Application of a modified Al2O3-supported PtZn bimetallic catalyst in propane dehydrogenation

CN122538112APending Publication Date: 2026-08-11DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610722701.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-25
Publication Date
2026-08-11

AI Technical Summary

Technical Problem

然而,这些策略在推动科学认识的同时,也暴露了与工业需求之间的鸿沟:分子筛材料本身存在制备成本高、水热稳定性有限、机械强度不足等固有限制;而更具工业载体潜力的氧化铝,却因其表面酸性强、与PtZn相互作用调控难,导致在其上构建同时具备高活性、高稳定性且能耐受再生的PtZn活性位点极具挑战

Benefits of technology

1.本发明中制备得到的Al2O3负载的PtZn双金属亚纳米催化剂,在低负载(0.3%)下,实现了远超其他PtZn/Al2O3的活性和稳定性。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122538112A_ABST
    Figure CN122538112A_ABST
Patent Text Reader

Abstract

This invention focuses on the application of a PtZn / Al2O3 bimetallic catalyst in the propane dehydrogenation reaction. A uniquely structured mixed oxide support was synthesized through a co-precipitation strategy incorporating an appropriate amount of silicon (Si), and metallic Pt was loaded using an equal-volume impregnation method. Benefiting from the uniform dispersion of Zn, Pt is atomically dispersed on the surface of Zn nanoclusters, improving metal utilization and catalytic efficiency. The introduction of Si significantly optimizes the metal-support interaction, greatly enhancing the catalyst's activity and stability. With catalyst particles of 20-40 mesh, it exhibits excellent catalytic performance, along with good high-temperature stability and resistance to carbon deposition. This preparation process is simple, reproducible, and achieves efficient and highly selective propylene production with low amounts of precious metals, demonstrating promising industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention pertains to the field of industrial applications and relates to the preparation of a catalyst and its performance in propane dehydrogenation. Specifically, it relates to the preparation of a modified Al₂O₃-supported PtZn bimetallic catalyst and its application in the direct dehydrogenation of propane to propylene. Background Technology

[0002] Propylene, as one of the most critical olefin feedstocks in the global chemical industry chain, is second only to ethylene in importance. It is the basic raw material for the production of polypropylene, acrylonitrile, propylene oxide, butanol, octanol, acrylic acid, and many other high-value-added chemicals, and is widely used in plastics, rubber, synthetic fibers, medical devices, building materials, and the automotive industry. With the continuous development of the global chemical industry, especially the rapid growth in demand for synthetic materials from emerging economies, global demand for propylene has exceeded 100 million tons annually and continues to climb at a rate of approximately 4% per year. Traditional propylene production methods, such as naphtha steam cracking and catalytic cracking, are gradually becoming unable to meet the growing market demand. Against this backdrop, propane direct dehydrogenation (PDH) technology, due to its strong feedstock specificity, high propylene selectivity, and adaptability to the emerging shale gas industry, has become the core technological path for increasing propylene production and diversifying the industry's feedstock and promoting a shift towards lighter-weight products. For China in particular, developing independently controllable PDH technology is of paramount strategic importance. my country is the world's largest producer and consumer of propylene, but has long relied on technology imports. Meanwhile, the PDH process is a strongly endothermic reaction (ΔH = +124 kJ / mol), requiring temperatures above 600℃, which presents challenges due to thermodynamic equilibrium limitations and high energy consumption. Therefore, developing efficient, stable, and low-energy-consumption PDH catalysts and processes is not only crucial for enhancing the core competitiveness of my country's chemical industry, but also an urgent need to promote the industry's green and low-carbon development.

[0003] The Oleflex and Catofin processes are two of the most representative technologies for direct propane dehydrogenation, holding a dominant position in global production capacity. The Oleflex process uses PtSn / Al2O3 as a catalyst. While facing the price issue of the precious metal Pt, the Pt-based alumina catalyst is recyclable, offering a high return on investment and being environmentally friendly. The Catofin process uses Cr2O3 / Al2O3 as a catalyst, which has a relatively lower cost, but its presence of the heavy metal chromium poses environmental challenges, and frequent catalyst regeneration increases operational complexity and costs. In contrast, Pt-based catalysts dominate industrial applications due to their high activity and selectivity, with PtSn catalysts exhibiting the best overall performance and a mature industrial system.

[0004] However, PtSn catalysts still face the challenge of simultaneously achieving high activity and high stability, as well as deactivation due to sulfur impurities in domestic feed gas. When catalysts deactivate due to sintering and carbon deposition of the active component Pt, frequent redispersion of Pt in an oxygen-chlorine atmosphere via chlorine-induced redispersion is required to restore their catalytic activity. This process leads to equipment corrosion and the generation of chlorine-containing pollutants, resulting in significant carbon emissions and high energy consumption.

[0005] To address key issues such as the sintering tendency of Pt-based catalysts at high temperatures and limited propylene selectivity, this study aims to enhance Pt stability and optimize product desorption behavior by selecting appropriate promoters and supports. A typical characteristic of PtSn catalysts is the gradual decrease in catalytic activity as the reaction proceeds, necessitating repeated redox regeneration. Designing highly stable PtSn catalysts requires clarifying the structure-activity relationship of PtSn under reaction conditions. Currently, the understanding of the active site structure of the PtSn system remains controversial in the literature, with proposals such as Pt-SnO... x Different structural models, such as Pt-Sn disordered alloys and various metallic compounds, have been developed. Based on this, precise control of the Pt atomic microenvironment—by changing the types (e.g., Zn, In, Ga) and distances of neighboring atoms—can further fine-tune the d-band center of Pt, achieving a balance between activity and selectivity. Simultaneously, the properties of the support play a crucial synergistic role: different support types (e.g., Al2O3 and molecular sieves), surface defect sites, and unique confinement effects can effectively anchor metal particles and stabilize active sites. Furthermore, exploring other metallic active components (such as noble metal Rh, or non-noble metals Ni, Co, etc.) as substitutes for Pt provides a broader space for material exploration in developing low-cost, high-stability catalyst systems.

[0006] Over the years, with the research on various additives, Zn has been regarded as an ideal additive with great potential to replace Sn. Among many Pt-M alloys, Pt-Zn alloys, due to their moderate atomic radius ratio and significant electronegativity difference, simultaneously achieve optimal electronic structure and spatial isolation at the atomic scale, theoretically exhibiting the best selectivity and catalytic performance. On the one hand, Zn can form thermodynamically more stable and structurally highly ordered intermetallic compounds such as Pt1Zn1 and Pt3Zn1 with Pt, which can effectively suppress multi-point adsorption of coke precursors, and ensure structural integrity at high temperatures through the exothermic formation of Pt-Zn bonds and low surface segregation. In particular, in the Pt1Zn1 intermetallic compound, the Pt atoms in the [PtZn4] structure on the surface are isolated by four Zn atoms, forming a single site, which effectively inhibits deep dehydrogenation of propylene. On the other hand, the ZnO component also endows the catalyst with a certain degree of resistance to sulfur poisoning, making it suitable for industrial environments with more relaxed requirements for the purity of feed gas. Therefore, the Pt-Zn system, with its more robust atomic structure and superior electronic control capabilities, offers a more promising solution to overcome the bottlenecks in high-temperature stability and regenerability of traditional Pt-Sn catalysts.

[0007] However, PtZn-based catalysts still face severe intrinsic and engineering challenges in their path to large-scale industrial application. The core issue lies in the dynamic evolution and instability of their thermodynamically metastable structure under harsh operating conditions: during long-term high-temperature reactions and multiple oxidation-regeneration cycles, Zn, due to its low boiling point, is prone to selective volatilization and loss, leading to the destruction of the precisely constructed structure, Pt particle agglomeration, and irreversible decline in catalytic activity. To address this challenge, research has mainly followed two paths: one is to utilize the rigid channels of molecular sieves (such as Silicalite-1 and Beta) to achieve atomic-level confinement, physically binding metal species; the other is to introduce a third component (such as La, Ge, or alkali metals) to inhibit Zn migration by forming stronger bonds. However, while these strategies advance scientific understanding, they also expose a gap between them and industrial needs: molecular sieve materials themselves have inherent limitations such as high preparation costs, limited hydrothermal stability, and insufficient mechanical strength; while alumina, which has greater potential as an industrial support, faces significant challenges in constructing PtZn active sites that simultaneously possess high activity, high stability, and the ability to withstand regeneration due to its strong surface acidity and difficulty in regulating interactions with PtZn. Therefore, the key to future breakthroughs lies in developing rational design principles for industrial applications, namely, how to manufacture PtZn-based catalysts that maintain structural integrity and performance stability in real reaction-regeneration cycles on inexpensive and robust alumina supports through surface and interface modification and multi-component synergistic regulation. This requires systematic innovation across multi-scale material design, in-situ characterization, and engineering verification. Summary of the Invention

[0008] The purpose of this invention is to provide a modified Al₂O₃-supported PtZn bimetallic sub-nano catalyst for propane dehydrogenation, in view of the aforementioned state of the prior art. This catalyst exhibits both high activity and high selectivity for propane dehydrogenation.

