Long-acting corrosion-resistant nano epoxy zinc-rich paint

By leveraging the synergistic effect of sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite and phytic acid, the problem of easy agglomeration of nanofillers in epoxy zinc-rich paint was solved, forming a dense coating, extending the sacrificial anode activity cycle of zinc powder, and improving the corrosion resistance of epoxy zinc-rich paint.

CN122356959BActive Publication Date: 2026-11-24SHANDONG HUADIAN ENERGY CONSERVATION TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610741120.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-05-27
Publication Date
2026-11-24
Estimated Expiration
2046-05-27

AI Technical Summary

Technical Problem

In traditional epoxy zinc-rich paints, the nanofillers tend to agglomerate in systems with high zinc powder and high pigment volume concentration, resulting in poor interfacial compatibility, coating defects, and a shortened protection cycle.

Method used

By employing the synergistic effect of sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite and phytic acid, the dispersion stability of nanofillers is improved through the combination of modified hydrotalcite materials and phytate, forming a dense coating and extending the active cycle of zinc powder sacrificial anodes.

Benefits of technology

It significantly extends the corrosion resistance life of epoxy zinc-rich paint and improves the corrosion resistance and environmental adaptability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122356959B_ABST
    Figure CN122356959B_ABST
Patent Text Reader

Abstract

This disclosure relates to the field of anti-corrosion paint technology, specifically a long-lasting corrosion-resistant nano-epoxy zinc-rich paint; the long-lasting corrosion-resistant nano-epoxy zinc-rich paint comprises the following components: component a: bisphenol A type epoxy resin or phenolic epoxy resin, zinc powder, modified hydrotalcite material, phytic acid and / or phytate, additives and a first solvent; component b: amine curing agent, curing accelerator and a second solvent; wherein, the mass ratio of component a to component b is (5-10):1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of anti-corrosion paint technology, specifically a long-lasting corrosion-resistant nano-epoxy zinc-rich paint. Background Technology

[0002] Metal corrosion is one of the main causes of industrial facility failure, and coating protection has become the preferred choice for long-term protection of steel structures due to its convenient application and controllable cost. Epoxy zinc-rich primers combine excellent adhesion, chemical resistance, and cathodic protection functions, and are widely used in heavily corrosive environments. Their anti-corrosion mechanism mainly relies on the sacrificial anode effect of high-content zinc powder and the physical shielding after epoxy resin curing. However, traditional epoxy zinc-rich paints have inherent defects: the zinc powder volume concentration is far higher than the critical value, making it difficult for the resin to completely fill the interparticle gaps, allowing corrosive media to easily penetrate along microchannels; zinc corrosion products expand in volume and have a loose structure, which can crack the coating and block conductive pathways, leading to a shortened protection cycle. Existing technologies introduce nanofillers (such as nano-silica, graphene, etc.) to improve performance, but in systems with high zinc powder and high pigment volume concentrations, nanofillers are prone to agglomeration and poor interfacial compatibility, which may instead become sources of coating defects.

[0003] Therefore, there is an urgent need to develop epoxy zinc-rich paint systems that combine long-lasting protection, stable nanofiller dispersion, and environmental adaptability. Summary of the Invention

[0004] The purpose of this disclosure is to provide a long-lasting, corrosion-resistant nano-epoxy zinc-rich paint to address the shortcomings of related technologies.

[0005] According to a first aspect of the present disclosure, a long-lasting corrosion-resistant nano-epoxy zinc-rich paint is provided, the long-lasting corrosion-resistant nano-epoxy zinc-rich paint comprising the following components: Component a: Bisphenol A type epoxy resin or phenolic epoxy resin, zinc powder, modified hydrotalcite material, phytic acid and / or phytate, additives and first solvent; Component b: amine curing agent, curing accelerator, and second solvent; Furthermore, the mass ratio of component a to component b is (5-10):1.

