A boron-nitrogen co-doped capacitor special carbon material and a preparation method thereof
By pretreatment of domestic sewage sludge and a multi-step doping process, a boron-nitrogen co-doped carbon material for capacitors with high specific capacity, excellent rate performance, and low self-discharge rate was prepared. This solved the problems of high impurity content and uneven doping in the existing technology and improved the performance of the capacitor.
Patent Information
- Application Number
- CN202610973567.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-01
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-07-01
AI Technical Summary
Existing technologies are insufficient to effectively reduce the impurity content in sewage sludge, achieve uniform co-doping of boron and nitrogen elements in the carbon framework, and optimize the pore structure, resulting in poor capacitor performance.
A mixed acid pretreatment method was adopted for domestic sewage sludge, combined with hydrothermal treatment and secondary heat treatment. Boric acid, polyvinyl alcohol and urea were used for doping to optimize the pore structure. Through a multi-step process, a special carbon material for boron-nitrogen co-doped capacitors was prepared.
The impurity content was reduced, which improved the capacitor's specific capacitance, rate performance, and self-discharge performance, thus meeting the practical application requirements of capacitors.
Smart Images

Figure REF-OBJ-1782895486728-000001 
Figure REF-OBJ-1782895486728-000002
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon materials technology, specifically to a boron-nitrogen co-doped carbon material for capacitors and its preparation method. Background Technology
[0002] Supercapacitors, as a novel energy storage device, possess advantages such as high power density, long cycle life, and fast charge / discharge speed, showing broad application prospects in portable electronic devices, hybrid vehicles, and renewable energy power generation. Electrode materials are one of the key factors determining the performance of supercapacitors. Among them, porous carbon materials have become the most widely used electrode materials due to their high specific surface area, good conductivity, excellent chemical stability, and relatively low cost. To further improve the electrochemical performance of supercapacitor carbon, heteroatom doping has proven to be an effective strategy. It can enhance the adsorption capacity of electrode materials for electrolyte ions by changing the electronic structure and surface chemistry of the carbon skeleton, thereby improving specific capacity and rate performance.
[0003] Activated carbon can be prepared from a wide range of raw materials, including coal, wood, nutshells, and various biomass. In recent years, the use of municipal sewage sludge as a carbon precursor in the preparation of carbon materials for capacitors, derived from waste resource recovery, has attracted attention. However, direct carbonization of municipal sewage sludge presents significant problems: it has a high inorganic ash content and contains impurities such as heavy metal ions. These components not only reduce the porosity and specific surface area of the resulting carbon material but also introduce side reactions, increase internal resistance, and lead to a severe decline in capacitance performance. While simple acid washing pretreatment can remove some ash in existing technologies, its efficiency is often limited, and it is difficult to simultaneously achieve the ordered control of the carbon framework.
[0004] Furthermore, for the preparation of boron-nitrogen co-doped carbon materials, there are reports of using a method of co-pyrolysis of boric acid or borates with nitrogen-containing precursors and carbon sources at high temperatures. However, this method often faces problems such as uneven doping, low doping concentration, and unsatisfactory distribution of doped atoms in the carbon matrix. Simultaneously, existing doping processes are often separated from the activation and pore-forming steps, resulting in poor synergy between doping and pore structure control. Ultimately, the rate performance and self-discharge performance of the material are insufficient to meet the practical application requirements of capacitors.
[0005] Therefore, how to utilize domestic sewage sludge, a low-value waste, to effectively reduce impurity content through reasonable pretreatment and doping processes, and to achieve uniform and stable co-doping of boron and nitrogen elements in the carbon skeleton, while optimizing the pore structure, in order to prepare capacitor-specific carbon materials with high specific capacity, excellent rate performance and low self-discharge rate, remains a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0006] The purpose of this invention is to provide a boron-nitrogen co-doped carbon material for capacitors and its preparation method, so as to solve the problems existing in the prior art.
