A multi-component polyimide resin and a method for preparing the same

CN122502644APending Publication Date: 2026-08-04ZIGONG ZHONGTIANSHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610870315.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-16
Publication Date
2026-08-04

AI Technical Summary

Technical Problem

[0004]本发明提供了一种多组分聚酰亚胺树脂及其制备方法,以解决上述现有技术的不足,解决了常规聚酰亚胺材料在耐热性能上存在局限及传统聚酰亚胺树脂的分子链刚性较大不易加工的问题

Benefits of technology

首先,多组分聚酰亚胺树脂采用了独特的分子结构设计,这种结构赋予了材料卓越的耐热性能,它们具有优异的耐热性能,能够在高温环境下保持结构稳定和性能不变,这对于航空航天、电子封装等对温度敏感的领域尤为重要。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122502644A_ABST
    Figure CN122502644A_ABST
Patent Text Reader

Abstract

A method for preparing a multi-component polyimide resin includes the steps of first preparing polyimide acid (PAA) and then preparing the multi-component polyimide resin. The multi-component polyimide resin employs a unique molecular structure design, which endows the material with excellent heat resistance. It exhibits superior heat resistance, maintaining structural stability and performance unchanged at high temperatures, which is particularly important for temperature-sensitive fields such as aerospace and electronic packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyimide preparation technology, and in particular to a multi-component polyimide resin and its preparation method. Background Technology

[0002] Polyimide (PI) resins, due to the presence of imide ring structures in their main chain, possess excellent heat resistance, mechanical properties, and electrical insulation properties, making them widely used in high-tech fields such as aerospace, microelectronics, automotive, and precision machinery. Traditional polyimide resins are typically produced by the condensation polymerization of single or simple dianhydrides and diamines. While this can meet the requirements of some conventional environments, several technical bottlenecks remain when addressing the stringent demands of modern industry for multifunctional and high-performance materials.

[0003] Specifically, existing conventional polyimide materials have limitations in heat resistance. Under ultra-high temperatures or long-term thermal aging, they are prone to molecular chain degradation or oxidation, leading to embrittlement and decreased dimensional stability, making them unsuitable for applications under extreme conditions. Furthermore, the high rigidity of traditional polyimide resin molecular chains results in poor melt flowability and a narrow processing window, making it difficult to mold into films or complex components using conventional thermoplastic processing methods. The high energy consumption and low efficiency of the curing process further increase manufacturing costs. Simultaneously, in terms of chemical stability, traditional polyimides lack sufficient resistance to certain organic solvents or strong acid / alkali environments, limiting their long-term reliability in fields such as chemical corrosion protection and pharmaceutical packaging. Summary of the Invention

[0004] This invention provides a multi-component polyimide resin and its preparation method to overcome the shortcomings of the prior art and solve the problems of the limitations of conventional polyimide materials in heat resistance and the large rigidity of the molecular chain of traditional polyimide resins, which makes them difficult to process.