[0006] In one aspect of this disclosure, based on the total mass of component a, the mass percentage of the bisphenol A type epoxy resin or phenolic epoxy resin is selected from 15%-25%; the mass percentage of the zinc powder is selected from 60%-72%; the mass percentage of the modified hydrotalcite material is selected from 1.5%-5%; the mass percentage of the phytic acid and / or phytate is selected from 0.3%-1%; the mass percentage of the additives is selected from 1%-7%; and the balance is the first solvent.

[0007] In one aspect of this disclosure, based on the total mass of component b, the mass percentage of the amine curing agent is selected from 45% to 65%; the mass percentage of the curing accelerator is selected from 1% to 5%; and the balance is a second solvent.

[0008] In one aspect of this disclosure, the first solvent is selected from one or more of aromatic solvents, alcohol solvents, ether ester solvents, and ketone solvents.

[0009] In one aspect of the embodiments of this disclosure, the second solvent is selected from one or more of aromatic solvents, alcohol solvents, and ether ester solvents.

[0010] In one aspect of the embodiments of this disclosure, the first solvent is selected from xylene, toluene, trimethylbenzene, tetramethylbenzene, heavy aromatic solvent oil, n-butanol, isobutanol, isopropanol, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, propylene glycol ethyl ether acetate, cyclohexanone, methyl isobutyl ketone, methyl ethyl ketone, isophorone, ethylene glycol butyl ether, propylene glycol methyl ether, or dipropylene glycol methyl ether.

[0011] In one aspect of the embodiments of this disclosure, the second solvent is selected from xylene, trimethylbenzene, heavy aromatic solvent oil, n-butanol, isobutanol, isopropanol, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, ethyl 3-ethoxypropionate, or cyclohexanone.

[0012] In one aspect of the embodiments of this disclosure, the amine curing agent is selected from one or more of aliphatic amines, alicyclic amines, aromatic amines, polyamides, phenolic amines, polyether amines, modified amine adducts, and amide amines.

[0013] In one aspect of the embodiments of this disclosure, the curing accelerator is selected from one or more of tertiary amines, imidazoles, quaternary ammonium salts, borate complexes, phenols, organic acids, and thiols.

[0014] In one aspect of the embodiments of this disclosure, the amine curing agent is selected from ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine, hexamethylenediamine, isophoronediamine, 1,3-cyclohexanedimethylamine, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, dimer acid polyamide, low molecular weight polyamide, difunctional polyetheramine, trifunctional polyetheramine, epoxy resin-amine adduct, ketimide, or aldehyde imide.

[0015] In one aspect of this disclosure, the curing accelerator is selected from 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, N,N-dimethylbenzylamine, N,N-dimethylethanolamine, N,N-dimethylcyclohexylamine, 2-ethyl-4-methylimidazole, 1-methylimidazole, 2-phenylimidazole, or benzyltriethylammonium chloride.

[0016] In one aspect of this disclosure, the modified hydrotalcite material is selected from sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite; the sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite is prepared through the following steps: Step 1-a: Dissolve the soluble magnesium salt, soluble aluminum salt, and soluble lanthanum salt in deionized water to prepare a mixed metal salt solution, wherein Mg... 2+ With Al 3+ The molar ratio is (2-4):1, Al 3+ with La 3+ The molar ratio is (5-20):1; Step 2-a: Dissolve sarcosine and an alkaline substance in deionized water to prepare a sarcosine-alkali mixed solution; the alkaline substance is selected from one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, and sodium bicarbonate; Step 3-a: Under conditions of 60℃-90℃, the sarcosine-base mixed solution is added dropwise to the mixed metal salt solution at a rate of 0.5-5 mL / min while stirring. After the addition is complete, the reaction is continued at a constant temperature for 12-48 hours. Step 4-a: Transfer all the products after the reaction to a reaction vessel and hydrothermally react at 120℃-180℃ for 6-24 hours; Step 5-a: After the reaction is complete, cool to room temperature, filter, wash and dry to obtain the sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite.

