Ceramic proppant with hydrogen sulfide scavenging function and method of making same
Patent Information
- Application Number
- CN202610991723.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-06
- Publication Date
- 2026-09-08
- Estimated Expiration
- 2046-07-06
AI Technical Summary
然而,该类覆膜支撑剂主要依赖物理屏障作用,对H2S的化学清除能力有限,且树脂涂层在高温高压、高速流体冲刷及含硫腐蚀环境下易发生软化、蠕变变形甚至剥落,导致防护功能失效
[0040] This invention introduces pretreated short-cut steel fibers into the inner core, utilizing their high modulus properties to effectively suppress microcrack propagation in the ceramic matrix through bridging and pull-out effects. Simultaneously, the walnut shell powder pore-forming agent, while reducing density, combined with the strong toughening effect of the steel fibers, ensures that the proppant maintains extremely high compressive strength and fracture toughness under high closure pressure in deep wells, significantly reducing the breakage rate and fine powder generation, thereby maintaining high conductivity of oil and gas fractures over the long term.
Smart Images

Figure CN122482837B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hydraulic fracturing in oil and gas engineering, specifically to a ceramic proppant with hydrogen sulfide removal function and its preparation method. Background Technology
[0002] Currently, with the continuous increase in oil and gas extraction depth, the downhole environment is becoming increasingly complex, and the performance requirements for ceramic proppant are becoming increasingly stringent.
[0003] However, existing technologies generally lack adaptability to complex geological environments, especially in terms of protection against harsh conditions containing hydrogen sulfide (H2S).
[0004] Existing technological research mainly focuses on reducing density, improving compressive strength, and low-temperature sintering. For example, a lightweight, high-strength ceramsite proppant based on composite coating and low-temperature densification, with application number CN202511393580.X, uses bauxite, perlite, composite sintering aids (MnO2 / TiO2), B2O3, and AlF3 as raw materials. A ceramsite matrix is prepared through graded granulation and sintering, and then coated on its surface with a composite coating layer composed of expanded perlite and epoxy resin, aiming to achieve low-temperature sintering, reduce density, and improve compressive strength. However, this type of coated proppant mainly relies on physical barrier effects, with limited chemical removal capabilities for H2S. Furthermore, the resin coating is prone to softening, creep deformation, and even peeling under high temperature, high pressure, high-speed fluid erosion, and sulfur-containing corrosive environments, leading to failure of its protective function.
[0005] Hydrogen sulfide is a common associated gas in oil and gas extraction, and its hazards are twofold: on the one hand, H2S is highly toxic, and leaks can easily lead to serious safety accidents; on the other hand, the weak acid formed when H2S dissolves in water can severely corrode downhole tubing and surface equipment, and cause hydrogen embrittlement fracture of the proppant itself. Relying solely on traditional physical propping methods not only fails to eliminate the hydrogen sulfide hazard in the formation, but during long-term service, the fine powder generated from proppant breakage may also react with sulfides, exacerbating formation damage.
[0006] Therefore, it is urgent to find a way to ensure the basic physical properties of ceramsite proppant, such as its lightweight and high strength, while also possessing the chemical function of efficiently removing hydrogen sulfide. Summary of the Invention
[0007] One objective of this invention is to provide a ceramic proppant with hydrogen sulfide removal function and its preparation method, thereby obtaining a lightweight, high-strength ceramic proppant that can efficiently remove hydrogen sulfide.
[0008] A method for preparing a ceramic proppant with hydrogen sulfide scavenging function includes the following steps:
[0009] Step 1: A first slurry is obtained by wet ball milling bauxite, coal gangue, interface-optimized composite sintering aid, pretreated chopped steel fibers, walnut shell powder, and deionized water; the first slurry is dried and then ground, and after grinding and sieving, a first powder is obtained.
[0010] Step 2: A second slurry is obtained by wet ball milling bauxite, coal gangue, interface-optimized composite sintering aid, walnut shell powder, and deionized water; the second slurry is dried and then ground, and after grinding and sieving, a second powder is obtained.
[0011] Step 3: Place the first powder in a sugar coating machine, granulate it through a polyvinyl alcohol solution, and sieve out a first green body with a mesh size of 70-80; evenly add the second powder and polyvinyl alcohol solution to the first green body so that the second powder coats the surface of the first green body, and sieve out a spherical second green body with a mesh size of 50-70.
[0012] Step 4: The second green body is subjected to gradient sintering under a protective atmosphere to obtain the inner layer structure. The gradient sintering specifically includes: the second green body is heated to 600℃ at 2℃ / min and held at that temperature for 30-60 minutes under a protective atmosphere to remove the binder. After removing the binder, the temperature is increased to 1000℃ at 5℃ / min, and then increased to 1255-1300℃ at 3℃ / min and held at that temperature for 60-90 minutes to obtain the inner layer structure.
[0013] Step 5: The treated zinc-containing dust and kaolin are placed in a planetary mill and mixed. After mixing, starch is added and mixed to obtain composite powder. The composite powder is then sieved to obtain shell functional powder.
[0014] Step 6: Add the inner layer structure to the coating machine, spray the adhesive solution intermittently to make the surface of the inner layer structure matte, then add the shell functional powder, roll it to make the inner layer structure free from adhesion, and complete the coating operation.
[0015] Step 7: Repeat step 6 to complete 5-8 coating operations to obtain the coated core-shell structure;
[0016] Step 8: Under a protective atmosphere, the coated core-shell structure is heated from room temperature to 450°C at a rate of 1.5°C / min and held at this temperature for 60-90 minutes to remove the adhesive. This process decomposes and removes all polyvinyl alcohol (PVA) and starch organic matter from the shell preform. Slow heating and sufficient holding prevent the rapid pyrolysis of organic matter from generating large amounts of gas, which could lead to bubbling, cracking, or even peeling from the core. This stage requires ensuring complete removal of organic matter to avoid carbon buildup.
