A wire electroforming-drawing synergic composite forming process

By employing a multi-pass gradient control process for online collaborative electroforming and drawing, the problems of coating oxidation and poor interfacial bonding in traditional processes have been solved, enabling the preparation of high-performance composite wires and improving processing stability and efficiency.

CN122400347APending Publication Date: 2026-07-17ZHEJIANG TRUMHE NEW MATERIAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610656362.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-13
Publication Date
2026-07-17

AI Technical Summary

Technical Problem

In the traditional metal composite wire manufacturing process, the separation of electroforming and drawing leads to coating oxidation and interface contamination, resulting in weak bonding between the coating and the substrate. It is difficult to achieve sufficient densification of the coating, and the mismatch of processing parameters leads to low dimensional accuracy and insufficient tensile strength, which cannot meet the requirements of high-end equipment.

Method used

A multi-pass gradient control process combining online electroforming and drawing is adopted. By connecting the electroforming and drawing devices online in series, combined with polycrystalline diamond molds and lubricating oil, a dense bond between the electroformed layer and the substrate is achieved. Annealing treatment forms an atomic interdiffusion transition layer, optimizing the interface performance.

Benefits of technology

It improves the density and interlayer bonding strength of composite filaments, solves the problems of coating oxidation and interface contamination, ensures the high performance and dimensional accuracy of composite filaments, adapts to a variety of substrates and coating materials, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122400347A_ABST
    Figure CN122400347A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal material processing technology. It discloses a synergistic composite forming process for metal wire electroforming and drawing, comprising the following steps: first, surface cleaning and activation treatment of the base metal wire to remove oxide layers, oil stains, and impurities; then, feeding the pretreated wire into an electroforming device to deposit a metal plating layer, obtaining an initial electroformed composite wire; subsequently, direct online radial high-pressure drawing to achieve a dense bond between the electroformed layer and the base metal; followed by annealing of the composite wire; repeating the electroforming, drawing, and annealing steps at least once to complete multiple synergistic cycles; finally, testing the dimensional accuracy, mechanical properties, and interlayer bonding force of the composite wire, and cutting it into finished products after passing the tests. This invention employs an online tandem synergistic process of electroforming and drawing, avoiding plating oxidation and interface contamination. Radial high-pressure drawing can compact the plating layer, eliminate porosity, and improve bonding density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal material processing technology, and in particular to a metal wire electroforming-drawing synergistic composite forming process. Background Technology

[0002] High-performance metal composite wires are fundamental materials in fields such as electronic components, aerospace, and precision machinery manufacturing. The uniformity of their coating, interlayer bonding strength, and mechanical properties directly determine the stability and service life of the end products. Traditional metal composite wire manufacturing often employs offline processes where electroforming and drawing are separate. Electroforming deposits a coating on the surface of the base metal wire, followed by drawing for densification after transport. These two processes are independent and cannot be coordinated. This production model easily leads to oxidation and interface contamination of the electroformed layer during transport, making it difficult to ensure the bonding state between the coating and the substrate. Furthermore, offline drawing cannot match the stress application conditions to the deposition state of the electroformed layer, making it difficult to achieve sufficient densification of the coating.

[0003] Existing composite wire forming processes suffer from problems such as mismatched processing parameters across multiple passes and insufficient control over interfacial bonding. Conventional electroforming processes lack a quantitative correlation between deposition rate and drawing stress, easily leading to insufficient coating compaction or cracking and deformation. Furthermore, annealing treatments often use a single temperature parameter, failing to adapt to the atomic diffusion requirements of different matrix materials and hindering the formation of a stable interfacial transition layer. In addition, composite wires produced by traditional processes generally exhibit defects such as low dimensional accuracy, insufficient tensile strength and elongation, and weak interlayer peel strength, resulting in frequent coating peeling and cracking, failing to meet the stringent requirements of high-end equipment for high-performance metal wires. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention discloses an integrated molding process for metal wire electroforming-drawing synergistic composite molding, which combines online electroforming and drawing with multi-pass gradient control, thereby improving the quality and production efficiency of metal composite wires.

[0005] This invention discloses a metal wire electroforming-drawing synergistic composite forming process, which includes the following steps:

[0006] Step 1: Pretreatment of the base metal wire: The base metal wire is cleaned and activated to remove the surface oxide layer, oil and impurities.

[0007] Step 2, Electroforming Layer Deposition: The pretreated base metal wire is fed into an electroforming device, and a metal plating layer is deposited on the surface of the base metal wire using an electroforming process to form the initial electroformed composite wire.

[0008] Step 3: Online radial high-pressure drawing densification: The initial electroformed composite wire obtained in Step 2 is directly fed into the drawing device. Radial compressive stress is applied to the electroformed layer through the drawing die to make the electroformed layer and the base metal wire densely bonded.

[0009] Step 4: Annealing treatment: Anneal the drawn composite wire.

[0010] Step 5, Multi-pass Cooperative Loop: Repeat steps 2 through 4 at least once;

[0011] Step 6: Finished Product Inspection and Cutting: The composite filament is tested for dimensional accuracy, mechanical properties and interlayer bonding strength. After passing the tests, it is cut to obtain the finished product.

[0012] Furthermore, in step two, the electroforming deposition rate is 0.5-5 μm / min, the electroforming solution temperature is 20-60℃, and the current density is 1-10 A / dm³. 2 The pH value of the electroforming solution is 3-8, and the thickness of each electroforming layer is 1-10μm.

[0013] Furthermore, in step three, the radial compressive stress applied by the drawing die is 50-300 MPa, the reduction rate of the drawing pass is 5%-25%, and the radial compressive stress is positively correlated with the electroforming deposition rate. For every 0.5 μm / min increase in the electroforming deposition rate, the radial compressive stress increases by 10-50 MPa.

[0014] Furthermore, in step four, the annealing temperature is 200-1200℃, the holding time is 10-60min, the cooling method is furnace cooling or air cooling, and the cooling rate is 5-20℃ / min, so that an atomic interdiffusion transition layer with a thickness of 0.1-1μm is formed at the interface between the electroformed layer and the base metal wire.

[0015] Furthermore, in step five, the number of cycles is 3-10, and as the number of cycles increases, the electroforming deposition rate gradually decreases, the area reduction rate of the drawing passes gradually decreases, and the annealing temperature gradually increases.

[0016] The final electroforming deposition rate is 0.5-1 μm / min, the drawing pass area reduction rate is 5%-10%, and the annealing temperature is 400-1200℃.

[0017] Furthermore, in step one, the base metal wire is a copper wire, iron wire, tungsten wire, or molybdenum wire with a diameter of 0.1-1 mm;

[0018] Surface cleaning is performed using an alkaline degreasing agent and ultrasonic degreasing, with an ultrasonic power of 100-300W and a time of 5-15 minutes;

[0019] The activation process involves immersing the sample in an acidic activation solution for 1-5 minutes, then rinsing it with deionized water and drying it.

[0020] Furthermore, in step two, the electroforming process is either direct current electroforming or pulse electroforming, with the pulse frequency of pulse electroforming being 100-1000Hz and the duty cycle being 30%-70%.

[0021] The electroformed layer is a composite layer of one or more of nickel, copper, cobalt, and gold, with a total thickness of 1-100 μm.

[0022] Furthermore, in step three, the drawing die is a polycrystalline diamond die with a cone angle of 8°-15° in the working area and a working area length of 5-15mm. Lubricating oil is used for drawing, with a lubricating oil temperature of 20-40℃ and a lubrication pressure of 0.3-1MPa.

