Composite fishing net twine made from sisal fibre

CN122504063APending Publication Date: 2026-08-04GUANGXI SUBTROPICAL CROPS RESEARCH INSTITUTE(GUANGXI SUBTROPICAL AGRICULTURAL PRODUCTS PROCESSING RESEARCH INSTITUTE)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610850112.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-12
Publication Date
2026-08-04

AI Technical Summary

Technical Problem

[0002]渔网是用于捕捞水生生物的工具,多采用尼龙(PA)、聚乙烯(HDPE)或聚酯(PET)制作,尼龙、聚乙烯或聚酯均为高分子材料,具有强度高、耐磨性好的优势,但其长期浸泡在水中,会产生微塑料颗粒进入水体,而这些微塑料颗粒会随水体进入水域生物体、农田、饮用水,然后进入人体内,微塑料颗粒进入人体后可能划伤组织或堵塞微小结构,引发局部炎症反应,也可能会产生化学毒性,影响人体发育或激素平衡

Benefits of technology

(1)本发明先用果胶酶去除剑麻纤维表面的果胶,让纤维质地柔软、松散,同时以柠檬酸在纤维表面形成刻蚀效果,使其具有更多的孔洞和空隙,使其在后续能更好地容纳二氧化硅;后续以溶胶-凝胶法制备二氧化硅并使其均匀地填充在剑麻纤维的孔洞和空隙中,提高剑麻纤维的韧性和抗冲击强度,填充了二氧化硅之后,再加入钙源形成硫酸钙沉淀,提升剑麻纤维的硬度以及与二氧化硅的固化效果;改善了剑麻纤维的韧性之后,再以硅烷偶联剂改善剑麻纤维,使其在剑麻纤维表面形成疏水膜提高其在水中的耐久性,最后设置蜡质防水层,使其能具有更好地防水效果,从而能更有效的延长其使用寿命。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses a composite fishing net line made from sisal fiber. The preparation method includes the following steps: sisal fiber is depectinized by pectinase; a mixture of ethanol and water containing tetraethyl orthosilicate is prepared, the pretreated sisal fiber is added, dilute sulfuric acid is added to react, and then an alkaline calcium source solution is added to react further, yielding sisal fiber after one treatment; silane coupling agent is used to modify the sisal fiber to obtain sisal fiber after a second treatment; a waxy waterproof layer is sprayed onto the surface of the sisal fiber after the second treatment, and it is dried to obtain sisal fiber monofilaments; the sisal fiber monofilaments are twisted and fixed to obtain the composite fishing net line. This invention uses sisal fiber as the main material to make fishing net lines, which can provide more options for reducing water pollution caused by microplastic particles from fishing nets, and also provides a good idea for expanding the field of deep processing of sisal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sisal fiber deep processing technology, and in particular to a composite fishing net line made from sisal fiber. Background Technology

[0002] Fishing nets are tools used to catch aquatic life. They are mostly made of nylon (PA), polyethylene (HDPE), or polyester (PET). Nylon, polyethylene, and polyester are all high-molecular materials with advantages such as high strength and good wear resistance. However, when they are soaked in water for a long time, microplastic particles will enter the water body. These microplastic particles will enter aquatic organisms, farmland, drinking water, and then enter the human body. After entering the human body, microplastic particles may scratch tissues or block tiny structures, causing local inflammatory reactions. They may also produce chemical toxicity, affecting human development or hormone balance.

[0003] Sisal fiber is extracted from sisal leaves and is mainly used to make industrial steel wire rope cores and polishing wheels. It has the advantages of corrosion resistance, abrasion resistance, and non-hardening and brittleness at low temperatures. Applying it to the production of fishing net lines could provide more options for reducing water pollution caused by microplastic particles from fishing nets. Summary of the Invention