[0017] In one aspect of this disclosure, the additive is selected from at least one of dispersants, wetting agents, anti-settling agents, defoamers, and leveling agents.

[0018] In one aspect of the embodiments of this disclosure, the dispersant is selected from polycarboxylate dispersants, polyurethane polymeric dispersants, polyether polymeric dispersants, polyamide dispersants, phosphate ester dispersants, or polyacrylate dispersants.

[0019] In one aspect of the embodiments of this disclosure, the wetting agent is selected from polyether-modified siloxane wetting agents, fluorocarbon-modified polysiloxane wetting agents, polyether wetting agents, acetylenic diol wetting agents, or sulfonate anionic wetting agents.

[0020] In one aspect of this disclosure, the anti-settling agent is selected from polyamide wax-based anti-settling agents, organobentonite-based anti-settling agents, or polyurea compound-based anti-settling agents.

[0021] In one aspect of the embodiments of this disclosure, the defoamer is selected from organosilicon defoamers, polyether-modified siloxane defoamers, mineral oil defoamers, polyether defoamers, polyacrylate defoamers, or alkynyl alcohol defoamers.

[0022] In one aspect of the embodiments of this disclosure, the leveling agent is selected from polyacrylate leveling agents, polyether-modified siloxane leveling agents, fluorinated acrylate leveling agents, or fluorinated polysiloxane leveling agents.

[0023] In one aspect of the embodiments of this disclosure, the phytate is selected from sodium phytate, potassium phytate, ammonium phytate, magnesium phytate, or zinc phytate.

[0024] The technical solutions provided by the embodiments of this disclosure may include the following beneficial effects: As can be seen from the above embodiments, this disclosure significantly extends the corrosion resistance life of epoxy zinc-rich paint through the synergistic effect of sarcosine intercalated hydrotalcite and phytic acid.

[0025] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit this disclosure. Attached Figure Description

[0026] Figure 1 This is a SEM image of the sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite prepared in Example 1 of this disclosure. Detailed Implementation

[0027] Exemplary embodiments will now be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this disclosure. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this disclosure as detailed in the appended claims.

[0028] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. The embodiments described herein are illustrative in nature and are used to provide a basic understanding of this application. The embodiments of this application should not be construed as limiting this application.

[0029] For the sake of brevity, this article only discloses a few specific numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.

[0030] In this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0031] In this description, unless otherwise stated, "above" and "below" include the stated number.

[0032] Unless otherwise stated, the terms used in this disclosure have their common meanings as commonly understood by those skilled in the art. Unless otherwise stated, the values ​​of the parameters mentioned in this disclosure can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this disclosure).

[0033] The term "about" is used to describe and indicate small variations. When used in conjunction with an event or situation, the term may refer to examples in which the event or situation occurred precisely or in examples in which the event or situation occurred very approximately. For example, when used in conjunction with numerical values, the term may refer to a range of variation less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. Additionally, quantities, ratios, and other numerical values ​​are sometimes presented in range format herein. It should be understood that such range format is for convenience and brevity and should be interpreted flexibly to include not only numerical values ​​explicitly specified as range limits but also all individual numerical values ​​or subranges covered within the range, as if each numerical value and subrange were explicitly specified.

[0034] The list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms can mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another instance, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.

[0035] The present disclosure will be further described below by way of specific embodiments. Unless otherwise specified, all chemical reagents used in the embodiments of the present disclosure are obtained through conventional commercial means. Unless otherwise specified, all contents mentioned below are mass contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.

[0036] Example Example 1 Example 1 includes the following steps: 1. Preparation of sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite: Weigh 21.15g of magnesium nitrate hexahydrate [Mg(NO3)2·6H2O] and 9.38g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O], dissolve them in 100mL of deionized water, add 1.84mL of lanthanum nitrate [La(NO3)3] solution with a concentration of 1.358mol / L, stir well, and prepare a mixed metal salt solution.

