Combined spinning treatment method for stress relief and strengthening of conical die forgings
By employing a combined cold spinning process, which integrates quenching, cold spinning, and aging treatment, the stress relief and strengthening issues of tapered forgings have been resolved. This approach achieves stress elimination and performance enhancement in tapered forgings, making them suitable for applications in aerospace, high-end machinery, and other fields.
Patent Information
- Application Number
- CN202610505074.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-16
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-04-16
AI Technical Summary
Existing technologies struggle to achieve uniform stress relief and simultaneous improvement of mechanical properties in tapered forgings without the need for specialized molds. Traditional methods suffer from high mold costs, incomplete stress relief, or limited depth of application.
A combined cold spinning process is employed, including quenching, cold spinning, and aging. By precisely controlling the amount of spinning deformation, the number of passes, and the cooling method, and by adjusting the structure and parameters of the spinning wheel, uniform deformation and stress relief of the tapered forging are achieved, while simultaneously triggering work hardening and grain refinement.
It achieves efficient elimination of residual stress and grain refinement in tapered forgings, significantly improving material strength and plasticity, shortening the production cycle, reducing process complexity, and enabling rapid adaptation to different product specifications.
Smart Images

Figure CN122279164B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a spinning composite treatment method for stress relief and strengthening of conical forgings, belonging to the field of hot working and surface strengthening treatment of metal materials. Background Technology
[0002] Conical forgings are widely used in aerospace, high-end equipment, and energy sectors. Typical examples include conical shells made of high-alloy aluminum alloys (such as 7075 and 7050) and conical joints made of titanium alloys. These forgings typically require quenching and aging heat treatment to achieve high strength. However, during quenching, the combined effects of thermal stress and phase transformation stress can easily introduce significant residual tensile stress into the conical wall, leading to deformation and dimensional instability during subsequent machining. In severe cases, cracking may even occur, significantly impacting product yield and service reliability.
[0003] To eliminate residual stress after quenching, traditional methods mainly adopt the following technical paths: (1) Natural aging or thermal aging: Although it can relax stress to a certain extent, the processing cycle is long, the stress is not completely eliminated, and the material strength cannot be improved at the same time.
[0004] (2) Local cold deformation using a dedicated cold pressing die: A dedicated cold pressing die is designed for tapered forgings, and compressive stress is applied to a localized area to counteract residual tensile stress. This method has significant drawbacks: The mold has extremely poor versatility; forgings with different tapers, wall thicknesses, and sizes all require separate molds, resulting in high mold costs. Local cold pressing can easily introduce new stress concentration points, which in turn exacerbates the risk of dimensional instability. This process only aims to relieve stress and cannot effectively improve the material strength while relieving stress.
[0005] (3) Surface strengthening techniques such as shot peening and rolling: Although surface compressive stress can be introduced, the depth of action is limited, making it difficult to eliminate the residual tensile stress of the entire conical wall, and it is difficult to implement in complex parts such as the inner wall of the conical wall.
[0006] Therefore, there is an urgent need to develop a new composite treatment method suitable for conical forgings that does not require special molds, can uniformly relieve stress throughout the entire part, and simultaneously improve mechanical properties. Summary of the Invention
[0007] To overcome the shortcomings of existing technologies, this invention provides a spinning composite treatment method for stress relief and strengthening of conical forgings. The technical solution of this invention is as follows: A method for combining stress relief and strengthening of conical forgings through spinning, comprising the following steps: S1. Quenching treatment: The conical forging is heated to the solution temperature and then rapidly cooled. S2. Cold spinning treatment: The quenched conical forging is placed in a spinning machine, and its conical wall is uniformly deformed by cold spinning. The specific steps are as follows: S2.1 Select spinning method: Use forward spinning or reverse spinning; S2.2 Install the spinning wheel: Select a spinning wheel with an arc or conical structure, with a fillet radius of R5 to R15 mm, and make a smooth transition with the contact surface of the forging; S2.3 Set the spinning process parameters: Set the spindle speed to 80~200 r / min and the spinning wheel feed ratio to 0.5~2.0 mm / r; S2.4 Perform multi-pass spinning: Set the spinning passes to 1, 2, or 3 passes, wherein the deformation amount of the first pass is controlled within 2% of the forging wall thickness, and the deformation amount of subsequent passes is increased to 3% to 5% of the forging wall thickness; S2.5 Forced Cooling: During the spinning process, water cooling or air cooling is used to force-cool the processing area to control the temperature rise to no more than 50°C; S2.6 Controlling form and position tolerances: After spinning, control the roundness error of the conical surface of the forging to be ≤0.3 mm, and the wall thickness uniformity error to be ≤±0.2 mm; S3. Aging treatment: Heat the spun tapered forging to 120-540℃ and hold for 6-24 hours to obtain the finished product.
