Boron-containing sodium supplement and electrolyte for sodium-ion battery and battery cell
By using sodium tetraphenylborate as a sodium replenisher for sodium-ion batteries, combined with carbonate electrolytes, the problem of sodium deficiency during the first charge and discharge process of sodium-ion batteries is solved, achieving efficient sodium compensation and improved battery performance, making it suitable for large-scale application of sodium-ion batteries.
Patent Information
- Application Number
- CN202610503395.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-16
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-04-16
AI Technical Summary
Sodium-ion batteries are in a sodium-deficient or sodium-poor state in the positive electrode material during the first charge and discharge process, resulting in the loss of active sodium. When the hard carbon negative electrode forms a solid electrolyte interface film, it irreversibly consumes active sodium, affecting cycle life and energy density. Existing sodium replenishment agents have high decomposition voltage or produce gaseous byproducts, which damage the interface stability.
Sodium tetraphenylborate is used as a sodium supplement agent. Combined with carbonate electrolyte, it decomposes and releases active sodium ions under electrochemical oxidation to form a stable interface film, which inhibits the collapse of the cathode material structure and improves cycle stability.
Sodium tetraphenylborate has a low decomposition voltage and high solubility, avoiding the formation of gaseous byproducts, significantly improving sodium compensation efficiency and battery cycle performance, increasing the first discharge specific capacity, providing excellent rate performance, and significantly improving energy density and cycle stability.
Smart Images

Figure CN122474740B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of sodium-ion battery technology, specifically relating to a boron-containing sodium supplement agent, an electrolyte, and a battery cell for sodium-ion batteries. Background Technology
[0002] Sodium-ion batteries (SIBs) are widely regarded as an important alternative to lithium-ion batteries (LIBs) in large-scale energy storage and low-speed electric vehicles due to their advantages such as abundant raw material resources and low manufacturing costs. In recent years, they have become one of the research hotspots in the field of electrochemical energy storage. However, sodium-ion batteries still face two major challenges in practical applications: First, common cathode materials are often in a sodium-deficient or sodium-poor state, requiring sodium replenishment during the first charge and discharge process; second, hard carbon anodes irreversibly consume active sodium when forming a solid electrolyte interphase (SEI) film, leading to further loss of the total amount of active sodium in the entire battery, which severely restricts their cycle life and energy density.
[0003] Current reported methods for pre-sodiuming cathodes typically involve introducing sodium-containing compounds into the cathode material as sodium replenishers, causing them to decompose and release active sodium during the first charge. For example, the paper "Achieving High-Capacity Cathode Presodiation Agent Via Triggering Anionic Oxidation Activity in Sodium Oxide," Advanced Materials, 2024, 36, 2407720, reports on sodium replenishers, represented by Na₂O, which achieve sodium compensation by inducing anionic oxidation reactions. The articles "Rational Design of Aqueous Na Ion Batteries Toward High Energy Density and Long Cycle Life," *Journal of the American Chemical Society*, 2025, 147 (8), 7039-7049, and "Synergistic dominant facet and consanguine carboncoating enable efficient Na2CO3 presodiation for sodium-ion batteries," *EnergyStorage Materials*, 2026, 86, 104981, report the use of sodium-containing compounds such as NaNO2, Na2C4O4, Na2C2O4, and Na2CO3 for cathode presodiation. However, these sodium presodifiers, such as Na2O, NaNO2, Na2C4O4, Na2C2O4, and Na2CO3, have the following significant drawbacks: First, their decomposition voltage is generally high (typically higher than 4.3V vs. Na2O). + The sodium release efficiency is poorly matched with the stable operating voltage window of most cathode materials, resulting in low sodium release efficiency and difficulty in achieving effective compensation. Secondly, the decomposition process is often accompanied by the generation of CO2 and NO. x Gaseous byproducts such as O2 can exacerbate side reactions at the electrode / electrolyte interface, causing electrode structure expansion and thus accelerating capacity decay and cycle performance degradation. Furthermore, alkaline substances derived from sodium-containing compounds remaining on the surface of the cathode material can further damage interfacial stability and affect the long-term cycle performance of the battery.
[0004] To improve electrode interface stability, existing technologies have attempted to introduce boron-containing sodium salt additives into the electrolyte. For example, the paper "Sodium Difluoro(oxalato)borate Additive-Induced Robust SEI and CEI Layers Enable Dendrite-Free and Long-Cycling Sodium-Ion Batteries," published in Advanced Functional Materials, 2024, 34, 2402310, reports the introduction of NaBF4, NaDFOB, and NaBOB into the electrolyte to improve battery cycle performance by forming a boron-rich inorganic interface film. However, these boron-containing sodium salt additives are mainly used for interface modulation, and they suffer from problems such as high decomposition voltage and limited solubility. Furthermore, they themselves are difficult to efficiently release active sodium at suitable voltages.