[0017] After debinding, the temperature is increased from 450℃ to 800-950℃ at a rate of 3℃ / min and held for 30 minutes. Within this temperature range, the kaolin completes dehydration and undergoes a preliminary solid-phase reaction, beginning to form a stable ceramic phase, which imparts a certain mechanical strength to the shell. Simultaneously, the zinc compounds in the zinc-containing flue dust are fully activated, transforming into highly reactive zinc oxide, which undergoes slight solid-phase diffusion with the core ceramic surface, whose main components are Al2O3 and SiO2, forming a preliminary chemical bonding interface, laying the foundation for a final strong bond. When the kaolin content in the shell formulation is high, 950℃ is selected to promote its transformation; if zinc oxide is the main component, 800-850℃ is selected to reduce its volatilization.
[0018] After initial heating, the temperature is increased to 1220-1250℃ at a rate of 5℃ / min and held for 15-30 minutes to obtain the ceramic proppant. This rapid heating stage is used to quickly overcome the temperature range where zinc oxide volatilization intensifies (>1100℃), preserving as many active components as possible in the shell layer. At the final sintering temperature, the shell material generates a suitable liquid phase, undergoing rapid densification, with zinc oxide particles tightly encapsulated and fixed within the dense ceramic framework. Simultaneously, the higher temperature promotes more complete elemental diffusion and solid-phase reaction at the interface between the shell and the core, forming a strong chemical bond and mechanical interlocking structure. Short holding time ensures sufficient shell densification while preventing excessive zinc oxide volatilization or grain coarsening, thus maintaining its large specific surface area and good H2S reactivity.
[0019] Preferably, the interface-optimized composite sintering aid includes spodumene and titanium dioxide. Spodumene releases active Li at high temperatures. + This reduces the liquid phase formation temperature, lowering the core pre-sintering temperature from the traditional 1300-1350℃ to 1255-1300℃, saving energy and reducing fiber oxidation; Li + The spodumene migrates to the surface of the steel fiber and reacts with Fe on the fiber surface and Al2O3 and SiO2 in the ceramic matrix to generate tough interfacial phases such as lithium iron spinel (LiFe5O8) or lithium iron olivine (Fe2SiO4) in situ at the interface. The generated interfacial phase has high toughness, forming a flexible interfacial layer that buffers the thermal expansion mismatch between ceramic and metal, and increases the interfacial shear strength to ≥15MPa. Among them, spodumene and TiO2 work together to reduce the sintering temperature while promoting matrix densification and fiber wetting.
[0020] Furthermore, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, pretreated chopped steel fiber, and walnut shell powder is (65~75): (26~35): (2~5): (0.5~2): (3~7): (4~6).
[0021] This invention utilizes high-modulus steel fibers to construct a three-dimensional network within a ceramic matrix. When the ceramic particles are subjected to formation closure pressure, the steel fibers consume a large amount of fracture energy through bridging and pull-out effects, forcibly preventing the propagation and penetration of microcracks.
[0022] Walnut shell powder, as a pore-forming agent, will be completely burned and decomposed during high-temperature sintering, leaving a large number of uniformly distributed micron-sized closed pores inside the dense ceramic matrix.
[0023] The micropores created by walnut shell powder effectively reduce the bulk density of the ceramsite, thus achieving a lightweight effect and solving the problem of excessive density in traditional high-strength ceramsite. Meanwhile, the high content of steel fibers compensates for the strength loss that may occur due to pore formation and the introduction of coal gangue, ensuring that the inner core has extremely high resistance to breakage. Furthermore, the invention utilizes a large amount of coal gangue and walnut shell powder, significantly reducing the amount of bauxite used and substantially lowering raw material costs.
[0024] Furthermore, in step 2, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is (65~75): (26~35): (2~5): (0.5~2): (0.5~1.5). Although the outer layer also needs to be lightweight, its density is crucial due to direct contact with sulfur-containing fluids. A very small amount of walnut shell powder is used only for fine-tuning density and assisting in material transport during sintering, avoiding the formation of excessive interconnected channels. The outer layer does not contain steel fibers to ensure the chemical homogeneity and density of the shell, prevent metal fibers from forming anodes for electrochemical corrosion on the surface, and ensure that the active zinc component is uniformly distributed in the continuous ceramic phase. The low porosity ensures that the shell has sufficient mechanical strength to resist fluid erosion, while ensuring the stability of the reaction between the active zinc component and hydrogen sulfide. The outer and inner layers are both composed of bauxite and coal gangue, which ensures that the core and shell have similar coefficients of thermal expansion during high-temperature sintering, preventing the core and shell from delaminating or peeling off due to differences in thermal stress.
[0025] In addition, in step 5, the industrial zinc-containing dust is washed with water to remove soluble chlorine and fluorine impurities. After washing, a precipitant is added to remove heavy metals. After calcination at 400-500 ℃, it is ground and homogenized to obtain the treated zinc-containing dust. The weight ratio of the treated zinc-containing dust, kaolin, and starch is (60-70):(25-30):(5-10). Industrial zinc-containing dust usually contains chloride ions, sulfate ions, and heavy metal impurities such as lead and cadmium. Washing and precipitants are used to remove these impurities and prevent chloride ions from corroding equipment at high temperatures or causing frost on the surface of the ceramsite. Calcination at 400-500 ℃ is to thoroughly remove organic matter and water of crystallization, improving the purity and reactivity of the raw materials.
[0026] This step effectively removes harmful impurities and enhances the activity of the zinc component, resulting in a stable, efficient, and environmentally friendly final product. Kaolin, acting as the ceramic binder and framework material for the shell, dehydrates during sintering and forms mullite and other crystalline phases, creating a robust network structure that firmly anchors the active zinc oxide particles, preventing them from detaching during use. Starch, acting as a pore-forming agent and green body reinforcing agent, decomposes at low temperatures. This not only creates abundant micro- and nano-scale pores within the shell, significantly increasing the specific surface area and the number of reactive sites, accelerating the diffusion of H2S gas to the zinc oxide particle surface, but also helps improve the initial strength of the shell after green body drying, preventing powder loss during subsequent transport.