[0009] To achieve the above objectives, the specific technical solution is as follows: the application of a modified Al2O3-supported PtZn bimetallic catalyst in the dehydrogenation of propane to propylene.

[0010] The catalyst was obtained by co-precipitation, in which a precursor solution impregnated with Pt on a Si and Zn-doped Al2O3 support was dried and then reduced in a hydrogen atmosphere.

[0011] Furthermore, the mass percentage of Zn in the catalyst support is 10%-20%, the mass percentage of Al is 20%-40%, and the mass percentage of Si is 2%-21% (among which the catalyst performance is excellent when the Si content is 10%-21%, and the performance is best when it is 15%-17%).

[0012] Furthermore, the Pt-impregnated precursor solution was impregnated using an equal-volume impregnation method, and the mass loading of Pt in the catalyst relative to the support was 0.2%-0.3%. The reduction process in a hydrogen atmosphere is as follows: reduction is carried out in a mixture of H2 and He with a hydrogen volume percentage of 10%-100% at 580-620℃ for 1-4 hours.

[0013] Furthermore, the preparation method of the Si,Zn-doped Al2O3 support includes the following steps: S1 To prepare metal salt solution A, weigh the soluble precursors of zinc and aluminum and water into a container and dissolve all the solids. S2 Prepare solution B by weighing sodium hydroxide, anhydrous sodium carbonate and water into a container and dissolving them completely. Heat the resulting solution to 60-80 ℃ and then add the silicon precursor to dissolve it. S3 Keep the prepared solution B at 60-80 ℃, and introduce the solution A prepared in step S1 into solution B, while continuously stirring solution B during the introduction process; S4: After the import is complete, stop stirring and continue to age at 60-80 ℃ for 20-30 h; S5: Filter the aged turbid liquid from step S4 while hot, and wash the filter cake with water until the filtrate is neutral. Place the obtained solid in an oven at 50-70 ℃ and dry for 20-30 hours. Grind and crush the dried solid, and calcine it at 500-600 ℃ for 2-3 hours to obtain ZnAlSiO2. x Carrier.

[0014] Furthermore, the precursor salt of Zn is zinc nitrate hexahydrate, the precursor salt of Al is aluminum nitrate nonahydrate, the precursor salt of Si is sodium silicate nonahydrate, and the precursor of Pt is H2PtCl6.

[0015] Furthermore, the concentrations of the solutions prepared in steps S1 and S2 are as follows: Aluminum nitrate (0.5-0.75 mol / L); Sodium hydroxide (1.5-2 mol / L), sodium carbonate (0.5-0.6 mol / L), sodium silicate (0.01-0.2 mol / L).

[0016] Furthermore, the preparation method of the aforementioned diatomic catalyst includes the following steps: S1: Take ZnAlSiO x The carrier was impregnated with a Pt precursor solution using an equal-volume impregnation method onto ZnAlSiO2. x On the carrier, continuously stir until a viscous paste is formed, let stand at room temperature for 2-12 h, and dry in an oven at 50-70 ℃ for 12-24 h to obtain the catalyst precursor; S2: The catalyst precursor obtained in step S1 is reduced at 580-620 °C in a mixture of H2 and He with a hydrogen volume percentage of 10% to 100% for 1-4 h to obtain Pt / ZnAlSiO2. x catalyst.

[0017] Furthermore, the specific process of step S2 is as follows: The catalyst precursor obtained in step S1 is tableted, crushed and sieved to select particles of 20-40 mesh; the particles are weighed and uniformly mixed with inert quartz sand (20-40 mesh) and placed in a U-shaped quartz tube of a fixed bed reactor; the mixture of H2 and He with a hydrogen volume percentage of 10% to 100% is reduced for 1-4 h at 580-620 °C.

[0018] Furthermore, the reaction conditions were 600 °C, with the following feed gas volume ratio: 14% C3H8, 14% H2; the balance being He, and the WHSV being 40 h⁻¹. -1 .

[0019] In this invention, a Si- and Zn-doped alumina support is prepared by co-precipitation, and then an equal volume of Pt precursor solution is impregnated to obtain a PtZn bimetallic catalyst. After reduction, the Pt and Zn interact, and after further reactant gas treatment, an alloy is formed between Pt and Zn. By adjusting the Si content ratio in the support, the acidic sites on the support surface can be controlled, thus both disrupting the carbon deposition bed and achieving atomic-level dispersion of Pt.

[0020] The preparation method of the PtZn bimetallic sub-nanometer catalyst of the present invention involves co-precipitation to obtain Si, Zn-doped Al2O3 support, and Pt loading by equal-volume impregnation. The active component Pt has a mass percentage content of 0.3%, a zinc-to-aluminum ratio of 1 / 5, and a Si mass percentage content of 0-20%. The Pt precursor solution used is an aqueous solution of H2PtCl6·6H2O. Drying conditions are oven drying at 60-120℃ for 6-30 h, and reduction conditions are reduction at 600℃ under 10-100% H2 / He conditions for 1-10 h.

[0021] The PtZn bimetallic sub-nano catalyst prepared by any of the above methods was used in the propane dehydrogenation reaction. The characteristic reaction conditions were: a reaction temperature of 600℃, a reaction gas volume ratio of 14% C3H8, 14% H2, with the balance being He, and a WHSV of 40 h⁻¹. -1 .

[0022] Compared with the prior art, the present invention has the following advantages: 1. The Al2O3-supported PtZn bimetallic sub-nano catalyst prepared in this invention achieves significantly higher activity and stability than other PtZn / Al2O3 catalysts at a low loading (0.3%).

[0023] 2. The composite oxide support prepared in this invention optimizes the pore structure through Si doping, achieving a more uniform pore size distribution.

[0024] 3. The PtZn bimetallic sub-nano catalyst prepared in this invention has Zn uniformly doped in an alumina support, which effectively improves the utilization rate of Pt by uniformly anchoring Pt in the bulk Zn.

[0025] 4. The PtZn bimetallic sub-nano catalyst prepared in this invention forms a PtZn alloy after the reaction, wherein Pt atoms are dispersed at the atomic level on the surface of Zn sub-nano clusters, effectively isolating active sites and significantly inhibiting deep dehydrogenation and carbon deposition of propylene, thereby improving propylene selectivity. The highly dispersed Pt atoms greatly enhance the metal utilization rate of Pt, resulting in high activity at low loading levels. Si doping further modulates the acidity and pore structure of the support surface, promoting the atomic-level dispersion of Pt and structural stability at high temperatures, enabling the catalyst to maintain high activity and anti-carbon deposition ability during long-term reactions at 600℃.

[0026] This catalyst employs a co-precipitation strategy involving the introduction of appropriate amounts of silicon (Si) to synthesize a uniquely structured mixed oxide support, which is then loaded with metallic Pt via an equal-volume impregnation method. Benefiting from the uniform dispersion of Zn, Pt is atomically dispersed on the surface of Zn nanoclusters, enhancing metal utilization and catalytic efficiency. The introduction of Si significantly optimizes the metal-support interaction, greatly improving the catalyst's activity and stability. With catalyst particles of 20-40 mesh, it exhibits excellent catalytic performance, along with good high-temperature stability and resistance to carbon deposition. This preparation process is simple, reproducible, and achieves efficient and highly selective propylene production with low amounts of precious metals, demonstrating promising prospects for industrial applications. Attached Figure Description

[0027] Figure 1 The graphs show the activity test results of Examples 6, 7, 8 and Comparative Example 6 after 30 h of reaction.

[0028] Figure 2 The regeneration stability test was conducted for Example 15 and Comparative Example 10.

[0029] Figure 3 The N2 adsorption isotherms are for the supports in Examples 1, 2, 3 and Comparative Example 1.

[0030] Figure 4 The images show the pore size distribution of the carriers in Examples 1, 2, 3 and Comparative Example 1.

[0031] Figure 5 The images show the XRD patterns of the carriers in Examples 1, 2, 3 and Comparative Example 1.

[0032] Figure 6 The images show the NMR spectra of the vectors in Examples 1, 2, 3 and Comparative Example 1.

[0033] Figure 7 The image shows the restored AC-HAADF-STEM from Example 2, along with the corresponding EDS mapping.

[0034] Figure 8 The images show AC-HAADF-STEM, HAADF-STEM, and particle size distribution after 30 hours of reaction in Example 7. Figure 9 EDS mapping of Example 7 after reaction at 600°C for 30 h.

[0035] Figure 10 The images show the NH3-TPD analysis results of the carriers in Examples 1, 2, 3, and Comparative Example 1.

