Preparation method of high-thermal-conductivity magnesium alloy plate

By employing a smelting-extrusion-rolling-annealing process and alloy composition design, high thermal conductivity magnesium alloy sheets were prepared, solving the problem of mismatch between the thermal conductivity and mechanical properties of magnesium alloy sheets and achieving efficient and low-cost production.

CN122503769APending Publication Date: 2026-08-04NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610744414.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-27
Publication Date
2026-08-04

AI Technical Summary

Technical Problem

Existing magnesium alloy sheets are difficult to match well between thermal conductivity and mechanical properties, and their manufacturing process is complex and costly, making it difficult to meet the lightweight and efficient heat dissipation requirements of drones and aerospace.

Method used

High thermal conductivity magnesium alloy sheets are prepared by using a melting-extrusion-rolling-annealing process, low-temperature extrusion and single-pass large reduction rolling, combined with alloy composition design, to refine grains and improve microstructure uniformity.

Benefits of technology

It significantly improves the thermal conductivity and mechanical properties of magnesium alloy sheets, shortens the process flow, reduces production costs, and meets the lightweight and efficient heat dissipation requirements of drones and aerospace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122503769A_ABST
    Figure CN122503769A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing high thermal conductivity magnesium alloy sheet, comprising: 1. preparing magnesium alloy raw materials and performing alloy melting, and casting to obtain a magnesium alloy billet; 2. homogenizing the magnesium alloy billet; 3. low-temperature extrusion of the homogenized magnesium alloy billet to obtain an extruded magnesium alloy slab; 4. high-temperature short-time heat treatment of the extruded magnesium alloy slab to obtain a heat-treated magnesium alloy sheet; 5. single-pass large-reduction rolling deformation of the heat-treated magnesium alloy sheet to obtain a rolled magnesium alloy sheet; 6. low-temperature short-time annealing of the rolled magnesium alloy sheet to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet. This invention employs a melting-extrusion-rolling-annealing process, effectively refining grains and improving the uniformity and density of the microstructure, enhancing forming quality, and obtaining a high thermal conductivity magnesium alloy sheet with good strength and ductility matching. Furthermore, the process is short and low-cost, making it suitable for 3C electronics, aerospace, and military applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material preparation and processing technology, and specifically relates to a method for preparing a high thermal conductivity magnesium alloy sheet. Background Technology

[0002] As low-altitude unmanned aerial vehicle (UAV) equipment develops towards lightweight, highly integrated, and long-endurance designs, higher demands are being placed on the thermal conductivity and lightweight properties of structural components such as electronic equipment housings and heat dissipation shells. Magnesium alloys, with their advantages of low density, high specific strength, and good shock absorption performance, have become ideal lightweight materials. However, traditional magnesium alloys generally have low thermal conductivity; for example, AZ-based magnesium alloys have a thermal conductivity of approximately 50–80 W / (m·K), and ZK-based magnesium alloys have a thermal conductivity of approximately 100–120 W / (m·K). Rare-earth magnesium alloys, due to their high content of rare-earth elements, typically have a thermal conductivity below 100 W / (m·K). These materials are insufficient to meet the heat dissipation requirements of high-power electronic components under high-load conditions, easily leading to excessive temperature rise, performance degradation, or even failure of the equipment. Therefore, developing magnesium alloy sheets with both high thermal conductivity and good mechanical properties has become a research hotspot in the UAV and aerospace fields.

[0003] Currently, the main approaches to improving the thermal conductivity of magnesium alloys include: optimizing alloy composition (reducing the scattering of electron heat transfer by solid solution atoms), and controlling grain size and texture through plastic deformation and heat treatment. For example, the thermal conductivity of pure magnesium can reach approximately 156 W / (m·K), but its mechanical properties are poor; while the thermal conductivity of commonly used magnesium alloys decreases significantly after strengthening with elements such as Al, Zn, and RE. In existing technologies, some studies have improved thermal conductivity while maintaining a certain strength by controlling the content of alloying elements and aging precipitation behavior, but this suffers from long preparation cycles and high costs, making industrial production difficult. In addition, existing magnesium alloy sheets are usually formed by multi-pass rolling, requiring frequent annealing between passes, resulting in complex processes; at the same time, research has focused more on improving the strength of the sheet, with insufficient attention paid to the systematic control of thermal conductivity.