[0027] The high weight percentage of zinc-containing dust after treatment is to provide sufficient reactive components such as zinc oxide to react with hydrogen sulfide. Kaolin serves as a high-temperature resistant binder skeleton, providing an aluminum-silicon source and forming a stable ceramic bond with the zinc-containing dust at high temperatures. Starch acts as a high-temperature pore-forming agent and green body binder. Starch decomposes and creates pores in the early stages of sintering, further reducing the shell density and, more importantly, forming an open microporous structure that significantly increases the specific surface area of the shell.
[0028] Therefore, the zinc-containing dust produced through purification and calcination in this step has extremely high activity. Combined with the abundant microporous channels formed by starch pore-forming, hydrogen sulfide gas can rapidly diffuse into the shell, fully contacting and reacting with the active zinc to form zinc sulfide, thus improving the removal efficiency of hydrogen sulfide. Furthermore, the pre-removal of heavy metals and harmful impurities avoids secondary environmental pollution caused by the proppant during its downhole operation, meeting the requirements of green mining.
[0029] In summary, the inner layer structure of this invention mainly provides physical support. By introducing short-cut steel fibers, bauxite, and coal gangue, the overall compressive strength is improved while ensuring low density by utilizing the toughening effect of steel fibers and the densification effect of sintering aids. The inner layer structure is also equipped with shell functional powder, which introduces active components such as zinc-containing dust to form highly efficient H2S adsorption / reaction sites.
[0030] The dense surface layer of the ceramsite proppant obtained by this invention bears the main load, while the inner layer structure buffers the stress. The ceramsite proppant forms a mechanical structure with a dense surface and porous interior, which helps to improve the overall fracture resistance and interfacial bonding strength; the inner layer structure is conducive to achieving low density.
[0031] Specifically, the first green body includes pretreated chopped steel fibers, which are derived from waste steel fibers (such as machined wire and cut waste) generated in industries such as machining and metal products. To address the issue of inconsistent morphology and size of the original waste steel fibers, this invention pretreats the chopped steel fibers, specifically by: screening fiber segments with a length of 0.05-0.1 mm and a diameter of 5-15 μm from the waste steel fibers; immersing the screened fiber segments in a 5-10 wt% NaOH solution at 60-80°C for 20-30 minutes; rinsing the fiber segments until neutral; immersing the neutralized fiber segments in a 5-10 wt% dilute hydrochloric acid solution for 5-15 minutes; rinsing them until neutral; drying them; and then phosphating them with a zinc-based phosphating solution at 50-70°C for 3-8 minutes to obtain the pretreated chopped steel fibers.
[0032] Zinc-based phosphating treatment forms a dense phosphate conversion film with a high specific surface area on the surface of steel fibers. This not only improves the corrosion resistance of the fibers, but more importantly, it greatly enhances the mechanical bonding force and interfacial compatibility between the steel fibers and inorganic powder slurries such as bauxite and coal gangue. This prevents interfacial debonding during subsequent high-temperature sintering, thereby ensuring that the steel fibers can effectively play their role in toughening and reinforcing.
[0033] The preferred particle size of the ceramic proppant prepared by this invention is 30-50 mesh. Its inner core layer contains chopped steel fibers pretreated with phosphate, forming a high-strength and high-toughness physical support skeleton that effectively resists breakage under closing pressure; while the outer shell layer utilizes the active zinc component in zinc-containing dust to achieve efficient in-situ removal of hydrogen sulfide, thus possessing both excellent mechanical properties and chemical protection functions.
[0034] Traditional ceramic proppant acts only as a physical support and cannot effectively remove highly toxic and corrosive hydrogen sulfide commonly found in formations. This invention utilizes the active zinc component in the outer shell to enable the proppant to remove hydrogen sulfide. When downhole fluids containing hydrogen sulfide flow across the proppant surface, the active zinc component reacts chemically with the hydrogen sulfide to form a stable zinc sulfide (ZnS) solid precipitate, converting the harmful gas into a harmless solid substance. This reduces the risk of safety accidents caused by hydrogen sulfide leaks and effectively protects downhole tubing and surface equipment from acid corrosion, achieving the dual effect of propping and desulfurization.
[0035] Existing technologies attempt to isolate hydrogen sulfide by coating the surface of ceramic particles with physical barriers such as epoxy resin. However, under the high temperature, high pressure, and high-speed fluid erosion environment of deep wells, organic resin coatings are prone to softening, creep deformation, and even peeling, leading to rapid failure of the protective function. This invention employs a high-temperature sintered inorganic mineralized shell, which is fused with the ceramic particle matrix through a gradient sintering process, forming a dense and stable chemically bonded interface. This structure exhibits good thermal stability and chemical inertness under the extreme environment of deep wells, and unlike organic coatings, it will not undergo physical softening or chemical degradation, ensuring the reliability and durability of the chemical protection function during long-term service.
[0036] Secondly, traditional ceramsite is prone to microcracks and propagation under long-term alternating loads, resulting in a high breakage rate. The generated fine powder can clog oil and gas flow channels, exacerbating damage to the formation. This invention addresses this by incorporating zinc-phosphated short-cut steel fibers. The bridging effect of the steel fibers effectively prevents the propagation of cracks in the ceramic matrix. Simultaneously, the phosphate treatment forms a porous phosphate conversion film on the steel fiber surface, enhancing the interfacial bonding between the metal fibers and the inorganic ceramic matrix, preventing interfacial debonding during high-temperature sintering and service. This allows the ceramsite proppant of this invention to maintain its lightweight nature while possessing excellent compressive strength and fracture toughness, significantly reducing the breakage rate and minimizing the damage to formation conductivity caused by broken fine powder.