[0036] Figure 11 Thermogravimetric analysis (TGA) diagrams of Examples 6, 7, 8 and Comparative Example 6 after 30 h of reaction.

[0037] The present invention will now be described in detail through specific embodiments. It should be noted that these embodiments are merely examples and do not constitute any limitation on the nature and scope of the present invention. The present invention can be implemented as long as it meets the conditions set forth in the content section. Therefore, the scope of protection of the present invention is determined by the claims. Detailed Implementation

[0038] Example 1. 0.3Pt / ZnAlSiO x Preparation of -10 particulate catalyst: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonhydrate into a 250 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide, 13.25 g of anhydrous sodium carbonate, and 3.9 g of sodium silicate nonhydrate into a 500 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind it, and calcine it at 550°C for 2 hours to obtain ZnAlSiO2. x -10 carrier.

[0039] X-ray fluorescence spectrometry was used to analyze ZnAlSiO x The -10 carrier was scanned to measure its elemental composition. The measurement results are shown in Table 1. The mass content of Al is 31.9%, the mass content of Zn is 15.2%, the mass content of Si is 9.7%, and the mass content of O is 43.2%.

[0040] X-ray diffraction was used to analyze ZnAlSiO x -10° carrier powder was continuously scanned to determine its crystal phase composition; the scanning range 2θ was 10-90°. (See attached...) Figure 2 As shown, only the characteristic diffraction peaks of Al2O3 are present, while those of ZnO and SiO2 are absent. This indicates that Zn and Si oxides may either be doped into the alumina lattice without forming an independent phase, or they may form an amorphous structure. Furthermore, the diffraction peaks of the support are shifted to lower angles relative to the alumina, indicating lattice expansion, which suggests that Zn has been doped into the alumina.

[0041] The ZnAlSiOx-10 support powder was collected using a solid-state nuclear magnetic resonance spectrometer. 29 Si nuclear magnetic resonance spectrum ( 29Si MASNMR was used to analyze the coordination environment and chemical state of silicon atoms in its framework structure. (See attached image.) Figure 6 As shown, no phase similar to SiO2 (which typically appears at -110 ppm, corresponding to Q) was observed. 4 The resonance signal corresponding to the species was detected. Instead, a characteristic signal centered at approximately -85 ppm was detected, which belongs to the Q series. 1 and Q 2 Silicon species (corresponding to Si atoms connecting one or two silicon-oxygen bridges respectively). This phenomenon indicates that SiO2 does not form an independent phase, but is uniformly doped into the amorphous network.

[0042] ZnAlSiO was analyzed using a multi-station fully automated specific surface area and porosity analyzer. x -10 carrier (20-40 mesh) was used for pore structure analysis, as shown in the attached figure. Figure 3 As shown, the pore size distribution curve indicates that the carrier exhibits typical mesoporous characteristics, with the pore size mainly distributed in the range of 2-60 nm, and a sharp peak at 3-4 nm.

[0043] ZnAlSiO was analyzed using a fully automated temperature-programmed chemisorption analyzer. x The -10 support (20-40 mesh) was characterized by ammonia-programmed temperature-rise desorption. 100 mg of catalyst was weighed and placed in a U-shaped quartz tube. After reduction at 600 °C for 1 h in an H2 / Ar atmosphere with a volume concentration of 10%, the temperature was lowered to 100 °C, and the atmosphere was switched to Ar for purging. The TCD signal was recorded online, and NH3 was manually pulsed until the peak area remained constant. Subsequently, the temperature was increased from room temperature to 800 °C at a rate of 10 °C / min, and the mass spectrometry signal was recorded simultaneously to detect the number of acidic sites on the support. As shown in Figure 9, the 100 °C-400 °C range contains moderately weakly acidic sites, which are important factors leading to carbon deposition, ZnAlSiO2. x The -10 carrier's weakly acidic sites are compared to ZnAlO x The carrier has been reduced.

[0044] Take 200mg ZnAlSiO x -10 The carrier was placed in a 5 ml centrifuge tube. At room temperature (approximately 25°C), 32.4 μL of an aqueous solution of H₂PtCl₆·6H₂O (Pt: 18.5 mg / mL) was pipetted into the 5 ml centrifuge tube. Then, 367.6 μL of ultrapure water was added and mixed thoroughly. The mixed impregnation solution was added dropwise to the carrier in batches using a pipette, and the mixture was stirred thoroughly until it reached a viscous paste. After standing overnight at room temperature, the mixture was placed in a 60°C oven and dried for 12 hours. The dried solid powder was then compressed, crushed, and sieved to select particles of 20-40 mesh.

[0045] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlSiO2 is obtained. x -10 particulate catalyst. (The preceding number 0.3 represents the mass loading of Pt in the catalyst relative to the support of 0.3%, the same below).

[0046] Example 2. 0.3Pt / ZnAlSiO x Preparation of -15 particulate catalyst: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonhydrate into a 250 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide, 13.25 g of anhydrous sodium carbonate, and 7.8 g of sodium silicate nonhydrate into a 500 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind, and calcine at 550°C for 2 hours to obtain ZnAlSiO2. x -15 carrier.

[0047] X-ray fluorescence spectrometry was used to analyze ZnAlSiO x The elemental composition of the carrier was measured by scanning at -15°C. The measurement results are shown in Table 1. The mass content of Al is 26.0%, the mass content of Zn is 13.0%, the mass content of Si is 16.2%, and the mass content of O is 44.8%.

[0048] X-ray diffraction was used to analyze ZnAlSiO x -15° carrier powder was continuously scanned to determine its crystal phase composition; the scanning range 2θ was 10-90°. (See attached image.) Figure 2 As shown, only the characteristic diffraction peaks of Al2O3 are present, while those of ZnO and SiO2 are absent. This indicates that Zn and Si oxides may either be doped into the alumina lattice without forming an independent phase, or they may form an amorphous structure. Furthermore, the diffraction peaks of the support are shifted to lower angles relative to the alumina, indicating lattice expansion, which suggests that Zn has been doped into the alumina.

[0049] The ZnAlSiOx-15 support powder was collected using a solid-state nuclear magnetic resonance spectrometer. 29 Si nuclear magnetic resonance spectrum ( 29 Si MASNMR was used to analyze the coordination environment and chemical state of silicon atoms in its framework structure. (See attached image.) Figure 6 As shown, no phase similar to SiO2 (which typically appears at -110 ppm, corresponding to Q) was observed. 4 The resonance signal corresponding to the species was detected. Instead, a characteristic signal centered at approximately -85 ppm was detected, which belongs to the Q series. 1 and Q 2 Silicon species (corresponding to Si atoms connecting one or two silicon-oxygen bridges respectively). This phenomenon indicates that SiO2 does not form an independent phase, but is uniformly doped into the amorphous network.

[0050] ZnAlSiO was analyzed using a multi-station fully automated specific surface area and porosity analyzer. x -15 carrier (20-40 mesh) was used for pore structure analysis, as shown in the attached figure. Figure 3 As shown, the pore size distribution curve indicates that the carrier exhibits typical mesoporous characteristics, with the pore size mainly distributed in the range of 2-65 nm, and a sharp peak at 3-4 nm.

[0051] ZnAlSiO was analyzed using a fully automated temperature-programmed chemisorption analyzer. x The -15 support (20-40 mesh) was characterized by ammonia temperature-programmed desorption. 100 mg of catalyst was weighed and placed in a U-shaped quartz tube. After reduction at 600 °C for 1 h in a 10% H₂ / Ar atmosphere, the temperature was lowered to 100 °C, and the atmosphere was switched to Ar for purging. The TCD signal was recorded online, and NH₃ was manually pulsed until the peak area remained constant. Subsequently, the temperature was increased from room temperature to 800 °C at a rate of 10 °C / min, and the mass spectrometry signal was recorded simultaneously. The number of acidic sites on the support was detected, as shown in Figure 9. The 100 °C-400 °C range represents the distribution sites of moderately weak acids, ZnAlSiO₂. x The -15 carrier has weakly acidic sites compared to ZnAlSiO x -10 carriers have decreased.

[0052] Take 200mg ZnAlSiO x-15. Place the carrier in a 5ml centrifuge tube. At room temperature (approximately 25°C), pipette 32.4μL (Pt: 18.5mg / mL) of H2PtCl6·6H2O aqueous solution into the 5ml centrifuge tube. Add 467.6μL of ultrapure water and mix thoroughly. Using a pipette, add the mixed impregnation solution dropwise to the carrier in batches, stirring thoroughly until a viscous paste is formed. After standing overnight at room temperature, place the mixture in a 60°C oven to dry for 12 hours. Compress, crush, and sieve the dried solid powder, selecting particles of 20-40 mesh.

[0053] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlSiO2 is obtained. x -15 particulate catalyst.