[0004] In summary, developing a method for preparing magnesium alloy sheets suitable for industrial production that can balance high thermal conductivity and good mechanical properties, and meeting the lightweight and efficient heat dissipation requirements of components such as the cabin of unmanned aerial vehicle (UAV) electronic equipment, has significant engineering application value and market prospects. Summary of the Invention

[0005] The technical problem to be solved by this invention is to provide a method for preparing high thermal conductivity magnesium alloy sheets, addressing the shortcomings of the prior art. This method employs a melting-extrusion-rolling-annealing process. By using low-temperature extrusion and single-pass high-reduction rolling, the grain size is effectively refined and the uniformity and density of the microstructure are improved, enhancing the forming quality and obtaining high thermal conductivity magnesium alloy sheets with good strength and plasticity matching. This significantly shortens the process flow, reduces production costs, and solves the problem of the difficulty in preparing existing high thermal conductivity magnesium alloy sheets.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing a high thermal conductivity magnesium alloy plate, characterized in that the method includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the design composition of the target product magnesium alloy sheet and carry out alloy melting and casting to obtain magnesium alloy billet; Step 2: Homogenize the magnesium alloy billet from Step 1. Step 3: The magnesium alloy billet after homogenization in Step 2 is subjected to low-temperature extrusion to obtain an extruded magnesium alloy slab. Step 4: Perform high-temperature short-time heat treatment on the extruded magnesium alloy slab from Step 3 to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large-reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4 to obtain the rolled magnesium alloy sheet. Step 6: Perform low-temperature short-time annealing on the rolled magnesium alloy sheet from Step 5 to obtain a magnesium alloy sheet; the tensile strength of the magnesium alloy sheet is greater than 270 MPa, the yield strength is greater than 230 MPa, the elongation is greater than 10%, and the thermal conductivity is greater than 145 W / (m·K).

[0007] The above-mentioned method for preparing a high thermal conductivity magnesium alloy sheet is characterized in that the design composition of the target product magnesium alloy sheet in step one includes the following components by mass percentage: Zn 1%~3%, Cu 0.1%~0.25%, Ce or / and Mn 0.2%~0.5%, with the balance being Mg.

[0008] The above-mentioned method for preparing a high thermal conductivity magnesium alloy sheet is characterized in that the homogenization treatment in step two is: holding at 400℃~450℃ for 18h.

[0009] The above-mentioned method for preparing a high thermal conductivity magnesium alloy sheet is characterized in that the process parameters for low-temperature extrusion in step three are: extrusion temperature 250℃~350℃, extrusion ratio 16, and extrusion speed 0.1mm / s~0.5mm / s.

[0010] The method for preparing a high thermal conductivity magnesium alloy sheet described above is characterized in that the high-temperature short-time heat treatment in step four is: holding at 400℃ for 1 hour. This high-temperature short-time heat treatment after extrusion reduces internal dislocations in the slab, lowers deformation resistance, and thus improves the forming quality of the sheet.

[0011] The above-mentioned method for preparing a high thermal conductivity magnesium alloy sheet is characterized in that the single-pass large reduction rolling deformation in step five is as follows: the heat-treated magnesium alloy sheet is first preheated to 380°C and held for 30 minutes, and then subjected to single-pass rolling deformation with a rolling reduction of 60%~80%.

[0012] The method for preparing a high thermal conductivity magnesium alloy sheet described above is characterized in that the low-temperature short-time annealing in step six is: holding at 180℃~200℃ for 20 minutes. This low-temperature short-time annealing after rolling promotes dislocation recovery, reduces residual stress, and thus improves the sheet's plasticity and thermal conductivity.

[0013] Compared with the prior art, the present invention has the following advantages: 1. This invention reduces the Zn content in magnesium alloy sheets and introduces low-solid-solubility elements Cu / Ce to form a second phase with Zn, thereby effectively reducing the degree of matrix lattice distortion and improving the thermal conductivity of the alloy from the source. At the same time, by adding trace amounts of Mn to refine the grains and improve the strength of the magnesium alloy sheets, the invention achieves an integrated design of high-strength, high-plasticity, and high-thermal-conductivity magnesium alloy sheets from the source of alloy design.

[0014] 2. This invention employs a low-temperature extrusion process to obtain extruded magnesium alloy slabs with fine grains and uniform, dense structure. This effectively reduces the generation of defects in the slabs during subsequent rolling, improves the forming quality of the final magnesium alloy slabs, and helps to simultaneously enhance the mechanical properties of magnesium alloy slabs, including strength and plasticity.