[0037] This invention uses zinc-containing dust from industrial solid waste as a raw material for removing hydrogen sulfide, which not only achieves the harmless and resource-based utilization of hazardous waste and solves the environmental pollution problem caused by its stockpiling and disposal, but also significantly reduces the raw material cost of functional ceramsite proppant.
[0038] Furthermore, the present invention proposes a second objective: to prepare a ceramic proppant using the above-described preparation method.
[0039] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0040] This invention introduces pretreated short-cut steel fibers into the inner core, utilizing their high modulus properties to effectively suppress microcrack propagation in the ceramic matrix through bridging and pull-out effects. Simultaneously, the walnut shell powder pore-forming agent, while reducing density, combined with the strong toughening effect of the steel fibers, ensures that the proppant maintains extremely high compressive strength and fracture toughness under high closure pressure in deep wells, significantly reducing the breakage rate and fine powder generation, thereby maintaining high conductivity of oil and gas fractures over the long term.
[0041] The active zinc component of this invention can rapidly undergo a chemical precipitation reaction with highly toxic hydrogen sulfide in downhole fluids to generate stable zinc sulfide solids, achieving active capture and in-situ harmless removal of hydrogen sulfide. This inorganic mineralized protective layer formed by high-temperature eutectic melting has excellent thermal stability and chemical inertness, solving the problems of short protective life and easy failure of organic coatings.
[0042] This invention avoids the risks of core-shell delamination, cracking, or peeling caused by differences in thermal stress. The microporous structure formed by starch pore-forming in the outer layer not only further reduces the weight of the shell but also significantly increases the specific surface area, providing ample channels for the diffusion and reaction of hydrogen sulfide, thus greatly improving desulfurization efficiency.
[0043] Furthermore, while achieving the harmless treatment of hazardous waste, this invention reduces the amount of expensive primary minerals such as bauxite and the raw material cost of functional proppant. Attached Figure Description
[0044] The accompanying drawings, which are included to provide a further understanding of embodiments of the invention and form part of this application, do not constitute a limitation thereof. In the drawings:
[0045] Figure 1 Here is a SEM image of the ceramsite proppant obtained in Example 1; Figure 1 (a) shows the cross-sectional morphology of the ceramsite proppant; Figure 1 (b) The distribution of steel fibers in the ceramsite proppant at 2000x magnification; Figure 1 (c) shows the morphology of the ceramsite proppant skeleton structure at 10,000x magnification; Figure 1 (d) shows the distribution of steel fibers in the ceramsite proppant at a magnification of 10,000.
[0046] Figure 2 Optical images of the ceramic proppant prepared in Example 1 with three different particle sizes: 30 mesh, 40 mesh, and 50 mesh.
[0047] Figure 3 Cross-sectional optical images of the ceramic proppant prepared in Example 1 with three different particle sizes: 30 mesh, 40 mesh, and 50 mesh. Detailed Implementation
[0048] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments and accompanying drawings. However, this does not limit the invention to the scope of the embodiments described. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.
[0049] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0050] Example 1
[0051] A method for preparing a ceramic proppant with hydrogen sulfide scavenging function, characterized by comprising the following steps:
[0052] Step 1: Prepare the inner layer structure;
[0053] Step 11: Prepare pretreated chopped steel fibers;
[0054] Fiber segments with a length of 0.05-0.1 mm and a diameter of 5-15 μm were screened from waste steel fibers. These segments were then immersed in a 5-10 wt% NaOH solution at 60-80℃ for 20-30 minutes with stirring to remove surface grease. Afterward, the fibers were rinsed with water until neutral and then subjected to alkaline washing to remove further grease. At room temperature, the neutralized fiber segments were immersed in a 5-10 wt% dilute hydrochloric acid solution for 5-15 minutes to remove the surface oxide layer and rust. They were then repeatedly rinsed with deionized water until neutral and dried in an oven at 80-100℃ for 1-2 hours. Finally, they were phosphated in a zinc-based phosphating solution at 50-70℃ for 3-8 minutes to form an active surface conducive to interfacial bonding. After rinsing with water and drying in an oven at 80℃, the pretreated chopped steel fibers were obtained.
[0055] Step 12: A planetary ball mill is used to wet-mill bauxite, coal gangue, an interface-optimized composite sintering aid, pretreated chopped steel fibers, walnut shell powder, and deionized water at 400 r / min for 4 hours to obtain a first slurry. The first slurry is then dried at 120℃ for 24 hours, ground, and passed through a 350-mesh sieve to obtain a first powder. The interface-optimized composite sintering aid includes spodumene and titanium dioxide. The weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, pretreated chopped steel fibers, and walnut shell powder is 70:30:3:1.5:5:5.
[0056] Step 13: A second slurry is obtained by wet milling bauxite, coal gangue, interface-optimized composite sintering aid, walnut shell powder, and deionized water in a planetary ball mill at 400 r / min for 4 hours. This slurry is then dried at 120℃ for 24 hours, ground, and passed through a 350-mesh sieve to obtain the second powder. The weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is 70:30:3:1.5:1.
[0057] Step 14: Place the first powder in a coating machine and roll it at 50 r / min. Spray it with a 1.5% polyvinyl alcohol solution for granulation and sieve out a 70-80 mesh first green body. Then, while continuing to roll, evenly add the second powder and polyvinyl alcohol solution to the first green body so that the second powder coats the surface of the first green body and sieve out a 50-70 mesh spherical second green body. The second green body is the gradient structure green body.
[0058] Step 15: The second green body is placed in a tube furnace and heated to 600°C at 2°C / min under a protective atmosphere for 30 minutes to remove the binder. Then, it is heated to 1000°C at 5°C / min and finally heated to 1280°C at 3°C / min and held for 70 minutes. The inner layer structure is obtained by cooling with the furnace.