[0005] Therefore, developing a sodium supplement that combines low decomposition voltage, high solubility in electrolyte, no gaseous byproducts during decomposition, and effective provision of active sodium is of great significance for solving the sodium deficiency problem in sodium-ion battery cathode materials, improving the energy density and cycle stability of the entire battery, and thus promoting its large-scale application. Summary of the Invention
[0006] In order to solve the problems mentioned in the background art, the present invention aims to provide a boron-containing sodium supplement agent, an electrolyte, and a battery cell for sodium-ion batteries.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: On the one hand, the present invention provides a boron-containing sodium supplement for sodium-ion batteries, wherein the boron-containing sodium supplement is sodium tetraphenylborate.
[0008] On the other hand, the present invention provides an electrolyte for sodium-ion batteries, comprising the boron-containing sodium supplementer and carbonate electrolyte described above for sodium-ion batteries; The mass ratio of the boron-containing sodium supplement agent and the carbonate electrolyte used in the sodium-ion battery is (5-22.8):100.
[0009] Furthermore, the carbonate electrolyte includes sodium perchlorate, propylene carbonate, and the film-forming additive vinylene carbonate.
[0010] Furthermore, the ratio of sodium perchlorate to propylene carbonate is 1 mol: 1 L; And / or, the mass of the vinylene carbonate is 1% of the total mass of sodium perchlorate and propylene carbonate.
[0011] On the other hand, the present invention provides a method for pre-intercalating sodium into a sodium-ion battery, comprising the following steps: Adding any of the electrolytes described above to a sodium-ion battery achieves pre-intercalation of sodium into the battery. During the initial charging of the sodium-ion battery, the boron-containing sodium supplement agent undergoes controlled decomposition under electrochemical oxidation, releasing active sodium ions by breaking its own sodium-containing chemical bonds. These active sodium ions can quickly intercalate into the crystal structure of the positive electrode material, efficiently compensating for sodium source during the initial cycle of the sodium-ion battery. The boron-containing sodium supplement agent for sodium-ion batteries has both sodium source supply and structural stability functions. While supplementing the sodium source, it can effectively suppress phase transitions and structural collapse during the cycling process of the positive electrode material, improving the electrochemical reversibility of the material. This solves the technical problem that the positive electrode material is prone to sodium source loss and insufficient structural stability in the initial cycle of sodium-ion batteries, thus limiting the battery's energy density and cycle performance.
[0012] The boron-containing sodium supplement agent of this invention for sodium-ion batteries undergoes the following reaction during the pre-sodium intercalation process: The boron-containing sodium supplement used in sodium-ion batteries produces no gaseous byproducts after oxidative decomposition.
[0013] In another aspect, the present invention provides a battery cell comprising the boron-containing sodium-supplementing agent for sodium-ion batteries described above or the electrolyte for sodium-ion batteries described above.
[0014] Furthermore, it includes positive electrode materials, negative electrode materials, and any of the electrolytes described above for sodium-ion batteries.
[0015] Furthermore, the cathode material includes P2 type cathode material, O3 type cathode material, or sodium vanadium phosphate cathode material.
[0016] Furthermore, the P2 type cathode material includes Na 0.67 Ni 0.08 Ti 0.12 Mn 0.8 O2; And / or, the O3-type cathode material includes NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0017] Furthermore, the negative electrode material includes hard carbon.
[0018] Compared with the prior art, the beneficial effects of the present invention are: (1) The sodium tetraphenylborate used in this invention has a decomposition voltage as low as ~3.2V, which can complete the low-voltage decomposition and sodium replenishment in the early stage of the first charge of the battery, avoiding electrolyte side reactions and electrode interface damage caused by high-voltage decomposition; no gaseous byproducts are generated during the decomposition process of sodium tetraphenylborate; the solubility of sodium tetraphenylborate is as high as 273.6 g·L -1 It can fully dissolve in the electrolyte to form a stable system, ensuring sufficient sodium compensator concentration and meeting the requirements for efficient sodium replenishment. In addition, sodium tetraphenylborate not only significantly reduces the decomposition voltage, but also achieves complete decomposition of boron-containing sodium compensator in the low-voltage range, and the decomposition products are all soluble substances. This avoids problems such as increased interfacial polarization and hindered ion transport caused by the formation of insoluble deposits on the electrode surface, thus ensuring the stability of the battery's electrochemical performance.
[0019] (2) Existing sodium-containing compounds (such as Na2O, NaNO2, Na2C4O4, Na2C2O4, Na2CO3, etc.) have excessively high decomposition voltages, and existing boron-containing sodium salt additives (such as NaBF4, NaDFOB, NaBOB, etc.) have excessively high decomposition voltages and low solubility in electrolytes, which cannot meet the sodium compensation requirements of P2-type cathode materials with severe sodium deficiency. The sodium tetraphenylborate used in this invention has a decomposition voltage as low as ~3.2V, which is highly matched with the working voltage range (2.0~4.3V) of P2-type cathode materials, and can be used for sodium compensation of P2-type cathode materials.