[0008] The material of the tapered forging is 7075 aluminum alloy, 7050 aluminum alloy, TC4 titanium alloy or ultra-high strength steel.
[0009] In the quenching process of step S1: for aluminum alloy materials, the heating temperature is 460-470℃, followed by water cooling after holding; for titanium alloy materials, the heating temperature is 900-950℃, followed by water cooling.
[0010] Before the S1 quenching process, the process also includes step S0: forging the tapered forging and removing the bottom skin.
[0011] The process before die forging also includes billet heating and pre-forming treatment. The billet heating temperature is 440-480℃ for aluminum alloys and 920℃ for titanium alloys. The pre-forming treatment is free forging, die forging, or ring forging.
[0012] In step S2, the cold spinning deformation is 3% to 5% of the wall thickness.
[0013] In step S2, the spinning process consists of two passes, with the deformation amount in the first pass being 1.5% to 2.0%, and the deformation amount in the second pass increasing to 3% to 5%.
[0014] In step S2, forced cooling is achieved using water cooling, and the temperature rise in the processing area does not exceed 30°C.
[0015] In step S3: for 7075 aluminum alloy or 7050 aluminum alloy, the heating temperature is 130-140℃ and the holding time is 18-20h; for TC4 titanium alloy, the heating temperature is 540℃ and the holding time is 6h.
[0016] After the cold spinning process in step S2, the cone surface roundness error of the tapered forging is ≤0.15 mm, and the wall thickness uniformity error is ≤±0.1 mm.
[0017] The advantages of this invention are: 1. The tapered wall of the tapered die forging is uniformly cold-deformed as a whole by cold spinning. The residual tensile stress introduced by quenching is precisely offset by the precisely controlled compressive strain field, thus avoiding the stress concentration caused by traditional local cold pressing.
[0018] 2. By precisely controlling the cold spinning deformation within the range of 3% to 5% of the forging wall thickness, a significant work hardening effect can be triggered while relieving stress, and the brittle second phase can be broken, refining the grain to grade 11.0 (aluminum alloy).
[0019] 3. There is no need to develop special cold pressing dies for forgings with different tapers and sizes. Different specifications of products can be quickly adapted simply by adjusting the parameters such as the spinning wheel trajectory, feed ratio, and number of passes of the spinning machine.
[0020] 4. The cold spinning treatment after quenching is organically integrated with the subsequent aging treatment, replacing the traditional multiple separation processes, reducing the number of workpiece transfers and clamping times, significantly shortening the production cycle, and reducing the complexity of the process.
[0021] 5. It achieves the optimal balance between stress relief, strengthening and plasticity, and has significant technical criticality and non-obviousness.
[0022] 6. The roundness error (≤0.3 mm) and wall thickness uniformity error (≤±0.2 mm) of the spun conical surface were quantitatively controlled, achieving a roundness error ≤0.15 mm and a wall thickness uniformity error ≤±0.1 mm, meeting the requirements of subsequent precision machining and assembly.
[0023] This invention deeply integrates the three steps of quenching, cold spinning, and aging, and precisely controls the deformation amount, pass distribution, forced cooling temperature rise, and dimensional and positional tolerances of cold spinning. It has significant technological advancements and broad industrial application prospects, and is especially suitable for the manufacturing needs of high-performance and high-reliability tapered forgings in aerospace, high-end machinery and other fields. Attached Figure Description
[0024] Figure 1 This is a photograph of the metallographic structure of Embodiment 1 of the present invention.
[0025] Figure 2 This is a photograph of the metallographic structure from another viewpoint of Embodiment 1 of the present invention.