[0005] In order to achieve the objectives of this invention, the following technologies are proposed: One aspect provides a method for preparing a multi-component polyimide resin, comprising the following steps: Step 01: Add 1,4-phenylenediamine P-PDA to N-methylpyrrolidone NMP and stir for 1 hour at a temperature of 5°C to 10°C under nitrogen protection to ensure complete dissolution. Step 02: Add 4,4′-diaminodiphenyl ether ODA to the solution prepared in step 01, and stir for 2 hours at a temperature of 5°C to 10°C under nitrogen protection to ensure complete dissolution. Step 03: Divide 4,4′-oxydiphthalic anhydride (ODPA) into four portions according to their total mass of 65%, 20%, 10% and 5%; Step 04: Divide 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride (PMDA) into four portions according to 90%, 7%, and 3% of its total mass; Step 05: Add the first portion of 4,4′-oxydiphthalic anhydride ODPA to the solution obtained in Step 02, and stir for 3 hours at a temperature of 5°C to 10°C under the protection of nitrogen, so that the anhydride group of ODPA undergoes a nucleophilic addition-elimination reaction with the amino groups of P-PDA and ODA to form amide bonds and release water molecules, gradually forming polyimide acid. Step 06: Add the second part of 4,4′-oxophthalic anhydride ODPA to the solution obtained in Step 05. After an interval of 30 minutes, add the third part of 4,4′-oxophthalic anhydride ODPA. Stir for 2 hours at a temperature of 5°C to 10°C under the protection of nitrogen. Step 07: Add the fourth part of 4,4′-oxydiphthalic anhydride ODPA to N-methylpyrrolidone NMP. When dissolving, the mass ratio of the fourth part of 4,4′-oxydiphthalic anhydride ODPA to N-methylpyrrolidone NMP is 1:1. Mix at a temperature of 5°C to 10°C for 30 minutes. Step 08: Add the solution obtained in step 07 dropwise to the reactants obtained in step 06, and stir for 10 hours under the protection of nitrogen at a temperature of 5°C to 10°C. Step 09: The reactants obtained in Step 08 are heated in a constant temperature water bath at 20°C to 30°C. Then, the first part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA is added to the reactants obtained in Step 08, and the mixture is stirred for 10 hours at 20°C to 30°C under nitrogen protection. Step 10: Add the second part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to the reactants obtained in Step 09 under the preparation conditions of Step 09, and stir for 10 hours at a temperature of 20°C to 30°C under nitrogen protection. Step 11: Add the third part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to N-methylpyrrolidone NMP. When dissolving, the mass ratio of the third part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to N-methylpyrrolidone NMP is 1:1. Mix at a temperature of 5°C to 10°C for 30 minutes. Step 12: Add the solution obtained in step 11 dropwise to the reactants obtained in step 10, and stir for 10 hours at a temperature of 20°C to 30°C under nitrogen protection to obtain polyimide PAA. Step 13: Place the polyimide PAA in an oil bath at 0°C to 5°C and stir at a stirring speed of 200r / min to 300r / min under nitrogen protection. Step 14: Add acetic anhydride to the polyimide PAA from step 13, and stir for 1 hour at a temperature of 0°C to 5°C, a stirring speed of 200 r / min to 300 r / min and under nitrogen protection. The amount of acetic anhydride added is 20% of the total mass of the polyimide PAA.

[0006] Step 15: Add benzopyridine to the reactants obtained in Step 14, and stir for 1 hour at a temperature of 0°C to 5°C, a stirring speed of 200 r / min to 300 r / min and under nitrogen protection to complete the imidization and ring closure of the resin, precipitate solid resin, and obtain a mixture of solid resin and liquid solvent, wherein the amount of benzopyridine added is 15% of the total mass of polyimide acid PAA.

[0007] Step 16: Perform solid-liquid separation on the mixed slurry obtained in step 15 to obtain solid primary resin. During filtration, a vacuum pump, a suction flask, and a Buchner funnel are used to separate the solid resin from the liquid solvent.

[0008] Step 17: Use N-methylpyrrolidone (NMP) four times the mass of the initial resin as a washing solution to wash the solid initial resin in order to remove impurities such as oligomers and unreacted monomers in the resin, so as to obtain the cleaned resin. Step 18: Use methanol, which is twice the mass of the cleaned resin, as the washing solution to wash the cleaned resin in order to remove small molecules, reaction solvents, etc. from the resin. Step 19: The resin obtained in step 18 is subjected to a vacuum of -0.998 MPa, a temperature of 190°C to 220°C and a duration of 10 to 20 hours to remove the solvent. Finally, it is subjected to a high-temperature treatment at 270°C to 280°C for 9 to 12 hours to obtain a multi-component polyimide resin powder.

[0009] Furthermore, the amount of 1,4-phenylenediamine P-PDA added accounts for 33% to 50% of the total molar amount of the diamine; The amount of 4,4′-diaminodiphenyl ether (ODA) added is 50% to 67% of the total molar amount of the diamine.

[0010] Furthermore, 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride (PMDA) accounts for 5% to 22% of the total molar amount of dianhydride; 4,4′-O-diphthalic anhydride (ODPA) accounts for 78% to 95% of the total molar amount of dianhydride.

[0011] Furthermore, the solid content of 1,4-phenylenediamine P-PDA, 4,4′-diaminodiphenyl ether ODA, 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA and 4,4′-oxobisphthalic anhydride ODPA in N-methylpyrrolidone NMP is 20% to 28%.

