A nickel-based chromium carbide powder and a method for producing the same, a coating

Nickel-based chromium carbide powder was prepared by pre-alloying and atomization powdering processes, which solved the problem of instability of chromium carbide in nickel-based alloy powder, improved wear resistance and high-temperature oxidation resistance, and reduced production costs.

CN122400577BActive Publication Date: 2026-11-24CHENGDU DAGUANG NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610818244.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-06-08
Publication Date
2026-11-24
Estimated Expiration
2046-06-08

AI Technical Summary

Technical Problem

When using tungsten carbide as a substitute material in existing nickel-based alloy powders, it is difficult to reduce costs while maintaining wear resistance. Furthermore, chromium carbide is unstable in nickel-containing molten metal, resulting in poor wear resistance of the product.

Method used

Large-particle pre-alloyed powder is prepared by forming a diffusion bond between nickel and chromium carbide at a temperature significantly lower than that of chromium carbide through a pre-alloying process. This powder is then added to the molten metal through an atomization process to form nickel-based chromium carbide powder, which inhibits the dissolution and phase transformation of chromium carbide and maintains its original hard particle morphology.

Benefits of technology

This improves the wear resistance and high-temperature oxidation resistance of nickel-based chromium carbide powder, ensuring the physical properties of the product and the uniformity of the coating, while reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122400577B_ABST
    Figure CN122400577B_ABST
Patent Text Reader

Abstract

This invention relates to the field of alloy powders, addressing the problem of difficulty in ensuring wear resistance when using chromium carbide to replace tungsten carbide. It provides a nickel-based chromium carbide powder, its preparation method, and a coating. A method for preparing nickel-based chromium carbide powder includes the following steps: S100, chromium carbide and nickel are subjected to a sintering process, a cooling process, and a pulverizing process to obtain pre-alloyed particles; S200, the pre-alloyed particles are added to a molten metal and then subjected to an atomization powdering process to obtain nickel-based chromium carbide powder; the molten metal contains nickel. In this invention, nickel and chromium carbide form pre-alloyed large particles through sintering, causing diffusion and metallurgical bonding on the surface of the nickel and chromium carbide particles, forming a nickel-based alloy coating layer. This not only improves the wettability of chromium carbide with the molten metal but also reduces the dissolution, precipitation, and recrystallization processes of chromium carbide, allowing chromium carbide to maintain its original crystal form in the molten metal as much as possible, thereby ensuring the wear resistance of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy powders, and more specifically, to a nickel-based chromium carbide powder, its preparation method, and its coating. Background Technology

[0002] Existing nickel-based alloy powders often increase wear resistance by adding different proportions of tungsten carbide particles. However, with the continuous increase in tungsten carbide prices, it is necessary to find alternative materials to reduce costs. Conventional chromium carbide is difficult to maintain stability in nickel-containing molten metal, exhibiting not only volume growth but also multi-directional crystal transformations, resulting in poor wear resistance and making it difficult to directly replace tungsten carbide in terms of performance.

[0003] There is an urgent need for a process that can replace tungsten carbide with chromium carbide, while ensuring wear resistance and reducing costs. Summary of the Invention

[0004] The purpose of this invention is to provide a nickel-based chromium carbide powder, its preparation method, and coating, thereby solving the problem that it is difficult to ensure wear resistance when using chromium carbide to replace tungsten carbide.

[0005] The embodiments of the present invention are achieved through the following technical solutions:

[0006] A method for preparing nickel-based chromium carbide powder includes the following steps:

[0007] S100, chromium carbide and nickel are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles;

[0008] S200: After the pre-alloyed particles are added to the molten metal, nickel-based chromium carbide powder is obtained through an atomization powdering process.

[0009] The molten metal contains nickel.

[0010] In existing technologies, tungsten carbide can maintain its crystalline form after being immersed in nickel-containing molten metal. However, tungsten carbide is expensive. The applicant hopes to replace tungsten carbide with chromium carbide, which would not only reduce production costs but also improve the product's lifespan in high-temperature environments. After oxidation at high temperatures, chromium carbide forms a dense chromium oxide layer on the product surface, preventing further oxidation. In contrast, tungsten carbide is difficult to oxidize to form a dense layer, thus improving product lifespan.

