Flame-retardant thermoplastic elastomer compound and method for producing the same

CN122502814APending Publication Date: 2026-08-04GUANGDONG SHENGJIA RUBBER & PLASTIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610773896.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-01
Publication Date
2026-08-04

AI Technical Summary

Technical Problem

本申请通过在热塑性弹性体胶料中添加特定的复合阻燃剂,能够在有效提高热塑性弹性体胶料阻燃性的同时,维持热塑性弹性胶体良好的力学性能,还能够进一步提高热塑性弹性胶体的耐水性,克服了现有阻燃性弹性体胶料的耐水性不足的问题

Benefits of technology

[0034]1. The flame-retardant thermoplastic elastomer compound of this application uses a blend of SEBS and PP as the matrix, combined with a composite flame retardant prepared by crosslinking and modifying SEBS with an intumescent flame retardant, barium metaphosphate, boron nitride, and triallyl isocyanurate. The components work synergistically to achieve excellent flame retardant effect with a low amount of flame retardant added. During combustion, a dense and stable intumescent char layer can be formed. With the obtained composite flame retardant, the flame retardant components exert a synergistic flame retardant effect, and the compound can obtain good flame retardant performance with a low amount of flame retardant added. This avoids the damage to the mechanical properties of the matrix caused by adding a large amount of flame retardant, and can simultaneously achieve good flame retardant effect and good mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of polymer materials technology, specifically disclosing a flame-retardant thermoplastic elastomer compound and its preparation method. The flame-retardant thermoplastic elastomer compound comprises 50-80 parts SEBS, 10-30 parts PP, 5-15 parts compatibilizer, 10-30 parts composite flame retardant, 3-10 parts plasticizer, 0.2-1 parts antioxidant, and 0.1-0.5 parts lubricant. The composite flame retardant is prepared by reacting and mixing an intumescent flame retardant, barium metaphosphate, boron nitride, triallyl isocyanurate, and SEBS. The flame-retardant thermoplastic elastomer compound of this application possesses good flame retardancy, mechanical properties, and water resistance stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, and in particular to a flame-retardant thermoplastic elastomer compound and its preparation method. Background Technology

[0002] Thermoplastic elastomers (TEBs), as promising polymer materials, have seen increasingly widespread applications in cable sheathing, sealing materials, and automotive interiors in recent years. SEBS, as the base material for TEBs, is inherently flammable with a low oxygen index, making it prone to molten dripping during combustion, which fails to meet the demands of applications requiring higher flame retardancy. Currently, the common modification method involves adding flame retardants to the SEBS matrix to improve flame retardancy. Traditional halogen-based flame retardants offer high flame retardancy efficiency, but release large amounts of toxic fumes and corrosive gases during combustion, causing environmental pollution and failing to meet current green and environmentally friendly development requirements. They are gradually being replaced by halogen-free flame retardant systems. Existing halogen-free flame retardant systems are mostly phosphorus-based, nitrogen-based, or inorganic flame retardants. Achieving ideal flame retardant effects often requires high addition amounts. However, adding large amounts of flame retardants severely damages the original mechanical properties of the TEB and increases raw material costs, failing to balance excellent flame retardancy with good basic material properties, and thus failing to meet the requirements for long-term use.

[0003] Therefore, developing a flame-retardant thermoplastic elastomer compound that simultaneously possesses good flame-retardant properties and mechanical properties is a technical problem that needs to be solved in this field. Summary of the Invention

[0004] To improve the flame retardancy of thermoplastic elastomer compounds, this application provides a flame-retardant thermoplastic elastomer compound and its preparation method. By adding specific composite flame retardants to the thermoplastic elastomer compound, this application effectively improves its flame retardancy while maintaining its good mechanical properties. Furthermore, it enhances the water resistance of the thermoplastic elastomer, overcoming the problem of insufficient water resistance in existing flame-retardant elastomer compounds. Due to its excellent flame retardancy, mechanical properties, and water resistance, the flame-retardant thermoplastic elastomer compound of this application is suitable for use in the production of cables and sealing materials where high flame retardancy ratings and mechanical stability are required, and can meet the performance requirements for long-term use.