[0012] Further, the total molar amount of 1,2,4,5-phenyltetracarboxylic acid dianhydride PMDA and 4,4′-oxobisphthalic anhydride ODPA : the total molar amount of 1,4-phenylenediamine P-PDA and 4,4′-diaminodiphenyl ether ODA = 0.992 to 0.998 : 1.

[0013] On the other hand, a multi-component polyimide resin is provided, which is prepared by a multi-component polyimide resin preparation method.

[0014] The advantages of the above technical solution are: First, multi-component polyimide resins employ a unique molecular structure design, which endows the materials with excellent heat resistance. They possess superior heat resistance and can maintain structural stability and performance unchanged in high-temperature environments, which is particularly important for temperature-sensitive fields such as aerospace and electronic packaging.

[0015] Secondly, multi-component polyimide resins exhibit excellent processing performance, possessing good processability and easily forming various forms such as films and composite materials to meet diverse application needs. This makes them widely applicable in fields such as electronic packaging, aerospace, and new energy. Simultaneously, their processing involves low energy consumption and high production efficiency, which helps reduce production costs and improve economic benefits.

[0016] Finally, multi-component polyimide resins exhibit strong chemical stability and resistance to a wide range of chemicals and solvents, making them widely applicable in industries such as chemical and pharmaceutical. Furthermore, their chemical resistance ensures the long-term performance of the products during extended use. Attached Figure Description

[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will now be described in further detail with reference to the accompanying drawings.

[0018] Figure 1 The DSC spectrum of the polyimide resin powder prepared in Example 1 is shown.

[0019] Figure 2 The flexural strength spectrum of the polyimide resin powder prepared in Example 1 is shown.

[0020] Figure 3 The tensile strength spectrum of the polyimide resin powder prepared in Example 1 is shown.

[0021] Figure 4 The compressive strength spectrum of the polyimide resin powder prepared in Example 1 is shown.

[0022] Figure 5The DSC spectrum of the polyimide resin powder prepared in Example 2 is shown.

[0023] Figure 6 The flexural strength spectrum of the polyimide resin powder prepared in Example 2 is shown.

[0024] Figure 7 The tensile strength spectrum of the polyimide resin powder prepared in Example 2 is shown.

[0025] Figure 8 The compressive strength spectrum of the polyimide resin powder prepared in Example 2 is shown.

[0026] Figure 9 The DSC spectrum of the polyimide resin powder prepared in Example 3 is shown.

[0027] Figure 10 The flexural strength spectrum of the polyimide resin powder prepared in Example 3 is shown.

[0028] Figure 11 The tensile strength spectrum of the polyimide resin powder prepared in Example 3 is shown.

[0029] Figure 12 The compressive strength spectrum of the polyimide resin powder prepared in Example 3 is shown.

[0030] Figure 13 The DSC spectrum of the polyimide resin powder prepared in Example 4 is shown.

[0031] Figure 14 The flexural strength spectrum of the polyimide resin powder prepared in Example 4 is shown.

[0032] Figure 15 The tensile strength spectrum of the polyimide resin powder prepared in Example 4 is shown.

[0033] Figure 16 The compressive strength spectrum of the polyimide resin powder prepared in Example 4 is shown. Detailed Implementation

[0034] Example 1 1,4-Phenylenediamine (P-PDA) and 4,4′-diaminodiphenyl ether (ODA) were used as polymerization monomers, with P-PDA comprising 50% and ODA 50% molar. 1,2,4,5-Phenylenetetramethylcarboxylic dianhydride (PMDA) and 4,4′-oxophthalic anhydride (ODPA) were used as polymerization monomers, with ODPA comprising 95% and PMDA 5% molar. N-methylpyrrolidone (NMP) was used as the polymerization solvent, and the polymerization solids content was 20 wt%. The multicomponent polyimide resin powder and its sheets were prepared through the following steps: Step 01: Add 1,4-phenylenediamine P-PDA to N-methylpyrrolidone NMP and stir for 1 hour at 5°C under nitrogen protection to ensure complete dissolution.

[0035] Step 02: Add 4,4′-diaminodiphenyl ether (ODA) to the solution prepared in step 01, and stir for 2 hours at 5°C under nitrogen protection to ensure complete dissolution.

[0036] Step 03: Divide 4,4′-oxydiphthalic anhydride (ODPA) into four portions according to their total mass of 65%, 20%, 10%, and 5%.

