A comb-shaped long-chain alkyl copolymer pitch inhibitor and its preparation method and application
Patent Information
- Application Number
- CN202610967590.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-01
- Publication Date
- 2026-08-04
AI Technical Summary
(1)小分子芳烃类溶剂:存在用量大、毒性高、闪点低等缺陷;
本发明提供了一种用于预防油田油井井下管柱因沥青质析出而造成管柱堵塞的梳形长链烷基共聚物沥青抑制剂及其制备方法与应用,抑制剂的抑制率>95%、原料易得、反应条件温和、适合大规模生产;制备方法仅需两步常规反应,无需高压及特殊纯化设备。
Smart Images

Figure CN122502562A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of oilfield chemical technology, specifically relating to a comb-shaped long-chain alkyl copolymer asphalt inhibitor, its preparation method, and its application. Background Technology
[0002] During oilfield extraction, as formation pressure decreases and crude oil is extracted, asphaltenes in the crude oil lose stability due to changes in temperature, pressure, and composition, causing them to precipitate and deposit. This asphaltenes deposit can clog wellbore tubing, formation pores, and surface facilities, severely impacting normal oilfield production and economic benefits. For example, in one offshore oilfield, formation pressure decreased by 7-12 MPa compared to the initial production period, a significant drop that was a major cause of asphaltenes precipitation.
[0003] Currently, commonly used methods for asphaltene inhibition include the use of dispersants and inhibitors. Industrially used asphalt inhibitors mainly include: (1) Small molecule aromatic solvents: have drawbacks such as large usage, high toxicity, and low flash point; (2) Organochlorine products: They have strong solubility and good short-term effects, but they can easily cause excessive levels of organochlorine in crude oil. Organochlorine can also easily cause problems such as catalyst poisoning and equipment corrosion in refineries. (3) Ionic or amphoteric surfactants: They have poor temperature and salt resistance, are easily adsorbed by the formation and become ineffective, and are very likely to cause oil-water emulsification in water-bearing oil wells, making it impossible to break the emulsion and dehydrate; (4) Dodecylbenzenesulfonic acid, Span, Tween and other surfactant inhibitors: their performance is unstable in harsh downhole environments (such as high temperature and high salinity), and they have problems such as high cost or environmental unfriendliness. (5) Conventional polymer-type inhibitors: have high molecular rigidity and insufficient compatibility with asphaltene, and their inhibition rate is generally lower than 80%.
[0004] Therefore, there is an urgent need to develop an asphalt inhibitor with a high inhibition rate (>95%), low cost, simple preparation process, and suitability for high temperature and high salinity environments. Summary of the Invention
[0005] This invention is proposed to solve the problems existing in the prior art, and its purpose is to provide a comb-shaped long-chain alkyl copolymer asphalt inhibitor, its preparation method and application.
[0006] This invention is achieved through the following technical solution: A method for preparing a comb-shaped long-chain alkyl copolymer asphalt inhibitor includes the following steps: S1, free radical copolymerization: Octadecyl methacrylate (SMA), maleic anhydride (MA), and styrene (St) were dissolved in a solvent at a molar ratio of 1:1:(0.1~0.5). The mixture was heated to 40℃~60℃ and stirred until completely dissolved. After purging with nitrogen to remove oxygen, the temperature was further increased to the reaction temperature of 70℃~95℃. An initiator was then added to carry out the polymerization reaction for 1h~5h to obtain the terpolymer SMA-MA-St. The reaction equation is as follows:
[0007] In the formula: x, y, and z are the mole fractions of octadecyl methacrylate, maleic anhydride, and styrene, respectively, x+y+z=1, and x:y:z=1:1:(0.1~0.5); S2, amidation grafting: The terpolymer obtained in step S1 was dissolved in a solvent with a molar ratio of 1:(0.1~0.5). After mixing and dissolving, a catalyst was added, and the mixture was heated to 120℃~140℃ and refluxed for 1h~5h to carry out an amidation reaction. After the reaction was completed, the mixture was purified by washing with small amounts of ethanol several times to obtain a pale yellow, waxy, comb-shaped long-chain alkyl copolymer asphalt inhibitor. The reaction equation is as follows:
[0008]
[0009] In the formula: x, y, and z are the mole fractions of octadecyl methacrylate, maleic anhydride, and styrene, respectively; x + y + z = 1, and x:y:z = 1:1:(0.1~0.5); the number-average molecular weight of the inhibitor is Mn = 1.0 × 10⁻⁶. 4 ~3.0×10 4 g / mol.