[0023] Furthermore, in step six, the finished product inspection includes: dimensional accuracy inspection, with the diameter tolerance of the composite filament being ±0.005-±0.02mm; and mechanical property inspection, with tensile strength ≥800MPa and elongation ≥10%.

[0024] Interlayer adhesion test: The interlayer peel strength in the peel test is ≥15MPa, and there is no coating peeling.

[0025] Furthermore, the electroforming unit and the drawing unit are connected in series online, with the discharge end of the electroforming unit connected to the feed end of the drawing unit, allowing electroforming deposition and radial high-pressure drawing to proceed continuously.

[0026] The beneficial effects of this invention are:

[0027] This invention employs a synergistic online electroforming and drawing process, achieving continuous and seamless operation of electroforming deposition and radial high-pressure drawing. This fundamentally solves the problems of coating oxidation and interface contamination caused by traditional offline processes. The online processing mode allows the electroformed layer to undergo high-pressure drawing directly before cooling and setting. Utilizing the structural design of the polycrystalline diamond mold, continuous and uniform radial compressive stress effectively compacts the electroformed layer, eliminating internal porosity defects and improving the bonding density between the coating and the substrate. This synergistic operation simplifies the production process, reduces surface damage caused by wire transfer and secondary clamping, ensures the continuity of the processing, and optimizes stress application, effectively avoiding coating cracking, peeling, and other defects, thus improving processing stability.

[0028] Multi-pass gradient cyclic processing combined with controlled annealing continuously optimizes the interfacial bonding performance and internal microstructure of the composite filament. With increasing cycle passes, the electroforming deposition rate, drawing area reduction, and annealing temperature are precisely adjusted to meet the coating formation requirements of different processing stages. Annealing effectively eliminates internal processing stress, promoting the formation of a stable atomic interdiffusion transition layer between the electroformed layer and the substrate, improving interlayer bonding strength, and addressing the pain points of weak interfacial bonding and easy coating detachment in traditional processes. The gradient parameter design also avoids substrate deformation and coating damage caused by single-pass processing, allowing the mechanical and interfacial properties of the composite filament to be gradually optimized.

[0029] A precise control of process parameters and a standardized testing system throughout the entire process ensure that the finished composite filaments possess excellent comprehensive performance and dimensional accuracy. The prepared filaments exhibit controllable diameter tolerances, improved tensile strength, elongation, and other mechanical properties, while interlayer bonding meets the stringent standards of high-end applications. This process is adaptable to the composite preparation of various substrates such as copper, iron, tungsten, and molybdenum with various metal coatings, broadening the material's applicability. The continuous production mode simultaneously improves processing efficiency and reduces production losses. The integral molding process breaks through the performance bottlenecks of traditional technologies, and the prepared composite filaments can meet the high-performance requirements of electronic components, aerospace, and precision machinery manufacturing, demonstrating promising prospects for industrial application. Attached Figure Description

[0030] Figure 1 This is a flowchart of a metal wire electroforming-drawing synergistic composite forming process in the embodiments of this application. Detailed Implementation

[0031] To enable those skilled in the art to better understand the present invention, the technical solutions in the specific embodiments of the present invention will be clearly and completely described below.

[0032] This invention discloses a metal wire electroforming-drawing synergistic composite forming process, which includes the following steps:

[0033] Step 1: Pretreatment of the base metal wire: The base metal wire is cleaned and activated to remove the surface oxide layer, oil and impurities.

[0034] Step 2, Electroforming Layer Deposition: The pretreated base metal wire is fed into an electroforming device, and a metal plating layer is deposited on the surface of the base metal wire using an electroforming process to form the initial electroformed composite wire.

[0035] Step 3: Online radial high-pressure drawing densification: The initial electroformed composite wire obtained in Step 2 is directly fed into the drawing device. Radial compressive stress is applied to the electroformed layer through the drawing die to make the electroformed layer and the base metal wire densely bonded.

[0036] Step 4: Annealing treatment: Anneal the drawn composite wire.

[0037] Step 5, Multi-pass Cooperative Loop: Repeat steps 2 through 4 at least once;

[0038] Step 6: Finished Product Inspection and Cutting: The composite filament is tested for dimensional accuracy, mechanical properties and interlayer bonding strength. After passing the tests, it is cut to obtain the finished product.

[0039] The base metal wire is subjected to pretreatment, electroforming layer deposition, online radial high-pressure drawing densification, annealing, multi-pass synergistic cycling, and finished product inspection and cutting operations in sequence to complete the electroforming-drawing synergistic composite forming of the metal wire. First, the base metal wire undergoes surface cleaning and activation treatment. Ultrasonic degreasing removes surface oil and impurities, followed by immersion in an acidic activation solution to remove the oxide layer, ensuring surface cleanliness and activity. The pretreated base metal wire is then fed into an electroforming device, where a metal plating layer is deposited on its surface using DC electroforming or pulse electroforming processes. By controlling parameters such as the electroforming deposition rate, electroforming solution temperature, and current density, a uniformly thick initial electroformed composite wire is formed. The initial electroformed composite wire is then directly fed into a drawing device connected to the electroforming device. A polycrystalline diamond drawing die applies radial compressive stress to the electroformed layer, achieving a dense bond between the electroformed layer and the base metal wire. Subsequently, the drawn composite wire is sent to an annealing furnace, where the annealing temperature, holding time, and cooling rate are controlled to complete the annealing process, forming an atomic interdiffusion transition layer at the interface between the electroformed layer and the base metal wire.

[0040] After completing a single electroforming, drawing, and annealing process, the composite wire undergoes a multi-pass coordinated cycle, repeatedly performing electroforming layer deposition, online radial high-pressure drawing for densification, and annealing. The number of cycles is set according to the performance of the composite wire and the required coating thickness. During the cycle, process parameters are gradually adjusted: the electroforming deposition rate gradually decreases with each cycle, the reduction rate of the drawing pass gradually decreases, and the annealing temperature gradually increases. The electroforming deposition rate, the reduction rate of the drawing pass, and the annealing temperature of the final pass are all controlled within a reasonable range. After the multi-pass coordinated cycle is completed, the composite wire undergoes comprehensive finished product inspection, sequentially testing dimensional accuracy, mechanical properties, and interlayer bonding strength. Once all indicators meet the standards, the composite wire is cut to obtain the finished metal composite wire.

[0041] This process employs a coordinated online electroforming and drawing operation, enabling continuous operation of electroforming layer deposition and radial high-pressure drawing. This effectively avoids problems such as coating oxidation and interface contamination caused by offline operations, resulting in a tighter bond between the electroformed layer and the base metal wire. Simultaneously, radial high-pressure drawing effectively compacts the electroformed layer, eliminating internal porosity defects and improving the density of the composite wire. The multi-pass gradient cyclic process design, combined with the atomic interdiffusion transition layer formed by annealing, continuously optimizes the interfacial bonding performance of the composite wire, improves interlayer peel strength, and prevents coating peeling and cracking. Full-process parameter control and standardized finished product inspection ensure the dimensional accuracy of the composite wire, improve tensile strength, elongation, and other mechanical properties, and make the various performance indicators of the finished composite wire more stable, meeting the actual application requirements of high-performance metal wires. Furthermore, the continuous process layout improves the production efficiency of metal composite wires and reduces performance losses during production.