[0037] Separately weigh 2.45 g of sarcosine and 9.38 g of sodium hydroxide, dissolve them in 100 mL of deionized water to prepare a sarcosine-sodium hydroxide mixed solution. Place the above mixed metal salt solution in an 80°C constant temperature water bath, and add the sarcosine-sodium hydroxide mixed solution dropwise at a rate of 2 mL / min using a peristaltic pump while continuously stirring. After the addition is complete, continue the reaction at 80°C for 24 hours.

[0038] The resulting slurry was then transferred to a high-pressure reactor and hydrothermally reacted at 170°C for 8 hours. After the reaction was complete, it was allowed to cool naturally to room temperature, filtered, and repeatedly washed with deionized water until the filtrate was neutral. The filter cake was then dried in an oven at 80°C for 10 hours to obtain a white powdery sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite; its SEM image is shown below. Figure 1 As shown.

[0039] 2. Preparation of the epoxy zinc-rich paint of this embodiment: Three parts by weight of sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite, 0.5 parts by weight of sodium phytate, 1 part by weight of BYK-154 dispersant, 7 parts by weight of xylene, and 3 parts by weight of n-butanol were mixed and dispersed at 1000 rpm for 30 min to obtain a pre-dispersed slurry. 40 parts by weight of spherical zinc powder and 25 parts by weight of flake zinc powder were added to the pre-dispersed slurry and dispersed at 800 rpm for 20 min. Then, 20 parts by weight of E-44 epoxy resin and 0.5 parts by weight of BYK-066N defoamer were added and dispersed at 1000 rpm for 15 min to obtain component a. Eight parts by weight of T-31 phenolic amine, 0.5 parts by weight of DMP-30, 4 parts by weight of xylene, and 2.5 parts by weight of n-butanol were mixed and stirred at 350 rpm for 10 min until clear and transparent to obtain component b. When using, mix component a and component b at a weight ratio of 100:15, stir at 500 r / min for 10 min, and let stand to defoam to obtain the nano epoxy zinc-rich paint of this embodiment.

[0040] Comparative Example 1 Comparative Example 1 includes the following steps: One part by weight of BYK-154 dispersant, seven parts by weight of xylene, and three parts by weight of n-butanol were mixed and dispersed at 1000 rpm for 30 min to obtain a pre-dispersed slurry. Forty-two parts by weight of spherical zinc powder and 26.5 parts by weight of flake zinc powder were added to the pre-dispersed slurry and dispersed at 800 rpm for 20 min. Then, 20 parts by weight of E-44 epoxy resin and 0.5 parts by weight of BYK-066N defoamer were added and dispersed at 1000 rpm for 15 min to obtain component a. Eight parts by weight of T-31 phenolic amine, 0.5 parts by weight of DMP-30, four parts by weight of xylene, and 2.5 parts by weight of n-butanol were mixed and stirred at 350 rpm for 10 min until clear and transparent to obtain component b. For use, component a and component b were mixed at a weight ratio of 100:15 and stirred at 500 rpm for 10 min. After standing to defoam, the nano-epoxy zinc-rich paint of this comparative example was obtained.

[0041] Comparative Example 2 Comparative Example 2 includes the following steps: 1. Preparation of magnesium aluminum lanthanum hydrotalcite: Weigh 21.15g of magnesium nitrate hexahydrate [Mg(NO3)2·6H2O] and 9.38g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O], dissolve them in 100mL of deionized water, add 1.84mL of lanthanum nitrate [La(NO3)3] solution with a concentration of 1.358mol / L, stir well, and prepare a mixed metal salt solution.