[0037] Step 04: Divide 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride (PMDA) into four portions according to 90%, 7%, and 3% of its total mass.

[0038] Step 05: Add the first portion of 4,4′-oxydiphthalic anhydride ODPA to the solution obtained in Step 02, and stir for 3 hours at 5°C under nitrogen protection, so that the anhydride group of ODPA undergoes a nucleophilic addition-elimination reaction with the amino groups of P-PDA and ODA to form an amide bond and release water molecules, gradually forming polyimide acid.

[0039] Step 06: Add the second part of 4,4′-oxophthalic anhydride ODPA to the solution obtained in Step 05. After an interval of 30 minutes, add the third part of 4,4′-oxophthalic anhydride ODPA. Stir for 2 hours at 5°C under nitrogen protection.

[0040] Step 07: Add the fourth part of 4,4′-oxophthalic anhydride ODPA to N-methylpyrrolidone NMP. When dissolving, the mass ratio of the fourth part of 4,4′-oxophthalic anhydride ODPA to N-methylpyrrolidone NMP is 1:1. Mix at 5°C for 30 minutes.

[0041] Step 08: Add the solution obtained in step 07 dropwise to the reactants obtained in step 06, and stir for 10 hours at 5°C under nitrogen protection.

[0042] Step 09: The reactants obtained in Step 08 are heated in a constant temperature water bath at 30°C. Then, the first portion of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA is added to the reactants obtained in Step 08, and the mixture is stirred for 10 hours at 30°C under nitrogen protection.

[0043] Step 10: Add a second part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to the reactants obtained in step 09, and stir for 10 hours at a temperature of 20°C to 30°C under nitrogen protection.

[0044] Step 11: Add the third part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to N-methylpyrrolidone NMP. When dissolving, the mass ratio of the third part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to N-methylpyrrolidone NMP is 1:1. Mix at 5°C for 30 min.

[0045] Step 12: Add the solution obtained in step 11 dropwise to the reactants obtained in step 10, and stir for 10 hours at 30°C under nitrogen protection to obtain polyimide PAA.

[0046] Step 13: Place the polyimide (PAA) in an oil bath at 5°C and stir at a stirring speed of 300 r / min under nitrogen protection.

[0047] Step 14: Add acetic anhydride to the polyimide PAA from step 13, and stir for 1 hour at 0°C, 300 rpm, and under nitrogen protection.

[0048] Step 15: Add benzopyridine to the reactants obtained in step 14, and stir for 1 hour at 0°C, 300 r / min, and under nitrogen protection to complete the imidization and ring closure of the resin, precipitating solid resin and obtaining a slurry of solid resin and liquid solvent.

[0049] Step 16: The mixed slurry obtained in step 15 is subjected to solid-liquid separation to obtain solid primary resin. During filtration, a vacuum pump, a suction flask, and a Buchner funnel are used to separate the solid resin from the liquid solvent.

[0050] Step 17: Use N-methylpyrrolidone (NMP) four times the mass of the initial resin as a washing solution to wash the solid initial resin to remove impurities such as oligomers and unreacted monomers from the resin, so as to obtain the cleaned resin.

[0051] Step 18: Use methanol, which is twice the mass of the cleaned resin, as the washing solution to wash the cleaned resin in order to remove small molecules, reaction solvents, etc. from the resin.

[0052] Step 19: The resin obtained in step 18 is subjected to a vacuum of -0.998 MPa, a temperature of 190°C and 20 hours to remove the solvent. Finally, it is subjected to a high-temperature treatment at 280°C for 12 hours to obtain a multi-component polyimide resin powder, which is then processed into sheets as needed.

[0053] The following steps are used for processing the sheet material: 1. Place the resin powder into the mold of the hot press. 2. Heat the hot press to 400℃ to melt the resin powder in the mold. 3. Apply pressure to the hot press, maintaining a pressure of 15 MPa per unit square area on the mold. Maintain this pressure for 25 minutes. 4. After the pressure holding time is complete, turn off the heating, keeping the pressure unchanged. Once the temperature drops below 50℃, depressurize the hot press, remove the mold, disassemble the mold, and then remove the sheet material.