[0054] Example 3. 0.3Pt / ZnAlSiO x Preparation of -20 particulate catalyst: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonhydrate into a 250 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide, 13.25 g of anhydrous sodium carbonate, and 11.7 g of sodium silicate nonhydrate into a 500 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind it, and calcine it at 550°C for 2 hours to obtain ZnAlSiO2. x -20 carrier.

[0055] X-ray fluorescence spectrometry was used to analyze ZnAlSiO x The -20 carrier was scanned to measure its elemental composition. The measurement results are shown in Table 1. The mass content of Al is 21.8%, the mass content of Zn is 11.4%, the mass content of Si is 20.9%, and the mass content of O is 45.9%.

[0056] X-ray diffraction was used to analyze ZnAlSiO x-20° carrier powder was continuously scanned to determine its crystal phase composition; the scanning range 2θ was 10-90°. (See attached image.) Figure 2 As shown, only the characteristic diffraction peaks of Al2O3 are present, while those of ZnO and SiO2 are absent. This indicates that Zn and Si oxides may either be doped into the alumina lattice without forming an independent phase, or they may form an amorphous structure. Furthermore, the diffraction peaks of the support are shifted to lower angles relative to the alumina, indicating lattice expansion, which suggests that Zn has been doped into the alumina.

[0057] The ZnAlSiOx-20 support powder was collected using a solid-state nuclear magnetic resonance spectrometer. 29 Si nuclear magnetic resonance spectrum ( 29 Si MASNMR was used to analyze the coordination environment and chemical state of silicon atoms in its framework structure. (See attached image.) Figure 6 As shown, no phase similar to SiO2 (which typically appears at -110 ppm, corresponding to Q) was observed. 4 The resonance signal corresponding to the species was detected. Instead, a characteristic signal centered at approximately -85 ppm was detected, which belongs to the Q series. 1 and Q 2 Silicon species (corresponding to Si atoms connecting one or two silicon-oxygen bridges respectively). This phenomenon indicates that SiO2 is not independently phased but uniformly doped into the amorphous network, and that silicon oxide and aluminum oxide are not physically mixed.

[0058] ZnAlSiO was analyzed using a multi-station fully automated specific surface area and porosity analyzer. x -20 carrier (20-40 mesh) was used for pore structure analysis, as shown in the attached figure. Figure 3 As shown, the pore size distribution curve indicates that the carrier exhibits typical mesoporous characteristics, with the pore size mainly distributed in the range of 2-60 nm, and a sharp peak at 3-4 nm.

[0059] ZnAlSiO was analyzed using a fully automated temperature-programmed chemisorption analyzer. x The -20 support (20-40 mesh) was characterized by ammonia temperature-programmed desorption. 100 mg of catalyst was weighed and placed in a U-shaped quartz tube. After reduction at 600 °C for 1 h in a 10% H₂ / Ar atmosphere, the temperature was lowered to 100 °C, and the Ar atmosphere was switched for purging. The TCD signal was recorded online, and NH₃ was manually pulsed until the peak area remained constant. Subsequently, the temperature was increased from room temperature to 800 °C at a rate of 10 °C / min, and the mass spectrometry signal was recorded simultaneously to detect the number of acidic sites on the support. See Figure 9. The 100 °C-400 °C range represents the distribution sites of moderately weak acids, ZnAlSiO₂. x The -20 carrier has weakly acidic sites compared to ZnAlSiO. x -15 carriers have decreased.

[0060] Take 200mg ZnAlSiO x -20 The carrier was placed in a 5 ml centrifuge tube. At room temperature (approximately 25°C), 32.4 μL of an aqueous solution of H₂PtCl₆·6H₂O (Pt: 18.5 mg / mL) was pipetted into the 5 ml centrifuge tube. Then, 527.6 μL of ultrapure water was added and mixed thoroughly. The mixed solution was then added dropwise to the carrier in batches using a pipette, stirring thoroughly until a thick paste was formed. After standing overnight at room temperature, the mixture was placed in a 60°C oven and dried for 12 hours. The dried solid powder was then compressed, crushed, and sieved to select particles of 20-40 mesh.

[0061] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlSiO2 is obtained. x -20 particulate catalyst.

[0062] Example 4. 0.3Pt / ZnAlSiO x -2 Preparation of particulate catalyst: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonahydrate into a 250 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide, 13.25 g of anhydrous sodium carbonate, and 0.78 g of sodium silicate nonahydrate into a 500 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind it, and calcine it at 550°C for 2 hours to obtain ZnAlSiO2. x -2 carrier.

[0063] X-ray fluorescence spectrometry was used to analyze ZnAlSiO x The carrier was scanned to measure its elemental composition. Measurement results: Al mass content was 38.6%, Zn mass content was 17.8%, Si mass content was 2.3%, and O mass content was 41.3%.

[0064] Take 200 mg ZnAlSiOx -2. Place the carrier in a 5 ml centrifuge tube. At room temperature (approximately 25°C), pipette 32.4 μL of an aqueous solution of H₂PtCl₆·6H₂O (Pt: 18.5 mg / mL) into the 5 ml centrifuge tube. Add 407.6 μL of ultrapure water and mix thoroughly. Using a pipette, add the mixed impregnation solution dropwise to the carrier in batches, stirring thoroughly until a thick paste is formed. After standing overnight at room temperature, place the mixture in a 60°C oven to dry for 12 hours. Compress the dried solid powder into tablets, crush, and sieve, selecting particles of 20-40 mesh.

[0065] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlSiO2 is obtained. x -2 Particle catalyst.

[0066] Example 5. 0.3Pt / ZnAlSiO x -3 Preparation of particulate catalyst: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonahydrate into a 250 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide, 13.25 g of anhydrous sodium carbonate, and 1.17 g of sodium silicate nonahydrate into a 500 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind, and calcine at 550°C for 2 hours to obtain ZnAlSiO2. x -3 carrier.

[0067] X-ray fluorescence spectrometry was used to analyze ZnAlSiO x The elemental composition of the carrier was measured by scanning with a -3 carrier. The results showed that the mass content of Al was 39.7%, Zn was 15.1%, Si was 2.8%, and O was 42.4%.

[0068] Take 200 mg ZnAlSiO x-3. Place the carrier in a 5 ml centrifuge tube. At room temperature (approximately 25°C), pipette 32.4 μL of an aqueous solution of H₂PtCl₆·6H₂O (Pt: 18.5 mg / mL) into the 5 ml centrifuge tube. Add 407.6 μL of ultrapure water and mix thoroughly. Using a pipette, add the mixed impregnation solution dropwise to the carrier in batches, stirring thoroughly until a thick paste is formed. After standing overnight at room temperature, place the mixture in a 60°C oven and dry for 12 hours. Compress the dried solid powder into tablets, crush, and sieve, selecting particles of 20-40 mesh.

[0069] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlSiO2 is obtained. x -3 Particle catalyst.

[0070] Example 6. 0.3Pt / ZnAlSiO2 prepared in Example 1 x -10 Particle Catalyst Activity Evaluation: A catalyst was loaded into a quartz reaction tube with an inner diameter of 7.6 mm in a fixed bed. The feed gas composition was 14% C3H8, 14% H2, and 72% He, and the feed gas space velocity was 40 h⁻¹. -1 The reaction temperature was 600℃, the reaction pressure was atmospheric pressure, and the reaction time was 30 hours.

[0071] The propane dehydrogenation performance evaluation is attached. Figure 1 As shown, 0.3Pt / ZnAlSiO x The activity of the -10 particulate catalyst decreased from 54.5% to 50.2% in the initial 2 h, and then slowly increased to about 63% and remained stable in the following 28 h; the selectivity remained at about 99% for 30 h.

[0072] Take 0.3Pt / ZnAlSiO after the reaction x -10 mg of catalyst was used to perform thermogravimetric analysis on the carbon deposits after the catalyst reaction using an SDT Q600 thermogravimetric analyzer. The temperature was increased from room temperature to 800 degrees Celsius at a rate of 10 °C / min in air atmosphere, and the mass change was recorded.

[0073] Example 7. 0.3Pt / ZnAlSiO2 prepared in Example 2 x -15 Particle Catalyst Activity Evaluation: The catalytic reaction process and conditions were the same as in Example 6.

[0074] The propane dehydrogenation performance evaluation is attached. Figure 1 As shown, 0.3Pt / ZnAlSiO x The conversion rate of the -15 particulate catalyst decreased from 57.6% to 55.6% in the initial 1 h, and then the activity slowly increased to around 74% and remained stable in the following 29 h; the selectivity remained at around 99% for 30 h.

[0075] Take 0.3Pt / ZnAlSiO after the reaction x -15 catalyst 10 mg, the thermogravimetric analysis of carbon deposits after catalyst reaction was performed using an SDT Q600 thermogravimetric analyzer. The temperature was increased from room temperature to 800 degrees at a rate of 10℃ / min in air atmosphere, and the mass change was recorded.