[0020] (3) The present invention uses sodium tetraphenylborate as a sodium replenishing agent, which can effectively compensate for the sodium source loss in the early stage of the positive electrode material cycle, so that the initial discharge specific capacity of the P2||HC coin cell increases from 65 mAh·g -1 Significantly increased to 163mAh·g -1 The sodium source compensation efficiency is significant. After sodium supplementation treatment with boron-containing sodium supplementing agent, the P2||HC coin cell has excellent rate performance and ultra-long cycle stability. After 3700 long-cycle cycles, the capacity retention rate still reaches 72.08%, which effectively solves the technical pain points of traditional cathode materials such as rapid capacity decay and limited rate performance caused by insufficient sodium source and poor structural stability. It also greatly improves the electrochemical reversibility and service life of the battery.
[0021] (4) The sodium tetraphenylborate used in this invention has been successfully tested under operating conditions, and a 5Ah-level electrolyte-deficient soft-pack battery has been successfully assembled with an energy density of 184Wh·kg. -1 The battery exhibits extremely high energy density and retains 81.65% of its capacity after 250 cycles. These results demonstrate that the invention is not only suitable for small laboratory battery systems but also adaptable to the design requirements of large-capacity, electrolyte-poor practical batteries. It ensures both high energy density and reliable cycle performance, providing key technological support for large-scale applications in sodium-ion battery energy storage and power batteries, and possesses broad industrialization prospects. Attached Figure Description
[0022] Figure 1 This is the CV curve of the 2032 coin cell in Embodiment 1 of the present invention; Figure 2 This is a charge-discharge curve of the 2032 coin cell in Embodiment 1 of the present invention; Figure 3 This is a cycle performance diagram of the P2||HC coin cell in Embodiment 1 and Comparative Example 1 of the present invention; Figure 4 These are rate performance diagrams of P2||HC coin cells in Embodiment 1 and Comparative Example 1 of the present invention; Figure 5 This is a cycle performance diagram of the P2||HC soft-pack battery in Embodiment 1 and Comparative Example 1 of the present invention; Figure 6 This is a charge-discharge curve of the P2||HC soft-pack battery in Embodiment 1 of the present invention; Figure 7 These are optical photographs of the electrolytes for sodium-ion batteries prepared in Examples 2-5 of this invention; Figure 8 These are the charge-discharge curves of the NVP||HC coin cells in Embodiment 6 and Comparative Example 2 of this invention. Figure 9 These are charge-discharge curves of the O3||HC coin cells in Embodiment 7 and Comparative Example 3 of the present invention; Figure 10 This is the CV curve of the 2032 coin cell in Comparative Example 4 of the present invention; Figure 11 These are the charge and discharge curves of the 2032 type button half-cell in Comparative Examples 4-6 of this invention; Figure 12 These are charge and discharge curves of the 2032 type button half-cell in Comparative Examples 7-9 of this invention. Detailed Implementation
[0023] To better understand the content of this invention, the following detailed description is provided in conjunction with specific implementation methods. However, the scope of protection of this invention is not limited to the following embodiments.
[0024] Example 1 Electrolytes used in sodium-ion batteries include sodium tetraphenylborate (NaBPh4) and carbonate electrolytes. The carbonate electrolyte is composed of sodium perchlorate (NaClO4), propylene carbonate (PC), and the film-forming additive vinylene carbonate (VC). The ratio of sodium perchlorate to propylene carbonate is 1 mol: 1 L, and the mass of vinylene carbonate is 1% of the total mass of sodium perchlorate and propylene carbonate.
[0025] Preparation of electrolyte for sodium-ion batteries: Slowly add 75 mg of sodium tetraphenylborate to a dry, sealed bottle containing 1 g of carbonate electrolyte (dried by molecular sieve, with a moisture content ≤10 ppm), place the bottle on a magnetic stirrer, and stir at 300 rpm at a constant temperature of 25°C for 30 min until the sodium tetraphenylborate is completely dissolved, forming a clear electrolyte that is transparent, free of turbidity and precipitation. Seal and store the electrolyte in an argon-protected desiccator for later use.
[0026] Pre-sodium insertion method for sodium-ion batteries: The electrolyte used in sodium-ion batteries described above is added to the sodium-ion battery to achieve pre-sodium insertion of the sodium-ion battery.
[0027] 2032 type button cell: All assembly operations were performed in an argon glove box with argon purity ≥99.999%, moisture content ≤0.01ppm, and oxygen content ≤0.01ppm. A 0.5mm thick sodium metal sheet was selected as the counter electrode and reference electrode, cut into 14mm diameter discs; carbon paper was selected as the working electrode, cut into 10mm diameter discs, and dried in a 120℃ vacuum oven for 12 hours before use to remove residual moisture; a 16mm diameter glass fiber diaphragm was vacuum dried at 100℃ for 8 hours before use. Assemble the 2032 coin cell in the following order: positive electrode shell → sodium metal sheet → glass fiber separator → 40μL electrolyte for sodium-ion batteries → carbon paper → gasket → spring sheet → negative electrode shell. During assembly, ensure that all components are aligned and centered to avoid short circuits. Use a coin cell sealing machine to seal the cells at a pressure of 1.2MPa. After sealing, place the cells in a glove box and let them stand for 24 hours to allow the electrolyte to fully wet the electrodes and separator.