[0004] This invention discloses a composite fishing net line made from sisal fiber. Using sisal fiber as the main material to make the fishing net line can provide more options for reducing water pollution caused by microplastic particles in fishing nets, and also provides a good idea for expanding the field of deep processing of sisal.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows: A composite fishing net line made from sisal fiber, the preparation method includes the following steps: (1) Dissolve citric acid and sodium citrate in water until the pH value is 3~5 to obtain a buffer solution, and then add 0.05~0.3% of pectinase by weight of the buffer solution to obtain an enzymatic hydrolysate; (2) Soak sisal fibers in an enzymatic hydrolysate for 30-120 minutes. After soaking, clean and dry them to obtain pretreated sisal fibers. (3) Prepare a mixture of ethanol and water containing tetraethyl orthosilicate, put the pretreated sisal fiber into it, add dilute sulfuric acid, react under ultrasonic vibration for 30-40 min, then stop the vibration and let it stand for 20-30 min. Repeat the reaction and standing operation under vibration for 1-2 times. After the operation is completed, continue to add alkaline calcium source solution until the pH value of the reaction system is 7.5-8.5, react under ultrasonic vibration for 30-40 min, and let it stand for 50-60 min. After standing, wash and dry to obtain sisal fiber that has been processed in one step. (4) Dissolve the silane coupling agent in a solvent, add acid to adjust the pH value to 6.2~6.8, stir evenly, and spray it onto the surface of the sisal fiber after the first treatment in the form of a spray to obtain the sisal fiber after the second treatment. (5) Spray a waxy waterproof layer on the surface of the sisal fiber after secondary treatment, dry it to obtain sisal fiber monofilament, and twist and fix the sisal fiber monofilament to obtain the composite fishing net line.

[0006] Preferably, the waxy waterproof layer comprises a wax emulsion layer; The wax emulsion layer is formed by spraying wax emulsion, which is composed of the following raw materials in parts by weight: 20-25 parts paraffin wax, 1-2 parts fatty amine polyoxyethylene ether, 0.5-1 part fatty alcohol polyoxyethylene ether, 0.005-0.01 parts acetic acid, and 18-25 parts water.

[0007] Preferably, the waxy waterproof layer further includes a waxy layer surrounding the wax emulsion layer, wherein the waxy layer is formed by spraying paraffin wax or carnauba wax.

[0008] More preferably, the fatty amine polyoxyethylene ether is selected from one or more of tetradecylamine polyoxyethylene ether, dodecylamine polyoxyethylene ether, tallow amine polyoxyethylene ether, and stearylamine polyoxyethylene ether.

[0009] More preferably, in step (4), the silane coupling agent is one or more of vinyltriisopropoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane; And / or, in step (4), the amount of silane coupling agent used is 0.1-0.5‰ of the weight of sisal fibers after one treatment.

[0010] More preferably, in step (4), after the silane coupling agent is sprayed, the sprayed sisal fiber is left to stand naturally or air-dried until the liquid content is 8-20% to obtain the sisal fiber after secondary treatment.

[0011] More preferably, after the wax emulsion layer is sprayed, it is dried before the wax layer is sprayed.

[0012] More preferably, the amount of wax emulsion used is 1-3.6% of the mass of the sisal fibers after secondary processing. More preferably, the weight of the waxy layer is 0.5 to 2% of the mass of the sisal fiber after secondary processing.

[0013] Preferably, in step (2), the weight ratio of sisal fiber to enzymatic hydrolysate is 1:(8~20).

[0014] Preferably, in step (3), the mass ratio of tetraethyl orthosilicate, ethanol and water is 1:(2~3):(5~8). And / or, the mass ratio of the ethanol and water mixture containing tetraethyl orthosilicate to the pretreated sisal fibers is 1:(15~20). And / or, in step (3), after adding dilute sulfuric acid, adjust the initial pH of the reaction system to 2.5~3.0.

[0015] The composite fishing net line made from sisal fiber described above has the following advantages: (1) In this invention, pectinase is first used to remove pectin from the surface of sisal fiber, making the fiber soft and loose. At the same time, citric acid is used to form an etching effect on the fiber surface, making it have more pores and gaps, so that it can better accommodate silica in the later stage. Then, silica is prepared by sol-gel method and uniformly filled into the pores and gaps of sisal fiber to improve the toughness and impact strength of sisal fiber. After filling with silica, calcium source is added to form calcium sulfate precipitate, which improves the hardness of sisal fiber and the curing effect with silica. After improving the toughness of sisal fiber, silane coupling agent is used to improve sisal fiber, so that a hydrophobic film is formed on the surface of sisal fiber to improve its durability in water. Finally, a wax waterproof layer is set to make it have better waterproof effect, thereby more effectively extending its service life.