[0076] Example 8. 0.3Pt / ZnAlSiO2 prepared in Example 3 x -20 Particle Catalyst Activity Evaluation: The catalytic reaction process and conditions were the same as in Example 6.

[0077] The propane dehydrogenation performance evaluation is attached. Figure 1 As shown, 0.3Pt / ZnAlSiO x The conversion rate of the -20 particulate catalyst increased from 30.7% to around 70% in the initial 15 h and remained stable in the following 15 h; the selectivity remained at around 99% for 30 h.

[0078] Take 0.3Pt / ZnAlSiO after the reaction x -20 catalyst 10 mg, the thermogravimetric analysis of carbon deposits after catalyst reaction was performed using an SDT Q600 thermogravimetric analyzer. The temperature was increased from room temperature to 800 degrees at a rate of 10℃ / min in air atmosphere, and the mass change was recorded.

[0079] Example 9. 0.3Pt / ZnAlSiO2 prepared in Example 2 x Long-term stability test of -15 particulate catalyst: The catalytic reaction process and conditions were the same as in Example 6. The difference was that the reaction time was 50 hours.

[0080] 0.3Pt / ZnAlSiO x The long-term stability test of the -15 particle catalyst showed that the activity remained basically the same as that of Example 7 in the first 30 h, and slowly decreased to about 70% within 30-50 h; the selectivity remained at about 99% within 50 h.

[0081] Example 10. 0.3Pt / ZnAlSiO2 prepared in Example 3 x Stability testing of -20 particulate catalyst: The catalytic reaction process and conditions were the same as in Example 6. The difference was that the reaction time was 36 hours.

[0082] 0.3Pt / ZnAlSiO x The long-term stability test of the -20 particle catalyst showed that the activity remained basically the same as that of Example 8 in the first 30 h, and slowly decreased to about 70% within 30-36 h; the selectivity remained at about 99% within 36 h.

[0083] Example 11. 0.3Pt / ZnAlSiO2 prepared in Example 2 x Activity evaluation of -15 particulate catalyst under different pretreatment conditions: The catalyst preparation process and conditions are the same as in Example 2, except that the pretreatment conditions are different from those in Example 2: the atmosphere is 100% H2 by volume, and the treatment lasts for 1 h.

[0084] The catalytic reaction process and conditions were the same as in Example 6. The difference was that the reaction time was 36 hours.

[0085] 0.3Pt / ZnAlSiO x The activity evaluation of the -15 particulate catalyst showed that the conversion rate dropped from 69.3% to 64.1% in the initial 3 h, the activity slowly increased to around 74% in 3-17 h, and remained stable at around 74% in the following 19 h; the selectivity remained at around 99% for 36 h.

[0086] Example 12. 0.3Pt / ZnAlSiO2 prepared in Example 2 x Activity evaluation of -15 particulate catalyst under different pretreatment conditions: The catalyst preparation process and conditions are the same as in Example 2, except that the pretreatment conditions are different from those in Example 2: the atmosphere is 100% H2 by volume, and the treatment lasts for 3 hours.

[0087] The process and conditions of the catalytic reaction were the same as in Example 6, except that the reaction time was 38 hours.

[0088] 0.3Pt / ZnAlSiO xThe activity evaluation of the -15 particulate catalyst showed that the conversion rate dropped from 74.7% to 64% in the initial 3 h, the activity slowly increased to around 70% in 3-15 h, and remained stable at around 70% in 15-38 h; the selectivity remained at around 99% within 38 h.

[0089] Example 13. 0.3Pt / ZnAlSiO2 prepared in Example 2 x -15 Particulate catalyst activity evaluation without pretreatment before use: The process and conditions of the catalytic reaction were the same as in Example 6, except that the reaction time was 70 hours.

[0090] 0.3Pt / ZnAlSiO x The activity evaluation of the -15 particulate catalyst showed that the conversion rate dropped from 41.5% to 31.6% in the initial 1 h, the activity slowly increased to around 67.9% from 1 to 36 h, the activity stabilized at around 68% from 36 to 66 h, and the activity slowly decreased from 68% to around 67% in the last 4 h.

[0091] Example 14. 0.3Pt / ZnAlSiO2 prepared in Example 2 x Activity evaluation of -15 particulate catalysts under different granulation pressures: Granulation conditions: Granulation at 15 MPa (all other embodiments and comparative examples of the present invention were granulated at 10 MPa).

[0092] The pretreatment conditions were the same as in Example 2.

[0093] The catalytic reaction conditions were the same as in Example 6, except that the reaction time was 24 hours.

[0094] 0.3Pt / ZnAlSiO x The activity evaluation of the -15 particulate catalyst showed that the conversion rate dropped from 59.3% to 55.3% in the initial 1 h, and then slowly increased to around 71% and remained stable in the following 23 h; the selectivity remained at around 99% for 30 h.

[0095] Example 15. 0.3Pt / ZnAlSiO2 prepared in Example 2 x -15 Particle Catalyst Regeneration Stability Test: The pretreatment conditions were the same as in Example 2.

[0096] Catalytic reaction conditions: After pretreatment, the feed gas composition (volume ratio) was 14% C3H8, 14% H2, and 72% He, and the feed gas space velocity was 40 h⁻¹. -1The reaction temperature was 600℃, and the reaction pressure was atmospheric pressure.

[0097] Regeneration conditions and procedures after each reaction stage: After the reaction, the feed gas was switched to 100% helium by volume for purging at a flow rate of 30 ml / min, and the mixture was allowed to cool naturally from 600℃ to room temperature. Then, helium was switched to O2 / He with 20% oxygen by volume, and the temperature was increased to 500℃ at 10℃ / min and held for 1 h. Finally, He was switched back to 600℃ and treated with H2 / He at 20% by volume for 1 h.

[0098] The test results are attached. Figure 2 As shown. In the first reaction stage, the activity decreased from 64% to 60% in the initial 3 hours, then slowly increased to 73% over the next 20 hours, stabilized around 73% for 15 hours, and then slowly decreased from 72% to 69% in the final 8 hours. Selectivity remained above 96% during the first reaction stage. After the regeneration process, the initial activity reached 82%, then rapidly decreased in the first 15 hours, eventually stabilizing at 61%. In the second reaction stage, selectivity remained above 94%. In the third reaction stage, the initial activity was 80%, then rapidly decreased in the first 15 hours, eventually stabilizing at 58%. Selectivity remained above 94%. In the fourth reaction stage, the initial activity was 78.5%, then rapidly decreased in the first 15 hours, eventually stabilizing at 55.6%. Selectivity remained above 92%. In the fifth reaction stage, the initial activity was 74%, then rapidly decreased in the first 15 hours, eventually stabilizing at 52%. Selectivity remained above 92%. In the sixth reaction stage, the initial activity was 66%, then decreased rapidly over the first 15 hours, eventually stabilizing at 50.6%. The selectivity remained above 92% during the sixth reaction stage. In the seventh reaction stage, the initial activity was 64.5%, then decreased rapidly over the first 15 hours, eventually stabilizing at 47%. The selectivity remained above 91% during the seventh reaction stage.

[0099] Example 16. 0.3Pt / ZnAlSiO2 prepared in Example 4 x -2 Particulate catalyst activity evaluation: The catalytic reaction process and conditions were the same as in Example 6, except that the reaction time was 18 h.

[0100] 0.3Pt / ZnAlSiO x -2 Propane dehydrogenation performance of particulate catalyst: The conversion rate decreased from 50% to around 35% in the initial 3 h, and remained stable in the following 15 h; the selectivity slowly increased from 87% to 94% in the first 9 h, and then remained at around 94%.

[0101] Example 17. 0.3Pt / ZnAlSiO2 prepared in Example 5 x -3 Activity evaluation of particulate catalysts: The catalytic reaction process and conditions were the same as in Example 6, except that the reaction time was 18 h.

[0102] 0.3Pt / ZnAlSiO x -3 Propane dehydrogenation performance of particulate catalyst: The conversion rate decreased from 52% to around 39% in the initial 3 h, and remained stable in the following 15 h; the selectivity remained around 96% within 18 h.

[0103] Comparative Example 1. 0.3Pt / ZnAlO x Preparation of particulate catalysts: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonahydrate into a 250 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide and 13.25 g of anhydrous sodium carbonate into a 500 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind it, and calcine it at 550°C for 2 hours to obtain ZnAlO. x Carrier.

[0104] X-ray fluorescence spectrometry was used to analyze ZnAlO x The carrier was scanned to measure its elemental composition. The measurement results are shown in Table 1. The mass content of Al was 40.8%, the mass content of Zn was 18.4%, and the mass content of O was 40.8%.

[0105] X-ray diffraction was used to analyze ZnAlO x The carrier powder was continuously scanned to determine its crystal phase composition, with a scanning range of 2θ of 10-90°; see attached. Figure 2 As shown, only the characteristic diffraction peaks of Al2O3 are present, while those of ZnO are absent. Furthermore, the diffraction peaks of the support are shifted to lower angles compared to the alumina, indicating lattice expansion. This suggests that Zn has been doped into the alumina lattice.