[0028] P2||HC button cell: ① Positive electrode: P2 type Na 0.67 Ni 0.08 Ti 0.12 Mn 0.8O2 active material, conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 90:5:5. N-methylpyrrolidone (NMP) solvent is added, and the mixture is stirred to form a uniform positive electrode slurry. The positive electrode slurry is coated onto a 12μm thick aluminum foil current collector, dried with hot air at 80℃ for 12 hours, then rolled under 8MPa pressure, and subsequently cut into 10mm diameter discs. Finally, it is dried in a 120℃ vacuum oven for 24 hours to remove residual solvent and moisture, and is ready for use. ② Negative electrode sheet: Hard carbon (HC), conductive agent Super P, and sodium alginate are mixed in a mass ratio of 94:1:5. Deionized water is added, and the mixture is stirred to form a uniform negative electrode slurry. The negative electrode slurry is coated onto a 10μm thick copper foil current collector, dried with hot air at 80℃ for 12 hours, then rolled under 6MPa pressure, cut into 12mm diameter discs, and dried in a 100℃ vacuum oven for 24 hours, and is ready for use. ③ The glass fiber separator (16mm in diameter) was vacuum dried at 100℃ for 8 hours and then set aside for use. All assembly operations were carried out in an argon glove box with argon purity ≥99.999%, moisture content ≤0.01ppm, and oxygen content ≤0.01ppm. The P2||HC coin cell was assembled in the following order: positive electrode shell → positive electrode sheet → glass fiber separator → 40μL electrolyte for sodium-ion batteries → negative electrode sheet → gasket → spring sheet → negative electrode shell. After assembly, the cells were sealed using a coin cell sealing machine at a sealing pressure of 1.2MPa. After sealing, the cells were placed in the glove box and left to stand for 24 hours to ensure that the electrolyte was fully impregnated.
[0029] P2||HC soft-pack battery: ① Positive electrode: P2 type Na 0.67 Ni 0.08 Ti 0.12 Mn 0.8O2 active material, conductive agent Super P, and binder PVDF are mixed in a mass ratio of 8:1:1, and NMP solvent is added to prepare a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil current collector with a thickness of 12μm, dried with hot air at 80℃ for 12h, rolled at 8MPa, and then cut into rectangular sheets of 7.5cm×6.1cm. Aluminum tabs are used and ultrasonically welded to the positive electrode current collector. Then, the sheets are dried in a vacuum oven at 120℃ for 24h for later use. ② Negative Electrode: Hard carbon, conductive agent Super P, and binder sodium carboxymethyl cellulose / styrene-butadiene rubber (CMC / SBR, CMC and SBR in a mass ratio of 1:1) are mixed at a mass ratio of 9:0.5:0.5, and deionized water is added to prepare the negative electrode slurry. The negative electrode slurry is coated onto a 10μm thick copper foil current collector, dried at 80℃ for 12h, and rolled at 6MPa. The resulting rectangular sheets (slightly larger than the positive electrode to avoid lithium dendrite precipitation) are then cut. Nickel tabs are used, ultrasonically welded to the negative electrode current collector, and dried in a 100℃ vacuum oven for 24h. Assembly is carried out in a drying room with a dew point of -50℃ and a relative humidity ≤1%. A glass fiber separator cut to 8.0cm × 6.8cm was selected and placed between the positive and negative electrode plates, ensuring that the separator completely covered the active material areas of both electrodes to obtain the electrode core. The stacked electrode core was placed in an aluminum-plastic film soft pack, and the three sides of the aluminum-plastic film soft pack were pre-sealed using a vacuum heat sealer at a temperature of 120℃, a pressure of 0.3MPa, and a time of 3s. Electrolyte for sodium-ion batteries (electrolyte dosage based on 2g·Ah) was injected into the pre-sealed aluminum-plastic film soft pack. -1 (Calculation), let stand for 30 minutes to allow the electrolyte to fully wet the electrode core; then place the aluminum-plastic film soft pack in a vacuum environment for 10 minutes to degas and remove residual air bubbles inside the electrode core; finally, use a vacuum heat sealer to seal the fourth side of the aluminum-plastic film soft pack at a sealing temperature of 130℃, a pressure of 0.4MPa, and a time of 5s to complete the assembly of the 5Ah-level low electrolyte soft pack battery.
[0030] Example 2 The difference between this embodiment and Embodiment 1 is that 50 mg of sodium tetraphenylborate is used instead of 75 mg of sodium tetraphenylborate in Embodiment 1.
[0031] Example 3 The difference between this embodiment and Embodiment 1 is that 100 mg of sodium tetraphenylborate is used instead of 75 mg of sodium tetraphenylborate in Embodiment 1.