[0011] After attempting to replace tungsten carbide with chromium carbide, the applicant found that chromium carbide was difficult to stabilize in nickel-containing molten metal. It not only exhibited volume growth but also multi-directional crystal transformations, resulting in poor wear resistance and making it difficult to directly replace tungsten carbide in terms of performance. The applicant hypothesizes that the reason is that tungsten carbide is relatively stable in liquid nickel, typically only undergoing minor dissolution at the edges while maintaining a hard, granular core. However, chromium carbide has an extremely strong chemical affinity for the nickel matrix. During high-temperature melting or sintering, chromium carbide undergoes diffusion reactions with other elements in the liquid nickel phase, such as iron and nickel itself, leading to its easy dissolution and phase transformation, such as from Cr3C2 to Cr7C3 or other complex metallic carbides. This intense chemical activity prevents it from existing as a stable, hard phase like tungsten carbide. During the aforementioned reaction process, the originally singular and regular chromium carbide crystal structure is disrupted, and various new carbides are generated in situ, such as elongated, lath-shaped, blocky, or fishbone-shaped eutectic carbides. The molar volume of the new phase generated by the chemical reaction is larger than that of the original chromium carbide, leading to abnormal volume growth. After the chromium carbide, which serves as the hard phase framework, is reduced or disappears, it is replaced by other carbides with different sizes, morphologies, and hardnesses, resulting in a significant decrease in the wear resistance of the product. The internal stress and microcracks caused by the volume growth process also reduce the mechanical properties of the product.

[0012] In addition, tungsten carbide is generally harder than chromium carbide, so to improve the overall wear resistance of the product, the amount of chromium carbide used needs to be increased.

[0013] To address the aforementioned issues, the applicant devised a pre-alloying technical solution. Nickel and chromium carbide are sintered to form pre-alloyed large particles. This process is not complete melting, but rather carried out at a temperature below the significant melting point of chromium carbide. This allows diffusion and metallurgical bonding between the nickel and chromium carbide particles, forming a nickel-based alloy coating. This not only improves the wettability of chromium carbide with the molten metal but also reduces the dissolution, precipitation, and recrystallization of chromium carbide, allowing it to maintain its original crystal form in the molten metal as much as possible, thus ensuring the wear resistance of the product. Furthermore, pre-alloying suppresses excessive dissolution and harmful phase transformations of chromium carbide in the metal at high concentrations, allowing a large amount of chromium carbide to remain in a stable, original hard particle form, thereby increasing the amount of chromium carbide used.

[0014] Tiny chromium carbide particles have a large specific surface area and high surface energy, making them thermodynamically unstable. They preferentially dissolve into the surrounding high-temperature nickel matrix. However, once the carbon and chromium concentrations in the nickel matrix reach saturation, these elements will re-precipitate on the surface using large chromium carbide particles as nuclei. This leads to a phenomenon where large particles absorb smaller particles, growing larger while the smaller particles gradually disappear. Therefore, larger particles are less prone to dissolution. However, directly using large chromium carbide particles results in a smaller interface between the particles and the nickel matrix, making them susceptible to brittle fracture or peeling off from the coating under external force. Therefore, this invention increases the particle volume when added to the molten metal through pre-alloying, thus suppressing the overall dissolution tendency of the particles.

[0015] The significant difference in composition and chemical potential between untreated chromium carbide and liquid nickel drives rapid dissolution of chromium carbide. During sintering, nickel atoms diffuse to the surface of the chromium carbide particles, while chromium and carbon atoms diffuse into the nickel matrix, forming a diffusion layer with a gradual compositional gradient around the chromium carbide particles. This means the surface of the chromium carbide particles is now coated with a diffusion layer whose composition is closer to that of the liquid nickel. Upon contact with liquid nickel, the compositional gradient between the two decreases, thus significantly reducing the chemical potential gradient driving dissolution and slowing the dissolution rate. Because the amount of dissolution is greatly limited, the number of free chromium and carbon atoms in the liquid phase decreases. Upon cooling, the system no longer has the conditions for large-scale, disordered recrystallization. The original surface state of the chromium carbide particles becomes more stable, preserving their original hard particle morphology to the greatest extent possible, rather than collapsing into a chaotic new phase, thereby ensuring wear resistance.