[0059] Step 2: Prepare the coated core-shell structure;
[0060] Step 21: Prepare the treated zinc-containing fume;
[0061] Zinc-containing fume dust was mixed with deionized water at a weight ratio of 1:5 and washed. After washing, the mixture was stirred at room temperature for 30 minutes and then filtered. This process was repeated 2-3 times until the Cl in the filtrate was reduced. - and F - The concentration is reduced to remove most of the soluble chlorine and fluorine impurities, resulting in a filter cake. Sodium sulfide solution is added to the filter cake, and the pH is controlled at 8-10. The mixture is stirred at 60-80℃ for 1-2 hours to cause heavy metal ions such as lead and cadmium to precipitate as insoluble sulfides. The precipitate is filtered, washed, and then calcined at 400-500℃ for 1.5-3 hours to convert amorphous or complex zincates into highly reactive zinc oxide, while removing residual organic matter and moisture. The calcined precipitate is ground to a particle size of ≤8μm and homogenized to obtain treated zinc-containing dust. The main active component of the treated zinc-containing dust is highly reactive zinc oxide, with a ZnO content ≥78wt%, total soluble chlorine and fluorine impurities ≤0.08wt%, and lead content ≤0.03wt%.
[0062] Step 22: Prepare shell functional powder;
[0063] The treated zinc-containing dust and kaolin were mixed in a planetary mill for 60 minutes. Starch was then added, and mixing continued for another 20 minutes to obtain a composite powder. This composite powder was then passed through a 300-mesh sieve to obtain the shell-forming functional powder. The weight ratio of the treated zinc-containing dust, kaolin, and starch was 70:25:5. Passing through a 300-mesh sieve effectively dispersed the soft agglomerates generated during mixing, resulting in a fine powder with excellent flowability, ensuring uniform adhesion to the core surface during coating.
[0064] Step 23, wrapping operation;
[0065] The inner layer structure is incorporated into the coating machine, with the machine parameters set as follows: pot rotation speed 40 rpm, temperature 60℃. The pot rotation speed is controlled at 30–50 rpm, at which point the core particles tumble in a rope-like pattern, facilitating even reception of the spray and powder, while preventing excessive rotation speed and centrifugal force that could cause particles to adhere to the walls. The pot heating temperature is set at 55–65℃ to gently evaporate surface moisture and prevent particle adhesion. Pressure spraying creates fine droplets, enabling precise wetting in small, multiple applications, avoiding localized over-wetting.
[0066] After intermittently spraying in an adhesive solution, namely a 1.5% PVA solution, to make the surface of the inner layer structure matte, add the shell functional powder, and roll and dry for 4 minutes to make the inner layer structure free of adhesion, thus completing the coating operation.
[0067] Repeat the coating process 5-8 times, sampling and sieving to monitor particle size every 6 cycles until the vast majority of particles reach a size of 30-50 mesh, then stop coating to obtain the coated core-shell structure. Compared to traditional one-time coating, the cyclic coating method effectively avoids problems such as powder agglomeration, uneven coating, and loose shell. A 1.5% PVA aqueous solution is used; too high a concentration will lead to poor spray atomization and excessively thick coating that easily sticks together; too low a concentration will result in insufficient adhesion. Fully dissolve the PVA particles in hot water above 90℃, and filter after cooling to remove incompletely dissolved gel particles, ensuring a clear solution with stable viscosity, thus forming uniform and fine droplets during spraying.
[0068] Step 3: Prepare ceramic proppant;
[0069] Under a protective atmosphere, the coated core-shell structure is heated from room temperature to 450°C at a rate of 1.5°C / min and held for 60-90 minutes to remove the adhesive. After adhesive removal, the temperature is increased from 450°C to 800-950°C at a rate of 3°C / min and held for 30 minutes. After holding, the temperature is increased to 1220-1250°C at a rate of 5°C / min and held for 15-30 minutes to obtain the ceramic proppant with a particle size of 30-50 mesh.
[0070] Example 2
[0071] Based on Example 1, in this example, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, pretreated chopped steel fibers, and walnut shell powder is 70: 30: 2: 0.5: 3: 4.
[0072] In step 13, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is 70: 30: 2: 0.5: 0.5.
[0073] The weight ratio of the treated zinc-containing dust, kaolin, and starch is 65:30:5.
[0074] The remaining steps are the same as in Example 1.
[0075] Example 3
[0076] Based on Example 1, in this example, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, pretreated chopped steel fibers, and walnut shell powder is 70:30:5:2:7:6.
[0077] In step 13, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is 70: 30: 5: 2: 1.5.
[0078] The weight ratio of the treated zinc-containing dust, kaolin, and starch is 60:30:10.
[0079] The remaining steps are the same as in Example 1.
[0080] Comparative Example 1
[0081] This comparative example uses a one-step molding and sintering method. Based on Example 1,
[0082] The comparative example uses the traditional one-time molding and sintering method: the shell functional powder of Example 1 is physically dry mixed with the second powder to obtain a mixture.
[0083] The first powder of Example 1 was placed in a sugar coating machine and rolled at a speed of 50 r / min. A 1.5% polyvinyl alcohol solution was sprayed on it for granulation, and a first green body of 70-80 mesh was screened out. Then, while keeping it rolling, the mixture and polyvinyl alcohol solution were evenly added to the first green body so that the mixture coated the surface of the first green body to obtain the green body.
[0084] The green body was placed in a tube furnace and heated to 600°C at 2°C / min for 30 min under a protective atmosphere. Then, the temperature was increased to 1000°C at 5°C / min and finally increased to 1280°C at 3°C / min and held for 70 min. The ceramsite support was obtained by cooling in the furnace.
[0085] Comparative Example 2
[0086] In this embodiment, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, pretreated chopped steel fibers, and walnut shell powder is 70:30:5:2:7:3.
[0087] In step 13, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is 70: 30: 5: 2: 3.
[0088] Comparative Example 3
[0089] Based on Example 1, this comparative example does not include pretreated chopped steel fibers. In step 12, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is 70:30:3:1.5:5.
[0090] Comparative Example 4
[0091] Based on Example 1, the pretreated chopped steel fibers were replaced with a composite additive of MnO2 and TiO2.