[0042] Separately weigh 9.35 g of sodium hydroxide and 1.185 g of sodium bicarbonate, dissolve them in 100 mL of deionized water to prepare an alkaline mixed solution. Place the above mixed metal salt solution in an 80°C constant temperature water bath, and add the above alkaline mixed solution dropwise at a rate of 2 mL / min using a peristaltic pump while continuously stirring. After the addition is complete, continue the reaction at 80°C for 12 hours.

[0043] The resulting slurry was then transferred to a high-pressure reactor and hydrothermally reacted at 170°C for 8 hours. After the reaction was complete, it was naturally cooled to room temperature, filtered, and repeatedly washed with deionized water until the filtrate was neutral. The filter cake was then dried in an oven at 80°C for 10 hours to obtain a white powdery unmodified magnesium aluminum lanthanum hydrotalcite.

[0044] 2. Preparation of the epoxy zinc-rich paint of this comparative example: Three parts by weight of magnesium aluminum lanthanum hydrotalcite, 0.5 parts by weight of sodium phytate, 1 part by weight of BYK-154 dispersant, 7 parts by weight of xylene, and 3 parts by weight of n-butanol were mixed and dispersed at 1000 rpm for 30 min to obtain a pre-dispersed slurry. 40 parts by weight of spherical zinc powder and 25 parts by weight of flake zinc powder were added to the pre-dispersed slurry and dispersed at 800 rpm for 20 min. Then, 20 parts by weight of E-44 epoxy resin and 0.5 parts by weight of BYK-066N defoamer were added and dispersed at 1000 rpm for 15 min to obtain component a. Eight parts by weight of T-31 phenolic amine, 0.5 parts by weight of DMP-30, 4 parts by weight of xylene, and 2.5 parts by weight of n-butanol were mixed and stirred at 350 rpm for 10 min until clear and transparent to obtain component b. When using, mix component a and component b at a weight ratio of 100:15, stir at 500 r / min for 10 min, and let stand to defoam to obtain the nano-epoxy zinc-rich paint of this comparative example.

[0045] Example 2 Example 2 includes the following steps: 1. Preparation of lactate-intercalated magnesium aluminum lanthanum hydrotalcite: Weigh 21.15g of magnesium nitrate hexahydrate [Mg(NO3)2·6H2O] and 9.38g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O], dissolve them in 100mL of deionized water, add 1.84mL of lanthanum nitrate [La(NO3)3] solution with a concentration of 1.358mol / L, stir well, and prepare a mixed metal salt solution.

[0046] Separately weigh 9.35 g of sodium hydroxide and 1.185 g of sodium bicarbonate, dissolve them in 100 mL of deionized water to prepare an alkaline mixed solution. Place the above mixed metal salt solution in an 80°C constant temperature water bath, and add the above alkaline mixed solution dropwise at a rate of 2 mL / min using a peristaltic pump while continuously stirring. After the addition is complete, continue the reaction at 80°C for 12 hours.

[0047] The resulting slurry was then transferred to a high-pressure reactor and hydrothermally reacted at 170°C for 8 hours. After the reaction was complete, it was naturally cooled to room temperature, filtered, and repeatedly washed with deionized water until the filtrate was neutral. The filter cake was then dried in an oven at 80°C for 10 hours to obtain unmodified carbonate-type magnesium aluminum lanthanum hydrotalcite.

[0048] Weigh 5.6 g of the unmodified carbonate-type magnesium aluminum lanthanum hydrotalcite powder and disperse it in 100 mL of ethylene glycol. Sonicate the dispersion for 30 min to obtain an LDH suspension. Weigh 3.74 g of a 60% sodium lactate aqueous solution and dissolve it in 50 mL of deionized water to prepare a sodium lactate solution. Slowly pour the sodium lactate solution into the LDH ethylene glycol suspension, stir until homogeneous, and then adjust the pH of the mixture to 4.5 with dilute nitric acid.