[0054] The final product is a multi-component polyimide resin powder and its sheet, the properties of which are shown in the table below: Detection categories Test Project Test data Remark Polyimide resin powder <![CDATA[η inh (dL g -1 )]]> 0.59 Polyimide resin powder <![CDATA[DSC(T g / o C)]]> 280.28 See the diagram. Figure 1 Polyimide resin sheets Bending strength (MPa) 98.4 See the diagram. Figure 2 Polyimide resin sheets Tensile strength (MPa) 78.9 See the diagram. Figure 3 Polyimide resin sheets Compressive strength (MPa) 144.2 See the diagram. Figure 4 Example 2 1,4-Phenylenediamine (P-PDA) and 4,4′-diaminodiphenyl ether (ODA) were used as polymerization monomers, with P-PDA comprising 50% and ODA comprising 50% in molar. 1,2,4,5-Phenylenetetramethylcarboxylic dianhydride (PMDA) and 4,4′-oxydiphthalic anhydride (ODPA) were used as polymerization monomers, with ODPA comprising 78% and PMDA comprising 22% in molar. N-methylpyrrolidone (NMP) was used as the polymerization solvent, and the polymerization solids content was 20 wt%. The multicomponent polyimide resin powder and its sheets were prepared by the steps described in Example 1. Detection categories Test Project Test data Remark Polyimide resin powder <![CDATA[η inh (dL g -1 )]]> 0.87 Polyimide resin powder <![CDATA[DSC(T g / o C)]]> 286.6 See the diagram. Figure 5 Polyimide resin sheets Bending strength (MPa) 137.6 See the diagram. Figure 6 Polyimide resin sheets Tensile strength (MPa) 98.9 See the diagram. Figure 7 Polyimide resin sheets Compressive strength (MPa) 160 See the diagram. Figure 8

[0055] Example 3 1,4-Phenylenediamine (P-PDA) and 4,4′-diaminodiphenyl ether (ODA) were used as polymerization monomers, with P-PDA accounting for 33% and ODA accounting for 67% molar. 1,2,4,5-Benzenetetramethylcarboxylic dianhydride (PMDA) and 4,4′-Oxybisphthalic anhydride (ODPA) were used as polymerization monomers, with ODPA accounting for 78% and PMDA accounting for 22% molar. N-methylpyrrolidone (NMP) was used as the polymerization solvent, and the polymerization solids content was 20 wt%. The multicomponent polyimide resin powder and its sheets were prepared by the steps described in Example 1. Detection categories Test Project Test data Remark Polyimide resin powder <![CDATA[η inh (dL g -1 )]]> 1.29 Polyimide resin powder <![CDATA[TGA(T d5% / o C)]]> 541.5 See the diagram. Figure 9 Polyimide resin sheets Bending strength (MPa) 145.1 See the diagram. Figure 10 Polyimide resin sheets Tensile strength (MPa) 104.2 See the diagram. Figure 11 Polyimide resin sheets Compressive strength (MPa) 165.4 See the diagram. Figure 12

[0056] Example 4 1,4-Phenylenediamine (P-PDA) and 4,4′-diaminodiphenyl ether (ODA) were used as polymerization monomers, with P-PDA comprising 33% and ODA comprising 67% molar. 1,2,4,5-Phenylenetetramethylcarboxylic dianhydride (PMDA) and 4,4′-oxydiphthalic anhydride (ODPA) were used as polymerization monomers, with ODPA comprising 78% and PMDA comprising 22% molar. N-methylpyrrolidone (NMP) was used as the polymerization solvent, and the polymerization solids content was 28 wt%. The multicomponent polyimide resin powder and its sheets were prepared by the steps described in Example 1. Detection categories Test Project Test data Remark Polyimide resin powder <![CDATA[η inh (dL g -1 )]]> 1.76 Polyimide resin powder <![CDATA[TGA(T d5% / o C)]]> 552.7 See the diagram. Figure 13 Polyimide resin sheets Bending strength (MPa) 154.5 See the diagram. Figure 14 Polyimide resin sheets Tensile strength (MPa) 113.3 See the diagram. Figure 15 Polyimide resin sheets Compressive strength (MPa) 226.9 See the diagram. Figure 16