[0005] Firstly, the flame-retardant thermoplastic elastomer compound provided in this application adopts the following technical solution:

[0006] A flame-retardant thermoplastic elastomer compound, comprising, by weight parts: 50-80 parts SEBS, 10-30 parts PP, 5-15 parts compatibilizer, 10-35 parts composite flame retardant, 3-10 parts plasticizer, 0.2-1 parts antioxidant, and 0.1-0.5 parts lubricant;

[0007] The composite flame retardant is prepared by mixing and reacting an intumescent flame retardant, barium metaphosphate, boron nitride, triallyl isocyanurate and SEBS in a mass ratio of (30~50):(10~20):(1~5):(1~3):100.

[0008] In the above technical solution, the composite flame retardant used in this application includes an intumescent flame retardant that can form a porous carbon layer during combustion, which serves to isolate oxygen and heat and inhibit dripping. Barium metaphosphate can promote the formation of the carbon layer and improve its density. Boron nitride is a highly thermally conductive inorganic filler that can form a thermally conductive pathway in the matrix, helping the material to dissipate heat quickly during combustion, while reducing the overall amount of flame retardant added. After crosslinking with SEBS, triallyl isocyanurate can have good compatibility with the SEBS matrix, improve the interfacial bonding force between the flame retardant component and the matrix, and avoid the impact of flame retardant agglomeration on the mechanical properties of the material. While ensuring flame retardant performance, it maintains the original good mechanical properties of the thermoplastic elastomer.

[0009] Furthermore, the study found that the flame-retardant thermoplastic elastomer compound exhibited better water resistance under the synergistic effect of barium metaphosphate, boron nitride, and triallyl isocyanurate. This is attributed to the fact that the SEBS matrix, after crosslinking modification with triallyl isocyanurate, better encapsulates barium metaphosphate, boron nitride, and especially the intumescent flame retardant, anchoring each flame-retardant component within the matrix. This significantly reduces the contact between the intumescent flame retardant and water molecules. Simultaneously, the filling of micropores within the material by barium metaphosphate and boron nitride reduces water molecule penetration channels, lowering the compound's affinity for water. The synergistic effect of these three components further isolates the intumescent flame retardant from water absorption, effectively improving the overall water resistance stability of the compound and extending its service life.

[0010] Preferably, the preparation method of the composite flame retardant includes the following steps:

[0011] Step 1: Place SEBS, barium metaphosphate and boron nitride in a two-roll mill and mix them evenly at 120~140℃ to obtain a primary mixture;

[0012] Step 2: Raise the temperature of the primary mixture to 140~145℃, add the peroxide, and then continue to raise the temperature to 145~155℃, add triallyl isocyanurate, and mix for 3~5 minutes to obtain the secondary mixture;

[0013] Step 3: Add an intumescent flame retardant to the secondary mixture, continue mixing for 2-5 minutes, and after cooling, obtain the composite flame retardant.

[0014] In the above technical solution, this application prepares a cross-linked SEBS-based flame retardant carrier by reacting triallyl isocyanurate and SEBS. Barium metaphosphate and boron nitride are uniformly dispersed and anchored in the carrier, which can effectively inhibit the migration and agglomeration of barium metaphosphate and boron nitride under mixing shear force. Then, it is blended with an intumescent flame retardant, which further isolates the contact between the intumescent flame retardant and the polar groups of the matrix, reduces water absorption sites, and also allows each flame retardant component to be more uniformly dispersed in the flame retardant thermoplastic elastomer compound, so as to better exert the synergistic flame retardant and water resistance improvement effects among the components, and avoid the decrease in mechanical properties caused by the agglomeration of flame retardant components when directly blended.