[0042] The polycrystalline diamond drawing die used in this process is the component that realizes radial compressive stress. Its working area is designed with a gradually tapered angle structure of 8°-15° and a working area length of 5-15mm. When the initial electroformed composite wire enters from the large-diameter end of the die and exits from the small-diameter end, the gradual contraction of the tapered angle will form a continuous extrusion effect on the electroformed layer on the surface of the wire, rather than a sudden pressure impact. The sizing zone of the die further ensures that the extrusive stress is evenly distributed in the circumferential direction of the wire, avoiding excessive or insufficient pressure in local areas, thus ensuring the uniformity of radial compressive stress from a structural perspective. At the same time, the die is made of polycrystalline diamond, which has the characteristics of high hardness and high wear resistance. It will not deform during continuous drawing and can stably maintain the magnitude and mode of action of the extrusive stress, providing structural protection for the continuous extrusive stress.

[0043] The online series connection design of the electroforming and drawing devices, combined with the continuous traction wire feeding system, is key to achieving continuous application of compressive stress. The initial composite wire after pretreatment and electroforming does not require offline transfer; it is directly fed into the drawing die at a uniform speed by the traction device. The traction speed is matched with the electroforming output speed and die specifications, ensuring the composite wire is always in a continuous state of forward movement and compression. The drawing process is uninterrupted and without jamming, resulting in continuous radial compressive stress on the electroformed layer throughout the entire process, creating a sustained compressive stress effect.

[0044] The lubrication measures and drawing parameter design in the process enhance the uniformity of radial compressive stress. During drawing, lubricating oil at 20-40℃ is used, and a lubrication pressure of 0.3-1MPa is applied. The high-pressure lubricating oil forms a uniform lubricating film between the composite wire and the inner wall of the die. This reduces the frictional resistance between the wire and the die, avoiding localized stress concentration caused by uneven friction, and allows the wire to maintain a centered forward movement within the die, ensuring consistent compressive stress on the electroformed layer at all circumferential positions. Simultaneously, the patent specifies a 5%-25% reduction in surface area per drawing pass, and a quantitative matching rule between radial compressive stress and electroforming deposition rate. This ensures that the magnitude of the compressive stress is compatible with the thickness and density of the electroformed layer, preventing cracking due to excessive pressure or insufficient densification due to insufficient pressure, thus guaranteeing the stability and uniformity of the compressive stress effect.

[0045] From the structural design of the mold to provide a foundation for uniform stress, to the continuous traction system connected in series to achieve continuous stress application, and then to the matching of lubrication methods and process parameters to eliminate stress concentration, the three work together to ultimately achieve the application of radial compressive stress on the electroformed layer by the drawing die, so that the electroformed layer is fully compacted and achieves a dense bond with the base metal wire.

[0046] The radial contact pressure of the die refers to the compressive stress perpendicular to the axial direction of the wire, applied by the working area of ​​the polycrystalline diamond die to the electroformed deposited layer on the wire surface during the drawing process, with its direction pointing towards the central axis of the wire. This pressure is generated when the wire passes through the conical working area of ​​the die. Because the die aperture is smaller than the outer diameter of the wire, the wire is forced to undergo plastic deformation under the action of traction force, and the inner wall of the die forms a uniform radial extrusion effect on the wire surface. The effect of this pressure is to close the pores inside the electroformed layer, refine and break the grains, and at the same time promote mechanical interlocking and atomic diffusion at the interface between the electroformed layer and the matrix, thereby achieving a dense metallurgical bond between the two. The 50-300MPa pressure range mentioned in this application is obtained by installing a high-precision tension sensor at the front end of the drawing traction device to measure the traction force in real time during the drawing process, and combining it with the die geometric parameters and material deformation resistance, and then calculating it by back-calculation using a mechanical model. During measurement, the average value of multiple consecutive data points under stable drawing conditions is taken, and the frictional resistance calibrated by the no-load drawing test is subtracted to ensure that the measurement results accurately reflect the actual radial contact pressure of the die on the wire.

[0047] In one implementation method, in step two, the electroforming deposition rate is 0.5-5 μm / min, the electroforming solution temperature is 20-60℃, and the current density is 1-10 A / dm³. 2 The pH value of the electroforming solution is 3-8, and the thickness of each electroforming layer is 1-10μm.

[0048] The pretreated base metal wire is continuously fed into the electroforming tank of the electroforming apparatus at a uniform speed, ensuring that the base metal wire is completely immersed in the electroforming solution and serves as the cathode. An anode corresponding to the coating metal material is then provided. Depending on the coating requirements, either direct current electroforming or pulse electroforming processes are selected for the electroforming layer deposition. The cathode current density is adjusted to maintain a stable range of 1-10 A / dm³. 2 Within the specified range, the temperature of the electroforming solution is kept constant at 20-60℃ using a temperature control system, and the pH value of the electroforming solution is controlled at 3-8 using an acid-base regulator. At the same time, the continuous feeding speed of the base metal wire is matched to adjust the electroforming deposition rate to 0.5-5μm / min. By controlling the operation time of a single electroforming pass, a metal coating with a thickness of 1-10μm is deposited on the surface of the base metal wire in each pass, thus completing the initial preparation of the electroformed composite wire.

[0049] During the electroforming process, the electroforming solution is continuously stirred and filtered to ensure a uniform distribution of metal ion concentration, avoiding uneven coating deposition caused by excessively low local concentrations. The pulse electroforming process simultaneously controls the pulse frequency and duty cycle to help maintain the stability of the deposition rate. For different combinations of base metal wire and coating metal, various parameters are flexibly adjusted within the above-mentioned range to adapt the electroforming process to the material characteristics of the base and coating. This ensures that the metal coating deposited in each pass adheres well to the surface of the base metal wire, free from defects such as pinholes, porosity, and peeling, guaranteeing the basic quality of the initial electroformed composite wire.

[0050] The parameter range allows for excellent process adaptability, meeting the deposition requirements of various base metal wires such as copper, iron, tungsten, and molybdenum, as well as different coating metals such as nickel, copper, cobalt, and gold. It is also compatible with multi-pass synergistic cycle process designs. The 1-10μm coating thickness design per pass matches the requirements of subsequent online radial high-pressure drawing, preventing cracking and detachment during drawing due to excessively thick coatings in a single pass. The synergistic control of deposition rate, current density, electroforming solution temperature, and pH effectively improves the density and surface smoothness of the electroformed layer, reducing internal porosity and inclusions. This lays a stable foundation for subsequent drawing densification and improved interfacial adhesion. Furthermore, the reasonable parameter range allows for process controllability, facilitating flexible adjustments based on finished product performance requirements.

[0051] In one implementation method, in step three, the radial compressive stress applied by the drawing die is 50-300 MPa, the reduction rate per drawing pass is 5%-25%, and the radial compressive stress is positively correlated with the electroforming deposition rate. For every 0.5 μm / min increase in the electroforming deposition rate, the radial compressive stress increases by 10-50 MPa, which can be adjusted within a certain range according to the material properties. This positive correlation applies to the same substrate material system, and the specific value can be fine-tuned according to the substrate strength and coating thickness.

[0052] The initial electroformed composite wire, after the electroforming layer deposition is completed, is directly fed from the discharge end of the electroforming unit into the connected drawing device. Utilizing the cone angle and working area structure design of the polycrystalline diamond drawing die, and in conjunction with the traction system adjustment, radial compressive stress is applied to the electroformed layer on the surface of the composite wire. By adjusting the traction force and the die's extrusion parameters, the applied radial compressive stress is controlled within the range of 50-300 MPa. Simultaneously, based on the initial dimensions of the composite wire and the die's sizing band specifications, the processing parameters of the drawing process are rationally adjusted to ensure that the reduction rate per drawing pass is consistently within the range of 5%-25%, achieving targeted densification of the electroformed layer.