[0016] The pre-alloyed large particles were not added directly during the molten metal process, but were added into the molten metal during the granulation process, which further reduced the dissolution process of chromium carbide in liquid nickel and improved the wear resistance of the product.

[0017] Atomization powder production is an existing technology that can achieve powder production through gas atomization or water atomization. Its principle is to break molten metal into micron-sized droplets through high-pressure airflow or liquid flow, which are then condensed to form metal or alloy powder.

[0018] Preferably, the average particle size of chromium carbide is 1-5 μm, the average particle size of nickel is 1-3 μm, and the average particle size of the pre-alloyed particles is 15-50 μm.

[0019] To ensure the performance of the final coating, this invention uses finer chromium carbide.

[0020] Preferably, by weight, 70-85 parts of chromium carbide and 15-30 parts of nickel are present.

[0021] An appropriate amount of nickel helps to effectively fill the voids between chromium carbide particles, promoting the formation and growth of sintering necks, thereby obtaining pre-alloyed particles with high density and good strength. Controlling the proportion of nickel helps to control the dissolution of chromium carbide during sintering and its precipitation during cooling, thereby controlling the structure of the pre-alloyed particles and minimizing their dissolution after being added to the molten metal.

[0022] Preferably, the sintering process includes: a first-stage sintering process and a second-stage sintering process;

[0023] The temperature of the first sintering process is 800-1000℃, and the time is 1-2 hours; the temperature of the second sintering process is 1150-1250℃, and the time is 2-3 hours.

[0024] Both the first and second sintering processes are carried out under an inert atmosphere.

[0025] In the first sintering process, nickel powder particles begin to bond through surface diffusion and grain boundary diffusion, and undergo preliminary interfacial reactions and alloying with the surface of chromium carbide particles. Moderate interfacial reactions can pin the chromium carbide particles and inhibit their excessive growth. In the second sintering process, the nickel phase flows plastically, filling the pores, and interdiffusion occurs between the nickel and chromium carbide interfaces, forming a chromium-rich solid solution transition layer.

[0026] An inert atmosphere prevents the oxidation of chromium carbide surfaces, which can lead to the formation of an oxide layer that hinders diffusion and affects the formation of a gradient diffusion layer.

[0027] Preferably, the cooling process includes: rapidly cooling to 600-800°C at a rate of 50-80°C / min, and then cooling to the furnace exit temperature at a rate of 10-20°C / min; the furnace exit temperature is <100°C.

[0028] Let it cool naturally after it comes out of the oven.

[0029] During the pre-alloying process of Cr3C2-Ni, a nickel-based solid solution forms at high temperatures. Chromium atoms dissolve from the chromium carbide particles and diffuse into the nickel binder phase. If the cooling rate is too slow, chromium atoms have sufficient time to precipitate from the supersaturated nickel solid solution. Therefore, this invention employs rapid cooling to an extremely low atomic diffusion rate followed by slow cooling. Rapid cooling leaves significant thermal stress within the material, necessitating slow cooling to allow sufficient time for stress relaxation. This ensures that chromium does not precipitate excessively, thereby achieving dimensional stability and structural integrity of the workpiece.

[0030] Preferably, in step S100, an additional 0.5-1 parts of vanadium carbide and 0.02-0.05 parts of carbon powder are added.

[0031] During sintering, vanadium carbide accumulates at the grain boundaries of chromium carbide, anchoring these boundaries and effectively suppressing abnormal grain growth. This results in a more dispersed and uniform distribution of chromium carbide within the pre-alloyed particles. This highly uniform microstructure allows the particles to melt and disperse more stably upon entering the molten metal, significantly improving the sphericity and compositional consistency of the atomized powder, directly enhancing the processing performance of the final powder product. The finer, more uniformly distributed chromium carbide particles also improve the wear resistance of the coating.

[0032] The direction of the crystal transformation of chromium carbide is related to the carbon atom concentration. By adding carbon powder, the chromium carbide in the product can be kept in the Cr3C2 crystal form as much as possible, reducing the precipitation of other brittle phases along the grain boundaries and improving the wear resistance of the material. In addition, the addition of carbon powder can suppress the decarburization phase transformation of chromium carbide at high temperatures.

[0033] Preferably, the composition of the molten metal, by weight percentage, includes: B 3%-4%, Si 3.5%-5.5%, C 0.5%-1.1%, Cr 15%-20%, Fe≤5%, and the balance Ni;

[0034] Pre-alloyed particles account for 30wt%-40wt% of the molten metal.