[0015] Preferably, the peroxide is dicumyl peroxide, and the mass ratio of dicumyl peroxide to SEBS is (0.5~1):100.

[0016] In the above technical solution, this application uses dicumyl peroxide as an initiator to initiate the cross-linking reaction of triallyl isocyanurate, and at the same time promotes the grafting of triallyl isocyanurate onto the SEBS molecular chain, so that the prepared secondary mixture carrier can better combine the inorganic flame retardant components. The cross-linked SEBS carrier has better compatibility with the SEBS matrix, is easier to disperse uniformly, and has less negative impact on the mechanical properties of the matrix.

[0017] Preferably, the intumescent flame retardant is one or more of piperazine pyrophosphate and melamine polyphosphate.

[0018] Preferably, the intumescent flame retardant is piperazine pyrophosphate.

[0019] In the above technical solution, piperazine pyrophosphate, as an intumescent flame retardant, has good char formation effect and excellent thermal stability. It can form a stable intumescent char layer during combustion, resulting in higher flame retardant efficiency. At the same time, piperazine pyrophosphate has a higher synergistic effect with barium metaphosphate and boron nitride, which can better improve the flame retardancy, mechanical properties and water resistance of flame retardant thermoplastic elastomers.

[0020] Preferably, the plasticizer is one or more of cycloalkyl mineral oil, dioctyl phthalate, and dioctyl sebacate.

[0021] In the above technical solutions, adding these plasticizers can reduce the melt viscosity of the SEBS matrix, improve processing performance, and adjust the hardness and elasticity of the material, so that the flame-retardant thermoplastic elastomer compound has the flexibility to meet the requirements of the application scenario and improves the convenience of processing and molding.

[0022] Preferably, the antioxidant is one or more of antioxidant 168, antioxidant 1010, and antioxidant BHT.

[0023] In the above technical solution, by adding the antioxidant, the thermal oxidative degradation of the SEBS matrix during processing and long-term use can be inhibited, thus avoiding the problems of material aging and hardening, and decline in mechanical properties, and extending the service life of the material.

[0024] Preferably, the lubricant is one or more of paraffin wax, zinc stearate, and polyethylene wax.

[0025] In the above technical solution, by adding the above-mentioned lubricant, this application can improve the processing fluidity of materials, reduce the adhesion of materials to equipment during extrusion processing, improve the surface quality of finished products, and increase processing efficiency.

[0026] Preferably, the compatibilizer is one or a mixture of two of maleic anhydride-grafted SEBS and ethylene-acrylate-maleic anhydride terpolymer.

[0027] In the above technical solution, by adding the above compatibilizer, this application can further improve the compatibility between the other components in the flame-retardant thermoplastic elastomer and the SEBS matrix, further enhance the interfacial bonding force between the components, avoid the mechanical properties from deterioration due to interfacial defects, and also further improve the overall water resistance stability of the rubber compound and reduce the problem of water molecules penetrating along the interface.

[0028] Secondly, this application provides a method for preparing a flame-retardant thermoplastic elastomer compound, which adopts the following technical solution:

[0029] A method for preparing a flame-retardant thermoplastic elastomer compound includes the following steps:

[0030] Step S1: Weigh each component material according to the formula, put them into an internal mixer, and mix them at 140~180℃ for 8~15 minutes;

[0031] Step S2: The mixed material is fed into a twin-screw extruder, the temperature is controlled at 150~190℃, the screw speed is controlled at 200~400r / min, and the flame-retardant thermoplastic elastomer compound is obtained after melt extrusion and granulation.

[0032] In the above technical solution, this application adopts a simple preparation process that is compatible with existing polymer material processing production lines, which is convenient for industrial-scale production. The resulting flame-retardant thermoplastic elastomer compound has uniform dispersion of each component, good flame retardancy, mechanical properties and water resistance, and can meet the requirements of industrial production.