[0053] The drawing process parameters are dynamically adjusted in real time in conjunction with the electroforming deposition rate. Before the drawing operation, the relevant parameters are adjusted according to the electroforming deposition rate determined in step two, following a quantitative matching rule. For every 0.5 μm / min increase in the electroforming deposition rate, the radial compressive stress increases by 10-50 MPa. This change is achieved by adjusting the traction power and the extrusion force of the die, ensuring that the magnitude of the radial compressive stress is matched to the deposition thickness and density of the electroformed layer. This guarantees that the electroformed layers formed at different deposition rates are subjected to uniform and appropriate radial extrusion.

[0054] This parameter setting and quantitative matching method ensures that the radial compressive stress closely matches the actual state of the electroformed layer, avoiding insufficient compaction due to insufficient pressure or cracking and deformation of the base metal wire due to excessive pressure, effectively improving the density of the electroformed layer. The 5%-25% reduction in surface area per drawing pass balances densification with dimensional control of the composite wire, reserving reasonable processing space for subsequent multi-pass cycles. The positive correlation between radial compressive stress and electroforming deposition rate is quantitatively designed to adapt to the gradient changes in deposition rate during multiple cycles, ensuring a dense bond between the electroformed layer and the substrate in each pass. This lays a solid foundation for subsequent annealing to form an interdiffusion transition layer, enhancing the interlayer bonding of the composite wire while ensuring the stability of its mechanical properties and dimensional accuracy.

[0055] After electroforming deposition, the wire surface is coated with electroforming solution and reaction products, requiring cleaning and drying before entering the drawing process. The cleaning process employs a three-stage countercurrent rinsing method: the first stage is deionized water spray cleaning, the second stage is deionized water ultrasonic cleaning, and the third stage is anhydrous ethanol immersion cleaning, with each stage lasting 30 to 60 seconds. After cleaning, the residual electroforming solution on the wire surface is less than 10 mg / m². The drying process uses a combination of hot air drying and infrared radiation drying. The hot air temperature is 80 to 120 degrees Celsius, the air velocity is 5 to 10 m / s, and the drying time is 1 to 3 minutes. Subsequently, the wire passes through an infrared radiation drying zone with an infrared power density of 0.5 to 1 watt per square centimeter for 30 to 60 seconds. After drying, the wire surface temperature is controlled at 40 to 60 degrees Celsius, and the surface moisture content is less than 0.1%. The cleaned and dried wire is immediately fed into the drawing die, with the time interval from drying completion to entry into the drawing die not exceeding 30 seconds to avoid oxidation or contamination of the coating surface. The cleaning and drying unit is connected in series with the electroforming unit and the drawing unit online to achieve continuous production.

[0056] In one implementation method, in step four, the annealing temperature is 200-1200℃, the holding time is 10-60min, the cooling method is furnace cooling or air cooling, and the cooling rate is 5-20℃ / min, so that an atomic interdiffusion transition layer with a thickness of 0.1-1μm is formed at the interface between the electroformed layer and the base metal wire.

[0057] The composite wire, after online radial high-pressure drawing, is fed into an annealing furnace. Based on the characteristics of the matrix and coating materials, the annealing temperature is controlled within the range of 200-1200℃ using the furnace temperature control system. A corresponding holding time is also set, allowing the composite wire to be held at this temperature for 10-60 minutes, providing sufficient time and temperature for atomic diffusion at the interface between the electroformed layer and the base metal wire. After holding, the cooling method—furnace cooling or air cooling—is selected according to process requirements. By adjusting the furnace cooling rate or controlling the air cooling environment, the cooling rate of the composite wire is stabilized at 5-20℃ / min, gradually completing the cooling process. This allows for sufficient atomic diffusion and fusion at the interface between the electroformed layer and the matrix, forming an atomically interdiffused transition layer with a thickness in the range of 0.1-1μm.

[0058] During the annealing process, specific process parameters are adjusted according to the changes in the number of passes in the multi-pass coordinated cycle. The annealing temperature is gradually increased with the increase of the number of passes, while the corresponding holding time and cooling rate are matched to ensure that the degree of atomic diffusion at the interface is adapted to the state of the composite wire after the previous electroforming and drawing processes. A stable heating environment is maintained in the annealing furnace to avoid uneven atomic diffusion caused by local temperature fluctuations, ensuring that the thickness of the interface transition layer in the circumferential direction of the composite wire is consistent, without any local thinning or thickening, thus guaranteeing the uniformity and stability of the interface bonding.

[0059] The parameter range design of this annealing process exhibits excellent process adaptability, meeting the atomic diffusion requirements of different substrates and coating metals, and adapting to the process rhythm of multi-pass synergistic cycles. Reasonable annealing temperature and holding time provide suitable thermodynamic conditions for interfacial atomic diffusion, promoting the formation of a stable interdiffusion transition layer, fundamentally improving the interlayer adhesion between the electroformed layer and the substrate, and preventing coating peeling during subsequent use. Controllable cooling rates and suitable cooling methods effectively reduce the internal stress generated in the composite wire during annealing, preventing deformation and cracking, and ensuring the dimensional accuracy and mechanical properties of the composite wire. Simultaneously, the 0.1-1μm interfacial transition layer thickness design ensures tight interlayer bonding without compromising the overall performance of the composite wire due to excessive transition layer thickness, resulting in superior overall performance of the finished composite wire.

[0060] The thickness of the interdiffusion transition layer described in this invention is characterized using scanning electron microscopy (SEM) combined with energy dispersive spectroscopy (EDS). The specific method involves axially slicing the composite filament sample, embedding and solidifying it, and then preparing a cross-sectional sample using an ion thinning instrument after grinding and polishing. The SEM operating voltage is set to 15-20 kV, and the beam current intensity is 1-2 nanoamps. EDS is performed in line scan mode, acquiring elemental composition data every 50 nanometers from the substrate material towards the coating. The transition layer thickness is defined as the width of the region where the mass fractions of both the substrate and coating elements are between 10% and 90%. For transition layers less than 0.5 micrometers thick, transmission electron microscopy (TEM) is used for supplementary verification. The TEM operating voltage is 200 kV, and high-resolution imaging is used to observe lattice structure changes. Elemental diffusion distribution is analyzed using electron energy loss spectroscopy. The two detection methods corroborate each other, ensuring that the measurement accuracy of the transition layer thickness reaches ±0.05 micrometers.

[0061] In one implementation, in step five, the number of cycles is 3-10, and as the number of cycles increases, the electroforming deposition rate gradually decreases, the reduction rate of the drawing pass gradually decreases, and the annealing temperature gradually increases.

[0062] The final electroforming deposition rate is 0.5-1 μm / min, the drawing pass area reduction rate is 5%-10%, and the annealing temperature is 400-1200℃.

[0063] After completing a single electroforming layer deposition, online radial high-pressure drawing densification, and annealing, based on the total coating thickness requirements and finished product performance standards of the composite wire, 3 to 10 coordinated cycle operations are set, repeating steps two through four. During each cycle, various process parameters are gradually adjusted with the increase in the number of cycles. The electroforming deposition rate is reduced according to a preset gradient, the drawing pass area reduction rate is simultaneously reduced according to a gradient, and the annealing temperature is increased according to a gradient. This ensures that the process parameters for each pass are adapted to the current coating state and interfacial bonding of the composite wire, achieving gradual optimization of the composite wire's performance.