[0057] The multi-component polyimide resin prepared by this invention, due to its multi-component monomer polymerization, has significant performance control advantages compared to single-monomer systems. Through monomer combination design, synergistic optimization of the material in terms of thermal stability, mechanical properties, processability, and optical transparency is achieved. The multi-component polyimide resin combines the heat resistance of thermosetting polyimides with the processability of thermoplastics. Compared to traditional polyimides, which require high-temperature and high-pressure molding and are not reprocessable, the multi-component polyimide resin supports conventional molding processes such as compression molding and extrusion, significantly improving manufacturability. The multi-component polyimide resin exhibits excellent thermal and mechanical properties, with a glass transition temperature exceeding 285℃, a 5% thermogravimetric temperature exceeding 550℃, a flexural strength exceeding 150 MPa, a tensile strength exceeding 110 MPa, and a compressive strength exceeding 200 MPa.

[0058] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Obviously, those skilled in the art can make various modifications and variations to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention also intends to include these modifications and variations.

Claims

1. A method for preparing a multi-component polyimide resin, characterized in that, The process includes the following steps: first, the preparation of polyimide acid (PAA), and then the preparation of multi-component polyimide resin.

2. The method for preparing the multi-component polyimide resin according to claim 1, characterized in that, The preparation steps of polyimide acid (PAA) include: Step 01: Add 1,4-phenylenediamine P-PDA to N-methylpyrrolidone NMP and stir for 1 hour at a temperature of 5°C to 10°C under nitrogen protection to ensure complete dissolution. Step 02: Add 4,4′-diaminodiphenyl ether ODA to the solution prepared in step 01, and stir for 2 hours at a temperature of 5°C to 10°C under nitrogen protection to ensure complete dissolution. Step 03: Divide the 4,4′-oxydiphthalic anhydride ODPA into four parts according to its total mass: the first part of 4,4′-oxydiphthalic anhydride ODPA, the second part of 4,4′-oxydiphthalic anhydride ODPA, the third part of 4,4′-oxydiphthalic anhydride ODPA, and the fourth part of 4,4′-oxydiphthalic anhydride ODPA. Step 04: Divide the 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA into three parts according to its total mass: a first part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA, a second part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA, and a third part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA. Step 05: Add the first portion of 4,4′-oxydiphthalic anhydride ODPA to the solution obtained in Step 02, and stir for 3 hours at a temperature of 5°C to 10°C under nitrogen protection. Step 06: Add the second part of 4,4′-oxophthalic anhydride ODPA to the solution obtained in Step 05. After an interval of 30 minutes, add the third part of 4,4′-oxophthalic anhydride ODPA. Stir for 2 hours at a temperature of 5°C to 10°C under the protection of nitrogen. Step 07: Add the fourth part of 4,4′-oxydiphthalic anhydride ODPA to N-methylpyrrolidone NMP and mix for 30 min at a temperature of 5°C to 10°C. Step 08: Add the solution obtained in step 07 dropwise to the reactants obtained in step 06, and stir for 10 hours under the protection of nitrogen at a temperature of 5°C to 10°C. Step 09: The reactants obtained in Step 08 are heated in a constant temperature water bath at 20°C to 30°C. Then, the first part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA is added to the reactants obtained in Step 08, and the mixture is stirred for 10 hours at 20°C to 30°C under nitrogen protection. Step 10: Add the second part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to the reactants obtained in step 09, and stir for 10 hours at a temperature of 20°C to 30°C under nitrogen protection. Step 11: Add the third part of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA to N-methylpyrrolidone NMP and mix for 30 min at a temperature of 5°C to 10°C. Step 12: Add the solution obtained in step 11 dropwise to the reactants obtained in step 10, and stir for 10 hours under the protection of nitrogen at a temperature of 20°C to 30°C to obtain polyimide PAA.