[0033] In summary, this application includes at least one of the following beneficial technical effects:

[0034] 1. The flame-retardant thermoplastic elastomer compound of this application uses a blend of SEBS and PP as the matrix, combined with a composite flame retardant prepared by crosslinking and modifying SEBS with an intumescent flame retardant, barium metaphosphate, boron nitride, and triallyl isocyanurate. The components work synergistically to achieve excellent flame retardant effect with a low amount of flame retardant added. During combustion, a dense and stable intumescent char layer can be formed. With the obtained composite flame retardant, the flame retardant components exert a synergistic flame retardant effect, and the compound can obtain good flame retardant performance with a low amount of flame retardant added. This avoids the damage to the mechanical properties of the matrix caused by adding a large amount of flame retardant, and can simultaneously achieve good flame retardant effect and good mechanical properties.

[0035] 2. The flame-retardant thermoplastic elastomer compound of this application exhibits better water resistance under the synergistic effect of barium metaphosphate, boron nitride, and triallyl isocyanurate. This is because the three components work synergistically in multiple ways, such as reducing the affinity of the compound surface for water, blocking the physical channels for water molecule penetration, forming an effective waterproof barrier, and constructing a three-dimensional network with high cross-linking density, thereby reducing the exposure of hydrophilic groups on the polymer chain. Together, they hinder the penetration of water molecules into the interior of the compound, prevent the internal components of the compound from dissolving outward, effectively reduce the water absorption rate of the compound, and improve the water resistance stability of the compound during long-term use.

[0036] 3. The flame-retardant thermoplastic elastomer compound of this application adopts a halogen-free flame-retardant system, which meets the requirements of green and environmentally friendly development. Moreover, the preparation process is simple, compatible with existing polymer material processing equipment, and easy to carry out industrial-scale production. It is suitable for application in the production of cables and sealing materials with high requirements for flame retardancy and mechanical stability. Detailed Implementation

[0037] To better illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0038] Preparation Example 1

[0039] A composite flame retardant comprises 400g of intumescent flame retardant, 200g of barium metaphosphate, 50g of boron nitride, 30g of triallyl isocyanurate and 1000g of SEBS.

[0040] The intumescent flame retardant is piperazine pyrophosphate, purchased from Chongqing Coal Technology Heavy Industry Co., Ltd. in China.

[0041] The barium metaphosphate was purchased from Chongqing Ruifu Food Additives Co., Ltd., and is of industrial grade with a particle size of less than 5μm.

[0042] Among them, boron nitride was purchased from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., item number: 102414.

[0043] Among them, triallyl isocyanurate was purchased from Hunan Zhenyuan Chemical Co., Ltd.

[0044] Among them, SEBS is the industrial-grade SEBS of Yueyang Baling Petrochemical Company, with the product number YH503.

[0045] The preparation method of the composite flame retardant includes the following steps:

[0046] Step 1: Place SEBS, barium metaphosphate and boron nitride in a two-roll mill and mix them evenly at 120°C to obtain a primary mixture.

[0047] Step 2: Raise the temperature of the primary mixture to 140°C, add 10g of dicumyl peroxide, then continue to raise the temperature to 150°C, add triallyl isocyanurate, and mix for 5 minutes to obtain the secondary mixture.

[0048] Step 3: Add an intumescent flame retardant to the secondary mixture, continue mixing for 3 minutes, and after cooling, obtain the composite flame retardant.

[0049] The diisopropylbenzene peroxide was purchased from Nanjing Reagent.

[0050] Preparation Example 2

[0051] A composite flame retardant, unlike Preparation Example 1, comprises 300g of an intumescent flame retardant, 100g of barium metaphosphate, 10g of boron nitride, 10g of triallyl isocyanurate, and 1000g of SEBS.

[0052] The preparation method of the composite flame retardant includes the following steps:

[0053] Step 1: Place SEBS, barium metaphosphate and boron nitride in a two-roll mill and mix them evenly at 140°C to obtain a primary mixture.