[0064] In the final pass of the multi-pass synergistic cycle, process parameters are adjusted to a preset range, stabilizing the electroforming deposition rate at 0.5 to 1 μm / min, adjusting the area reduction rate of the drawing pass to 5 to 10%, and increasing the annealing temperature to 400 to 1200℃. The parameters for this final pass remain stable throughout the process, ensuring a thin and uniform electroforming layer, a gentle densification process during drawing, and sufficient interfacial atomic diffusion during annealing, thus finalizing the properties of the composite wire.

[0065] This process design achieves gradual accumulation of composite filament coating thickness through 3 to 10 synergistic cycles, meeting the total coating thickness requirements from 1 to 100 μm. Furthermore, by adjusting parameters in a gradient manner, it avoids problems such as coating cracking and substrate deformation caused by high-rate deposition and large area reduction during single-pass drawing, ensuring a dense bond between the electroformed layer and the substrate in each pass. The low deposition rate and small area reduction in the final pass effectively improve the surface smoothness and dimensional accuracy of the composite filament, while the high annealing temperature promotes full interdiffusion of interfacial atoms, further thickening and stabilizing the interdiffusion transition layer and enhancing interlayer bonding. The overall gradient cycling process gradually optimizes the mechanical properties and interfacial bonding performance of the composite filament with each cycle, ultimately ensuring that all indicators of the finished product meet high-performance requirements, with better process stability and repeatability.

[0066] In one embodiment, in step one, the base metal wire is a copper wire, iron wire, tungsten wire, or molybdenum wire with a diameter of 0.1-1 mm;

[0067] Surface cleaning is performed using an alkaline degreasing agent and ultrasonic degreasing, with an ultrasonic power of 100-300W and a time of 5-15 minutes;

[0068] The activation process involves immersing the sample in an acidic activation solution for 1-5 minutes, then rinsing it with deionized water and drying it.

[0069] First, based on the performance requirements of the finished composite filament, copper wire, iron wire, tungsten wire, or molybdenum wire is selected as the base metal wire, and the diameter of the base metal wire is controlled within the range of 0.1 to 1 mm. After determining the suitable base material and specifications, subsequent pretreatment operations are carried out. Then, a surface cleaning operation is performed. The base metal wire is placed in an ultrasonic cleaning device containing an alkaline degreasing agent. The equipment parameters are adjusted to stabilize the ultrasonic power at 100 to 300 W. The cavitation effect of ultrasonic vibration is used to degrease the base metal wire. The degreasing time is controlled at 5 to 15 minutes to fully remove oil, dust, and various impurities adhering to the surface of the base metal wire.

[0070] After surface degreasing, the base metal wire is removed and immersed in an acidic activation solution for activation. The immersion time is strictly controlled between 1 and 5 minutes. The acidic activation solution removes the oxide layer on the surface of the base metal wire, fully exposing the fresh metal surface of the base. After immersion and activation, the base metal wire is immediately rinsed repeatedly with deionized water to thoroughly remove any residual acidic activation solution. Then, the base metal wire is thoroughly dried by blowing air to ensure that there is no liquid residue or impurities adhering to the base surface.

[0071] The substrate selection and pretreatment parameter design are adaptable to the substrate requirements of composite filaments in different application scenarios. The diameter range of 0.1 to 1 mm also provides reasonable processing space for subsequent multi-pass electroforming and drawing operations. Controllable power and duration ultrasonic degreasing can efficiently clean the surface while avoiding damage to the substrate, while immersion in an acidic activating solution thoroughly removes the oxide layer and enhances the surface activity of the substrate. Subsequent deionized water rinsing and drying operations prevent secondary contamination and corrosion caused by residual solutions, keeping the substrate surface clean and activated. This lays a crucial foundation for the uniform deposition and tight bonding of the subsequent electroformed layer, effectively avoiding defects such as peeling and poor bonding of the electroformed layer caused by substrate surface problems.

[0072] In one implementation, in step two, the electroforming process is direct current electroforming or pulse electroforming, with the pulse frequency of pulse electroforming being 100-1000Hz and the duty cycle being 30%-70%.

[0073] The electroformed layer is a composite layer of one or more of nickel, copper, cobalt, and gold, with a total thickness of 1-100 μm.

[0074] When performing electroforming layer deposition, either DC electroforming or pulse electroforming processes are selected based on the material characteristics of the base metal wire and the performance requirements of the finished composite wire. When using DC electroforming, a DC power supply system directly provides a stable current to the electroforming device to complete the coating deposition. When using pulse electroforming, the pulse frequency and duty cycle are adjusted by the pulse power supply, stabilizing the pulse frequency between 100 and 1000 Hz and controlling the duty cycle between 30 and 70%, achieving coating deposition through pulsed current output. Simultaneously, depending on the application requirements, a single metal or a combination of metals from nickel, copper, cobalt, and gold is selected to deposit a single-layer or composite electroformed layer on the surface of the base metal wire. By adjusting the electroforming operation parameters for multiple cycles, such as controlling the total thickness through the number of cycles and the thickness of each pass, the total thickness of the electroformed composite layer can be controlled within the range of 1 to 100 μm.

[0075] To address different metal coating requirements, corresponding electroforming deposition methods are employed to prepare composite layers. Multiple metal composite layers can be achieved through stepwise or co-deposition, ensuring tight bonding between different metal layers and uniform overall coating thickness. During pulse electroforming, the pulse frequency and duty cycle are continuously monitored and fine-tuned to avoid uneven coating deposition caused by parameter fluctuations. DC electroforming maintains stable current output to ensure coating density. Combining a multi-pass synergistic cycle process design, the deposition thickness of each electroformed layer is controlled, and after multiple cycles, the total electroformed layer thickness reaches a preset range of 1 to 100 μm. This process is coordinated with parameters such as electroforming deposition rate and current density throughout.

[0076] This process design allows for highly flexible selection of electroforming methods and coating materials, adapting to the performance requirements of composite wires in various applications. DC electroforming enables efficient coating deposition, improving production efficiency, while pulse electroforming, by controlling the frequency and duty cycle, effectively refines the coating grains, improving the density and surface smoothness of the electroformed layer and reducing internal defects. Single or composite coatings of nickel, copper, cobalt, and gold can impart different properties to the composite wire, such as wear resistance, conductivity, and corrosion resistance, meeting diverse application needs. A total composite layer thickness range of 1 to 100 μm, matched with a multi-pass synergistic cycle process rhythm, avoids the problems of loose coating and weak bonding caused by excessively thick single-pass deposition. Simultaneously, a reasonable thickness range allows for better composite effects between the electroformed layer and the base metal wire, laying a good foundation for subsequent drawing densification and annealing treatments, and improving the overall mechanical and performance properties of the finished composite wire.

[0077] In one implementation method, in step three, the drawing die is a polycrystalline diamond die with a cone angle of 8°-15° in the working area and a working area length of 5-15mm. Lubricating oil is used for drawing, with a lubricating oil temperature of 20-40℃ and a lubrication pressure of 0.3-1MPa.

[0078] When performing online radial high-pressure drawing densification, polycrystalline diamond drawing dies are selected as the processing components. The structural parameters of the die are strictly controlled, with the cone angle of the working area controlled between 8 and 15° and the length of the working area adjusted between 5 and 15 mm to ensure that the die structure is compatible with the drawing process requirements. During the drawing process, lubricating oil is continuously supplied to the working area of ​​the die. The temperature of the lubricating oil is stabilized between 20 and 40°C using a temperature control device, while the supply pressure of the lubricating oil is controlled using a pressure regulating component, maintaining it between 0.3 and 1 MPa. This ensures that the lubricating oil fully covers the contact area between the die and the wire as the composite wire advances, completing the lubrication preparation and parameter control before drawing.