[0035] Preferably, in step S200, the temperature of the molten metal is 1400-1600℃, and the time from the addition of the pre-alloyed particles to the end of the atomization powdering process does not exceed 20 minutes; the atomization powdering process uses atomizing gas with a pressure of 0.6-1.6 MPa, a guide tube diameter of 7-12 mm, and a cooling rate of 1×10⁻⁶. 4 -3×10 4 K / s.

[0036] To minimize the time from pre-alloyed particles to the end of powder production, the initial amount of molten metal can be adjusted adaptively according to the processing efficiency of the atomizing powder production equipment.

[0037] After the pre-alloyed particles are added to the molten metal, they are uniformly mixed using electromagnetic stirring. Argon or nitrogen is used as the atomizing gas to prevent oxidation. The gas pressure and the diameter of the guide tube are matched to control the flow rate and product fineness. A high cooling rate can effectively inhibit grain growth, which is beneficial for obtaining amorphous, nanocrystalline, or extremely fine microstructures. However, an excessively rapid cooling rate may cause some fine droplets to solidify before they are fully spheroidized, or to collide with larger droplets that are still in a semi-molten state after solidification, forming satellite powders attached to the surface of large particles, which significantly reduces the powder's flowability and bulk density.

[0038] A nickel-based chromium carbide powder prepared by the aforementioned method.

[0039] A coating prepared from the aforementioned nickel-based chromium carbide powder exhibits a wear loss weight of 100-128 mg and a high-temperature oxidation resistance of 1.7-2.5 mg / cm². 2 .

[0040] The present invention has at least the following beneficial effects:

[0041] In this invention, nickel and chromium carbide are sintered to form pre-alloyed large particles. This process is not complete melting, but rather carried out at a temperature below the significant melting point of chromium carbide. This allows diffusion and metallurgical bonding between the nickel and chromium carbide particles, forming a nickel-based alloy coating. This not only improves the wettability of chromium carbide with the molten metal but also reduces the dissolution, precipitation, and recrystallization of chromium carbide, allowing it to maintain its original crystal form in the molten metal as much as possible. This ensures the wear resistance of the product. Suppressing disordered recrystallization also significantly improves the uniformity of product distribution, thereby enhancing the physical properties and weather resistance of the coating. Furthermore, pre-alloying inhibits excessive dissolution and harmful phase transformation of chromium carbide in the metal at high concentrations, allowing a large amount of chromium carbide to remain in a stable, original hard particle form, thus providing a certain amount of chromium carbide dosage. By increasing the particle volume when added to the molten metal through pre-alloying, the overall dissolution tendency of the particles is suppressed. The significant difference in composition and chemical potential between untreated chromium carbide and liquid nickel drives the rapid dissolution of chromium carbide. During sintering, nickel atoms diffuse to the surface of chromium carbide particles, while chromium and carbon atoms diffuse into the nickel matrix, forming a diffusion layer with a gradual compositional change around the chromium carbide particles. This means the surface of the chromium carbide particles is now coated with a diffusion layer whose composition is closer to that of the molten nickel. When in contact with the molten nickel, the compositional gradient between the two decreases, thus significantly reducing the chemical potential gradient driving dissolution and slowing the dissolution rate. Due to the significantly limited amount of dissolution, the number of free chromium and carbon atoms in the molten nickel is reduced. Upon cooling, the system no longer has the conditions for large-scale, disordered recrystallization. The original surface state of the chromium carbide particles becomes more stable, preserving their original hard particle morphology to the greatest extent possible, rather than collapsing into a chaotic new phase, thereby ensuring wear resistance. The pre-alloyed large particles are not added directly during the molten metal melting process but are added into the molten metal during granulation, further reducing the dissolution process of chromium carbide in the molten nickel and improving the wear resistance of the product. Attached Figure Description

[0042] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0043] Figure 1Electron micrographs of tungsten carbide in existing technologies;

[0044] Figure 2 Electron micrograph of chromium carbide directly replacing tungsten carbide;

[0045] Figure 3 This is an electron microscope image of a coating formed using nickel-based chromium carbide powder provided by the present invention. Detailed Implementation

[0046] To make the objectives, methods, and advantages of the embodiments of the present invention clearer, the methods in the embodiments of the present invention will be clearly and completely described. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.