[0106] ZnAlO was analyzed using a multi-station fully automated specific surface area and porosity analyzer. x The pore structure of the carrier (20-40 mesh) was analyzed, as shown in the attached figure. Figure 3As shown, the pore size distribution curve indicates that the carrier exhibits typical mesoporous characteristics, with the pore size mainly distributed in the range of 2-60 nm, and showing a sharp peak at 3-4 nm and 5-7 nm.

[0107] ZnAlO was analyzed using a fully automated temperature-programmed chemisorption analyzer. x The support (20-40 mesh) was characterized by ammonia-programmed temperature-rise desorption. 100 mg of catalyst was weighed and placed in a U-shaped quartz tube. After reduction at 600 °C for 1 h in an atmosphere of 10% H₂ / Ar (volume concentration), the temperature was lowered to 100 °C, and the atmosphere was switched to Ar for purging. The TCD signal was recorded online, and NH₃ was manually pulsed until the peak area remained constant. Subsequently, the temperature was increased from room temperature to 800 °C at a rate of 10 °C / min, and the mass spectrometry signal was recorded simultaneously to detect the number of acidic sites on the support. (See Figure 9). The 100 °C-400 °C range represents the distribution sites of moderately to weakly acidic ZnAlO₂. x The vector has the most relatively weakly acidic sites.

[0108] Take 200mg ZnAlO x The carrier was placed in a 5 ml centrifuge tube. At room temperature (approximately 25°C), 32.4 μL of an aqueous solution of H₂PtCl₆·6H₂O (Pt: 18.5 mg / mL) was pipetted into the 5 ml centrifuge tube. Then, 407.6 μL of ultrapure water was added and mixed thoroughly. The mixture was then added dropwise to the carrier in batches using a pipette, stirring thoroughly until a thick paste was formed. After standing overnight at room temperature, the mixture was dried in a 60°C oven for 12 hours. The dried solid powder was then compressed, crushed, and sieved to select particles of 20-40 mesh.

[0109] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlO is obtained. x Particulate catalyst.

[0110] Comparative Example 2. 0.3Pt / ZnAlO x Preparation of powdered catalysts: Weigh 200 mg of ZnAlO prepared in Comparative Example 1 xThe carrier was placed in a 5 ml centrifuge tube. At room temperature (approximately 25°C), 32.4 μL of (Pt: 18.5 mg / mL) H2PtCl6·6H2O aqueous solution was pipetted into the 5 ml centrifuge tube. Then, 407.6 μL of ultrapure water was added and mixed thoroughly. The mixed impregnation solution was added dropwise to the carrier in batches using a pipette. The mixture was stirred thoroughly until it became a viscous paste. After standing overnight at room temperature, the mixture was placed in a 60°C oven and dried for 12 hours.

[0111] Pretreatment before use: Weigh 100 mg of the powder into a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm, and place it in a mixed atmosphere of H2 and He with a hydrogen volume percentage of 20% at 600 °C, with a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlO is obtained. x Powdered catalyst.

[0112] Comparative Example 3. 0.3PtZn / AlSiO x Preparation of particulate catalysts: Weigh 46.9 g of aluminum nitrate nonahydrate into a 250 ml beaker, add 200 ml of water and stir until the solid is completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide, 13.25 g of anhydrous sodium carbonate, and 7.8 g of sodium silicate nonahydrate into a 500 ml beaker, add 216 ml of water and stir until the solid is completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 60°C oven overnight, grind, and calcine at 550°C for 2 hours to obtain AlSiO2. x Carrier.

[0113] Take 200 mg AlSiO x The carrier was placed in a 5 ml centrifuge tube. At room temperature (approximately 25°C), 32.4 μL (Pt: 18.5 mg / mL) of H₂PtCl₆·6H₂O aqueous solution and 467.5 μL (Zn: 55.43 mg / mL) of zinc nitrate hexahydrate solution were pipetted into the 5 ml centrifuge tube and mixed thoroughly. The mixed solution was then added dropwise to the carrier in batches using a pipette, and stirred thoroughly until a thick paste was formed. After standing overnight at room temperature, the mixture was placed in a 60°C oven and dried for 12 hours. The dried solid powder was then compressed, crushed, and sieved to select particles of 20-40 mesh.

[0114] Pretreatment before use: Weigh 100 mg (20-40 mesh) of the particles and mix them evenly with 1000 mg of inert quartz sand (20-40 mesh). Place the mixture in a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm and conduct the reaction at 600 °C under a mixed atmosphere of H2 and He (20% hydrogen by volume) at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlO is obtained. x Particulate catalyst.

[0115] Comparative Example 4. 0.3Pt / ZnAlO x Preparation of powdered catalyst at -0.06K: Weigh 200 mg of ZnAlO prepared in Comparative Example 1 x The carrier was placed in a 5 ml centrifuge tube. At room temperature (approximately 25°C), 32.4 μL of (Pt: 18.5 mg / mL) H2PtCl6·6H2O aqueous solution and 30 μL of (K: 66.7 mg / mL) KCl aqueous solution were pipetted into the 5 ml centrifuge tube. Then, 377.6 μL of ultrapure water was added and mixed thoroughly. The mixed impregnation solution was added dropwise to the carrier in batches using a pipette. The mixture was stirred thoroughly until it became a viscous paste. After standing overnight at room temperature, the carrier was dried in a 60°C oven for 12 hours.

[0116] Pretreatment before use: Weigh 100 mg of the powder into a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm, and react it at 600 °C in a mixed atmosphere of H2 and He with a hydrogen volume percentage of 20% at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.3Pt / ZnAlO is obtained. x -0.06K powdered catalyst.

[0117] Comparative Example 5. (Not the present invention) 0.85Pt / ZnAlO x Preparation of -1 / 5 powdered catalyst: Weigh 7.44 g of zinc nitrate hexahydrate and 46.9 g of aluminum nitrate nonahydrate into a 1000 ml beaker, add 200 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution A. Weigh 15 g of sodium hydroxide and 13.25 g of anhydrous sodium carbonate into a 1000 ml beaker, add 216 ml of water and stir until the solids are completely dissolved. Name the resulting solution Solution B. Place Solution B in a 70°C water bath and pump Solution A into Solution B using a constant flow pump at a rate of 3 ml / min, stirring continuously. Once Solution A has been completely pumped into Solution B, stop stirring and continue aging in the 70°C water bath for 24 hours. Filter the resulting white turbid liquid while hot and wash with ultrapure water until the filtrate is neutral. Dry the resulting white solid in a 120°C oven overnight, grind it, and calcine it at 550°C for 2 hours to obtain ZnAlO. x -1 / 5 carrier. Take 1g ZnAlO x -1 / 5 of the carrier was placed in a 25ml beaker. At room temperature (approximately 25°C), 287μL of (Pt: 29.6mg / mL) H2PtCl6·6H2O aqueous solution was pipetted into a 2ml centrifuge tube. Then, 800μL of ultrapure water was added and mixed thoroughly. The mixed impregnation solution was added dropwise to the carrier in batches using a pipette. The mixture was stirred thoroughly with a glass rod until it became a thick paste. After standing overnight at room temperature, the mixture was placed in a 60°C oven and dried for 12 hours.

[0118] Pretreatment before use: Weigh 100 mg of the powder into a fixed-bed quartz reaction tube with an inner diameter of 7.6 mm, and react it at 600 °C in a mixed atmosphere of H2 and He with a hydrogen volume percentage of 20% at a space velocity of 18,000 mL·h⁻¹. -1 ·g -1 After reduction for 1 hour, 0.85Pt / ZnAlO is obtained. x -1 / 5 powdered catalyst.

[0119] Comparative Example 6. Comparative Example 1 prepared 0.3Pt / ZnAlO x Particulate catalyst activity evaluation: The catalytic reaction process and conditions were the same as in Example 6.

[0120] The propane dehydrogenation performance evaluation is attached. Figure 1 As shown, 0.3Pt / ZnAlO x The conversion rate of the particulate catalyst decreased from 51.6% to 36.5% in the initial 1 h, and the activity slowly decreased to 16% in the following 29 h; the selectivity gradually increased as the reaction proceeded, slowly rising from 88% to around 94%-95%.

[0121] Take 0.3Pt / ZnAlO after the reaction x10 mg of catalyst was subjected to thermogravimetric analysis of carbon deposits after the catalyst reaction using an SDT Q600 thermogravimetric analyzer. The temperature was increased from room temperature to 800 degrees Celsius at a rate of 10 °C / min in air atmosphere, and the mass change was recorded.

[0122] Comparative Example 7. Comparative Example 2 prepared 0.3Pt / ZnAlO x Powder catalyst activity evaluation: The catalytic reaction process and conditions were the same as in Example 6. The difference was that the reaction time was 18 hours.