[0079] The initial composite wire, after electroforming, is directly fed from the electroforming device into a polycrystalline diamond drawing die. The wire advances at a uniform speed along the cone angle of the die's working area. The die's structural parameters are coordinated with the drawing speed to achieve stable application of radial compressive stress to the electroformed layer. Based on the specifications of the base metal wire, the thickness and density of the electroformed layer, the cone angle and length of the die's working area are flexibly adjusted within a preset parameter range. Simultaneously, the temperature and pressure of the lubricating oil are adjusted to ensure a high degree of synchronization between lubrication and the drawing rhythm. This prevents drawing failures caused by insufficient lubrication or parameter mismatch, ensuring a continuous and stable drawing process.

[0080] Polycrystalline diamond (PCD) material possesses high hardness and wear resistance, maintaining the structural precision of the die over a long period. This prevents die deformation during drawing from affecting the uniformity of compressive stress. The combination of an 8-15° working zone cone angle and a 5-15mm working zone length allows for a gradual application of radial compressive stress, effectively preventing stress concentration and cracking of the electroplated layer. A lubricating oil temperature of 20-40°C and a lubrication pressure of 0.3-1MPa, in conjunction with these parameters, forms a uniform lubricating film between the wire and the die's inner wall, reducing drawing friction resistance and preventing scratches or peeling of the plating. Simultaneously, a stable supply of lubricating oil cools the die's working area, reducing high-temperature wear. The overall die and lubrication parameter design ensures that the electroplated layer is fully compacted and densely bonded to the substrate, while also improving the stability and repeatability of the drawing process, extending die life, and reducing production losses.

[0081] As one implementation method, step six includes finished product inspection: dimensional accuracy inspection, with the diameter tolerance of the composite filament being ±0.005-±0.02mm; and mechanical property inspection, with tensile strength ≥800MPa and elongation ≥10%.

[0082] Interlayer adhesion test: The interlayer peel strength in the peel test is ≥15MPa, and there is no coating peeling.

[0083] After undergoing multiple rounds of coordinated cycling, the composite filament enters the finished product inspection stage, where dimensional accuracy testing, mechanical property testing, and interlayer bonding strength testing are carried out sequentially. For dimensional accuracy testing, a laser diameter gauge is used to measure the diameter of the composite filament, strictly controlling the diameter tolerance within the range of ±0.005 to ±0.02 mm. For mechanical property testing, an electronic universal testing machine is used to perform tensile tests on the composite filament, determining its tensile strength and elongation, ensuring that the finished product's tensile strength is not less than 800 MPa and the elongation is not less than 10%. For interlayer bonding strength testing, a coating peel strength tester is used to conduct peel tests, recording the interlayer peel strength while observing the coating condition. The peel strength is required to be not less than 15 MPa, and there should be no coating peeling off the surface of the composite filament.

[0084] During the testing process, standardized testing procedures were followed, and multi-point, multi-segment dimensional accuracy checks were performed on the composite filaments to avoid local dimensional deviations affecting the overall judgment and to ensure that the diameter of the filaments was uniform and met the standards throughout. Mechanical property testing involved strict control of test conditions throughout to ensure the accuracy and reference value of the test data, accurately reflecting the actual mechanical properties of the composite filaments. In the interlayer bonding strength test, not only was the peel strength value judged, but the presence of potential defects such as localized peeling or flaking of the coating was also visually inspected. Composite filaments failing to meet any of the standards were rejected. Only composite filaments meeting all test standards were sent to the cutting process and cut to the preset specifications to obtain the finished product.

[0085] The testing indicators and methods for this finished product comprehensively control the quality of the composite wire from three dimensions: size, mechanical properties, and interlayer bonding effect. Strict diameter tolerances ensure the dimensional accuracy of the finished product, meeting the specifications required for high-precision industrial applications. Tensile strength and elongation performance requirements ensure the composite wire possesses excellent mechanical properties, enhancing its structural stability and resistance to deformation during use. Limitations on interlayer peel strength and visual inspection of the coating state provide dual protection for the tight bonding between the electroformed layer and the base metal wire, fundamentally preventing coating peeling and failure during subsequent use. Simultaneously, standardized testing and defective product rejection processes effectively improve the yield rate, ensuring that the prepared composite wire meets the standards for high-performance metal wires, adapting to diverse application needs.

[0086] In one implementation, the electroforming device and the drawing device are connected in series online, with the discharge end of the electroforming device connected to the feed end of the drawing device, so that electroforming deposition and radial high-pressure drawing can be carried out continuously.

[0087] An integrated online series layout is adopted for the electroforming and drawing devices. The wire feeding stations of the two devices are calibrated to ensure that their central axes remain coaxial. The discharge end of the electroforming device and the feed end of the drawing device are directly connected. A gapless transition conveyor structure is set at the connection point, eliminating the intermediate offline transfer link in the traditional process, thus forming a continuous metal wire processing production line. At the same time, a unified continuous traction wire feeding system is provided for the series-connected devices, allowing the initial electroformed composite wire after electroforming layer deposition to directly enter the transition conveyor structure from the discharge end of the electroforming device and be smoothly and uninterruptedly fed into the feed end of the drawing device, realizing the continuous operation of electroforming deposition and radial high-pressure drawing processes.

[0088] The electroforming and drawing units, connected in series, share a single traction wire feeding system. This system's wire feeding speed is dynamically adjusted in real-time in conjunction with the electroforming deposition rate and various drawing parameters, ensuring the composite wire moves at a constant speed without interruption or jamming within both units. This allows for a high degree of synchronization between the electroforming layer deposition and radial high-pressure drawing operations. Auxiliary guide components are installed at the transition conveyor structure to maintain the composite wire's conveying posture, preventing processing deviations caused by wire offset. Furthermore, the discharge end of the electroforming unit is positioned flush with the die inlet of the drawing unit, ensuring that the composite wire immediately enters the drawing die for radial high-pressure drawing upon completion of the electroforming layer deposition, truly achieving seamless integration of the two processes.

[0089] Connecting the electroforming and drawing devices in series online allows composite wires to directly enter the drawing process after electroforming layer deposition without offline transport. This effectively avoids oxidation and impurity contamination on the electroformed layer surface during offline placement, ensuring interface cleanliness between the electroformed layer and the base metal wire from the source and improving subsequent bonding. Simultaneously, subjecting the electroformed layer to radial high-pressure drawing before cooling and structural stabilization results in better densification, more easily eliminating internal porosity defects and achieving a tighter bond between the electroformed layer and the base. Furthermore, the simultaneous and continuous operation of the processes shortens the overall processing time, improves the production efficiency of metal composite wires, and the integrated series layout allows for a more compact production space, reducing secondary clamping and transport of the wires and avoiding surface damage and dimensional deviations during transport, thus ensuring the stability of the composite wire processing quality.

[0090] Example

[0091] Example 1: Copper-based nickel electroformed composite wire

[0092] Step 1: Pretreatment of the base metal wire

[0093] Pure copper wire with a diameter of 0.3mm was selected as the substrate. A CNC ultrasonic cleaner was used to clean its surface. An alkaline degreasing agent was added, and the ultrasonic power was set to 200W. The ultrasonic degreasing was performed for 10 minutes to remove surface oil, dust and impurities. Then, it was soaked in an acidic activating solution for 3 minutes to remove the surface oxide layer. After soaking, it was rinsed with deionized water and dried to ensure that the substrate surface was free of oil, oxide layer and residual impurities.