[0032] Example 4 The difference between this embodiment and Embodiment 1 is that 150 mg of sodium tetraphenylborate is used instead of 75 mg of sodium tetraphenylborate in Embodiment 1.
[0033] Example 5 The difference between this embodiment and Embodiment 1 is that 228 mg of sodium tetraphenylborate is used instead of 75 mg of sodium tetraphenylborate in Embodiment 1.
[0034] Example 6 The difference between this embodiment and Embodiment 1 is that sodium vanadium phosphate (NVP) is used instead of the P2 type Na in Embodiment 1. 0.67 Ni 0.08 Ti 0.12 Mn 0.8 O2 active material is used to assemble an NVP||HC coin cell.
[0035] Example 7 The difference between this embodiment and Embodiment 1 is that: O3-type cathode material (NaNi) is used. 1 / 3 Fe 1 / 3 Mn 1 / 3 O2) replaces the P2 type Na in Example 1 0.67 Ni 0.08 Ti 0.12 Mn 0.8 O2 active material is assembled into an O3||HC coin cell.
[0036] Comparative Example 1 The carbonate electrolyte is composed of sodium perchlorate (NaClO4), propylene carbonate (PC), and film-forming additive vinylene carbonate (VC). The ratio of sodium perchlorate to propylene carbonate is 1 mol: 1 L, and the mass of vinylene carbonate is 1% of the total mass of sodium perchlorate and propylene carbonate. The carbonate electrolyte is dried using molecular sieves, and the moisture content is ≤10 ppm.
[0037] P2||HC button cell: ① Positive electrode: P2 type Na 0.67 Ni 0.08 Ti 0.12 Mn 0.8O2 active material, conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 90:5:5. N-methylpyrrolidone (NMP) solvent is added, and the mixture is stirred to form a uniform positive electrode slurry. The positive electrode slurry is coated onto a 12μm thick aluminum foil current collector, dried with hot air at 80℃ for 12 hours, then rolled under 8MPa pressure, and subsequently cut into 10mm diameter discs. Finally, it is dried in a 120℃ vacuum oven for 24 hours to remove residual solvent and moisture, and is ready for use. ② Negative electrode sheet: Hard carbon, conductive agent Super P, and sodium alginate are mixed in a mass ratio of 94:1:5. Deionized water is added, and the mixture is stirred to form a uniform negative electrode slurry. The negative electrode slurry is coated onto a 10μm thick copper foil current collector, dried with hot air at 80℃ for 12 hours, then rolled under 6MPa pressure, cut into 12mm diameter discs, and dried in a 100℃ vacuum oven for 24 hours, and is ready for use. ③ The glass fiber separator (16mm in diameter) was vacuum dried at 100℃ for 8 hours and then set aside for use. All assembly operations were carried out in an argon glove box with argon purity ≥99.999%, moisture content ≤0.01ppm, and oxygen content ≤0.01ppm. The P2||HC coin cell was assembled in the following order: positive electrode shell → positive electrode plate → glass fiber separator → 40μL carbonate electrolyte → negative electrode plate → gasket → spring plate → negative electrode shell. After assembly, the cells were sealed using a coin cell sealing machine at a sealing pressure of 1.2MPa. After sealing, the cells were placed in the glove box and left to stand for 24 hours to ensure that the electrolyte was fully impregnated.
[0038] P2||HC soft-pack battery: ① Positive electrode: P2 type Na 0.67 Ni 0.08 Ti 0.12 Mn 0.8O2 active material, conductive agent Super P, and binder PVDF are mixed in a mass ratio of 8:1:1, and NMP solvent is added to prepare a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil current collector with a thickness of 12μm, dried with hot air at 80℃ for 12h, rolled at 8MPa, and then cut into rectangular sheets of 7.5cm×6.1cm. Aluminum tabs are used and ultrasonically welded to the positive electrode current collector. Then, the sheets are dried in a vacuum oven at 120℃ for 24h for later use. ② Negative Electrode: Hard carbon, conductive agent Super P, and binder sodium carboxymethyl cellulose / styrene-butadiene rubber (CMC / SBR, CMC and SBR in a mass ratio of 1:1) are mixed at a mass ratio of 9:0.5:0.5, and deionized water is added to prepare the negative electrode slurry. The negative electrode slurry is coated onto a 10μm thick copper foil current collector, dried at 80℃ for 12h, and rolled at 6MPa. The resulting rectangular sheets (slightly larger than the positive electrode to avoid lithium dendrite precipitation) are then cut. Nickel tabs are used, ultrasonically welded to the negative electrode current collector, and dried in a 100℃ vacuum oven for 24h. Assembly is carried out in a drying room with a dew point of -50℃ and a relative humidity ≤1%. A glass fiber separator cut to 8.0cm × 6.8cm was selected and placed between the positive and negative electrode plates, ensuring that the separator completely covered the active material areas of both electrodes to obtain the electrode core. The stacked electrode core was placed in an aluminum-plastic film soft package, and the three sides of the aluminum-plastic film soft package were pre-sealed using a vacuum heat sealer at a temperature of 120℃, a pressure of 0.3MPa, and a time of 3s. Carbonate electrolyte was injected into the pre-sealed aluminum-plastic film soft package (electrolyte dosage was 2g·Ah). -1 (Calculation), let stand for 30 minutes to allow the electrolyte to fully wet the electrode core; then place the aluminum-plastic film soft pack in a vacuum environment for 10 minutes to degas and remove residual air bubbles inside the electrode core; finally, use a vacuum heat sealer to seal the fourth side of the aluminum-plastic film soft pack at a sealing temperature of 130℃, a pressure of 0.4MPa, and a time of 5s to complete the assembly of the 5Ah-level low electrolyte soft pack battery.