[0016] (2) The present invention further selects a vinyl silane coupling agent, which can form a reactive silanol intermediate after hydrolysis. It can crosslink with the hydroxyl groups on the surface of sisal fiber and the hydroxyl groups on the surface of silica, and firmly graft onto the surface of sisal fiber. After hydrolysis, it carries a slight negative charge, which can be more firmly combined with the wax emulsion with slight cations in the wax waterproof layer, thereby improving the adhesion effect of the wax emulsion on the surface of sisal fiber and better improving the water resistance of fishing net line.

[0017] (3) This invention uses pure natural sisal fiber as the main material and does not introduce polymer materials such as nylon, polyethylene, and polyester as raw materials. This can avoid the water entering the fishing net during fishing, reduce the pollution of water by microplastic particles in the fishing net, and is environmentally friendly. It provides an environmentally friendly option for the production of fishing nets and also provides a good idea for expanding the field of deep processing of sisal. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0019] Example 1

[0020] A composite fishing net line made from sisal fiber, the preparation method includes the following steps: (1) Dissolve citric acid and sodium citrate in water until the pH value is 4.5 to obtain a buffer solution, and then add 0.1% of pectinase by weight of the buffer solution to obtain an enzymatic hydrolysate; (2) Soak sisal fiber in enzymatic hydrolysate. The weight ratio of sisal fiber to enzymatic hydrolysate is 1:12. The soaking time is 120 min. After soaking, wash with water and dry to obtain pretreated sisal fiber. (3) Prepare a mixture of ethanol and water containing tetraethyl orthosilicate. The mass ratio of tetraethyl orthosilicate, ethanol and water is 1:3:6.5. Add pretreated sisal fibers. The mass ratio of the mixture of ethanol and water containing tetraethyl orthosilicate to the pretreated sisal fibers is 1:18. Add dilute sulfuric acid. After adding dilute sulfuric acid, adjust the initial pH of the reaction system to 2.5. React under ultrasonic vibration (frequency 22kHz) for 40min. Then stop the vibration and let it stand for 30min. Repeat the reaction and standing operation under vibration conditions once. After the operation is completed, continue to add saturated Ca (OH)2 solution until the pH of the reaction system is 8.0. React under ultrasonic vibration for 35min. Let it stand for 60min. After standing, wash once with water and once with ethanol. Dry at 75℃ for 3h to obtain sisal fibers that have been treated once. (4) Dissolve vinyltriisopropoxysilane in ethanol, add glacial acetic acid to adjust the pH value to 6.2, stir evenly, and spray it onto the surface of the sisal fiber after one treatment in the form of a spray. The amount of silane coupling agent is 0.3‰ of the weight of the sisal fiber after one treatment. In step (4), after the spraying is completed, place the sprayed sisal fiber naturally or air dry it until the liquid content is 12% to obtain the sisal fiber after two treatments. (5) Spray a wax emulsion layer onto the surface of the sisal fiber after secondary treatment. The wax emulsion is composed of the following raw materials in parts by weight: 22 parts of paraffin (58#), 1.5 parts of dodecylamine polyoxyethylene ether, 0.8 parts of fatty alcohol polyoxyethylene ether (AEO-15), 0.01 parts of glacial acetic acid, and 20 parts of water. The amount of wax emulsion used is 2.5% of the mass of the sisal fiber after secondary treatment. After spraying, dry at 40°C for 5 hours to obtain sisal fiber monofilaments. Twist and fix the sisal fiber monofilaments to obtain composite fishing net line.

[0021] Example 2

[0022] Example 2 is basically the same as Example 1, except that after drying at 40°C for 5 hours after spraying, a wax layer is sprayed on in the form of a spray. The wax layer is made of paraffin wax and the amount used is 1.2% of the mass of the sisal fiber after secondary treatment.