[0054] Step 2: Raise the temperature of the primary mixture to 145°C, add 5g of dicumyl peroxide, then continue to raise the temperature to 155°C, add triallyl isocyanurate, and mix for 5 minutes to obtain the secondary mixture.

[0055] Step 3: Add intumescent flame retardant to the secondary mixture, continue mixing for 2 minutes, and after cooling, obtain the composite flame retardant.

[0056] Preparation Example 3

[0057] A composite flame retardant, unlike Preparation Example 1, comprises 500g of intumescent flame retardant, 150g of barium metaphosphate, 40g of boron nitride, 20g of triallyl isocyanurate and 1000g of SEBS.

[0058] The preparation method of the composite flame retardant includes the following steps:

[0059] Step 1: Place SEBS, barium metaphosphate and boron nitride in a two-roll mill and mix them evenly at 120°C to obtain a primary mixture.

[0060] Step 2: Raise the temperature of the primary mixture to 140°C, add 7g of dicumyl peroxide, then continue to raise the temperature to 145°C, add triallyl isocyanurate, and mix for 3 minutes to obtain the secondary mixture.

[0061] Step 3: Add an intumescent flame retardant to the secondary mixture, continue mixing for 5 minutes, and after cooling, obtain the composite flame retardant.

[0062] Comparative Preparation Example 1

[0063] A composite flame retardant, which differs from Preparation Example 1 in that barium metaphosphate is replaced with an intumescent flame retardant in equal amounts, while the remaining steps are consistent with Preparation Example 2.

[0064] Comparative Preparation Example 2

[0065] A composite flame retardant, which differs from Preparation Example 1 in that boron nitride is replaced in an equal amount with an intumescent flame retardant, while the remaining steps are consistent with Preparation Example 2.

[0066] Comparative preparation example 3

[0067] A composite flame retardant, which differs from Preparation Example 1 in that barium metaphosphate and boron nitride are replaced with intumescent flame retardants in equal amounts, while the remaining steps are consistent with Preparation Example 2.

[0068] Comparative preparation example 4

[0069] A composite flame retardant, differing from Preparation Example 1 in that triallyl isocyanurate is replaced with an equal amount of SEBS, is prepared by the following steps:

[0070] Step 1: Place SEBS, barium metaphosphate and boron nitride in a two-roll mill and mix them evenly at 120°C to obtain a primary mixture.

[0071] Step 2: Raise the temperature of the primary mixture to 140°C, add 10g of dicumyl peroxide, and then continue to raise the temperature to 150°C. After mixing for 5 minutes, a secondary mixture is obtained.

[0072] Step 3: Add an intumescent flame retardant to the secondary mixture, continue mixing for 3 minutes, and after cooling, obtain the composite flame retardant.

[0073] Comparative preparation example 5

[0074] A composite flame retardant, which differs from Preparation Example 1 in that barium metaphosphate is replaced with an equal amount of aluminum metaphosphate, while the remaining steps are consistent with Preparation Example 2.

[0075] The aluminum metaphosphate was purchased from Nantong Herun Biotechnology Co., Ltd., and is of industrial grade with a particle size of less than 5μm.

[0076] Comparative preparation example 6

[0077] A composite flame retardant, which differs from Preparation Example 1 in that boron nitride is replaced with an equal amount of aluminum nitride, while the remaining steps are consistent with Preparation Example 2.

[0078] Aluminum nitride was purchased from Zhejiang Yamei Nanotechnology Co., Ltd.

[0079] Comparative preparation example 7

[0080] A composite flame retardant, which differs from Preparation Example 1 in that triallyl isocyanurate is replaced in equal amounts with trimethylolpropane trimethacrylate.

[0081] Trimethylolpropane trimethacrylate was purchased from Guangzhou Shanghe Chemical Technology Co., Ltd.