[0026] Figure 3 This is a low-magnification SEM image of the cold-spinned part of Embodiment 1 of the present invention.
[0027] Figure 4 This is a high-magnification SEM image of the cold spinning process of Embodiment 1 of the present invention. Detailed Implementation
[0028] The present invention will be further described below with reference to specific embodiments, and the advantages and features of the present invention will become clearer as a result. However, these embodiments are merely exemplary and do not constitute any limitation on the scope of the present invention. Those skilled in the art should understand that modifications or substitutions can be made to the details and form of the technical solutions of the present invention without departing from the spirit and scope of the present invention, but all such modifications and substitutions fall within the protection scope of the present invention.
[0029] This invention provides a method for a combined stress-relieving and strengthening spinning process for tapered forgings, comprising the following steps performed sequentially: S1. Quenching treatment: The conical forging is heated to the solution temperature and then rapidly cooled. For aluminum alloys, the heating temperature is 460-470℃, followed by water cooling after holding at that temperature; for titanium alloys, the heating temperature is 900-950℃, followed by water cooling.
[0030] S2. Cold spinning treatment: The quenched conical forging is placed in a spinning machine, and its conical wall is uniformly deformed by cold spinning. The specific steps are as follows: S2.1 Select spinning method: Use forward spinning or reverse spinning; S2.2 Install the spinning wheel: Select a spinning wheel with an arc or conical structure, with a fillet radius of R5 to R15 mm, and make a smooth transition with the contact surface of the forging; S2.3 Set the spinning process parameters: Set the spindle speed to 80~200 r / min and the spinning wheel feed ratio to 0.5~2.0 mm / r; S2.4 Perform multi-pass spinning: Set the spinning passes to 1, 2, or 3 passes, wherein the deformation amount of the first pass is controlled within 2% of the forging wall thickness, and the deformation amount of subsequent passes is increased to 3% to 5% of the forging wall thickness; S2.5 Forced cooling: During the spinning process, water cooling or air cooling is used to force-cool the processing area to control the temperature rise to no more than 50°C (preferably no more than 30°C). S2.6 Controlling form and position tolerances: After spinning, control the roundness error of the conical surface of the forging to be ≤0.3 mm (preferably ≤0.15 mm), and the wall thickness uniformity error to be ≤±0.2 mm (preferably ≤±0.1 mm).
[0031] S3. Aging treatment: Heat the spun tapered forging to 120-540℃ and hold for 6-24 hours to obtain the finished product.
[0032] Before step S1, step S0 is also included: forging the tapered forging and removing the bottom skin. Before forging, the billet is heated and pre-formed. The billet heating temperature is 440-480℃ for aluminum alloys and 920℃ for titanium alloys. The pre-formation process is free forging, die forging, or ring forging.
[0033] I. Metallographic Observation and Brittle Phase Analysis To verify the effect of the cold spinning treatment of the present invention on the microstructure of the conical forging, metallographic observation was conducted on the sample treated by the method of the present invention (taking a 7075 aluminum alloy conical forging as an example, treated according to the process of Example 1).
[0034] (a) Metallographic photograph Figure 1 and Figure 2 These are metallographic photographs of different fields of view taken at the same magnification in Embodiment 1 of the present invention. Figure 1 and Figure 2 It can be seen that: After being cold-spun and deformed by 3% to 5% according to the present invention, the grains of the conical forging are significantly elongated and refined along the deformation direction, with a grain size of 11.0 grade, which is significantly better than the unspun comparative example (grain size of 8.0 grade). The dislocation density inside the grains and at the grain boundaries increases significantly, forming work-hardened microstructure characteristics. The tissue uniformity was good across different fields of view, with no obvious local over-deformation or cracking observed.
[0035] (ii) Photographs of brittle phase fragmentation after cold rotation Figure 3 and Figure 4 These are photographs taken at different magnifications after cold spinning, used to show the fragmentation morphology of the brittle phase. Figure 3 and Figure 4 It can be clearly seen that: After being cold-spun and deformed by 3% to 5% according to the present invention, the brittle second phase (such as Al2CuMg, Al2Cu, etc.) that was originally distributed in a continuous network or coarse block shape is significantly broken under the intense shearing and compressive stress of the spinning wheel, and is transformed into fine particles that are dispersed and uniformly distributed in the matrix. Figure 3 The image is a low-magnification SEM image, showing the macroscopic homogeneity of brittle phase fragmentation; Figure 4 These are high-magnification SEM images, clearly showing the fineness of the brittle phase particles and their bonding state with the matrix.