[0049] The mixture was transferred to a three-necked flask and refluxed at 120°C for 3 hours. After the reaction was complete, the mixture was filtered, and the filter cake was repeatedly washed with deionized water until the filtrate was neutral. The filter cake was then dried in a 100°C drying oven for 12 hours to obtain a white powder of lactate-intercalated magnesium aluminum lanthanum hydrotalcite.

[0050] 2. Preparation of the epoxy zinc-rich paint of this embodiment: The steps here are the same as in Example 1, except that sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite is replaced with an equal mass of lactate-intercalated magnesium aluminum lanthanum hydrotalcite.

[0051] Example 3: Example 3 includes the following steps: 1. Preparation of SDBS intercalated magnesium aluminum lanthanum hydrotalcite: Weigh 21.15 g of magnesium nitrate hexahydrate [Mg(NO3)2·6H2O] and 9.38 g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O], dissolve them in 100 mL of deionized water, add 1.84 mL of lanthanum nitrate [La(NO3)3] solution with a concentration of 1.358 mol / L, stir well, and prepare a mixed metal salt solution.

[0052] Separately, dissolve 9.35 g of sodium hydroxide in 100 mL of deionized water that has been boiled to remove carbon dioxide, thus preparing an alkaline solution. While continuously stirring, add the above mixed metal salt solution dropwise to the alkaline solution at a rate of 2 mL / min, controlling the pH of the system to approximately 9.5. After the addition is complete, continue stirring for 0.5 hours.

[0053] The resulting slurry was placed in a constant temperature water bath at 80℃ and reacted for 12 hours. It was then transferred to a high-pressure reactor and hydrothermally reacted at 170℃ for 8 hours. After the reaction was complete, it was allowed to cool naturally to room temperature, filtered, and repeatedly washed with boiled deionized water until the filtrate was neutral. The filter cake was then dried in a 65℃ oven for 10 hours, ground, and the resulting magnesium aluminum lanthanum hydrotalcite (nitrate type) was obtained and stored in a desiccator for later use.

[0054] Weigh 3.0 g of the above-mentioned nitrate-type magnesium aluminum lanthanum hydrotalcite powder, disperse it in 100 mL of deionized water, and sonicate for 30 min to obtain an LDH suspension. Weigh 3.82 g of sodium dodecylbenzenesulfonate (SDBS), dissolve it in 100 mL of deionized water to prepare an SDBS solution. Slowly pour the above SDBS solution into the LDH suspension, stir vigorously under nitrogen protection, control the pH of the system to 7-8, and react at 65℃ for 24 hours. After the reaction is complete, filter, and repeatedly wash the filter cake with deionized water until the filtrate is free of foam (indicating that the free SDBS has been washed away). Place the filter cake in a vacuum drying oven at 65℃ and dry for 12 hours to obtain SDBS intercalated magnesium aluminum lanthanum hydrotalcite.

[0055] 2. Preparation of the epoxy zinc-rich paint of this embodiment: The steps here are the same as in Example 1, except that sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite is replaced with an equal mass of lactate-intercalated magnesium aluminum lanthanum hydrotalcite.

[0056] Example 4 Example 4 includes the following steps: 1. Preparation of sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite: The steps here are the same as in Example 1.

[0057] 2. Preparation of the epoxy zinc-rich paint of this embodiment: 3.5 parts by weight of sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite, 1 part by weight of BYK-154 dispersant, 7 parts by weight of xylene, and 3 parts by weight of n-butanol were mixed and dispersed at 1000 r / min for 30 min to obtain a pre-dispersed slurry. 40 parts by weight of spherical zinc powder and 25 parts by weight of flake zinc powder were added to the above pre-dispersed slurry and dispersed at 800 r / min for 20 min. Subsequently, 20 parts by weight of E-44 epoxy resin and 0.5 parts by weight of BYK-066N defoamer were added and dispersed at 1000 r / min for 15 min to obtain component a. 8 parts by weight of T-31 phenolic amine, 0.5 parts by weight of DMP-30, 4 parts by weight of xylene, and 2.5 parts by weight of n-butanol were mixed and stirred at 350 r / min for 10 min until clear and transparent to obtain component b. When using, mix component a and component b at a weight ratio of 100:15, stir at 500 r / min for 10 min, and let stand to defoam to obtain the nano epoxy zinc-rich paint of this embodiment.