[0010] In the above technical solution, the solvents in steps S1 and S2 are the same, and are selected from any one of toluene, xylene or high-boiling-point aromatic hydrocarbons.
[0011] In the above technical solution, the total mass ratio of octadecyl methacrylate (SMA), maleic anhydride (MA), and styrene (St) to the solvent in step S1 is 1:(5-30).
[0012] In the above technical solution, the initiator in step S1 is benzoyl peroxide (BPO) or azobisisobutyronitrile (AIBN); the mass of the initiator in step S1 is 0.5% to 3% of the total mass of octadecyl methacrylate, maleic anhydride and styrene.
[0013] In the above technical solution, the long-chain alkylamine in step S2 is tetradecylamine or octadecylamine.
[0014] In the above technical solution, the catalyst in step S2 is concentrated sulfuric acid or p-toluenesulfonic acid; the mass of the catalyst in step S2 is 0.5% to 2% of the total mass of the terpolymer and the long-chain alkylamine.
[0015] A comb-shaped long-chain alkyl copolymer asphalt inhibitor prepared by the aforementioned method, the inhibitor having a comb-shaped molecular structure comprising a polymer backbone composed of octadecyl methacrylate, maleic amide, and styrene, and side-chain long-chain alkyl groups attached to the backbone; the maleic amide is generated by reacting maleic anhydride with a long-chain alkyl amine; the side-chain long-chain alkyl groups are derived from octadecyl methacrylate and grafted amines; The inhibitor has the following general structural formula:
[0016] In the formula: x, y, and z are the mole fractions of octadecyl methacrylate, maleic anhydride, and styrene, respectively; x + y + z = 1, and x:y:z = 1:1:(0.1~0.5); the number-average molecular weight of the inhibitor is Mn = 1.0 × 10⁻⁶. 4 ~3.0×10 4 g / mol.
[0017] Application of a comb-shaped long-chain alkyl copolymer asphalt inhibitor prepared by the aforementioned method in preventing or inhibiting asphalt deposition and blockage during oilfield exploitation.
[0018] The beneficial effects of this invention are: This invention provides a comb-shaped long-chain alkyl copolymer asphalt inhibitor for preventing wellbore blockage caused by asphalt precipitation in oil fields, as well as its preparation method and application. The inhibitor has an inhibition rate of >95%, readily available raw materials, mild reaction conditions, and is suitable for large-scale production. The preparation method requires only two conventional reaction steps and does not require high pressure or special purification equipment.
[0019] The inhibitor of this invention has high inhibition efficiency: the copolymer combines multiple mechanisms of action, the molecular design is "comb-shaped", and the side chain of the ternary copolymer contains long-chain alkyl and benzene rings, which can simultaneously provide polar hydrogen bonding sites, π-π stacking sites and steric hindrance, synergistically breaking apart planar overlapping aggregates of asphaltenes, with an inhibition rate of >95%; The inhibitor of this invention has good stability: the long-chain alkyl group in the molecule has good compatibility with the crude oil hydrocarbon phase, and the polymer structure is stable with good temperature resistance, making it suitable for harsh downhole environments; The inhibitor of this invention is inexpensive and easy to produce: the raw materials are all industrial-grade bulk chemicals, which are low in cost, the reaction conditions are mild, and the preparation process is a conventional solution polymerization and amidation reaction. It does not require special equipment such as high pressure and hydrogenation. The steps are simple, the conditions are mild, and it is easy to control, making it suitable for large-scale industrial production. The inhibitor product of this invention has good oil solubility, contains no surfactant, and is resistant to temperatures up to 180 ℃ and salt concentrations up to 2.0 × 10⁻⁶. 5 mg / L, suitable for high-temperature and high-salinity oil reservoirs; the concentration required for on-site injection is only 50 ppm to 150 ppm, which is far lower than the dosage of conventional solvent-based inhibitors, resulting in significant economic benefits. Attached Figure Description
[0020] Figure 1 These are the infrared spectra of the products of Examples 1 and 2 of the present invention (red line represents Example 1, blue line represents Example 2). Figure 2 This is a GPC outflow curve diagram of Embodiment 1 of the present invention; Figure 3 This is the GPC outflow curve of Embodiment 2 of the present invention.