[0007] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for preparing a boron-nitrogen co-doped carbon material for capacitors, comprising the following preparation steps: Pre-dry domestic sewage sludge with a moisture content of 75%~85% at 105℃ to constant weight, crush it, add mixed acid at a liquid-to-solid ratio of 10~15mL / g (mixed acid: dry sludge mass), stir at 60-100℃ for 1-3h, then vacuum filter, wash the solid with deionized water at 60~70℃ until the pH of the wash liquid is ≥4.5, dry at 105℃ to constant weight and take the dry material; First, boric acid and polyvinyl alcohol are dissolved separately in deionized water at 80-90℃, and then mixed with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.15-0.30:0.05-0.15, and the amount of water is 8-12 times the total mass of the three. The mixture is transferred to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. It is then heat-treated at 140-160℃ for 12-18 hours. After cooling, it is directly concentrated under reduced pressure at 60-80℃ and dried to obtain a boron-containing precursor. Take the boron-containing precursor from step (2), mix it with the additives and urea, and ball mill it until the D50 is 30-50 μm. Under an inert atmosphere, pre-carbonize it at 450-550℃ for 1-2 hours. Then add potassium hydroxide, mix it thoroughly, and heat it to 700-800℃ at a heating rate of 1-5℃ / min under a nitrogen or argon atmosphere and keep it at that temperature for 4 hours. Let it cool naturally to room temperature, wash it three times with 10wt% hydrochloric acid solution, and then wash it thoroughly with 80℃ deionized water until it is neutral. Dry it in a 105℃ constant temperature oven until it reaches constant weight. The carbon material obtained in step (3), boric acid, urea and polyvinyl alcohol are dispersed in deionized water at a mass ratio of 1:0.05-0.15:0.10-0.30:0.02-0.05. Vacuum is drawn and maintained for 30-60 minutes. After restoring normal pressure, the mixture is stirred for a period of time, then evaporated under reduced pressure to remove water, dried, and subjected to segmented heat treatment under an inert atmosphere.
[0008] Furthermore, the mixed acid in step (1) includes 0.5-1.5M hydrochloric acid, 0.1-0.5M citric acid, 0.1-0.3M oxalic acid, and the remainder is water.
[0009] Furthermore, in step (1), the mixed acid is added at a liquid-to-solid ratio of 10-15 mL / g (mixed acid: dry sludge mass).
[0010] Furthermore, in step (2), the mass ratio of dry material, boric acid and polyvinyl alcohol is 1:0.15-0.30:0.05-0.15.
[0011] Furthermore, the amount of water used in step (2) is 8-12 times the total mass of the three components.
[0012] Furthermore, in step (2), the heat treatment temperature is 140-160℃ and the heat treatment time is 12-18h.
[0013] Furthermore, the adjuvant in step (3) is one of starch, cellulose, lignin, sucrose, glucose and fructose.
[0014] Furthermore, in step (3), the mass ratio of the boron-containing precursor to the auxiliaries and urea is 1:0.2-0.8:0.1-0.5.
[0015] Furthermore, the amount of potassium hydroxide used in step (3) is 1-4 times the mass of the boron-containing precursor.
[0016] Further, the specific steps of the secondary heat treatment in step (4) are as follows: the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) are dispersed in deionized water at a mass ratio of 1:0.05-0.15:0.10-0.30:0.02-0.05, vacuum is drawn and maintained for 30-60 minutes, after restoring normal pressure, the mixture is stirred for a period of time, then the water is removed by vacuum evaporation, dried, and then subjected to segmented heat treatment under an inert atmosphere.
[0017] Compared with the prior art, the beneficial effects achieved by the present invention are: This invention uses domestic sewage sludge as the main carbon source, which can realize waste regeneration. Through mixed acid pretreatment and subsequent acid washing and water washing, the content of ash, inorganic salts and metal impurities in the sludge can be reduced, the adverse effects of impurities on carbonization, activation and electrochemical performance can be reduced, and the pyrolysis and activation reaction activity of the organic components of the sludge can be improved.
[0018] This invention utilizes domestic sewage sludge as raw material and boric acid and urea as additives to achieve boron-nitrogen doping, which can promote the adsorption of electrolyte ions by activated carbon, thereby increasing the capacity of activated carbon materials and optimizing self-discharge performance.
[0019] This invention involves hydrothermally treating pretreated sludge with boric acid and polyvinyl alcohol to promote uniform dispersion and fixation of the boron source in the organic matrix of the sludge, thereby reducing the migration and loss of the boron source during subsequent high-temperature treatment. Polyvinyl alcohol can also supplement the carbon source and improve the char-forming properties of the precursor, which is beneficial for obtaining a boron-containing carbon precursor with uniform composition and stable structure. Then, it is mixed with urea, the supplemented carbon source, and the activator and calcined to achieve doping and pore expansion at the same time.