[0058] Performance testing: 1. The acid mist resistance test shall be conducted in accordance with the requirements of GB / T1771.

[0059] 2. Impact resistance test: Apply each group of coatings to carbon steel test plates with a dry film thickness of 80-100μm. After curing for 7 days, place the test plates with the paint film facing up on the base of the impact testing machine. Raise a weight (1.0kg) to the specified height and drop it freely. The impact point should be no less than 15mm from the edge of the test plate. Raise the weight by 5cm for each test. Record the maximum drop height at which the paint film does not crack or peel as the impact resistance value.

[0060] 3. Cathodic Protection Effective Period Test: Each group of coatings was applied to carbon steel test plates with a dry film thickness of 80-100 μm. After curing for 7 days, the test plates were immersed in a 3.5% NaCl solution as the working electrode. A saturated calomel electrode (SCE) was used as the reference electrode, and a platinum electrode as the auxiliary electrode. The self-corrosion potential of the coating / steel substrate system was continuously monitored using an electrochemical workstation. The duration for which the potential remained below -900 mV (vs. SCE) was recorded as the effective period of cathodic protection. The results are shown in Table 1.

[0061] Table 1

[0062] As can be seen, Example 1 exhibits excellent long-term corrosion resistance; this is because sarcosine ions capture Cl through ion exchange. - and in the anode region with Zn 2+ / Fe 2+ Insoluble coordination complexes are formed to passivate the interface; phytate groups form a metal-ligand complex layer on the LDH surface, inhibiting premature dissolution of the lamination; both work synergistically to extend the active cycle of the zinc powder sacrificial anode and densify the coating pores, thus resulting in optimal corrosion resistance. The performance of Example 2 is significantly inferior to Example 1 but superior to Example 3 and the comparative example, indicating that lactate groups can provide a certain chelating and ion exchange capacity through carboxyl groups. The performance of Example 3 is similar to that of Comparative Example 2, both significantly lower than that of Example 1. This is because SDBS only improves dispersibility through long-chain alkyl groups, therefore its performance is close to that of the unmodified Comparative Example 2.

[0063] Other embodiments of this disclosure will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This disclosure is intended to cover any variations, uses, or adaptations of this disclosure that follow the general principles of this disclosure and include common knowledge or customary techniques in the art not disclosed herein.

Claims

1. A long-lasting, corrosion-resistant nano-epoxy zinc-rich paint, characterized in that, The long-lasting corrosion-resistant nano-epoxy zinc-rich paint comprises the following components: Component a: Bisphenol A type epoxy resin or phenolic epoxy resin, zinc powder, modified hydrotalcite material, phytic acid and / or phytate, additives and first solvent; Component b: amine curing agent, curing accelerator, and second solvent; Furthermore, the mass ratio of component a to component b is (5-10):1; Based on the total mass of component a, the mass percentage of the bisphenol A type epoxy resin or phenolic epoxy resin is selected from 15%-25%; the mass percentage of the zinc powder is selected from 60%-72%; the mass percentage of the modified hydrotalcite material is selected from 1.5%-5%; the mass percentage of the phytic acid and / or phytate is selected from 0.3%-1%; the mass percentage of the additives is selected from 1%-7%; the balance is the first solvent; The modified hydrotalcite material is selected from sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite; the sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite is prepared through the following steps: Step 1-a: Dissolve the soluble magnesium salt, soluble aluminum salt, and soluble lanthanum salt in deionized water to prepare a mixed metal salt solution, wherein Mg... 2+ With Al 3+ The molar ratio is (2-4):1, Al 3+ with La 3+ The molar ratio is (5-20):1; Step 2-a: Dissolve sarcosine and an alkaline substance in deionized water to prepare a sarcosine-alkali mixed solution; the alkaline substance is selected from one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, and sodium bicarbonate; Step 3-a: Under conditions of 60°C-90°C, the sarcosine-base mixed solution is added dropwise to the mixed metal salt solution at a rate of 0.5-5 mL / min while stirring. After the addition is complete, the reaction is continued at a constant temperature for 12-48 hours. Step 4-a: Transfer all the products after the reaction to a reaction vessel and hydrothermally react at 120°C-180°C for 6-24 hours; Step 5-a: After the reaction is complete, cool to room temperature, filter, wash and dry to obtain the sarcosine-intercalated magnesium aluminum lanthanum hydrotalcite.