3. The method for preparing the multi-component polyimide resin according to claim 2, characterized in that: The first portion of 4,4′-oxophthalic anhydride ODPA accounts for 65% of the total mass of 4,4′-oxophthalic anhydride ODPA; The second portion of 4,4′-oxophthalic anhydride ODPA accounts for 20% of the total mass of 4,4′-oxophthalic anhydride ODPA. The third portion of 4,4′-oxophthalic anhydride ODPA accounts for 10% of the total mass of 4,4′-oxophthalic anhydride ODPA. The fourth component, 4,4′-oxophthalic anhydride (ODPA), accounts for 5% of the total mass of 4,4′-oxophthalic anhydride (ODPA); the first component, 1,2,4,5-benzenetetramethylcarboxylic dianhydride (PMDA), accounts for 90% of the total mass of 1,2,4,5-benzenetetramethylcarboxylic dianhydride. The second portion of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride (PMDA) accounts for 7% of the total mass of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride. The third component, 1,2,4,5-benzenetetramethylcarboxylic dianhydride (PMDA), accounts for 3% of the total mass of 1,2,4,5-benzenetetramethylcarboxylic dianhydride.

4. The method for preparing the multi-component polyimide resin according to claim 2, characterized in that, The total molar amounts of 1,2,4,5-phenyltetramethylcarboxylic acid dianhydride PMDA and 4,4′-oxobisphthalic anhydride ODPA: the total molar amounts of 1,4-phenylenediamine P-PDA and 4,4′-diaminodiphenyl ether ODA = 0.992 to 0.998:

1.

5. The method for preparing the multi-component polyimide resin according to claim 2, characterized in that, In step 7, during dissolution, the mass ratio of the fourth part of 4,4′-oxophthalic anhydride ODPA to N-methylpyrrolidone NMP is 1:1; In step 11, during dissolution, the mass ratio of the third portion of 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride (PMDA) to N-methylpyrrolidone (NMP) is 1:

1.

6. The method for preparing the multi-component polyimide resin according to claim 2, characterized in that: In step 14, the amount of acetic anhydride added is 20% of the total mass of polyimide PAA; In step 15, the amount of benzopyridine added is 15% of the total mass of polyimide acid (PAA).

7. The method for preparing the multi-component polyimide resin according to claim 2, characterized in that: The amount of 1,4-phenylenediamine P-PDA added is 33% to 50% of the total molar amount of the diamine; The amount of 4,4′-diaminodiphenyl ether ODA added accounts for 50% to 67% of the total molar amount of the diamine; 1,2,4,5-Benzenetetramethylcarboxylic acid dianhydride (PMDA) accounts for 5% to 22% of the total molar amount of dianhydride; 4,4′-O-diphthalic anhydride (ODPA) accounts for 78% to 95% of the total molar amount of dianhydride.

8. The method for preparing the multi-component polyimide resin according to claim 2, characterized in that, The solid content of 1,4-phenylenediamine P-PDA, 4,4′-diaminodiphenyl ether ODA, 1,2,4,5-benzenetetramethylcarboxylic acid dianhydride PMDA and 4,4′-oxobisphthalic anhydride ODPA in N-methylpyrrolidone NMP is 20% to 28%.

9. The method for preparing the multi-component polyimide resin according to claim 1, characterized in that, The preparation steps of multi-component polyimide resin include: Step 13: Place the polyimide PAA in an oil bath at 0°C to 5°C and stir at a stirring speed of 200r / min to 300r / min under nitrogen protection. Step 14: Add acetic anhydride to the polyimide PAA from step 13, and stir for 1 hour at a temperature of 0°C to 5°C, a stirring speed of 200 r / min to 300 r / min, and under nitrogen protection. Step 15: Add benzopyridine to the reactants obtained in step 14, and stir for 1 hour at a temperature of 0°C to 5°C, a stirring speed of 200 r / min to 300 r / min and under nitrogen protection to obtain a slurry of solid resin and liquid solvent. Step 16: Perform solid-liquid separation on the solid resin and liquid solvent mixture obtained in step 15 to obtain solid primary resin. Step 17: Wash the solid primary resin with four times the mass of N-methylpyrrolidone (NMP) as washing solution to obtain cleaned resin. Step 18: Wash the cleaned resin with methanol, which is twice the mass of the cleaned resin. Step 19 involves removing the solvent from the resin obtained in Step 18 by subjecting it to a vacuum of -0.998 MPa, a temperature of 190°C to 220°C, and a duration of 10 to 20 hours. Finally, the resin is subjected to a high-temperature treatment at 270°C to 280°C for 9 to 12 hours to obtain a multi-component polyimide resin.

10. A multi-component polyimide resin, characterized in that, It is prepared by the method for preparing multi-component polyimide resin as described in any one of claims 1 to 9.