[0023] Example 3

[0024] A composite fishing net line made from sisal fiber, the preparation method includes the following steps: (1) Dissolve citric acid and sodium citrate in water until the pH value is 3 to obtain a buffer solution, and then add 0.05% of pectinase by weight of the buffer solution to obtain an enzymatic hydrolysate; (2) Soak sisal fibers in an enzymatic hydrolysate with a weight ratio of sisal fibers to enzymatic hydrolysate of 1:20 and a soaking time of 90 min. After soaking, rinse with water and dry to obtain pretreated sisal fibers. (3) Prepare a mixture of ethanol and water containing tetraethyl orthosilicate. The mass ratio of tetraethyl orthosilicate, ethanol and water is 1:2:5. Add pretreated sisal fibers. The mass ratio of the mixture of ethanol and water containing tetraethyl orthosilicate to the pretreated sisal fibers is 1:15. Add dilute sulfuric acid. After adding dilute sulfuric acid, adjust the initial pH of the reaction system to 2.5. React under ultrasonic vibration (frequency 22kHz) for 30min. Then stop the vibration and let stand for 30min. Repeat the reaction and standing operation under vibration conditions twice. After the operation is completed, continue to add saturated Ca (OH)2 solution until the pH of the reaction system is 7.5. React under ultrasonic vibration for 30min. Let stand for 60min. After standing, wash once with water and once with ethanol. Dry at 75℃ for 3h to obtain sisal fibers that have been treated once. (4) Dissolve vinyltriisopropoxysilane in ethanol, add glacial acetic acid to adjust the pH value to 6.5, stir evenly, and spray it onto the surface of the sisal fiber after one treatment in the form of a spray. The amount of silane coupling agent is 0.5‰ of the weight of the sisal fiber after one treatment. In step (4), after spraying, place the sprayed sisal fiber naturally or air dry it until the liquid content is 10% to obtain the sisal fiber after two treatments. (5) Spray a wax emulsion layer onto the surface of the sisal fiber after secondary treatment. The wax emulsion is composed of the following raw materials in parts by weight: 20 parts of paraffin (58#), 2 parts of dodecylamine polyoxyethylene ether, 1 part of fatty alcohol polyoxyethylene ether (AEO-15), 0.01 parts of glacial acetic acid, and 18 parts of water. The amount of wax emulsion used is 3.6% of the mass of the sisal fiber after secondary treatment. After spraying, dry at 40°C for 5 hours to obtain sisal fiber monofilaments. Twist and fix the sisal fiber monofilaments to obtain composite fishing net line.

[0025] Example 4

[0026] Example 4 is basically the same as Example 3, except that after drying at 40°C for 5 hours after spraying, a wax layer is sprayed on in the form of a spray. The wax layer is made of paraffin wax and the amount used is 1.5% of the mass of the sisal fiber after secondary treatment.

[0027] Comparative Example 1

[0028] Comparative Example 1 uses the pretreated sisal fiber from Example 1 as the sisal fiber monofilament, and the sisal fiber monofilament is twisted and fixed to obtain the fishing net line.

[0029] Comparative Example 2

[0030] Comparative Example 2 uses sisal fibers processed in one step as sisal fiber monofilaments, and the sisal fiber monofilaments are twisted and fixed to obtain fishing net lines.

[0031] Comparative Example 3

[0032] Comparative Example 3 uses sisal fibers that have undergone secondary processing in Example 1, dried as sisal fiber monofilaments, and twists and fixes the sisal fiber monofilaments to obtain fishing net lines.

[0033] Comparative Example 4

[0034] Comparative Example 4 uses untreated sisal fiber as sisal fiber monofilament, and the sisal fiber monofilament is twisted and fixed to obtain fishing net line.

[0035] The mechanical properties of the fishing net lines (0.2 mm in diameter) prepared in Examples 1-4 and Comparative Examples 1-4 were tested. The breaking strength was tested according to standard SC / T 4022-2007 "Determination of Breaking Strength and Knot Breaking Strength of Fishing Net Lines", and the breaking elongation was tested according to SC / T 4023-2007 "Determination of Elongation of Fishing Net Lines". The test results are shown in Table 1. Table 1. Test results of mechanical performance of fishing net line

[0036] The fishing net lines prepared in Examples 1-4 and Comparative Examples 1-4 were subjected to a 400-hour exposure aging test. The fishing net lines were placed in an accelerated UV aging chamber using UVA-340 lamps. The distance between the fishing net line sample and the lamp was 50mm ± 2mm. The humidity was controlled at 48 ± 2%, and the temperature at 60 ± 2℃. The net lines were exposed to rainwater for 20 minutes every two hours for a total of 400 hours. After the test, the breaking strength of the fishing net line samples was measured. The test results are shown in Table 2. Table 2 Aging Test

[0037] As can be seen from Table 2, the anti-aging properties of sisal fiber are significantly improved after pectin removal, filling, modification with silane coupling agent, and spraying with a wax waterproof layer. This allows sisal fiber to better extend its service life when used in the production of fishing net lines.