[0092] In this comparative example, in step 12, the weight ratio of bauxite, coal gangue, MnO2, TiO2, and walnut shell powder is 70:30:5.5:1:5.
[0093] Comparative Example 5
[0094] Based on Example 1, this comparative example does not include treated zinc-containing dust. The shell functional powder comprises kaolin and starch in a weight ratio of 25:5.
[0095] Comparative Example 6
[0096] Based on Example 1, this comparative example replaces the treated zinc-containing fume with inert ceramic powder.
[0097] The shell functional powder comprises calcined α-alumina powder, kaolin, and starch. The weight ratio of calcined α-alumina powder, kaolin, and starch is 65:30:5.
[0098] Comparative Example 7
[0099] Based on Example 1, this comparative example omits step 15. In step 23, the second green preform is added to the coating machine to complete the coating operation; under a protective atmosphere, the coated second green preform is heated from room temperature to 450°C at a heating rate of 1.5°C / min and held for 60-90 minutes to remove the glue; after glue removal, the temperature is increased from 450°C to 800-950°C at a heating rate of 3°C / min and held for 30 minutes; after holding, the temperature is increased to 1220-1280°C at a heating rate of 5°C / min and held for 15-30 minutes to obtain the ceramsite support agent.
[0100] Comparative Example 8
[0101] Based on Example 1, the ceramic proppant is prepared in step 3 of this comparative example;
[0102] Under a protective atmosphere, the coated core-shell structure is heated from room temperature to 450°C at a heating rate of 1.5°C / min and held at that temperature for 60-90 minutes to remove the adhesive. After removing the adhesive, the temperature is increased to 1220-1280°C at a heating rate of 5°C / min and held at that temperature for 15-30 minutes to obtain the ceramic proppant.
[0103] Experimental Example
[0104] The ceramic proppant obtained in Examples 1-3 and Comparative Examples 1-8 were tested for bulk density, apparent density, fragmentation rate after H2S removal simulation, and H2S removal capacity assessment. Bulk density and apparent density were determined according to the People's Republic of China Petroleum and Natural Gas Industry Standard SY / T5108-2014 "Test Methods for Fracturing Proppants". The fragmentation rate after H2S removal simulation was tested according to SY / T5108-2014, under a closing pressure of 52 MPa.
[0105] The breakage rate of the proppant after H2S removal was determined using a simulated heat treatment method. The specific steps were as follows: Equal masses of ceramic proppant samples were taken and treated at 150℃ for 48 hours under a nitrogen atmosphere to simulate the thermal history environment of H2S removal; subsequently, the samples were dried at 80℃ for 2 hours, and the breakage rate under a closure pressure of 52 MPa was tested according to the SY / T5108-2014 standard. The scientific basis of this method is that the volume expansion (approximately 66%) during the reaction of ZnO with H2S to form ZnS in the shell can be completely buffered and absorbed by the microporous structure (porosity approximately 25%) formed by starch pores in the shell, without damaging the integrity of the ceramic framework. Therefore, the mechanical properties of the sample after simulated heat treatment are consistent with those of the sample after the actual reaction.
[0106] The H2S chemical scavenging capacity was assessed using an indirect evaluation method. Specifically, 5g of proppant sample was ground to a fineness below 200 mesh, and the mass fraction W of ZnO was determined by X-ray fluorescence spectroscopy (XRF). ZnO (Unit: wt%). Each sample was measured in triplicate, and the average value was taken.
[0107] Based on the stoichiometric ratio, each mole of ZnO (81.38 g / mol) can remove 1 mole of H₂S (34.08 g / mol). The theoretical maximum adsorption capacity Q. max Calculate using the following formula:
[0108] ;
[0109] The thermal behavior of the sample under simulated reaction conditions was verified using a thermogravimetric analyzer (TGA). 10 mg of sample was heated to 150 °C at a rate of 10 °C / min under a nitrogen atmosphere, held at this temperature for 30 min to remove physically adsorbed water, and then the mass change was recorded at this temperature. Since no chemical reaction occurs in nitrogen, this step aims to confirm that the sample does not undergo thermal decomposition at 150 °C (mass loss <0.5 wt%), thus ensuring the reliability of the stoichiometric calculation of ZnO. Combining the data from the literature (Ciro, Erwin, Dell'Era, et al. Kinetics and thermodynamics of wet desulfurization reaction of ZnO adsorbent at high temperature [J]. Energies, 2023, Vol. 16(2): 792.) and the analysis of the shell structure in this invention, the reaction conversion efficiency of ZnO and H2S in the shell can reach over 85% (conservative value) under 150 °C and atmospheric pressure conditions, therefore η = 85%. Actual saturated adsorption capacity Q 实际 This is the H2S chemical scavenging capacity assessment value.
[0110] Q 实际 =Q max ×η;
[0111] The test results are shown in Table 1.
[0112]
[0113] As shown in Table 1, Examples 1-3 all exhibited low densities, i.e., 1.40-1.45 g / cm³. 3 The invention features a low breakage rate and excellent H2S removal capability. This is because the inner layer of the invention utilizes a three-dimensional toughened network constructed with high-modulus phosphated chopped steel fibers, combined with walnut shell powder for pore creation. This achieves lightweight design while significantly enhancing compressive strength through fiber bridging and pull-out effects, resulting in an extremely low breakage rate. The outer layer utilizes zinc-containing dust to provide ample active ZnO, combined with microporous channels formed by starch pore creation, ensuring extremely high H2S chemical removal efficiency.
[0114] Comparative Example 1 showed a significantly increased density and a substantial increase in breakage rate, from 9.1% to 12.5%, along with a decrease in H2S removal capacity. Comparative Example 1 employed a traditional one-step molding and sintering method, directly incorporating the shell functional powder into the inner layer. Due to the high proportion of heavy metal oxides in the shell, direct mixing resulted in a significant increase in overall density, negating its lightweight advantage. Furthermore, the active ZnO component was dispersed throughout the matrix, failing to form an efficient desulfurization enrichment layer on the surface and disrupting the continuity of the inner ceramic matrix and the toughening effect of the steel fibers, leading to a sharp deterioration in mechanical properties.