[0036] The beneficial effects of brittle phase fragmentation: The fragmentation of brittle phase significantly reduces stress concentration sources, which is beneficial to suppressing crack initiation and propagation; at the same time, the fine particles after fragmentation promote the uniform entanglement of dislocations, enhancing the work hardening effect; in addition, the dispersed brittle phase provides more precipitation nucleation sites for subsequent aging treatment, promoting the uniform distribution of precipitates, thereby improving strength while maintaining good plasticity.
[0037] The technical effects of the present invention are verified below with reference to five specific embodiments. Each embodiment adopts the basic implementation method described above, and the specific process parameters and test results are as follows.
[0038] Example 1 (7075 aluminum alloy, deformation amount 3.2%) Material: 7075 aluminum alloy tapered forging. Process parameters are as follows: Billet heating: 460℃, hold for 2 hours; Pre-forming: free forging; Remove bottom skin after die forging; Quenching (S1): 465℃, hold for 1.5 hours, water cooling; Cold spinning (S2): forward spinning, arc-shaped spinning wheel (R10 mm), spindle speed 120 r / min, feed ratio 1.0 mm / r, 2-pass spinning (deformation of 1.8% in the first pass and 3.2% in the second pass), water-cooled forced cooling (temperature rise ≤28℃), roundness error after spinning 0.12 mm, wall thickness uniformity error ±0.08 mm; Aging (S3): 135℃, heat preservation for 20 h.
[0039] The test results are as follows: Stress relief rate: 91%; Grain size: 11.2 grade; Tensile strength: 585 MPa; Yield strength: 505 MPa; Elongation: 8.6%; Brinell hardness: 162 HBW.
[0040] Example 2 (7050 aluminum alloy, deformation 4.0%): Material: 7050 aluminum alloy conical forging.
[0041] The process parameters are as follows: Billet heating: 470℃, holding for 2h; Pre-forming: die forging; Remove bottom skin after die forging; Quenching (S1): 468℃, holding for 1.5h, water cooling; Cold spinning (S2): reverse spinning, conical spinning wheel (R12 mm), spindle speed 100 r / min, feed ratio 1.2 mm / r, 2-pass spinning (deformation amount of 2.0% in the first pass, and increased to 4.0% in the second pass), forced air cooling (temperature rise ≤35℃), roundness error after spinning 0.14 mm, wall thickness uniformity error ±0.10 mm; Aging (S3): 138℃, holding for 19h.
[0042] The test results are as follows: stress relief rate: 87%; grain size: grade 10.8; tensile strength: 570 MPa; yield strength: 500 MPa; elongation: 9.0%; Brinell hardness: 160 HBW.
[0043] Example 3 (TC4 titanium alloy, deformation amount 4.5%) Material: TC4 titanium alloy conical forging.
[0044] The process parameters are as follows: Billet heating: 920℃, holding for 2h; Pre-forming: ring forging; after die forging, remove the bottom skin; Quenching (S1): 930℃, water cooling; Cold spinning (S2): forward spinning, arc-shaped spinning wheel (R8 mm), spindle speed 80 r / min, feed ratio 0.8 mm / r, 2-pass spinning (deformation amount of 1.5% in the first pass, and increased to 4.5% in the second pass), forced water cooling (temperature rise ≤25℃), roundness error after spinning 0.10 mm, wall thickness uniformity error ±0.07 mm; Aging (S3): 540℃, holding for 6h.
[0045] Test results: Stress relief rate: 89%; Grain size: 9.8 grade; Tensile strength: 1035 MPa; Yield strength: 925 MPa; Elongation: 11.5%; Brinell hardness: 345 HBW.
[0046] Example 4 (7075 aluminum alloy, deformation amount 4.8%) Material: 7075 aluminum alloy conical forging.