[0094] Step 2: Electroforming layer deposition

[0095] Pretreated pure copper wire is fed into a continuous electroforming production line, where a nickel electroforming layer is deposited on the surface of the copper wire using a DC electroforming process. The process parameters are controlled as follows: electroforming deposition rate 2 μm / min, electroforming solution temperature 40℃, and current density 5 A / dm³. 2 The electroforming solution has a pH of 5.5, and the single-pass electroforming layer thickness is 5μm. After deposition, the initial electroformed composite wire is obtained.

[0096] Step 3: Online radial high-pressure drawing densification

[0097] The initial electroformed composite wire obtained in step two is directly fed into the drawing unit of the online electroforming-drawing tandem device to achieve online collaborative operation of electroforming and drawing. Polycrystalline diamond drawing dies are used for drawing, with a cone angle of 10° and a working area length of 10mm. The radial compressive stress applied during the drawing process is 120MPa (matching the electroforming deposition rate), and the reduction rate of the drawing pass is 15%. Lubricating oil is used during drawing, with a lubricating oil temperature of 20-40℃ and a lubrication pressure of 0.6MPa. Through the radial high pressure, the loose nickel electroformed layer is compacted and densely bonded to the copper matrix.

[0098] Step 4: Annealing

[0099] The drawn composite wire was sent into a box annealing furnace for annealing treatment at a temperature of 350℃ and a holding time of 30 min. The cooling method was air cooling at a rate of 12℃ / min, which formed an atomic interdiffusion transition layer with a thickness of 0.5μm at the interface between the nickel electroplated layer and the copper substrate, further enhancing the interlayer bonding force.

[0100] Step 5: Multi-pass Cooperative Loop

[0101] Repeat steps two through four for a total of five cycles. As the number of cycles increases, the electroforming deposition rate gradually decreases, the reduction rate of the drawing pass gradually decreases, and the annealing temperature gradually increases. The electroforming deposition rate of the last pass is 0.8 μm / min, the reduction rate of the drawing pass is 8%, and the annealing temperature is 450℃, ensuring that the performance of the composite wire is gradually optimized.

[0102] Step Six: Finished Product Inspection and Cutting

[0103] The dimensional accuracy of the composite wire was tested using a laser diameter gauge, the mechanical properties were tested using an electronic universal testing machine, the interlayer bonding strength was tested using a coating peel strength tester, and the thickness and elemental distribution of the interface transition layer were observed using a scanning electron microscope (SEM) combined with an energy dispersive spectroscopy (EDS). After passing the tests, the copper-based nickel electroformed composite wire was cut into finished products.

[0104] Example 2: Tungsten-based copper electroformed composite wire

[0105] Step 1: Pretreatment of the base metal wire. The base metal wire is 0.1mm diameter tungsten wire; the base metal wire is ultrasonically degreased with an alkaline degreasing agent at a power of 100W for 5 minutes; the base metal wire is soaked in an acidic activating solution for 1 minute, then rinsed and dried.

[0106] Step 2: Electroforming layer deposition was performed using pulsed electroforming (pulse frequency 500Hz, duty cycle 50%); the deposition rate was 0.5μm / min, the electroforming solution temperature was 20℃, and the current density was 1A / dm³. 2 pH value 3, single-pass electroforming layer thickness 1μm, electroforming layer is pure copper layer.

[0107] Step 3: Online radial high-pressure drawing to densify polycrystalline diamond mold (cone angle 8°, working area length 5mm); radial compressive stress 50MPa, surface reduction rate 5%; lubricating oil temperature 20℃, lubrication pressure 0.3MPa.

[0108] Step 4: Annealing treatment. The annealing temperature is 1000℃. During the annealing process, a protective atmosphere is introduced to prevent oxidation. The temperature is held for 10 minutes and then cooled in the furnace at a rate of 5℃ / min. A 0.1μm transition layer is formed at the interface.

[0109] Step 5: Perform three multi-pass synergistic cycles; for the final pass, the electroforming deposition rate is 0.5 μm / min, the surface area reduction is 5%, and the annealing temperature is 900℃. During the annealing process, a protective atmosphere is introduced to prevent oxidation.

[0110] Step Six: Finished Product Inspection and Cutting. After passing the inspection, cut the finished product.

[0111] Example 3: Iron-based copper-nickel composite electroformed wire

[0112] Step 1: Pretreatment of the base metal wire. The base metal wire is selected as 0.5mm diameter iron wire; the alkaline degreasing agent is ultrasonically degreased at 300W for 15 minutes; the base metal wire is soaked in acidic activating solution for 5 minutes, then rinsed and dried.

[0113] Step 2: Electroforming layer deposition using DC electroforming; deposition rate 5 μm / min, electroforming solution temperature 60℃, current density 10 A / dm³ 2 The pH value is 8, the thickness of the single-pass electroforming layer is 10μm, and the electroforming layer is a copper-nickel composite layer.

[0114] Step 3: Online radial high-pressure drawing to densify polycrystalline diamond mold (cone angle 15°, working area length 15mm); radial compressive stress 300MPa (matching deposition rate), area reduction rate 25%; lubricating oil temperature 40℃, lubrication pressure 1MPa.

[0115] Step 4: Annealing treatment. Annealing temperature 550℃, hold for 60 min, air cool at a rate of 20℃ / min, forming a 1μm transition layer at the interface.

[0116] Step 5: Perform 10 cycles of multi-pass synergistic cycling; for the final pass, the electroforming deposition rate is 1 μm / min, the surface area reduction is 10%, and the annealing temperature is 600℃.

[0117] Step Six: Finished Product Inspection and Cutting. After passing the inspection, cut the finished product.

[0118] Example 4: Molybdenum-based cobalt electroformed composite wire

[0119] Step 1: Pretreatment of the base metal wire. The base metal wire is a 0.8mm diameter molybdenum wire; ultrasonic power 250W, degreasing for 12 minutes; soaking in acidic activation solution for 4 minutes, rinsing and drying.

[0120] Step 2: Electroforming layer deposition via pulsed electroforming (frequency 1000Hz, duty cycle 70%); deposition rate 3μm / min, electroforming solution temperature 50℃, current density 7A / dm³ 2 The pH value is 6.5, the thickness of the single-pass electroforming layer is 7μm, and the electroforming layer is a pure cobalt layer.

[0121] Step 3: Online radial high-pressure drawing to densify polycrystalline diamond mold (cone angle 12°, working area length 12mm); radial compressive stress 180MPa, surface reduction rate 20%; lubricating oil temperature 35℃, lubrication pressure 0.8MPa.

[0122] Step 4: Annealing treatment. The annealing temperature is 950℃. During the annealing process, a protective atmosphere is introduced to prevent oxidation. The temperature is held for 40 minutes and then cooled in the furnace at a rate of 15℃ / min. A 0.7μm transition layer is formed at the interface.

[0123] Step 5: Repeat the multi-pass synergistic cycle 7 times; the final pass electroforming deposition rate is 0.9 μm / min, the surface area reduction rate is 9%, the annealing temperature is 1100℃, and a protective atmosphere is introduced during the annealing process to prevent oxidation.

[0124] Step Six: Finished Product Inspection and Cutting. After passing the inspection, cut the finished product.

[0125] Example 5: Copper-based nickel-cobalt composite electroformed wire

[0126] Step 1: Pretreatment of the base metal wire. The base metal wire is a pure copper wire with a diameter of 1mm; ultrasonic power of 150W, degreasing for 8 minutes; soaking in acidic activation solution for 2 minutes, rinsing and drying.