[0047] Example 1: A method for preparing nickel-based chromium carbide powder, comprising the following steps (parts by weight):

[0048] S100, 70 parts of chromium carbide and 15 parts of nickel are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles.

[0049] The sintering process includes: a first-stage sintering process and a second-stage sintering process;

[0050] The temperature of the first sintering process is 800℃ and the time is 1 hour; the temperature of the second sintering process is 1150℃ and the time is 2 hours.

[0051] Both the first and second sintering processes are carried out under an argon atmosphere.

[0052] The cooling process includes: rapidly cooling to 600°C at a rate of 50°C / min, and then cooling down to the furnace exit temperature at a rate of 10°C / min; the furnace exit temperature is 80°C.

[0053] S200: After adding the pre-alloyed particles to molten metal at 1400℃, nickel-based chromium carbide powder is obtained through an atomization powdering process; the time from adding the pre-alloyed particles to the end of the atomization powdering process is 20 minutes; the atomization powdering process uses atomizing gas with a pressure of 0.6 MPa, a guide tube diameter of 7 mm, and a cooling rate of 1×10⁻⁶. 4 K / s;

[0054] The average particle size of chromium carbide is 1 μm, the average particle size of nickel is 1 μm, and the average particle size of pre-alloyed particles is 15 μm.

[0055] The composition of the molten metal by weight percentage includes: B 3%, Si 3.5%, C 0.5%, Cr 15%, Fe 5%, and the balance Ni; the pre-alloyed particles account for 30 wt% of the molten metal.

[0056] Example 2: A method for preparing nickel-based chromium carbide powder, comprising the following steps (parts by weight):

[0057] S100, 85 parts of chromium carbide and 30 parts of nickel are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles;

[0058] The sintering process includes: a first-stage sintering process and a second-stage sintering process;

[0059] The temperature of the first sintering process is 1000℃ and the time is 2 hours; the temperature of the second sintering process is 1250℃ and the time is 3 hours.

[0060] Both the first and second sintering processes are carried out under an argon atmosphere.

[0061] The cooling process includes: rapidly cooling to 800°C at a rate of 80°C / min, and then cooling down to the furnace exit temperature at a rate of 20°C / min; the furnace exit temperature is 90°C.

[0062] S200: After adding the pre-alloyed particles to molten metal at 1600℃, nickel-based chromium carbide powder is obtained through an atomization powdering process; the time from adding the pre-alloyed particles to the end of the atomization powdering process is 18 minutes; the atomization powdering process uses atomizing gas with a pressure of 1.6 MPa, a guide tube diameter of 12 mm, and a cooling rate of 3 × 10⁻⁶. 4 K / s;

[0063] The average particle size of chromium carbide is 5 μm, the average particle size of nickel is 3 μm, and the average particle size of pre-alloyed particles is 50 μm.

[0064] The composition of the molten metal by weight percentage includes: B 4%, Si 5.5%, C 1.1%, Cr 20%, Fe 4%, and the balance Ni, with pre-alloyed particles accounting for 40 wt% of the molten metal.

[0065] Example 3: A method for preparing nickel-based chromium carbide powder, comprising the following steps (parts by weight):

[0066] S100, 78 parts of chromium carbide and 26 parts of nickel are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles;

[0067] The sintering process includes: a first-stage sintering process and a second-stage sintering process;

[0068] The first sintering process is carried out at a temperature of 900℃ for 1.5 hours; the second sintering process is carried out at a temperature of 1200℃ for 2.5 hours.

[0069] Both the first and second sintering processes are carried out under an argon atmosphere.

[0070] The cooling process includes: rapidly cooling to 700°C at a rate of 65°C / min, and then cooling down to the furnace exit temperature at a rate of 15°C / min; the furnace exit temperature is 85°C.

[0071] S200: After adding the pre-alloyed particles to molten metal at 1500°C, nickel-based chromium carbide powder is obtained through an atomization powdering process; the time from adding the pre-alloyed particles to the end of the atomization powdering process is 15 minutes; the atomization powdering process uses atomizing gas with a pressure of 1.2 MPa, a guide tube diameter of 10 mm, and a cooling rate of 2 × 10⁻⁶. 4 K / s;

[0072] The average particle size of chromium carbide is 3 μm, the average particle size of nickel is 2 μm, and the average particle size of pre-alloyed particles is 30 μm.