[0047] The process parameters are as follows: Billet heating: 465℃, holding for 2h; Pre-forming: free forging; after die forging, remove the bottom skin; Quenching (S1): 470℃, holding for 1.5h, water cooling; Cold spinning (S2): reverse spinning, arc-shaped spinning wheel (R14 mm), spindle speed 150r / min, feed ratio 1.5 mm / r, 3-pass spinning (deformation amount of 1.5% in the first pass, 1.5% in the second pass, and increased to 4.8% in the third pass), water cooling forced cooling (temperature rise ≤30℃), roundness error after spinning 0.11 mm, wall thickness uniformity error ±0.09 mm; Aging (S3): 130℃, holding for 18h.
[0048] Test results: Stress relief rate: 93%; Grain size: 11.5; Tensile strength: 592 MPa; Yield strength: 512 MPa; Elongation: 8.2%; Brinell hardness: 166 HBW.
[0049] Example 5 (Ultra-high strength steel 30CrMnSiNi2A, deformation amount 3.5%) Material: 30CrMnSiNi2A ultra-high strength steel conical forging.
[0050] The process parameters are as follows: Billet heating: 850℃, holding for 2.5h; Pre-forming: die forging; Remove bottom skin after die forging; Quenching (S1): 880℃, oil cooling; Cold spinning (S2): forward spinning, conical spinning wheel (R6 mm), spindle speed 180 r / min, feed ratio 1.8 mm / r, 2-pass spinning (deformation amount of 1.6% in the first pass, and increased to 3.5% in the second pass), forced air cooling (temperature rise ≤40℃), roundness error after spinning 0.13 mm, wall thickness uniformity error ±0.11 mm; Aging (S3): 150℃, holding for 6h.
[0051] Test results: Stress relief rate: 86%; Grain size: 10.2 grade; Tensile strength: 1620 MPa; Yield strength: 1380 MPa; Elongation: 10.5%; Brinell hardness: 480 HBW.
[0052] II. Comparative Example Comparative Example 1 (Traditional Cold Press Stress Relief): Material: 7075 aluminum alloy conical forging. Process: After quenching, local cold pressing with a special cold pressing die is used to relieve stress. Spinning is not performed. Subsequent aging treatment is the same as in Example 1.
[0053] Test results: Stress relief rate: 73%; Grain size: 8.0 grade; Tensile strength: 545 MPa; Yield strength: 475 MPa; Elongation: 8.0%; Brinell hardness: 151 HBW.
[0054] Comparative Example 2 (spinning deformation insufficient, 1%): Material: 7075 aluminum alloy conical forging. Process: Same as Example 1, but the spinning deformation amount is 1%.
[0055] The test results are as follows: Stress relief rate: 65%; Grain size: 8.5 grade; Tensile strength: 530 MPa; Yield strength: 460 MPa; Elongation: 8.2%; Brinell hardness: 148 HBW.
[0056] Comparative Example 3 (excessive spinning deformation, 8%): Material: 7075 aluminum alloy conical forging. Process: Same as Example 1, but the spinning deformation is 8%.
[0057] The test results are as follows: Stress relief rate: 92%; Grain size: 11.5 grade; Tensile strength: 590 MPa; Yield strength: 515 MPa; Elongation: 4.5%; Brinell hardness: 165 HBW.
[0058] A comparison of Examples 1-5 and Comparative Examples 1-3 shows that: 1. Positive correlation between brittle phase fragmentation and mechanical properties: metallographic micrographs ( Figure 1 , Figure 2 ) and photographs of brittle phase fragmentation ( Figure 3 , Figure 4 This study confirms that after cold spinning treatment according to the present invention, the grains are significantly refined (grain size reaches grade 11.0 or above), and the brittle phase changes from a continuous network or coarse blocky structure to a dispersed distribution of fine particles. This microstructural change is the intrinsic mechanism by which the present invention achieves a synergistic improvement in mechanical properties.
[0059] 2. When the content is below 3% (Comparative Example 2), the brittle phase is not sufficiently broken, resulting in insufficient stress relief and strengthening effects; when the content is above 5% (Comparative Example 3), although the brittle phase is completely broken and the stress is thoroughly eliminated, the plastic damage is unacceptable. Therefore, 3% to 5% is the critical window for achieving a balance between stress relief, strengthening, and plasticity in this invention.