[0123] 0.3Pt / ZnAlO x The powder catalyst activity evaluation showed that the conversion rate dropped from 55.3% to around 30% in the initial 2 h, and the activity slowly decreased from 30% to 21% in the following 16 h; the selectivity slowly increased from the initial 89% to around 94%.

[0124] Comparative Example 8. Comparative Example 4 prepared 0.3Pt / ZnAlO x -0.06K powder catalyst activity evaluation: The catalytic reaction process and conditions were the same as in Example 6. The difference was that the reaction time was 70 h.

[0125] 0.3Pt / ZnAlO x The powder catalyst activity evaluation showed that the conversion rate remained around 37% and the selectivity remained around 96% within 70 h.

[0126] Comparative Example 9. (Not the present invention) Comparative Example 5 prepared 0.85Pt / ZnAlO x -1 / 5 powder catalyst activity evaluation: The catalytic reaction process and conditions were the same as in Example 6. The difference was that the reaction time was 16 hours.

[0127] 0.85Pt / ZnAlO x The activity evaluation of the -1 / 5 powder catalyst showed that the conversion gradually increased from 30.5% to 35.3% within 16 h of reaction and remained stable, while the selectivity remained around 99%.

[0128] Comparative Example 10. Comparative Example 3 prepared 0.3PtZn / AlSiO x Regeneration stability test of particulate catalyst: The pretreatment conditions were the same as those in Comparative Example 3.

[0129] Catalytic reaction conditions: After pretreatment, the feed gas composition (volume ratio) was 14% C3H8, 14% H2, and 72% He, and the feed gas space velocity was 40 h⁻¹. -1 The reaction temperature was 600℃, and the reaction pressure was atmospheric pressure.

[0130] Catalyst regeneration conditions and process after each reaction stage: After the reaction, the feed gas was switched to 100% helium (by volume) for purging at a flow rate of 30 ml / min, and the mixture was allowed to cool naturally from 600 °C to room temperature. Then, helium was switched to O2 / He (20% oxygen by volume), and the temperature was increased to 500 °C at a rate of 10 °C / min and held for 1 h. Finally, He was switched back to 600 °C and treated with H2 / He (20% H2 by volume) for 1 h.

[0131] The test results are attached. Figure 2 As shown. In the first reaction stage, the activity increased from 33% to 60.8% in the initial 12 hours, then slowly increased to 69% in the next 13 hours, stabilized around 69% for 10 hours, and then slowly decreased from 69% to 64% in the final 20 hours. Selectivity remained above 98% during the first reaction stage. After the regeneration process, the initial activity was 65%, then rapidly decreased in the first 8 hours, eventually stabilizing at 52%. In the second reaction stage, selectivity remained above 97%. In the third reaction stage, the initial activity was 64%, then rapidly decreased in the first 8 hours, eventually stabilizing at 48%. Selectivity remained above 97% during the third reaction stage. In the fourth reaction stage, the initial activity was 58%, then rapidly decreased in the first 8 hours, eventually stabilizing at 44%. Selectivity remained above 96% during the fourth reaction stage. In the fifth reaction stage, the initial activity was 48%, then rapidly decreased in the first 8 hours, eventually stabilizing at 35%. Selectivity remained above 94% during the fifth reaction stage.

[0132] The conversion rates, selectivity, and reaction conditions for the examples and comparative examples are shown in the table below (the catalytic performance at the starting and ending points is statistically analyzed; for specific variations, please refer to the descriptions of the examples and comparative examples above).

[0133] Table 1 shows the XRF test results of the elemental content in the carriers of Examples 1, 2, 3 and Comparative Example 1.

[0134] Table 2 shows the physical adsorption test results of the carriers in Examples 1, 2, 3 and Comparative Example 1. Table 3 shows the thermogravimetric analysis results of Examples 6, 7, 8 and Comparative Example 6 after 30 h of reaction. Comparing the performance of catalysts with different silicon contents, Example 7 (0.3Pt / ZnAlSiO) shows that... x -15) exhibited the best overall performance, with propane conversion significantly increasing from 57.61% to 74.17% within 30 h, while propylene selectivity remained above 98.73%, indicating that the catalyst gradually activated and stabilized during the reaction, forming a highly efficient single-atom alloy structure. Example 6 (0.3Pt / ZnAlSiO) x The conversion rate of -10) increased from 54.51% to 62.97%, but the increase was limited, and the final activity was below 0.3Pt / ZnAlSiO x -15 indicates that while 10% silicon doping improves performance, the structural control is not yet optimal. Example 8 (0.3Pt / ZnAlSiO) x -20) The initial activity was low (30.78%), but it increased significantly to 73.26% as the reaction proceeded, indicating that the high silicon content delayed the formation of active sites, but still achieved a high activity level. It is noteworthy that the propylene selectivity of the silicon-doped systems (Examples 6-8) remained consistently above 98.6%, significantly better than the undoped comparative example 6 (0.3Pt / ZnAlO). x The latter's activity dropped sharply from 51.6% to 16.06%, and its selectivity was only 88.36%-94.32%. This clearly shows that the introduction of silicon not only significantly improved the catalyst stability but also significantly suppressed side reactions and improved propylene selectivity. This may be attributed to silicon's regulation of the interaction between the acidic support surface and the metal support, optimization of the pore structure, and inhibition of carbon deposition.

[0135] In the stability test, Example 9 (0.3Pt / ZnAlSiO) x -15) exhibited excellent steady-state performance during a 50-h reaction: its propane conversion, after a slight fluctuation from 57.53%, stabilized at approximately 70%, showing only a slight decreasing trend, while the propylene selectivity remained consistently high at 98.67%–98.2%, indicating that the catalyst not only possesses high activity and high selectivity but also good structural stability and resistance to deactivation. In contrast, Example 10 (0.3Pt / ZnAlSiO) x -20) During the 36 h reaction process, the activity significantly increased from the initial 36.51% to 71.94%. Although its final activity was similar to that of 0.3Pt / ZnAlSiO x -15 is close, and the selectivity also remains high (98.39%–98.74%), but 0.3Pt / ZnAlSiO xThe -15 catalyst reaches a high activity plateau without prolonged activation during the reaction and exhibits more stable performance over long-term operation. This indicates that while the introduction of silicon improves overall catalytic performance, there is an optimal doping level: 20% silicon content achieves the best balance between active site formation rate, structural stability, and long-term resistance to deactivation, making it the component with the best overall performance in this system.

[0136] Regarding the impact of pretreatment conditions on long-term stability, Example 13 (no pretreatment, 70 h) exhibited a slow activation process, gradually increasing from 41.48% to 66.84%, and maintained high activity for 70 hours, indicating that even without H2 pretreatment, the catalyst can still form an active structure during the reaction, but the activation period is significantly prolonged. In contrast, Examples 11 (100% H2, 1 h) and 12 (100% H2, 3 h) both showed high initial activity (approximately 69-74%) with minimal fluctuations within 36 h, suggesting that strong reduction pretreatment facilitates the rapid formation of highly active PtZn alloys. Although the activity of Example 11 gradually increased from 41.48% to 66.84%, the activation period was as long as approximately 30 h, resulting in lower industrial efficiency.

[0137] Furthermore, Example 14 (15 MPa high-pressure granulation conditions) and conventional 10 MPa granulation of 0.3Pt / ZnAlSiO x The -15 catalyst exhibits comparable activity and selectivity, indicating that the catalyst system has a wide process operating window in terms of molding pressure parameters, which is beneficial for process control and scale-up in actual production.

[0138] The deactivation trend of Comparative Example 7 (0.3Pt / ZnAlOx powder catalyst) was similar to that of Comparative Example 6, but its initial activity was slightly higher, possibly due to limited mass transfer after granulation. Comparative Example 8 (0.3Pt / ZnAlOx powder catalyst) x The -0.06K powder catalyst, by introducing the alkali metal K to attempt to modulate the surface acidity, maintained a conversion rate of around 37% and a selectivity of 96% within 70 h. Although this was an improvement over the undoped system, the activity level was still far lower than that of the silicon-doped system, indicating that the modification effect of K is limited and cannot replace the deep optimization of pore structure and metal-support interaction by Si. Comparative Example 9 (0.85Pt / ZnAlO x The -1 / 5 powder catalyst exhibited catalytic behavior at a higher Pt loading (0.85%), but its conversion rate only increased slightly from 30.5% to 35.3% within 16 hours, with activity far lower than that of the silicon-doped catalyst with low loading (0.3%). This fully demonstrates that the high metal utilization and structural stability achieved by the present invention through Si doping can obtain better catalytic performance while significantly reducing the amount of precious metals used.

[0139] Figure 1 The activity test results of Examples 6, 7, 8 and Comparative Example 6 are shown after 30 hours of reaction. The figures clearly reflect the effect of different silicon doping amounts on catalyst performance.