[0082] Example 1

[0083] A flame-retardant thermoplastic elastomer compound comprising: 800g SEBS, 200g PP, 80g compatibilizer, 300g composite flame retardant, 60g plasticizer, 8g antioxidant, and 2g lubricant.

[0084] Among them, SEBS is the industrial-grade SEBS of Yueyang Baling Petrochemical Company, with the product number YH503.

[0085] Among them, PP is Basel's industrial-grade PP, part number: Hifax TYC 1338X.

[0086] The compatibilizer is SEBS-g-MAN, purchased from Dongguan Kadar Plastic Raw Materials Co., Ltd., item number: M500SE.

[0087] The plasticizer is a naphthenic mineral oil, purchased from Shandong Zhuyou Lubrication Technology Co., Ltd., product number: N4010.

[0088] The antioxidant in question is Antioxidant 1010, which was purchased from Nanjing Milan Chemical Co., Ltd.

[0089] The lubricant is paraffin wax, purchased from Wuhan Xindongyi Chemical Co., Ltd., with a density of 0.9 g / cm³.

[0090] The composite flame retardant was prepared in Preparation Example 1.

[0091] The preparation method of flame-retardant thermoplastic elastomer compound includes the following steps:

[0092] Step S1: Weigh each component material according to the formula, put them into an internal mixer, and mix them at 180°C for 10 minutes.

[0093] Step S2: The mixed material is fed into a twin-screw extruder, the temperature is controlled at 180℃ and the screw speed is controlled at 400r / min. After melt extrusion and granulation, the flame-retardant thermoplastic elastomer compound is obtained.

[0094] Example 2

[0095] A flame-retardant thermoplastic elastomer compound, which differs from Example 1, comprises: 800g SEBS, 200g PP, 50g compatibilizer, 350g composite flame retardant, 100g plasticizer, 5g antioxidant, and 3g lubricant.

[0096] The composite flame retardant was prepared in Preparation Example 2.

[0097] The preparation method of flame-retardant thermoplastic elastomer compound includes the following steps:

[0098] Step S1: Weigh each component material according to the formula, put them into an internal mixer, and mix them at 150°C for 15 minutes.

[0099] Step S2: The mixed material is fed into a twin-screw extruder, the temperature is controlled at 190℃ and the screw speed is controlled at 400r / min. After melt extrusion and granulation, the flame-retardant thermoplastic elastomer compound is obtained.

[0100] Example 3

[0101] A flame-retardant thermoplastic elastomer compound, which differs from Example 1, comprises: 500g SEBS, 100g PP, 100g compatibilizer, 100g composite flame retardant, 30g plasticizer, 2g antioxidant, and 1g lubricant.

[0102] The composite flame retardant was prepared in Preparation Example 3.

[0103] The preparation method of flame-retardant thermoplastic elastomer compound includes the following steps:

[0104] Step S1: Weigh each component material according to the formula, put them into an internal mixer, and mix them at 170°C for 12 minutes.

[0105] Step S2: The mixed material is fed into a twin-screw extruder, the temperature is controlled at 180℃ and the screw speed is controlled at 300r / min. After melt extrusion and granulation, the flame-retardant thermoplastic elastomer compound is obtained.

[0106] Comparative Example 1

[0107] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 1.

[0108] Comparative Example 2

[0109] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 2.

[0110] Comparative Example 3

[0111] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 3.

[0112] Comparative Example 4

[0113] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 4.

[0114] Comparative Example 5

[0115] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 5.

[0116] Comparative Example 6

[0117] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 6.

[0118] Comparative Example 7

[0119] A thermoplastic elastomer compound, which differs from Example 1 in that the composite flame retardant is prepared from Comparative Preparation Example 7.

[0120] Performance testing

[0121] This application tested the flame retardant properties, mechanical properties, and water resistance of the thermoplastic elastomer colloids of Examples 1-3 and Comparative Examples 1-7 above. The performance evaluation methods and test standards are as follows:

[0122] The flame-retardant thermoplastic elastomer compound, which was extruded and granulated, was placed in a forced-air drying oven and dried at 50 °C for 3 h. It was then injection molded at a suitable temperature using an injection molding machine and a special mold to prepare test samples. For each performance test of each example, 5 parallel samples were guaranteed, and the average value of the test results was taken.