[0115] The data for Comparative Example 2 fall between those of Example 1 and Example 3, showing good overall performance, but slightly inferior to the optimal Example 1. Comparative Example 2 adjusted the proportions of spodumene, titanium dioxide, steel fiber, and the shell layer. The data indicate that although the present invention has good tolerance within a certain range, the formulation of Example 1 maximizes the synergistic effect of mechanical strength and chemical desulfurization efficiency while ensuring lightweight properties.
[0116] Comparative Example 3 had a similar density to Example 1, but its breakage rate was significantly higher. The H2S removal capacity of Comparative Example 3 was assessed at 130 mg / g, slightly lower than that of Example 1. Pretreated chopped steel fibers were removed from the inner layer formulation of Comparative Example 3. Although the pore-forming effect of the walnut shell powder still ensured the product's lightweight nature, the loss of the bridging and toughening effect of the steel fibers in the ceramic matrix led to a significant decrease in the material's fracture toughness under a high closure pressure of 52 MPa, resulting in a substantial increase in the breakage rate. However, the shell formulation remained unchanged, therefore the desulfurization capacity was unaffected.
[0117] Comparative Example 4 replaced the phosphated steel fibers with a composite additive of MnO2 and TiO2, resulting in a slight decrease in density, but a significantly higher breakage rate than Example 1. Without the physical toughening effect of the steel fibers, conventional sintering aids alone could not effectively inhibit crack propagation in the ceramic matrix, leading to a decrease in strength. This indirectly confirms that the introduction of high-modulus steel fibers for physical toughening in this invention has irreplaceable advantages over simply relying on chemical composition adjustments in improving the fracture resistance of the proppant.
[0118] Comparative Example 5, lacking zinc-containing dust in its shell, exhibited almost zero H2S removal capacity (<5 mg / g) and a higher breakage rate. The shell's loss of active ZnO directly resulted in the product losing its core H2S removal function. Furthermore, the removal of a high proportion of zinc-containing dust from the shell formulation, leaving only kaolin and starch, led to insufficient strength in the resulting ceramic skeleton after sintering. The porous structure was also prone to collapse under high pressure, failing to effectively distribute the load, thus increasing the overall breakage rate. This demonstrates that zinc-containing dust is not only a functional component for desulfurization but also a crucial element in maintaining the shell's structural strength.
[0119] Comparative Example 6 replaced zinc-containing flue dust with inert α-alumina powder, resulting in an H2S removal capacity assessment value of less than 5 mg / g and a breakage rate increase to 8.5%. Similar to Comparative Example 5, replacing the active component led to the failure of the desulfurization function. Although inert alumina powder has high hardness, its thermal expansion coefficient is poorly matched with that of the inner core, and it cannot form a good solid-phase diffusion bond with the matrix during sintering like the active zinc component, resulting in a weakened interfacial bond between the shell and the core. Under the thermal stress and external high pressure following the simulated H2S reaction, the shell is prone to cracking and peeling, leading to a sharp deterioration in the breakage rate.
[0120] Comparative Example 7, employing a one-step encapsulation molding process, resulted in a higher breakage rate than Example 1. Direct integral encapsulation and sintering leads to a significant difference in thermal stress between the inner layer (containing steel fibers) and the outer layer during sintering shrinkage. Due to the lack of a stable framework formed by pre-sintering, microcracks or delamination easily occur at the interface between the inner and outer layers. This structural defect becomes a stress concentration point during high-pressure testing, causing premature breakage of the proppant.
[0121] Comparative Example 8, which involved direct rapid heating and sintering, exhibited the highest breakage rate. This resulted in the rapid decomposition of organic matter in the shell at high temperatures, generating a large amount of gas that could not be expelled in time, leading to blistering or microcracks within the shell. Simultaneously, there was insufficient solid-phase diffusion time between the shell and the core, resulting in extremely weak interfacial chemical bonding. These process defects directly led to increased internal defects, poor interfacial adhesion, and a complete collapse of mechanical properties in the product.
[0122] On the other hand, the SEM image of the ceramsite proppant obtained in Example 1 is as follows: Figure 1 As shown, where, Figure 1 (a) shows the cross-sectional morphology of the ceramsite proppant. From Figure 1 In (a), a distinct gradient distribution is clearly observed within the material. The density and composition change from the center to the edge. The core region exhibits a relatively dense matrix with dispersed pores and reinforcing phases, providing primary mechanical support. From the core to the surface, the structure gradually becomes more porous; this gradient helps alleviate stress concentration. The outermost layer displays a different microstructure, is rich in active components, and has a well-developed pore structure. Figure 1 (c) shows the morphology of the ceramsite proppant framework at 10,000x magnification, obtained through... Figure 1 (c) It can be seen that good sintering has occurred between the particles, forming a continuous ceramic skeleton.
[0123] Figure 1 (b) The distribution of steel fibers in the ceramsite proppant at a magnification of 2000. Figure 1 (b) It can be seen that the steel fiber is tightly wrapped by the ceramic matrix and is well bonded to the matrix, without obvious agglomeration. Figure 1 (d) Distribution of steel fibers in the ceramsite proppant at 10000x magnification. Figure 1 (d) It can be seen that the surface of the steel fiber is rough, forming a mechanical interlock with the surrounding ceramic particles. The steel fiber not only has a dense sintered neck, but also retains a certain microporous structure.
[0124] Figure 2 Ceramsite proppant prepared in Example 1 with three different particle sizes: 30 mesh, 40 mesh, and 50 mesh. From... Figure 2It can be seen that particles of different mesh sizes all maintain good sphericity, with relatively smooth but slightly rough surfaces and uniform particle size, which meets the industrial standard screening requirements.