[0073] The composition of the molten metal by weight percentage includes: B 3.22%, Si 4.31%, C 0.72%, Cr 16.67%, Fe 4.59%, and the balance Ni, with pre-alloyed particles accounting for 35 wt% of the molten metal.

[0074] Example 4: The difference from Example 3 is that S100, 78 parts of chromium carbide, 26 parts of nickel, 0.5 parts of vanadium carbide and 0.02 parts of carbon powder are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles.

[0075] Example 5: The difference from Example 3 is that S100, 78 parts of chromium carbide, 26 parts of nickel, 1 part of vanadium carbide and 0.05 parts of carbon powder are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles.

[0076] Example 6: The difference from Example 3 is that S100, 78 parts of chromium carbide, 26 parts of nickel, 0.7 parts of vanadium carbide and 0.03 parts of carbon powder are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles.

[0077] Comparative Example 1: The difference from Example 6 is that step S100 is omitted, and 78 parts of chromium carbide are directly added to the molten metal and then nickel-based chromium carbide powder is obtained through an atomization powdering process.

[0078] Comparative Example 2: The difference from Example 6 is that the time from the addition of pre-alloyed particles to the end of the atomization powdering process is 30 minutes.

[0079] Comparative Example 3: The difference from Example 6 is that the amount of nickel in step S100 is 40 parts.

[0080] Comparative Example 4: The difference from Example 6 is that the temperature of the two-stage sintering process is 1500°C.

[0081] Comparative Example 5: The difference from Example 6 is that the cooling rate of the cooling process is always maintained at 15°C / min.

[0082] Comparative Example 6: The difference from Example 6 is that the cooling rate of the cooling process is always maintained at 65°C / min.

[0083] Comparative Example 7: The difference from Example 6 is that the cooling rate of the atomization powder preparation process is 8 × 10⁻⁶. 3 K / s.

[0084] Comparative Example 8: The difference from Example 6 is that it contains no toner.

[0085] Blank example: Existing nickel-based tungsten carbide powder.

[0086] Experiments: Nickel-based chromium carbide powder was prepared according to the preparation methods provided in Examples 1-6 and Comparative Examples 1-8. The powder application rate of nickel-based chromium carbide powder and existing nickel-based tungsten carbide powder during supersonic flame spraying was tested. The wear resistance of the sprayed coating (300±10μm) was tested according to Method A in ASTM G65-04. The high-temperature oxidation weight gain test was used to test the high-temperature oxidation resistance of the sprayed coating (300±10μm). The test method was to expose the coating sample to static air at 800°C for 50 hours and measure the increase in mass per unit area. All test results are shown in Table 1.

[0087] Table 1

[0088] Example 1 Example 2 Example 3 Example 4 Example 5 Powder application rate / % 59.2 62.7 64.0 73.3 75.1 Wear loss weight / mg 127.9 122.0 118.6 105.8 102.4 <![CDATA[Weight gain / (mg / cm 2 )]]> 2.4 2.5 2.3 1.9 1.7 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Powder application rate / % 76.4 42.7 61.0 71.5 75.8 Wear loss weight / mg 100.5 180.2 124.5 116.1 157.3 <![CDATA[Weight gain / (mg / cm 2 )]]> 1.7 5.6 3.2 2.8 2.1 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Blank example Powder application rate / % 63.9 70.3 65.8 67.1 72.9 Wear loss weight / mg 146.0 127.7 130.5 121.4 98.5 <![CDATA[Weight gain / (mg / cm 2 )]]> 2.5 1.9 2.0 2.0 8.7

[0089] The test results of Examples 1-6 show that the nickel-based chromium carbide provided by the present invention has a good powder application rate, and the coating obtained therefrom has good wear resistance. A comparison of the test results of Examples 3-6 with the blank example shows that the coating obtained from the nickel-based chromium carbide powder provided by the present invention has comparable wear resistance to existing nickel-based tungsten carbide powders, and also exhibits better high-temperature oxidation resistance.

[0090] A comparison of the results from Comparative Example 1 and Example 6 shows that directly adding chromium carbide to the molten metal significantly reduced the powder coating rate, wear resistance, and oxidation resistance. The applicant hypothesizes that this is due to the influence of morphological uniformity, crystal form changes, coating density, and uniformity.