[0123] Flame retardant performance: Tested according to GB / T2046.2-2009, the test indicators are limiting oxygen index (LOI) and vertical burning test (UL94). The standard sample size for the limiting oxygen index (LOI) test is 150×6.5×3.2mm. 3The standard test sample size for the vertical burning test (UL94) is 100×5×1.6mm. 3 .

[0124] Mechanical properties: Tested according to GB / T 528-2009 using an electronic universal tensile testing machine. The test parameters are tensile strength and elongation at break. The standard sample size for tensile strength and elongation at break is 75×5×1.6mm. 3 Barbell shape.

[0125] Water resistance: Tested according to GB / T1034, the test indicators are water absorption rate (%), mass loss rate (%), and tensile strength and elongation at break after immersion for 72 hours. The standard sample size for water absorption rate (%) and mass loss rate (%) is 100×100×1.6mm. 3 The standard sample size for testing tensile strength and elongation at break is 75×5×1.6mm. 3 Barbell shape.

[0126] The test results are shown in Table 1.

[0127] Table 1:

[0128] Group Limiting Oxygen Index (LOI) Vertical flammability rating UL94 Tensile strength (MPa) Tensile strength after soaking (MPa) Elongation at break % Elongation at break after soaking (%) Water absorption rate % Quality loss rate % Example 1 34 V-0 16.2 15.7 672 620 0.31 0.28 Example 2 30 V-0 16.1 15.2 674 603 0.39 0.32 Example 3 32 V-1 16.7 15.9 686 619 0.35 0.31 Comparative Example 1 22 V-0 16.0 13.3 671 516 0.83 1.27 Comparative Example 2 20 V-1 15.9 12.8 683 540 0.76 1.14 Comparative Example 3 18 V-0 16.4 12.2 675 494 1.15 2.64 Comparative Example 4 16 V-2 13.1 9.4 571 390 0.94 1.48 Comparative Example 5 28 V-1 14.3 12.3 624 518 0.72 1.03 Comparative Example 6 24 V-1 14.1 12.4 618 521 0.68 0.92 Comparative Example 7 26 V-2 13.9 11.6 602 491 0.82 1.18

[0129] According to the test results in Table 1, the flame-retardant thermoplastic elastomer compounds prepared in Examples 1-3 of this application have a higher limiting oxygen index, can reach V-0 rating when burned vertically, have higher tensile strength and elongation at break, and lower water absorption and mass loss rate. The retention of tensile strength and elongation at break after soaking for 72 hours is also better. The flame-retardant thermoplastic elastomer compounds in Examples 1-3 of this application simultaneously take into account good flame-retardant properties, mechanical properties and water resistance stability, indicating that the synergistic effect of each component in this application can obtain flame-retardant thermoplastic elastomer compounds with good flame-retardant properties, mechanical properties and water resistance.

[0130] A detailed comparative analysis of Example 1 and Comparative Examples 1-4 reveals that Example 1 exhibits excellent flame retardant, water resistance, and mechanical properties. This analysis suggests that the simultaneous presence of barium metaphosphate, boron nitride, and triallyl isocyanurate allows them to function effectively from multiple dimensions, including physical barrier, synergistic flame retardancy, and cross-linking network construction, collectively enhancing the overall performance of the flame-retardant thermoplastic elastomer. The absence of any one component disrupts this synergistic effect, reducing the flame retardant effect and water barrier capacity, ultimately leading to a significant decline in the tested properties. This further validates that the technical solution of using barium metaphosphate and boron nitride in combination, and further introducing triallyl isocyanurate cross-linked SEBS as a synergistic flame retardant component, can effectively improve the flame retardant, mechanical properties, and water resistance of the flame-retardant thermoplastic elastomer.