[0140] Figure 2 It demonstrated 0.3Pt / ZnAlSiO x -15 and 0.3PtZn / AlSiO x Regeneration stability test. (Compared with 0.3PtZn / AlSiO2) x Compared to 0.3Pt / ZnAlSiO x -15 exhibits superior catalytic activity, higher operational stability, and better regeneration capability. This demonstrates that the Zn-doped support preparation strategy can achieve excellent catalytic performance.

[0141] Figure 3 The N2- adsorption-desorption isotherms are for the supports of Examples 1, 2, 3, and Comparative Example 1. All ZnAlSiO2 supports... x The supports were all mesoporous materials (exhibiting a type IV isotherm with an H2-type hysteresis loop). As the Si content increased from 0 wt% to 20 wt%, the BET specific surface area increased from 231 m² / s². 2 / g gradually decreased to 74 m 2 / g, the mesopore volume also increased from 0.52 cm³. 3 / g decreased to 0.24 cm 3 / g. This densification phenomenon is attributed to Si 4+ The incorporation of [a substance] forms shorter and stronger Si-O-Al or Si-O-Zn tetrahedral bonds, which leads to the shrinkage of the oxide network.

[0142] Figure 4 The images show the pore size distribution of the supports in Examples 1, 2, 3, and Comparative Example 1. Si doping resulted in a more uniform pore structure. After Si addition, the average pore size decreased from 7.4 nm to 5.7-5.9 nm, subsequently for ZnAlSiO2. x The -20 sample further increased to 7.0 nm, indicating a structural transformation under high Si content. The pore size distribution map shows a sharp peak at 3-4 nm in the Si-containing support, which is consistent with the Si-free ZnAlO4 sample. x The wide pore size distribution in the carrier provides a striking contrast, indicating that Si contributes to the formation of a more uniform pore structure.

[0143] Figure 5The XRD patterns of the supports in Examples 1, 2, 3, and Comparative Example 1 are shown. The diffraction patterns of all supports are consistent with nanocrystalline ZnAl₂O₄ spinel, and no ZnO or SiO phases were detected, indicating that Zn and Si are uniformly dispersed. As the Si content increases from 0 wt% to 20 wt%, the diffraction peaks of the spinel gradually broaden and weaken, indicating that more Si has entered the spinel, disrupting the crystal structure.

[0144] Figure 6 The carriers of Examples 1, 2, 3 and Comparative Example 1 29 Si MAS NMR spectrum. No SiO2 phase was observed (typically appearing at -110 ppm, corresponding to Q). 4 The resonance signal corresponding to the species was detected. Instead, a characteristic signal centered at approximately -85 ppm was detected, which belongs to the Q spectrum. 1 and Q 2 Silicon species (corresponding to Si atoms connecting one or two silicon-oxygen bridges, respectively). This phenomenon indicates that Si is uniformly dispersed in the amorphous network.

[0145] Figure 7 This is the AC-HAADF-STEM image after reduction in Example 2, along with the corresponding EDS mapping. It can be clearly seen that pt is distributed in single-atom form on the Zn nanoparticles; and exists in sub-nano cluster form.

[0146] Figure 8 The AC-HAADF-STEM, HAADF-STEM, and particle size distribution diagrams after 30 hours of reaction in Example 7 show that Pt is atomically dispersed on nanoclusters with an average particle size of approximately 1.1 nm.

[0147] Figure 9 The EDS mapping of Example 7 after 30 h of reaction shows that Zn, Al, and Si elements are uniformly distributed in the support, indicating that the co-precipitation method achieves uniform doping of multiple components; at the same time, Pt exhibits a highly dispersed state.

[0148] Figure 10 The images show the NH3-TPD analysis results of the supports in Examples 1, 2, 3, and Comparative Example 1. The temperature range of 100℃-400℃ represents the distribution sites of moderately to weakly acidic substances; the number of acidic sites gradually decreases with the addition of Si.

[0149] Figure 11 Thermogravimetric analysis (TGA) plots of Examples 6, 7, 8 and Comparative Example 6 after 30 h of reaction, 0.3Pt / ZnAlO x The carbon deposition weight loss was 18.94%, while that of 0.3Pt / ZnAlSiO x -10, 0.3Pt / ZnAlSiO x-15 and 0.3Pt / ZnAlSiO x The carbon deposits at -20 were reduced to 8.23%, 7.11%, and 5.09%, respectively, indicating that the introduction of silicon significantly inhibited carbon deposit formation and improved the catalyst's resistance to carbon deposits.

[0150] In summary, the introduction of Si significantly improves the stability and propylene selectivity of the PtZn catalyst, with the best overall performance achieved at a Si content of 15%, exhibiting high activity, high selectivity, and good long-term stability. By controlling the support structure and optimizing Pt dispersion and electronic states, highly efficient and stable catalysis was achieved under low platinum loading (0.3%). This system demonstrates significant performance advantages and potential for industrial PDH applications.

Claims

1. The application of a modified Al2O3-supported PtZn bimetallic catalyst in propane dehydrogenation, characterized in that: The catalyst was obtained by co-precipitation, in which a precursor solution impregnated with Pt on a Si and Zn-doped Al2O3 support was dried and then reduced in a hydrogen atmosphere.

2. The application as described in claim 1, characterized in that: The mass percentage of Zn in the catalyst support is 10%-20%, the mass percentage of Al is 20%-40%, and the mass percentage of Si is 2%-21% (among which the catalyst performance is excellent when the Si content is 10%-21%, and the performance is best when it is 15%-17%).

3. The application as described in claim 1, characterized in that: The precursor solution impregnated with Pt was prepared using an equal-volume impregnation method, and the mass loading of Pt in the catalyst relative to the support was 0.2%-0.3%. The reduction process in a hydrogen atmosphere is as follows: reduction is carried out in a mixture of H2 and He with a hydrogen volume percentage of 10%-100% at 580-620℃ for 1-4 hours.

4. The application as described in claim 1, characterized in that: The preparation method of the Si, Zn-doped Al2O3 support includes the following steps: S1 To prepare metal salt solution A, weigh the soluble precursors of zinc and aluminum and water into a container and dissolve all the solids. S2 Prepare solution B by weighing sodium hydroxide, anhydrous sodium carbonate and water into a container and dissolving them completely. Heat the resulting solution to 60-80 ℃ and then add the silicon precursor to dissolve it. S3 Keep the prepared solution B at 60-80 ℃, and introduce the solution A prepared in step S1 into solution B, while continuously stirring solution B during the introduction process; S4: After the import is complete, stop stirring and continue to age at 60-80 ℃ for 20-30 h; S5: Filter the aged turbid liquid from step S4 while hot, and wash the filter cake with water until the filtrate is neutral. Place the obtained solid in an oven at 50-70 ℃ and dry for 20-30 h. Grind and crush the dried solid, and calcine it at 500-600 ℃ for 2-3 h to obtain ZnAlSiO2. x Carrier.

5. The application as described in claim 4, characterized in that: The precursor salt for Zn is zinc nitrate hexahydrate, the precursor salt for Al is aluminum nitrate nonahydrate, the precursor salt for Si is sodium silicate nonahydrate, and the precursor salt for Pt is H2PtCl6.

6. The application as described in claim 4 or 5, characterized in that: The concentrations of the solutions prepared in steps S1 and S2: Aluminum nitrate (0.5-0.75 mol / L); Sodium hydroxide (1.5-2 mol / L), sodium carbonate (0.5-0.6 mol / L), sodium silicate (0.01-0.2 mol / L).

7. The application as described in claim 1, characterized in that: The preparation method of the aforementioned diatomic catalyst includes the following steps: S1: Take ZnAlSiO x The carrier was impregnated with a Pt precursor solution using an equal-volume impregnation method onto ZnAlSiO2. x On the carrier, continuously stir until a viscous paste is formed, let stand at room temperature for 2-12 h, and dry in an oven at 50-70 ℃ for 12-24 h to obtain the catalyst precursor; S2: The catalyst precursor obtained in step S1 is reduced at 580-620 °C in a mixture of H2 and He with a hydrogen volume percentage of 10% to 100% for 1-4 h to obtain Pt / ZnAlSiO2. x catalyst.

8. The application as described in claim 7, characterized in that: The specific process of step S2 is as follows: The catalyst precursor obtained in step S1 is tableted, crushed and sieved to select particles of 20-40 mesh; the particles are weighed and uniformly mixed with inert quartz sand (20-40 mesh) and placed in a U-shaped quartz tube of a fixed bed reactor; the mixture of H2 and He with a hydrogen volume percentage of 10% to 100% is reduced for 1-4 h at 580-620 °C.

9. The application as described in any one of claims 1-8, characterized in that: The reaction conditions were 600 °C, with the following feed gas volume ratio: 14% C3H8, 14% H2; the balance being He, and a WHSV of 40 h⁻¹. -1 .