[0021] For those skilled in the art, other related figures can be obtained from the above figures without any creative effort. Detailed Implementation
[0022] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0023] Example 1
[0024] A method for preparing a comb-shaped long-chain alkyl copolymer asphalt inhibitor includes the following steps: S1. In a four-necked flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet tube, add 50g of toluene, 20.0g of octadecyl methacrylate (0.06mol), maleic anhydride (5.9g, 0.06mol), and styrene (1.6g, 0.015mol). Under nitrogen protection, stir and heat to 50°C to dissolve the monomers; add 0.4g of benzoyl peroxide (BPO), heat to 85°C and react for 3 hours to obtain a viscous copolymer solution. S2. Add octadecylamine (8.1 g, 0.03 mol) and 0.2 g p-toluenesulfonic acid to the above copolymer solution reaction system, heat to 130 °C, and continue the reaction for 3 h. After the reaction is complete, pour the product into excess ethanol to precipitate, filter, and dry the solid product under vacuum at 50 °C to constant weight to obtain a pale yellow waxy solid product, which is the comb-shaped long-chain alkyl copolymer asphalt inhibitor (denoted as inhibitor A). Its infrared spectrum is shown below. Figure 1 As shown, the GPC effluent curve is as follows Figure 2 As shown.
[0025] Example 2
[0026] Based on the method of Example 1, in this example, toluene is replaced with an equal mass of xylene, the initiator is replaced with 0.5g AIBN, the polymerization temperature is changed to 90℃, and the reaction time is 2h; In the amidation reaction, octadecylamine was replaced with an equimolar amount of tetradecylamine (6.4 g, 0.03 mol), the reaction temperature was set at 125 °C, and the reaction time was 4 h. The other steps are the same as in Example 1, and the product is obtained, denoted as inhibitor B, whose infrared spectrum is shown below. Figure 1 As shown, the GPC effluent curve is as follows Figure 3 As shown.
[0027] Example 3
[0028] Based on the method of Example 1, the monomer feed ratio was adjusted in this example: octadecyl methacrylate (20.0g, 0.06mol), maleic anhydride (5.9g, 0.06mol), and styrene (6.2g, 0.06mol). The polymerization reaction was carried out at 80°C for 4 hours; The amount of octadecylamine used in the amidation reaction was 2.7 g (0.01 mol); The other steps are the same as in Example 1, and the product is obtained, which is denoted as inhibitor C.
[0029] Comparative Example 1: Commercially available dodecylbenzenesulfonic acid, analytical grade.
[0030] Performance tests were conducted on the inhibitors of Examples 1-3 and Comparative Example 1: I. Experimental reagents: xylene (AR), n-heptane (AR), and field asphalt (extracted from heavy oil in a certain oil field).
[0031] II. Experimental instruments: 100ml dehydration bottle (minimum graduation mark 0.05ml), ultrasonic constant temperature water bath, electronic balance, stopwatch, 100-1000ul pipette, 5ml pipette.
[0032] III. Simulated Oil: Prepare a xylene solution containing 10 wt% asphaltene as simulated oil.
[0033] IV. Experimental Testing: S1. Dissolve the inhibitors A, B, and C prepared in this invention, as well as the commercially available asphalt dispersant (dodecylbenzene sulfonic acid) of Comparative Example 1, in xylene at a concentration of 1 wt% and keep them homogeneous for later use.
[0034] S2. At room temperature (around 25℃), take 100ul xylene and 200ul asphalt solution, add them to the dehydration bottle, tighten the cap, mix well, place in a 60℃ constant temperature water bath for ultrasonic dispersion for 5 minutes, then remove, add 9.7ml n-heptane, tighten the cap, mix well, place in a 60℃ constant temperature water bath for ultrasonic dispersion for 5 minutes, then remove and let stand at room temperature to observe the color of the different interfaces at the top and bottom of the dehydration bottle. The darker liquid at the bottom of the interface is considered as undispersed asphalt. After 60 minutes, read the volume V1.
[0035] S3. At room temperature (around 25℃), take 100ul of asphalt inhibitor test solution and 200ul of asphalt solution, add them to the dehydration bottle, tighten the cap, mix well, place in a 60℃ constant temperature water bath for ultrasonic dispersion for 5 minutes, then remove, add 9.7ml of n-heptane, tighten the cap, mix well, place in a 60℃ constant temperature water bath for ultrasonic dispersion for 5 minutes, then remove, and observe the color of the different interfaces at the top and bottom of the dehydration bottle at room temperature. The darker liquid at the bottom of the interface is considered as undispersed asphalt. After 60 minutes, read the volume V2.
[0036] The inhibition efficiency can be estimated using the following formula: Asphalt inhibition rate X = [(V1-V2) / V1] * 100% The higher the value, the stronger the inhibitor's anti-precipitation ability and the better the inhibitory effect.
[0037] V. Experimental Test Results: The inhibitors of Examples 1-3 and Comparative Example 1 were tested according to the aforementioned experimental methods, and the test results are shown in Table 1.