[0038] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A composite fishing net line made from sisal fibers, characterized in that, The preparation method includes the following steps: (1) Dissolve citric acid and sodium citrate in water until the pH is 3-5 to obtain a buffer solution, and then add 0.05-0.3% of pectinase by weight of the buffer solution to obtain an enzymatic hydrolysate; (2) Soak sisal fibers in an enzymatic hydrolysate for 30-120 minutes. After soaking, clean and dry them to obtain pretreated sisal fibers. (3) Prepare a mixture of ethanol and water containing tetraethyl orthosilicate, put the pretreated sisal fiber into it, add dilute sulfuric acid, react under ultrasonic vibration for 30-40 min, then stop the vibration and let it stand for 20-30 min. Repeat the reaction and standing operation under vibration for 1-2 times. After the operation is completed, continue to add alkaline calcium source solution until the pH value of the reaction system is 7.5-8.5, react under ultrasonic vibration for 30-40 min, and let it stand for 50-60 min. After standing, wash and dry to obtain sisal fiber that has been processed in one step. (4) Dissolve the silane coupling agent in a solvent, add acid to adjust the pH value to 6.2~6.8, stir evenly, and spray it onto the surface of the sisal fiber after the first treatment in the form of a spray to obtain the sisal fiber after the second treatment. (5) Spray a waxy waterproof layer on the surface of the sisal fiber after secondary treatment, dry it to obtain sisal fiber monofilament, and twist and fix the sisal fiber monofilament to obtain the composite fishing net line.

2. The composite fishing net line prepared using sisal fiber according to claim 1, characterized in that, The waxy waterproof layer includes a wax emulsion layer; The wax emulsion layer is formed by spraying wax emulsion, which is composed of the following raw materials in parts by weight: 20-25 parts paraffin wax, 1-2 parts fatty amine polyoxyethylene ether, 0.5-1 part fatty alcohol polyoxyethylene ether, 0.005-0.01 parts acetic acid, and 18-25 parts water.

3. The composite fishing net line prepared using sisal fiber according to claim 2, characterized in that, The waxy waterproof layer also includes a waxy layer surrounding the wax emulsion layer, which is formed by spraying paraffin wax or palm wax.

4. The composite fishing net line prepared using sisal fiber according to claim 2, characterized in that, In step (4), the silane coupling agent is one or more of vinyltriisopropoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane; And / or, in step (4), the amount of silane coupling agent used is 0.1-0.5‰ of the weight of sisal fibers after one treatment.

5. The composite fishing net line prepared using sisal fiber according to any one of claims 1 to 4, characterized in that, In step (4), after the silane coupling agent is sprayed, the sprayed sisal fiber is left to stand naturally or air-dried until the liquid content is 8-20%, and the sisal fiber after secondary treatment is obtained.

6. The composite fishing net line prepared using sisal fiber according to claim 3, characterized in that, After the wax emulsion layer is sprayed and dried, the wax layer is then sprayed on.

7. The composite fishing net line prepared using sisal fiber according to claim 1, characterized in that, In step (2), the weight ratio of sisal fiber to enzymatic hydrolysate is 1:(8~20).

8. The composite fishing net line prepared using sisal fiber according to claim 1, characterized in that, In step (3), the mass ratio of tetraethyl orthosilicate, ethanol and water is 1:(2~3):(5~8); And / or, the mass ratio of the ethanol and water mixture containing tetraethyl orthosilicate to the pretreated sisal fibers is 1:(15~20). And / or, in step (3), after adding dilute sulfuric acid, adjust the initial pH of the reaction system to 2.5~3.

0.

9. The composite fishing net line prepared using sisal fiber according to claim 2, characterized in that, The amount of wax emulsion used is 1 to 3.6% of the mass of the sisal fiber after secondary processing.

10. The composite fishing net line prepared using sisal fiber according to claim 2, characterized in that, The weight of the waxy layer is 0.5 to 2% of the mass of the sisal fiber after secondary processing.