2. The long-lasting corrosion-resistant nano-epoxy zinc-rich paint according to claim 1, characterized in that, Based on the total mass of component b, the mass percentage of the amine curing agent is selected from 45% to 65%; the mass percentage of the curing accelerator is selected from 1% to 5%; and the balance is a second solvent.

3. The long-lasting corrosion-resistant nano-epoxy zinc-rich paint according to claim 1 or 2, characterized in that, The first solvent is selected from one or more of aromatic solvents, alcohol solvents, ether ester solvents, and ketone solvents; the second solvent is selected from one or more of aromatic solvents, alcohol solvents, and ether ester solvents.

4. The long-lasting corrosion-resistant nano-epoxy zinc-rich paint according to claim 3, characterized in that, The first solvent is selected from xylene, toluene, trimethylbenzene, tetramethylbenzene, heavy aromatic solvent oil, n-butanol, isobutanol, isopropanol, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, propylene glycol ethyl ether acetate, cyclohexanone, methyl isobutyl ketone, methyl ethyl ketone, isophorone, ethylene glycol butyl ether, propylene glycol methyl ether, or dipropylene glycol methyl ether; The second solvent is selected from xylene, trimethylbenzene, heavy aromatic solvent oil, n-butanol, isobutanol, isopropanol, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, ethyl 3-ethoxypropionate, or cyclohexanone.

5. The long-lasting corrosion-resistant nano-epoxy zinc-rich paint according to claim 1 or 2, characterized in that, The amine curing agent is selected from one or more of aliphatic amines, alicyclic amines, aromatic amines, polyamides, phenolic amines, polyether amines, modified amine adducts, and amide amines; the curing accelerator is selected from one or more of tertiary amines, imidazoles, quaternary ammonium salts, borate complexes, phenols, organic acids, and thiols.

6. The long-lasting corrosion-resistant nano-epoxy zinc-rich paint according to claim 5, characterized in that, The amine curing agent is selected from ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine, hexamethylenediamine, isophoronediamine, 1,3-cyclohexanedimethylamine, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, dimer acid polyamide, low molecular weight polyamide, difunctional polyetheramine, trifunctional polyetheramine, epoxy resin-amine adduct, ketimide or aldehyde imide; The curing accelerator is selected from 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, N,N-dimethylbenzylamine, N,N-dimethylethanolamine, N,N-dimethylcyclohexylamine, 2-ethyl-4-methylimidazole, 1-methylimidazole, 2-phenylimidazole or benzyltriethylammonium chloride.

7. The long-lasting corrosion-resistant nano-epoxy zinc-rich paint according to claim 1, characterized in that, The additive is selected from at least one of dispersants, wetting agents, anti-settling agents, defoamers, and leveling agents.

Citation Information

Patent Citations

  • Stable epoxy anticorrosive paint can be used for painting on rusty surfaces

    CN107189639A

  • Economical heavy-duty coating and preparation method thereof

    CN109679450A

  • Weather-resistant water-based vehicle body paint and preparation method thereof

    CN119019901A