[0038] Table 1: Performance Comparison of Different Inhibitors
[0039] The results show that the comb-shaped long-chain alkyl copolymer asphalt inhibitors (A, B, C) prepared in this invention all exhibit excellent asphaltene inhibition performance, and their anti-precipitation ability is significantly higher than that of commercially available traditional products. The inhibitory effect is significant, verifying the effectiveness of this invention.
[0040] The principle of this invention: This invention first uses octadecyl methacrylate, maleic anhydride, and styrene as monomers to copolymerize, and then prepares a comb-shaped long-chain alkyl copolymer asphalt inhibitor through an amidation reaction of the copolymer with tetradecylamine and octadecylamine. The polar groups such as ester and amine groups, with their strong ability to form hydrogen bonds, penetrate and disperse into the spaces between the asphaltene and resinous flakes, partially breaking down the planar overlapping aggregates and forming irregularly stacked flake molecules, resulting in a looser structure, reduced order, and decreased spatial extension. Styrene binds to the aromatic structure of asphaltene through π-π interactions, enhancing adsorption capacity. The numerous hydrophobic side chains surrounding the asphaltene after adsorption effectively increase the steric hindrance between the asphaltene molecules, resulting in an inhibition rate of >95% for the asphaltene inhibitor.
[0041] The raw materials used in this invention are readily available and inexpensive, and the reaction process is simple and easy to control, making it suitable for large-scale production.
[0042] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a comb-shaped long-chain alkyl copolymer asphalt inhibitor, characterized in that: Includes the following steps: S1. Dissolve octadecyl methacrylate, maleic anhydride and styrene in a solvent, heat and stir until completely dissolved, remove oxygen by purging with nitrogen and continue heating to the polymerization reaction temperature, add an initiator to carry out the polymerization reaction, and obtain a terpolymer. S2. The terpolymer obtained in step S1 is dissolved in a solvent with a long-chain alkylamine. After mixing and dissolving, a catalyst is added to carry out an amidation reaction. After the reaction is completed, the mixture is purified to obtain a comb-shaped long-chain alkyl copolymer asphalt inhibitor.
2. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: The solvents used in steps S1 and S2 are the same, and are selected from any one of toluene, xylene, or high-boiling-point aromatic hydrocarbons.
3. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: In step S1, the molar ratio of octadecyl methacrylate, maleic anhydride, and styrene is 1:1:(0.1~0.5); the mass ratio of the total mass of octadecyl methacrylate, maleic anhydride, and styrene to the mass of the solvent in step S1 is 1:(5~30).
4. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: The initiator in step S1 is benzoyl peroxide or azobisisobutyronitrile; the mass of the initiator in step S1 is 0.5% to 3% of the total mass of octadecyl methacrylate, maleic anhydride and styrene.
5. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: The stirring temperature in step S1 is 40℃~60℃; the polymerization reaction temperature in step S1 is 70℃~95℃; and the polymerization reaction time is 1h~5h.
6. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: In step S2, the long-chain alkylamine is tetradecylamine or octadecylamine; the catalyst in step S2 is concentrated sulfuric acid or p-toluenesulfonic acid.
7. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: In step S2, the molar ratio of the terpolymer to the long-chain alkylamine is 1:(0.1~0.5); the mass of the catalyst in step S2 is 0.5%~2% of the total mass of the terpolymer and the long-chain alkylamine.
8. The method for preparing the comb-shaped long-chain alkyl copolymer asphalt inhibitor according to claim 1, characterized in that: The temperature of the amidation reaction in step S2 is 120℃~140℃; the reaction time is 1h~5h.
9. A comb-shaped long-chain alkyl copolymer asphalt inhibitor prepared by the method according to any one of claims 1 to 8, characterized in that: The inhibitor has a comb-shaped molecular structure, which includes a polymer backbone composed of octadecyl methacrylate, maleic amide and styrene, and long-chain alkyl side chains attached to the backbone. The inhibitor has the following general structural formula: In the formula: x, y, and z are the mole fractions of octadecyl methacrylate, maleic anhydride, and styrene, respectively, x+y+z=1, and x:y:z=1:1:(0.1~0.5); The number-average molecular weight of the inhibitor, Mn, is 1.0 × 10⁻⁶. 4 g / mol ~ 3.0 × 10 4 g / mol.
10. The application of a comb-shaped long-chain alkyl copolymer asphalt inhibitor prepared by the method according to any one of claims 1 to 8 in the prevention or inhibition of asphalt deposition and blockage during oilfield exploitation.