[0015] 3. This invention uses single-pass large reduction rolling to achieve one-time forming of the sheet metal, eliminating the frequent intermediate annealing process required for multi-pass rolling of traditional magnesium alloy sheets, significantly shortening the process flow and reducing the production cost of the sheet metal.

[0016] 4. The magnesium alloy sheet prepared by this invention has a thermal conductivity of over 145 W / (m·K) and maintains a tensile strength of over 270 MPa and an elongation of over 10%, exhibiting excellent strength-plasticity-thermal conductivity matching, which can meet the lightweight and thermal conductivity requirements of UAV components.

[0017] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] Figure 1Metallographic image of the extruded magnesium alloy slab prepared in Example 1 of the present invention.

[0019] Figure 2 Metallographic image of the rolled magnesium alloy sheet prepared in Example 1 of the present invention.

[0020] Figure 3 Metallographic image of the extruded magnesium alloy slab prepared in Example 2 of the present invention.

[0021] Figure 4 Metallographic image of the rolled magnesium alloy sheet prepared in Example 2 of the present invention.

[0022] Figure 5 Metallographic image of the extruded magnesium alloy slab prepared in Example 3 of the present invention.

[0023] Figure 6 This is a metallographic image of the rolled magnesium alloy sheet prepared in Example 3 of the present invention. Detailed Implementation

[0024] Example 1 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 1%, Cu 0.1%, Ce 0.2%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 400℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 250℃, extrusion ratio 16, extrusion speed 0.1mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 80% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 180℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0025] Figure 1 The image shown is a metallographic image of the extruded magnesium alloy slab prepared in this embodiment. Figure 1It can be seen that the alloy grains in the extruded magnesium alloy slab are significantly refined, and the microstructure is dense and uniform, which can effectively reduce defects in the subsequent rolling process.

[0026] Figure 2 Here is a metallographic image of the rolled magnesium alloy sheet prepared in this embodiment, from... Figure 2 It can be seen that the grains of the rolled magnesium alloy sheet are larger and the precipitates are more numerous than those of the extruded magnesium alloy slab, which is beneficial to the improvement of the thermal conductivity of the magnesium alloy sheet.

[0027] Example 2 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 3%, Cu 0.1%, Mn 0.2%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 450℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 350℃, extrusion ratio 16, extrusion speed 0.2mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 60% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 200℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0028] Figure 3 The image shown is a metallographic image of the extruded magnesium alloy slab prepared in this embodiment. Figure 3 It can be seen that the alloy grains in the extruded magnesium alloy slab are also significantly refined.

[0029] Figure 4 Here is a metallographic image of the rolled magnesium alloy sheet prepared in this embodiment, from... Figure 4 It can be seen that the rolled magnesium alloy sheet also has a fine-grained structure and a large number of precipitates, which improves the mechanical and thermal conductivity of the magnesium alloy sheet.

[0030] Example 3 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 1%, Cu 0.1%, Ce 0.2%, Mn 0.2%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 420℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 280℃, extrusion ratio 16, extrusion speed 0.3mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 75% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 180℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0031] Figure 5 The image shown is a metallographic image of the extruded magnesium alloy slab prepared in this embodiment. Figure 5 It can be seen that the alloy grains in the extruded magnesium alloy slab are significantly refined, which lays the foundation for the large reduction in the subsequent rolling process.

[0032] Figure 6 Here is a metallographic image of the rolled magnesium alloy sheet prepared in this embodiment, from... Figure 6 It can be seen that the rolled magnesium alloy sheet also has a fine-grained structure and a large number of precipitates, which improves the mechanical and thermal conductivity of the magnesium alloy sheet.