[0131] A detailed comparative analysis of Example 1 and Comparative Examples 5-7 reveals that after replacing barium metaphosphate with aluminum metaphosphate, boron nitride with aluminum nitride, and triallyl isocyanurate with trimethylolpropane trimethacrylate, the overall performance of the flame-retardant thermoplastic elastomer compound is inferior to that of Example 1. This indicates that the technical solution of this application, which uses barium metaphosphate and boron nitride in combination and further introduces triallyl isocyanurate crosslinked SEBS as a synergistic flame-retardant component, is specific. The synergistic effect of specific components is worse than other similar replacement components. Only the specific component combination of this application can effectively improve the flame-retardant performance, mechanical properties, and water resistance stability of the flame-retardant thermoplastic elastomer compound.

[0132] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A flame-retardant thermoplastic elastomer compound, characterized in that, By weight, the flame-retardant thermoplastic elastomer compound comprises the following components: 50-80 parts SEBS, 10-30 parts PP, 5-15 parts compatibilizer, 10-35 parts composite flame retardant, 3-10 parts plasticizer, 0.2-1 parts antioxidant, and 0.1-0.5 parts lubricant; The composite flame retardant is prepared by mixing and reacting an intumescent flame retardant, barium metaphosphate, boron nitride, triallyl isocyanurate and SEBS in a mass ratio of (30~50):(10~20):(1~5):(1~3):

100.

2. The flame-retardant thermoplastic elastomer compound according to claim 1, characterized in that, The preparation method of the composite flame retardant includes the following steps: Step 1: Place SEBS, barium metaphosphate and boron nitride in a two-roll mill and mix them evenly at 120~140℃ to obtain a primary mixture; Step 2: Raise the temperature of the primary mixture to 140~145℃, add the peroxide, and then continue to raise the temperature to 145~155℃, add triallyl isocyanurate, and mix for 3~5 minutes to obtain the secondary mixture; Step 3: Add an intumescent flame retardant to the secondary mixture, continue mixing for 2-5 minutes, and after cooling, obtain the composite flame retardant.

3. The flame-retardant thermoplastic elastomer compound according to claim 2, characterized in that, The peroxide is dicumyl peroxide, and the mass ratio of dicumyl peroxide to SEBS is (0.5~1):

100.

4. The flame-retardant thermoplastic elastomer compound according to claim 1, characterized in that, The intumescent flame retardant is one or more of piperazine pyrophosphate and melamine polyphosphate.

5. The flame-retardant thermoplastic elastomer compound according to claim 4, characterized in that, The intumescent flame retardant is piperazine pyrophosphate.

6. The flame-retardant thermoplastic elastomer compound according to claim 1, characterized in that, The plasticizer is one or more of cycloalkyl mineral oil, dioctyl phthalate, and dioctyl sebacate.

7. The flame-retardant thermoplastic elastomer compound according to claim 1, characterized in that, The antioxidant is one or more of antioxidant 168, antioxidant 1010, and antioxidant BHT.

8. The flame-retardant thermoplastic elastomer compound according to claim 1, characterized in that, The lubricant is one or more of paraffin wax, zinc stearate, and polyethylene wax.

9. The flame-retardant thermoplastic elastomer compound according to claim 1, characterized in that, The compatibilizer is one or a mixture of two of maleic anhydride-grafted SEBS and ethylene-acrylate-maleic anhydride terpolymer.

10. A method for preparing a flame-retardant thermoplastic elastomer compound as described in any one of claims 1 to 9, characterized in that, Includes the following steps: Step S1: Weigh each component material according to the formula, put them into an internal mixer, and mix them at 140~180℃ for 8~15 minutes; Step S2: The mixed material is fed into a twin-screw extruder, and after melt extrusion and granulation, the flame-retardant thermoplastic elastomer compound is obtained.