[0039] Comparative Example 2 The carbonate electrolyte is composed of sodium perchlorate (NaClO4), propylene carbonate (PC), and film-forming additive vinylene carbonate (VC). The ratio of sodium perchlorate to propylene carbonate is 1 mol: 1 L, and the mass of vinylene carbonate is 1% of the total mass of sodium perchlorate and propylene carbonate. The carbonate electrolyte is dried using molecular sieves, and the moisture content is ≤10 ppm.
[0040] NVP||HC coin cell: ① Positive electrode: Sodium vanadium phosphate (NVP), conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 90:5:5. N-methylpyrrolidone (NMP) solvent is added and stirred to form a uniform positive electrode slurry. The positive electrode slurry is coated on an aluminum foil current collector with a thickness of 12μm, dried with hot air at 80℃ for 12h, rolled under a pressure of 8MPa, and then cut into round pieces with a diameter of 10mm. Finally, it is dried in a vacuum oven at 120℃ for 24h to remove residual solvent and moisture and is ready for use. ② Negative electrode sheet: Hard carbon, conductive agent Super P, and sodium alginate are mixed at a mass ratio of 94:1:5, and deionized water is added and stirred to form a uniform negative electrode slurry. The negative electrode slurry is coated onto a copper foil current collector with a thickness of 10μm, dried with hot air at 80℃ for 12h, rolled under 6MPa pressure, cut into 12mm diameter discs, and dried in a vacuum oven at 100℃ for 24h for later use. ③ The glass fiber diaphragm (16mm diameter) is dried in a vacuum oven at 100℃ for 8h for later use. All assembly operations are carried out in an argon glove box with argon purity ≥99.999%, moisture content ≤0.01ppm, and oxygen content ≤0.01ppm. Assemble the NVP||HC button cell in the following order: positive electrode shell → positive electrode sheet → glass fiber separator → 40μL carbonate electrolyte → negative electrode sheet → gasket → spring sheet → negative electrode shell. After assembly, seal the cells using a button cell sealing machine at a pressure of 1.2MPa. After sealing, place the cells in a glove box and let them stand for 24 hours to ensure that the electrolyte is fully impregnated.
[0041] Comparative Example 3 The carbonate electrolyte is composed of sodium perchlorate (NaClO4), propylene carbonate (PC), and film-forming additive vinylene carbonate (VC). The ratio of sodium perchlorate to propylene carbonate is 1 mol: 1 L, and the mass of vinylene carbonate is 1% of the total mass of sodium perchlorate and propylene carbonate. The carbonate electrolyte is dried using molecular sieves, and the moisture content is ≤10 ppm.
[0042] O3||HC coin cell: ① Positive electrode: O3 type positive electrode material (NaNi) is used. 1 / 3 Fe 1 / 3 Mn 1 / 3O2), conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 90:5:5. N-methylpyrrolidone (NMP) solvent is added, and the mixture is stirred to form a uniform positive electrode slurry. The positive electrode slurry is coated onto a 12μm thick aluminum foil current collector, dried with hot air at 80℃ for 12h, rolled under 8MPa pressure, and then cut into 10mm diameter discs. Finally, it is dried in a vacuum oven at 120℃ for 24h to remove residual solvent and moisture, and is ready for use. ② Negative electrode sheet: Hard carbon, conductive agent Super P, and sodium alginate are mixed in a mass ratio of 94:1:5. Deionized water is added, and the mixture is stirred to form a uniform negative electrode slurry. The negative electrode slurry is coated onto a 10μm thick copper foil current collector, dried with hot air at 80℃ for 12h, rolled under 6MPa pressure, cut into 12mm diameter discs, and dried in a vacuum oven at 100℃ for 24h, and is ready for use. ③ The glass fiber separator (16mm in diameter) was vacuum dried at 100℃ for 8 hours and then set aside for use. All assembly operations were carried out in an argon glove box with argon purity ≥99.999%, moisture content ≤0.01ppm, and oxygen content ≤0.01ppm. The O3||HC coin cell was assembled in the following order: positive electrode shell → positive electrode plate → glass fiber separator → 40μL carbonate electrolyte → negative electrode plate → gasket → spring plate → negative electrode shell. After assembly, the cells were sealed using a coin cell sealing machine at a sealing pressure of 1.2MPa. After sealing, the cells were placed in the glove box and left to stand for 24 hours to ensure that the electrolyte was fully impregnated.