[0127] Step 2: Electroforming layer deposition using DC electroforming; deposition rate 1.5 μm / min, electroforming solution temperature 35℃, current density 4 A / dm³ 2 The pH value is 4.5, the thickness of the single-pass electroforming layer is 4μm, and the electroforming layer is a nickel-cobalt composite layer.

[0128] Step 3: Online radial high-pressure drawing to densify polycrystalline diamond mold (cone angle 9°, working area length 8mm); radial compressive stress 100MPa, surface reduction rate 12%; lubricating oil temperature 25℃, lubrication pressure 0.5MPa.

[0129] Step 4: Annealing treatment. Annealing temperature 300℃, hold for 25 min, air cool at a rate of 10℃ / min, forming a 0.4μm transition layer at the interface.

[0130] Step 5: Perform 4 cycles of multi-pass synergistic cycling; the final pass electroforming deposition rate is 0.7 μm / min, the surface area reduction rate is 7%, and the annealing temperature is 420℃.

[0131] Step Six: Finished Product Inspection and Cutting. After passing the inspection, cut the finished product.

[0132] Comparative Example

[0133] Comparative Example 1: Traditional offline electroforming process (no drawing, no circulation)

[0134] Substrate: 0.3mm pure copper wire, conventionally degreased and activated;

[0135] Electroforming: Pure nickel layer, deposition rate 2μm / min, total thickness 25μm, offline electroforming followed by natural air drying;

[0136] Post-processing: No pulling, no multi-pass cycles, no matched annealing;

[0137] Finished product: Directly cut and inspected.

[0138] Comparative Example 2: Single Drawing Process

[0139] Substrate: 0.3mm pure copper wire, standard pretreatment;

[0140] Process: Only a 15% reduction in surface area per single drawing pass, without electroforming, online coordination, or cyclic annealing;

[0141] Finished product: Directly cut and inspected.

[0142] Comparative Example 3: Electroforming and Offline Drawing Processes

[0143] Substrate: 0.3mm pure copper wire, standard pretreatment;

[0144] Electroforming: Pure nickel layer, total thickness 25μm, placed for 24 hours after offline electroforming;

[0145] Pulling: Offline ordinary pulling, without radial high-pressure matching, without multi-pass cycles;

[0146] Annealing: Anneal at a single temperature of 350℃ for 30 minutes, without gradient temperature increase;

[0147] Finished product: Directly cut and inspected.

[0148] Performance testing methods

[0149] Dimensional accuracy inspection: In accordance with GB / T4909-2021 "Measurement of diameter, cross-sectional area and weight of steel wire", a laser diameter gauge is used to measure the diameter of the composite wire and the diameter tolerance is recorded.

[0150] Mechanical property testing: In accordance with GB / T228.1-2021 "Metallic materials - Tensile testing - Part 1: Test method at room temperature", tensile strength, yield strength and elongation were tested using an electronic universal testing machine.

[0151] Interlayer adhesion test: According to GB / T5270-2005 "Test method for adhesion of metal coatings on metal substrate", a coating peel strength tester was used to conduct peel test, record peel strength, and observe whether the coating peels off.

[0152] Interface transition layer detection: The thickness of the atomic interdiffusion transition layer at the interface between the electroformed layer and the substrate metal wire was observed using scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS).

[0153] The performance test results are shown in Table 1 below.

[0154]

[0155] Table 1

[0156] The composite metal wire prepared by the electroforming-drawing synergistic composite forming process of this invention has far superior dimensional accuracy, tensile strength, elongation, and interlayer bonding force compared to existing traditional processes. The coating is tightly bonded to the substrate without peeling off, and a stable atomic interdiffusion transition layer is formed at the interface, which meets the requirements for high-performance metal wires.

[0157] It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A metal wire electroforming-drawing synergistic composite forming process, characterized in that, Includes the following steps: Step 1: Pretreatment of the base metal wire: The base metal wire is cleaned and activated to remove the surface oxide layer, oil and impurities. Step 2, Electroforming Layer Deposition: The pretreated base metal wire is fed into an electroforming device, and a metal plating layer is deposited on the surface of the base metal wire using an electroforming process to form the initial electroformed composite wire. Step 3: Online radial high-pressure drawing densification: The initial electroformed composite wire obtained in Step 2 is directly fed into the drawing device. Radial compressive stress is applied to the electroformed layer through the drawing die to make the electroformed layer and the base metal wire densely bonded. Step 4: Annealing treatment: Anneal the drawn composite wire. Step 5, Multi-pass Cooperative Loop: Repeat steps 2 through 4 at least once; Step 6: Finished Product Inspection and Cutting: The composite filament is tested for dimensional accuracy, mechanical properties and interlayer bonding strength. After passing the tests, it is cut to obtain the finished product.

2. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step two, the electroforming deposition rate is 0.5-5 μm / min, the electroforming solution temperature is 20-60℃, and the current density is 1-10 A / dm³. 2 The pH value of the electroforming solution is 3-8, and the thickness of each electroforming layer is 1-10μm.

3. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step three, the radial compressive stress applied by the drawing die is 50-300 MPa, the reduction rate of the drawing pass is 5%-25%, and the radial compressive stress is positively correlated with the electroforming deposition rate. For every 0.5 μm / min increase in the electroforming deposition rate, the radial compressive stress increases by 10-50 MPa.

4. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step four, the annealing temperature is 200-1200℃, the holding time is 10-60min, the cooling method is furnace cooling or air cooling, and the cooling rate is 5-20℃ / min, so that an atomic interdiffusion transition layer with a thickness of 0.1-1μm is formed at the interface between the electroformed layer and the base metal wire.

5. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step five, the number of cycles is 3-10, and as the number of cycles increases, the electroforming deposition rate gradually decreases, the area reduction rate of the drawing pass gradually decreases, and the annealing temperature gradually increases. The final electroforming deposition rate is 0.5-1 μm / min, the drawing pass area reduction rate is 5%-10%, and the annealing temperature is 400-1200℃.

6. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step one, the base metal wire is made of copper, iron, tungsten, or molybdenum, with a diameter of 0.1-1 mm; Surface cleaning is performed using an alkaline degreasing agent and ultrasonic degreasing, with an ultrasonic power of 100-300W and a time of 5-15 minutes; The activation process involves immersing the sample in an acidic activation solution for 1-5 minutes, then rinsing it with deionized water and drying it.

7. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step two, the electroforming process is either direct current electroforming or pulse electroforming. The pulse frequency of pulse electroforming is 100-1000Hz, and the duty cycle is 30%-70%. The electroformed layer is a composite layer of one or more of nickel, copper, cobalt, and gold, with a total thickness of 1-100 μm.

8. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: In step three, the drawing die is a polycrystalline diamond die with a cone angle of 8°-15° in the working area and a working area length of 5-15mm. Lubricating oil is used for drawing, with a lubricating oil temperature of 20-40℃ and a lubrication pressure of 0.3-1MPa.

9. The electroforming-drawing synergistic composite forming process for metal wire according to claim 1, characterized in that: Step six includes finished product inspection: dimensional accuracy inspection, with the diameter tolerance of the composite filament being ±0.005-±0.02mm; and performance inspection, with tensile strength ≥800MPa and elongation ≥10%. Interlayer adhesion test: The interlayer peel strength in the peel test is ≥15MPa, and there is no coating peeling.

10. A metal wire electroforming-drawing synergistic composite forming process according to any one of claims 1 to 9, characterized in that: The electroforming device and the drawing device are connected in series online, with the discharge end of the electroforming device connected to the feed end of the drawing device, so that electroforming deposition and radial high-pressure drawing can be carried out continuously.