[0125] Figure 3 Cross-sectional optical images of the ceramic proppant prepared in Example 1 with three different particle sizes: 30 mesh, 40 mesh, and 50 mesh. Figure 3 In the white ceramic matrix, dark dots are uniformly distributed, representing the cross-sections of steel fibers. The steel fibers are evenly distributed, both at the center and near the edges of the particles, without significant segregation. Therefore, through... Figure 3 It is evident that the raw materials of the present invention are thoroughly mixed, and the steel fibers do not undergo severe sedimentation or aggregation during the molding process.
[0126] In summary, the bulk density of the ceramsite proppant prepared by this invention is 1.40-1.45 g / cm³. 3 Its apparent density is 2.26-2.29 g / cm³. 3 The fracturing rate under a 52MPa closure pressure is 3.2%-3.8%, and the chemical removal capacity for hydrogen sulfide (H2S) is assessed at 118-145 mg H2S / g. After H2S removal simulation, the fracturing rate under a 52MPa closure pressure is 3.6%-4.3%. Therefore, the ceramic proppant prepared in this invention is suitable for fracturing operations in medium-deep sulfur-bearing oil and gas reservoirs. It can effectively support fractures, maintain conductivity, actively remove H2S, protect downhole equipment, and improve the overall safety and economy of production.
[0127] The above description is merely some specific embodiments of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a ceramic proppant with hydrogen sulfide scavenging function, characterized in that, Includes the following steps: Step 1: A first slurry is obtained by wet ball milling bauxite, coal gangue, interface-optimized composite sintering aid, pretreated chopped steel fibers, walnut shell powder, and deionized water; the first slurry is dried and then ground, and after grinding and sieving, a first powder is obtained. Step 2: A second slurry is obtained by wet ball milling bauxite, coal gangue, interface-optimized composite sintering aid, walnut shell powder, and deionized water; the second slurry is dried and then ground, and after grinding and sieving, a second powder is obtained. Step 3: Place the first powder in a sugar coating machine, granulate it through a polyvinyl alcohol solution, and sieve out a first green body with a mesh size of 70-80; evenly add the second powder and polyvinyl alcohol solution to the first green body so that the second powder coats the surface of the first green body, and sieve out a spherical second green body with a mesh size of 50-70. Step 4: The second green body is subjected to gradient sintering under a protective atmosphere to obtain the inner layer structure; Step 5: The treated zinc-containing dust and kaolin are mixed in a planetary mill. After mixing, starch is added and mixed to obtain composite powder. The composite powder is then sieved to obtain shell functional powder. Step 6: Add the inner layer structure to the coating machine, spray the adhesive solution intermittently to make the surface of the inner layer structure matte, then add the shell functional powder, roll it to make the inner layer structure free from adhesion, and complete the coating operation. Step 7: Repeat step 6 to complete 5-8 coating operations to obtain the coated core-shell structure; Step 8: Under a protective atmosphere, the coated core-shell structure is heated from room temperature to 450°C at a heating rate of 1.5°C / min and held for 60-90 minutes to remove the adhesive. After removing the adhesive, the temperature is increased from 450°C to 800-950°C at a heating rate of 3°C / min and held for 30 minutes. After holding, the temperature is increased to 1220-1250°C at a heating rate of 5°C / min and held for 15-30 minutes to obtain the ceramic proppant.
2. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 1, characterized in that, In step 1, the pretreatment of chopped steel fibers includes the following steps: Fiber segments with a length of 0.05-0.1 mm and a diameter of 5-15 μm were screened from waste steel fibers. The screened fiber segments were placed in a 5-10 wt% NaOH solution and soaked at 60-80℃ for 20-30 minutes. The fiber segments were then rinsed until neutral. After rinsing the fiber segments to neutrality, immerse them in a 5-10 wt% dilute hydrochloric acid solution for 5-15 minutes, rinse them to neutrality, dry them, and then phosphate them in a zinc-based phosphate solution at 50-70℃ for 3-8 minutes to obtain pretreated chopped steel fibers.
3. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 1, characterized in that, In step 1, the interface-optimized composite sintering aid includes spodumene and titanium dioxide.
4. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 3, characterized in that, In step 1, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, pretreated chopped steel fiber, and walnut shell powder is (65~75): (26~35): (2~5): (0.5~2): (3~7): (4~6).
5. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 3, characterized in that, In step 2, the weight ratio of bauxite, coal gangue, spodumene, titanium dioxide, and walnut shell powder is (65~75): (26~35): (2~5): (0.5~2): (0.5~1.5).
6. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 1, characterized in that, In step 5, the industrial zinc-containing dust is washed with water, and a precipitant is added to remove heavy metals. After being roasted at 400-500℃, it is ground and homogenized to obtain the treated zinc-containing dust.
7. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 1, characterized in that, In step 5, the weight ratio of the treated zinc-containing dust, kaolin, and starch is (60-70):(25-30):(5-10).
8. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 1, characterized in that, In step 8, the particle size of the ceramsite proppant is 30-50 mesh.
9. The method for preparing a ceramic proppant with hydrogen sulfide scavenging function according to claim 1, characterized in that, In step 4, gradient sintering specifically includes: the second green body is heated to 600℃ at 2℃ / min and held for 30-60 minutes under a protective atmosphere to remove the binder; after removing the binder, the temperature is increased to 1000℃ at 5℃ / min, and then increased to 1255-1300℃ at 3℃ / min and held for 60-90 minutes to obtain the inner layer structure.
10. Ceramsite proppant prepared by any one of the preparation methods according to claims 1-9.
Citation Information
Patent Citations
Lightweight high-strength ceramic proppant based on composite coating and low-temperature densification and preparation method thereof
CN120865880B
Ceramsite proppant for well producing coalbed methane from coal gangue and preparation method thereof
CN105885820A
Lightweight core-shell structure ceramsite proppant and preparation method thereof
CN121046065A