[0043] Comparative Example 4 The difference between this comparative example and Example 1 is that 50 mg of sodium tetra(4-fluorophenyl)borate is used instead of 75 mg of sodium tetraphenylborate in Example 1; and the composition of the carbonate electrolyte is changed to: sodium perchlorate (NaClO4), ethylene carbonate (EC), and dimethyl carbonate (DMC), with a sodium perchlorate concentration of 1 mol / L and a volume ratio of ethylene carbonate to dimethyl carbonate of 1:1.
[0044] Comparative Example 5 The difference between this comparative example and Example 1 is that 150 mg of sodium tetra(4-fluorophenyl)borate was used instead of 75 mg of sodium tetraphenylborate in Example 1; and the composition of the carbonate electrolyte was changed to: sodium perchlorate (NaClO4), ethylene carbonate (EC), and dimethyl carbonate (DMC), with the concentration of sodium perchlorate being 1 mol / L and the volume ratio of ethylene carbonate to dimethyl carbonate being 1:1.
[0045] Comparative Example 6 The difference between this comparative example and Example 1 is that 250 mg of sodium tetra(4-fluorophenyl)borate was used instead of 75 mg of sodium tetraphenylborate in Example 1; and the composition of the carbonate electrolyte was changed to: sodium perchlorate (NaClO4), ethylene carbonate (EC), and dimethyl carbonate (DMC), with the concentration of sodium perchlorate being 1 mol / L and the volume ratio of ethylene carbonate to dimethyl carbonate being 1:1.
[0046] Comparative Example 7 The difference between this comparative example and Example 1 is that 50 mg of sodium tetra(4-fluorophenyl)borate is used instead of 75 mg of sodium tetraphenylborate in Example 1; and the composition of the carbonate electrolyte is changed to sodium perchlorate (NaClO4) and propylene carbonate (PC), with the concentration of sodium perchlorate being 1 mol / L.
[0047] Comparative Example 8 The difference between this comparative example and Example 1 is that 50 mg of sodium tetra(4-fluorophenyl)borate is used instead of 75 mg of sodium tetraphenylborate in Example 1; and the composition of the carbonate electrolyte is changed to: sodium hexafluorophosphate (NaPF6), ethylene carbonate (EC), and dimethyl carbonate (DMC), with the concentration of sodium hexafluorophosphate being 1 mol / L and the volume ratio of ethylene carbonate to dimethyl carbonate being 1:1.
[0048] Comparative Example 9 The difference between this comparative example and Example 1 is that 50 mg of sodium tetra(4-fluorophenyl)borate was used instead of 75 mg of sodium tetraphenylborate in Example 1; and the composition of the carbonate electrolyte was changed to sodium perchlorate (NaClO4) and diethylene glycol dimethyl ether (DIGLYME), with the concentration of sodium perchlorate being 1 mol / L.
[0049] The 2032 coin cell prepared in Example 1 was subjected to cyclic voltammetry (CV) and charge-discharge tests, and the results are as follows: Figure 1 and Figure 2 As shown. Test results show that sodium tetraphenylborate at ~3.2V (vs. Na + The charging decomposition begins at / Na) and is completely decomposed before 3.4V. Low-voltage sodium replenishment is completed in the early stage of the first charge of the battery to avoid electrolyte side reactions caused by high-voltage decomposition and to meet the core potential requirements of the pre-intercalated sodium material.
[0050] Cyclic performance and rate performance tests were conducted on the P2||HC coin cells in Example 1 and Comparative Example 1. The results are as follows: Figure 3 and Figure 4 As shown. Electrochemical performance test results show that after adding sodium tetraphenylborate, the initial discharge specific capacity of the P2||HC coin cell in Example 1 increased from 65 mAh·g in Comparative Example 1. -1Significantly increased to 163mAh·g -1 The sodium source compensation efficiency is significant, effectively compensating for the sodium source loss in the early stages of cycling of the P2-type cathode material; in the rate performance test, the specific capacity of the P2||HC coin cell in Example 1 remained at 136 mAh·g at current densities of 0.2C, 0.5C, 1C, 2C and 5C. -1 130mAh·g -1 116mAh·g -1 100mAh·g -1 and 67mAh·g -1 It exhibits excellent rate adaptability; after long-cycle testing at 2C current density, after 3700 cycles, the capacity retention rate of the P2||HC coin cell in Example 1 is still 72.08%, which is much higher than that of Comparative Example 1 (which has a retention rate of less than 50% after 1000 cycles).