[0060] 3. The method of the present invention can achieve a stress relief rate of 85% to 93%, increase the yield strength by 8% to 12%, improve the grain size by 2 to 3 grades, improve the dimensional stability by more than 40%, and at the same time maintain the elongation at more than 8.2% (aluminum alloy / steel) or 11.5% (titanium alloy), thus avoiding the plasticity loss caused by traditional methods or improper deformation.
[0061] In summary, this invention achieves the dual goals of efficiently eliminating residual stress and synergistically improving mechanical properties in tapered forgings by deeply integrating quenching, cold spinning (deformation amount 3% to 5%), and aging, and by utilizing the brittle phase breakage and grain refinement during the spinning process. It has significant technological advancements and industrial application value.
[0062] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A combined stress relief and strengthening method of a conical swaged part, characterized by, Includes the following steps: S1. Quenching treatment: The conical forging is heated to the solution temperature and then rapidly cooled. S2. Cold spinning treatment: The quenched conical forging is placed in a spinning machine, and its conical wall is uniformly deformed by cold spinning. The specific steps are as follows: S2.1 Select spinning method: Use forward spinning or reverse spinning; S2.2 Install the spinning wheel: Select a spinning wheel with an arc or conical structure, with a fillet radius of R5 to R15 mm, and make a smooth transition with the contact surface of the forging; S2.3 Set the spinning process parameters: Set the spindle speed to 80~200 r / min and the spinning wheel feed ratio to 0.5~2.0mm / r; S2.4 Perform multi-pass spinning: Set the spinning passes to 2 or 3, wherein the deformation amount of the first pass is controlled within 2% of the forging wall thickness, and the deformation amount of subsequent passes is increased to 3% to 5% of the forging wall thickness; S2.5 Forced Cooling: During the spinning process, water cooling or air cooling is used to force-cool the processing area to control the temperature rise to no more than 50°C; S2.6 Controlling form and position tolerances: After spinning, control the roundness error of the conical surface of the forging to be ≤0.3mm, and the wall thickness uniformity error to be ≤±0.2mm; S3. Aging treatment: Heat the spun tapered forging to 120-540℃ and hold for 6-24 hours to obtain the finished product. The material of the tapered forging is 7075 aluminum alloy, 7050 aluminum alloy, TC4 titanium alloy or ultra-high strength steel.
2. The combined stress-relieving and strengthening spinning process of a conical die forging according to claim 1, characterized by, In the quenching process of step S1: for aluminum alloy materials, the heating temperature is 460-470℃, followed by water cooling after holding; for titanium alloy materials, the heating temperature is 900-950℃, followed by water cooling.
3. The method for combined stress relief and strengthening of conical forgings by spinning according to claim 1, characterized in that, Before the quenching process in step S1, step S0 is also included: forging the tapered forging and removing the bottom skin.
4. The method for combined stress relief and strengthening of conical forgings by spinning according to claim 3, characterized in that, The process before die forging also includes billet heating and pre-forming treatment. The billet heating temperature is 440-480℃ for aluminum alloys and 920℃ for titanium alloys. The pre-forming treatment is free forging, die forging, or ring forging.
5. The method for combined stress relief and strengthening of conical forgings by spinning according to claim 1, characterized in that, In step S2, forced cooling is achieved using water cooling, and the temperature rise in the processing area does not exceed 30°C.
6. The method for combined stress relief and strengthening of conical forgings by spinning according to claim 1, characterized in that, In step S3: for 7075 aluminum alloy or 7050 aluminum alloy, the heating temperature is 120-140℃ and the holding time is 18-20h; for TC4 titanium alloy, the heating temperature is 540℃ and the holding time is 6h.
7. The method for combined stress relief and strengthening of conical forgings by spinning according to claim 1, characterized in that, After the cold spinning process in step S2, the cone surface roundness error of the tapered forging is ≤0.15 mm, and the wall thickness uniformity error is ≤±0.1 mm.
Citation Information
Patent Citations
Preparation method of stainless steel thin-walled cylinder
CN114473370A
Method for producing tube material for high strength front fork outer tube, and tube material obtained by the production method
JP2011006736A