[0091] A comparison of the results of Comparative Example 2 and Example 6 shows that as the time from the addition of pre-alloyed particles to the end of the atomization powdering process increases, the powder application rate, wear resistance, and oxidation resistance decrease.

[0092] A comparison of the results of Comparative Example 3 and Example 6 shows that excessive nickel during pre-alloying can also affect the wear resistance of the coating.

[0093] A comparison of the results from Comparative Example 4 and Example 6 shows that excessively high temperatures in the two-stage sintering process severely affect the wear resistance of the coating. The applicant hypothesizes that the diffusion layer structure of nickel-coated chromium carbide in the pre-alloyed particles is disrupted.

[0094] A comparison of the results of Comparative Examples 5-7 and Example 6 shows that the cooling rate of the cooling process and the cooling rate of the atomization powdering process both affect the powder application rate, wear resistance, and oxidation resistance.

[0095] A comparison of the results of Comparative Example 8 and Example 6 shows that without toner, the powder application rate, wear resistance, and oxidation resistance all decrease to some extent.

[0096] Figure 1 The image shown is the electron microscope image corresponding to the blank example, i.e., the electron microscope image when tungsten carbide is used. Figure 2 The images are electron microscope images corresponding to Comparative Example 1. As can be seen from the two images, when chromium carbide is used to directly replace tungsten carbide, chromium carbide exhibits irregular aggregation and poor distribution uniformity.

[0097] Figure 3 The image shown is an electron microscope image corresponding to Example 6. As can be seen from the image, chromium carbide forms small aggregates, and the small aggregates are evenly distributed.

[0098] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing nickel-based chromium carbide powder, characterized in that, Includes the following steps: S100, chromium carbide and nickel are processed through sintering, cooling and crushing processes to obtain pre-alloyed particles; S200: After the pre-alloyed particles are added to the molten metal, nickel-based chromium carbide powder is obtained through an atomization powdering process. By weight, 70-85 parts chromium carbide and 15-30 parts nickel; The composition of the molten metal, by weight percentage, includes: B 3%-4%, Si 3.5%-5.5%, C 0.5%-1.1%, Cr 15%-20%, Fe≤5%, and the balance Ni; Pre-alloyed particles account for 30wt%-40wt% of the molten metal; The sintering process includes: a first-stage sintering process and a second-stage sintering process; The temperature of the first sintering process is 800-1000℃, and the time is 1-2 hours; the temperature of the second sintering process is 1150-1250℃, and the time is 2-3 hours. Both the first and second sintering processes are carried out under an inert atmosphere.

2. The preparation method according to claim 1, characterized in that, The average particle size of chromium carbide is 1-5 μm, the average particle size of nickel is 1-3 μm, and the average particle size of pre-alloyed particles is 15-50 μm.

3. The preparation method according to claim 1, characterized in that, The cooling process includes: rapidly cooling to 600-800℃ at a rate of 50-80℃ / min, and then cooling down to the furnace exit temperature at a rate of 10-20℃ / min; the furnace exit temperature is <100℃.

4. The preparation method according to any one of claims 1-3, characterized in that, In step S100, an additional 0.5-1 part of vanadium carbide and 0.02-0.05 parts of carbon powder are added.

5. The preparation method according to claim 4, characterized in that, In step S200, the temperature of the molten metal is 1400-1600℃, and the time from the addition of the pre-alloyed particles to the end of the atomization powdering process does not exceed 20 minutes. The atomization powdering process uses atomizing gas with a pressure of 0.6-1.6 MPa, a guide tube diameter of 7-12 mm, and a cooling rate of 1×10⁻⁶. 4 -3×10 4 K / s.

6. A nickel-based chromium carbide powder prepared by the preparation method according to any one of claims 1-5.

7. A coating prepared from nickel-based chromium carbide powder as described in claim 6, characterized in that, The wear loss of the coating is 100-128 mg, and the high-temperature oxidation resistance is 1.7-2.5 mg / cm³. 2 .

Citation Information

Patent Citations

  • Method for producing chromium carbide-nickel chromium atomized powder

    CN1186723A

  • Sintered P / M products containing pre-alloyed titanium carbide additives