[0051] Cyclic performance tests were conducted on the P2||HC pouch cells in Example 1 and Comparative Example 2, and the results are as follows: Figure 5 As shown. Charge-discharge tests were performed on the P2||HC pouch battery in Example 1, and the results are as follows. Figure 6 As shown. The performance test results of the P2||HC pouch battery in Example 1 show that the actual energy density of the P2||HC pouch battery reaches 184 Wh·kg. -1 (Based on total battery mass calculations), this is at an exceptionally high level in the industry; after 250 cycles, the battery capacity retention rate is 81.65%, and there are no obvious abnormalities such as bulging or leakage during the cycling process. The test results confirm that the pre-sodium intercalation method of this invention is not only suitable for small coin cells in the laboratory, but can also be stably adapted to large-capacity, electrolyte-poor practical soft-pack battery systems, demonstrating outstanding prospects for industrial application.
[0052] Optical photographs of the electrolytes prepared for sodium-ion batteries in Examples 2-5 are shown below. Figure 7 As shown. From Figure 7 As can be seen, sodium tetraphenylborate exhibits extremely high solubility in carbonate electrolytes, with a solubility as high as 273.6 g·L⁻¹. -1 It can form a stable and homogeneous system in carbonate electrolytes, ensuring sufficient sodium compensator concentration and providing a material basis for efficient sodium supplementation.
[0053] Charge-discharge tests were performed on the NVP||HC coin cells in Example 6 and Comparative Example 2, and the results are as follows: Figure 8 As shown. From Figure 8 As can be seen, sodium tetraphenylborate can efficiently supplement sodium in the NVP||HC system.
[0054] Charge-discharge tests were performed on the O3||HC coin cells in Example 7 and Comparative Example 3, and the results are as follows: Figure 9 As shown. From Figure 9 As can be seen, sodium tetraphenylborate can efficiently supplement sodium in the O3||HC system.
[0055] CV tests were performed on the 2032 coin cell in Comparative Example 4, and the results are as follows: Figure 10 As shown. From Figure 10 As can be seen from this, sodium tetra(4-fluorophenyl)borate at ~3.75V (vs. Na + Charging decomposition begins at / Na), with an oxidation peak still present near 4.0V. Its complete decomposition potential is high, making it prone to high-voltage decomposition and triggering side reactions in the electrolyte.
[0056] Charge-discharge tests were conducted on the 2032 coin cell half-cells in Comparative Examples 4-6, and the results are as follows: Figure 11 As shown. From Figure 11 It can be seen that sodium tetra(4-fluorophenyl)borate with different contents has a high decomposition potential and is difficult to efficiently replenish sodium.
[0057] Charge-discharge tests were conducted on the 2032 type coin cells in Comparative Examples 7-9, and the results are as follows: Figure 12 As shown. From Figure 12 As can be seen, sodium tetra(4-fluorophenyl)borate has good compatibility with different electrolytes, but it is still difficult to efficiently replenish sodium.
[0058] In summary, compared to sodium tetra(4-fluorophenyl)borate, sodium tetraphenylborate completes low-voltage sodium replenishment and has a higher sodium replenishment specific capacity during the initial charging of the battery, avoiding electrolyte side reactions caused by high-voltage decomposition and meeting the core potential requirements of pre-intercalated sodium materials.
[0059] The above description is only a specific embodiment of the present invention and not all embodiments. Any equivalent modifications made by those skilled in the art to the technical solutions of the present invention by reading the present invention specification shall be covered by the claims of the present invention.
Claims
1. An electrolyte for sodium-ion batteries, characterized in that, This includes boron-containing sodium replenishing agents and carbonate electrolytes used in sodium-ion batteries; The boron-containing sodium supplement is sodium tetraphenylborate; The carbonate electrolyte comprises sodium perchlorate, propylene carbonate, and vinylene carbonate; the ratio of sodium perchlorate to propylene carbonate is 1 mol: 1 L; the mass of vinylene carbonate is 1% of the total mass of sodium perchlorate and propylene carbonate. The mass ratio of the boron-containing sodium supplement agent and the carbonate electrolyte used in the sodium-ion battery is (5-22.8):
100.
2. A method for pre-intercalating sodium into a sodium-ion battery, characterized in that, Includes the following steps: The electrolyte for sodium-ion batteries as described in claim 1 is added to a sodium-ion battery to achieve pre-sodium intercalation in the sodium-ion battery.
3. A battery cell, characterized in that, Includes the electrolyte for sodium-ion batteries as described in claim 1.
4. The battery cell according to claim 3, characterized in that, It includes positive electrode material, negative electrode material, and the electrolyte for sodium-ion batteries as described in claim 1.
5. The battery cell according to claim 4, characterized in that, The cathode material includes P2 type cathode material, O3 type cathode material or sodium vanadium phosphate cathode material.
6. The battery cell according to claim 5, characterized in that, The P2 type cathode material includes Na. 0.67 Ni 0.08 Ti 0.12 Mn 0.8 O2; And / or, the O3-type cathode material includes NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
7. The battery cell according to claim 4, characterized in that, The negative electrode material includes hard carbon.
Citation Information
Patent Citations
Method for pre-embedding sodium into sodium-ion battery at low temperature
CN121769241A