[0033] Example 4 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 3%, Cu 0.25%, Ce 0.5%, Mn 0.5%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 450℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 350℃, extrusion ratio 16, extrusion speed 0.5mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 60% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 200℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0034] Example 5 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 2%, Cu 0.2%, Mn 0.2%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 430℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 320℃, extrusion ratio 16, extrusion speed 0.3mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 72% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 180℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0035] Example 6 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 2%, Cu 0.25%, Ce 0.25%, Mn 0.25%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 450℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 350℃, extrusion ratio 16, extrusion speed 0.3mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 65% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 190℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0036] Example 7 This embodiment includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the designed composition of the target product magnesium alloy sheet and perform alloy melting using gravity casting method. After casting, a cylindrical magnesium alloy billet is obtained. The designed composition of the target product magnesium alloy sheet includes the following components by mass percentage: Zn 1%, Cu 0.25%, Ce 0.2%, Mn 0.5%, with the balance being Mg. Step 2: Homogenize the magnesium alloy billet from Step 1 by holding it at 400℃ for 18 hours. Step 3: Perform low-temperature extrusion on the magnesium alloy billet after homogenization treatment in Step 2: extrusion temperature 300℃, extrusion ratio 16, extrusion speed 0.3mm / s, to obtain extruded magnesium alloy slab. Step 4: The extruded magnesium alloy slab from Step 3 is subjected to high-temperature short-time heat treatment at 400℃ for 1 hour to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4. First, preheat the heat-treated magnesium alloy sheet to 380℃ and hold for 30 minutes, then perform single-pass rolling deformation with a rolling reduction of 80% to obtain the rolled magnesium alloy sheet. Step 6: The rolled magnesium alloy sheet from Step 5 is subjected to low-temperature short-time annealing at 180℃ for 20 minutes to obtain a high-strength, high-ductility, and high-thermal-conductivity magnesium alloy sheet.

[0037] The thermal conductivity and mechanical properties of the magnesium alloy plates prepared in Examples 1-7 of this invention were tested, and the results are shown in Table 1.

[0038] Table 1

[0039] As shown in Table 1, the magnesium alloy sheets prepared in Examples 1-7 of this invention all have thermal conductivity higher than 145 W / (m·K) and tensile strength greater than 230 MPa, which are significantly better than existing commercial magnesium alloys and publicly reported high thermal conductivity magnesium alloys. Among them, the magnesium alloy sheet in Example 1 has a tensile strength of over 280 MPa, an elongation of over 10%, and a thermal conductivity of 156 W / (m·K), demonstrating excellent matching of thermal conductivity and mechanical properties.

[0040] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing a high thermal conductivity magnesium alloy sheet, characterized in that, The method includes the following steps: Step 1: Prepare magnesium alloy raw materials according to the design composition of the target product magnesium alloy sheet and carry out alloy melting and casting to obtain magnesium alloy billet; Step 2: Homogenize the magnesium alloy billet from Step 1. Step 3: The magnesium alloy billet after homogenization in Step 2 is subjected to low-temperature extrusion to obtain an extruded magnesium alloy slab. Step 4: Perform high-temperature short-time heat treatment on the extruded magnesium alloy slab from Step 3 to obtain heat-treated magnesium alloy sheet. Step 5: Perform single-pass large-reduction rolling deformation on the heat-treated magnesium alloy sheet from Step 4 to obtain the rolled magnesium alloy sheet. Step 6: Perform low-temperature short-time annealing on the rolled magnesium alloy sheet from Step 5 to obtain a magnesium alloy sheet; the tensile strength of the magnesium alloy sheet is greater than 270 MPa, the yield strength is greater than 230 MPa, the elongation is greater than 10%, and the thermal conductivity is greater than 145 W / (m·K).

2. The method for preparing a high thermal conductivity magnesium alloy sheet according to claim 1, characterized in that, The design composition of the target product magnesium alloy sheet mentioned in step one includes the following components by mass percentage: Zn 1%~3%, Cu 0.1%~0.25%, Ce and / or Mn 0.2%~0.5%, with the balance being Mg.

3. The method for preparing a high thermal conductivity magnesium alloy sheet according to claim 1, characterized in that, The homogenization process described in step two involves maintaining the temperature at 400℃~450℃ for 18 hours.

4. The method for preparing a high thermal conductivity magnesium alloy sheet according to claim 1, characterized in that, The process parameters for low-temperature extrusion in step three are: extrusion temperature 250℃~350℃, extrusion ratio 16, and extrusion speed 0.1mm / s~0.5mm / s.

5. The method for preparing a high thermal conductivity magnesium alloy sheet according to claim 1, characterized in that, The high-temperature short-time heat treatment mentioned in step four is: holding at 400℃ for 1 hour.

6. The method for preparing a high thermal conductivity magnesium alloy sheet according to claim 1, characterized in that, The single-pass large reduction rolling deformation described in step five is as follows: first, the heat-treated magnesium alloy sheet is preheated to 380℃ and held for 30 minutes, and then a single-pass rolling deformation is performed, with a rolling reduction of 60%~80%.

7. The method for preparing a high thermal conductivity magnesium alloy sheet according to claim 1, characterized in that, The low-temperature short-time annealing described in step six is: holding at 180℃~200℃ for 20 minutes.