixing and curing equipment must be calibrated regularly to ensure precise parameter control; coupled environment simulation curing parameters must be determined based on on-site survey data to ensure consistency with the actual service environment.

[0112] Although specific embodiments of the present invention have been described above, those skilled in the art should understand that these are merely illustrative examples, and various changes or modifications can be made to these embodiments without departing from the spirit and scope of the present invention, which is defined only by the appended claims.

Claims

1. A method for concrete mix design in an underground environment coupled with loads, characterized in that, Includes the following steps: The parameters of the coupling environment are quantified and classified into three levels: weak coupling, medium coupling, and strong coupling. The criteria for weak coupling are: sulfate ≤ 500 mg / L, chloride ≤ 100 mg / L, and stress ratio. α s ≤0.3, wet-dry cycle frequency ≤2 times / year, dynamic load frequency ≤1Hz, dynamic load amplitude α d ≤0.15; The criteria for determining intermediate coupling are: 500 mg / L < sulfate ≤ 2000 mg / L, 100 mg / L < chloride ≤ 500 mg / L, and 0.3 < stress ratio. α s ≤0.6, wet-dry cycle frequency 3 times / year to 12 times / year, 1Hz < dynamic load frequency < 5Hz, 0.15 < dynamic load amplitude α d ≤0.35; The criteria for strong coupling are: sulfate > 2000 mg / L, chloride > 500 mg / L, and stress ratio. α s >0.6, wet-dry cycle frequency >12 times / year, dynamic load frequency >5Hz, dynamic load amplitude α d >0.35; In the case of weak coupling, the concrete mix proportions are as follows: 320-350 parts of P·O 42.5 ordinary Portland cement, 80-110 parts of composite admixture, 1100-1300 parts of recycled aggregate, 178-198 parts of water, and 6-12 parts of admixture. In the intermediate coupling, the concrete mix proportion is: 280-320 parts of P·O 52.5 ordinary Portland cement, 110-130 parts of composite admixture, 1100-1300 parts of recycled aggregate, 169-178 parts of water and 6-12 parts of admixture; Strong coupling, the concrete mix proportion is: 280-320 parts of P·O 52.5 ordinary Portland cement, 130-150 parts of composite admixture, 1100-1300 parts of recycled aggregate, 148-169 parts of water and 6-12 parts of admixture; The composite admixture is a combination of fly ash, slag powder and silica fume; the admixture is a polycarboxylate-based high-efficiency water-reducing agent.

2. The concrete mix design method for underground environments coupled with loads as described in claim 1, characterized in that, Under weak coupling conditions, the composite admixture accounts for 20%–25% of the mass of the cementitious material; under medium coupling conditions, the composite admixture accounts for 25%–35% of the mass of the cementitious material; and under strong coupling conditions, the composite admixture accounts for 35%–45% of the mass of the cementitious material. The cementitious material consists of cement and composite admixtures.

3. The concrete mix design method for underground environments coupled with loads as described in claim 1, characterized in that, For high-salinity groundwater strongly coupled environments with chloride concentrations >1000 mg / L, the concrete mix proportion is: 300 parts of P·O 52.5 ordinary Portland cement, 140 parts of composite admixture, 1100-1300 parts of recycled aggregate, 161 parts of water, 12.25 parts of admixture, and 17.5-28 parts of metakaolin modifier; Among them, the active alumina content in the metakaolin modifier is ≥40%.

4. The concrete mix design method for underground environments coupled with loads as described in claim 1, characterized in that, For strong dynamic load coupling environment with dynamic load frequency > 2Hz, the concrete mix proportion is: 310 parts of P·O 52.5 ordinary Portland cement, 147 parts of composite admixture, 1100-1300 parts of recycled aggregate, 157.5 parts of water, 10.85 parts of admixture and 2.8-4.2 parts of basalt fiber modifier; The basalt fiber modifier has a length of 6mm to 12mm and a tensile strength of ≥3500MPa.

5. The concrete mix design method for underground environments coupled with loads as described in claim 1, characterized in that, To adapt to the coupling environment dominated by sulfate attack, 7 to 10.5 parts of nano silica modifier are added, with a particle size of 20 nm to 50 nm.

6. The concrete mix design method for underground environments coupled with loads as described in claim 1, characterized in that, The mass ratio of fly ash, slag powder, and silica fume is 5:3:2; among which, the fly ash is Class F, Grade I, with a specific surface area ≥350 m². 2 / kg; Slag powder is grade S95, with a specific surface area ≥400m². 2 / kg; Silica fume specific surface area ≥18000m² 2 / kg.

7. The concrete mix design method for underground environments coupled with loads as described in claim 1, characterized in that, The recycled aggregate is made from crushed construction waste, with a particle size of 5mm~25mm, a crushing index of ≤20%, a water absorption rate of ≤3%, and is saturated and surface-dried before use.

8. A concrete production method based on the concrete mix design method for underground environment and load coupling environment as described in claim 1, characterized in that, Includes the following steps: The recycled aggregate is dried and then subjected to saturated surface drying treatment to obtain pretreated recycled aggregate. The composite admixture was passed through a 45μm sieve; Preheat the cement to 20℃~30℃ in advance; First, mix the pretreated recycled aggregate, cement, and composite admixture, and dry mix for 2 to 3 minutes until the mixture is uniform; then add 70% water and admixtures, and wet mix for 3 to 4 minutes; then add the remaining 30% water and continue mixing for 2 to 3 minutes at a mixing speed of 60 to 80 r / min. After casting, let it stand for 12h~24h in an environment of 20±2℃ and relative humidity ≥90%, and then carry out gradient temperature curing: first raise the temperature from room temperature to 40℃ at a rate of 5℃ / h and keep it at a constant temperature for 12h; then raise the temperature to 60℃ at a rate of 3℃ / h and keep it at a constant temperature for 24h; finally, let it cool naturally to room temperature at a rate of ≤5℃ / h. The gradient-cured concrete was placed in a curing box simulating the target underground coupled environment. The simulation parameters were consistent with the actual underground environment, and the curing time was ≥7 days.

9. The manufacturing method according to claim 8, characterized in that, The mixing temperature of the pretreated recycled aggregate, cement, composite admixture, water and additives is 15℃~25℃.

10. The manufacturing method according to claim 8, characterized in that, Gradient curing uses steam curing with a steam pressure of 0.1MPa~0.15MPa.