[0020] This invention can replenish the boron and nitrogen elements lost during the activation process through secondary heat treatment, and improve the uniformity and stability of doping distribution. It also enables heteroatom doping and pore structure regulation to work together to further improve the capacity retention, rate performance and cycle performance of the material. Detailed Implementation
[0021] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0022] Example 1
[0023] (1) Pre-dry the domestic sludge with a moisture content of 75% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 10mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.0.2:0.05, and the amount of water is 8 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 140°C for 12 hours, cool, concentrate under reduced pressure at 80°C and dry to constant weight to obtain boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with cellulose and urea at a mass ratio of 1:0.2:0.1 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 450℃ for 2h. Then add potassium hydroxide with a mass of 1 times that of the boron-containing precursor and mix it thoroughly. Under a nitrogen atmosphere, heat it to 700℃ at a heating rate of 1℃ / min and keep it at that temperature for 4h. Cool it naturally to room temperature, wash it three times with 10wt% hydrochloric acid solution, and then wash it thoroughly with deionized water at 80℃ until it is neutral. Dry it in a constant temperature oven at 105℃ until it reaches constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.05:0.10:0.02, evacuate to -0.09 MPa and maintain for 30 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 650℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0024] Example 2
[0025] (1) Pre-dry the domestic sludge with a moisture content of 80% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 11mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.30:0.15, and the amount of water is 10 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 140°C for 18 hours, cool, concentrate under reduced pressure at 80°C and dry to constant weight to obtain boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with lignin and urea at a mass ratio of 1:0.8:0.5 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 450℃ for 2h. Then add potassium hydroxide with a mass of 4 times that of the boron-containing precursor and mix it thoroughly. Under an argon atmosphere, heat it to 800℃ at a heating rate of 5℃ / min and keep it at that temperature for 4h. Let it cool naturally to room temperature. First wash it three times with 10wt% hydrochloric acid solution, then wash it thoroughly with 80℃ deionized water until it is neutral. Dry it in a 105℃ constant temperature oven until it reaches constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.1:0.10:0.03, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 650℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0026] Example 3
[0027] (1) Pre-dry the domestic sludge with a moisture content of 85% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 12mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.30:0.1, and the amount of water is 12 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 150°C for 18 hours, cool, concentrate under reduced pressure at 80°C and dry to constant weight to obtain a boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with sucrose and urea at a mass ratio of 1:0.5:0.3 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 550℃ for 1h. Then add potassium hydroxide with a mass of 2 times that of the boron-containing precursor and mix it thoroughly. Under a nitrogen atmosphere, heat it to 750℃ at a heating rate of 3℃ / min and keep it at that temperature for 4h. Cool it naturally to room temperature, wash it three times with 10wt% hydrochloric acid solution, and then wash it thoroughly with deionized water at 80℃ until it is neutral. Dry it in a constant temperature oven at 105℃ until it reaches constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.15:0.15:0.04, evacuate to -0.09 MPa and maintain for 50 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 670℃ at 3℃ / min and keep warm for 1 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0028] Example 4
[0029] (1) Pre-dry the domestic sludge with a moisture content of 85% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 14mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.2:0.1, and the amount of water is 10 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 150°C for 16 hours, cool, concentrate under reduced pressure at 80°C and dry to constant weight to obtain boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with glucose and urea at a mass ratio of 1:0.8:0.1 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 500℃ for 2h. Then add potassium hydroxide with a mass of 4 times that of the boron-containing precursor and mix it thoroughly. Under an argon atmosphere, heat it to 700℃ at a heating rate of 1℃ / min and keep it at that temperature for 4h. Let it cool naturally to room temperature. First wash it 3 times with 10wt% hydrochloric acid solution, then wash it thoroughly with 80℃ deionized water until it is neutral. Dry it in a 105℃ constant temperature oven until it reaches constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.12:0.2:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 700℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0030] Example 5
[0031] (1) Pre-dry the domestic sludge with a moisture content of 75% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 15mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.25:0.1, and the amount of water is 12 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 150°C for 16 hours, cool, concentrate under reduced pressure at 80°C and dry to constant weight to obtain a boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with starch and urea at a mass ratio of 1:0.2:0.5 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 500℃ for 2h. Then add potassium hydroxide with a mass of 1 times that of the boron-containing precursor and mix it thoroughly. Under a nitrogen atmosphere, heat it to 800℃ at a heating rate of 5℃ / min and keep it at that temperature for 4h. Let it cool naturally to room temperature. First wash it three times with 10wt% hydrochloric acid solution, then wash it thoroughly with 80℃ deionized water until it is neutral. Dry it in a 105℃ constant temperature oven until it reaches constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.10:0.30:0.04, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0032] Example 6
[0033] (1) Pre-dry the domestic sludge with a moisture content of 80% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 15mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.30:0.15, and the amount of water is 12 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 160°C for 16 hours, cool, and then concentrate under reduced pressure at 80°C and dry to constant weight to obtain a boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with fructose and urea at a mass ratio of 1:0.6:0.4 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 550℃ for 1h. Then add potassium hydroxide with a mass of 3 times that of the boron-containing precursor and mix it thoroughly. Under an argon atmosphere, heat it to 780℃ at a heating rate of 4℃ / min and keep it at that temperature for 4h. Let it cool naturally to room temperature. Wash it three times with 10wt% hydrochloric acid solution, then wash it thoroughly with deionized water at 80℃ until it is neutral. Dry it in a constant temperature oven at 105℃ until it reaches constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.15:0.30:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0034] Comparative Example 1 (1) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80℃, and then mix them with dry materials. The mass ratio of domestic sludge, boric acid and polyvinyl alcohol is 1:0.30:0.15, and the amount of water is 12 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 160℃ for 16 hours, cool and then concentrate under reduced pressure at 80℃ and dry to constant weight to obtain boron-containing precursor. (2) Take the boron-containing precursor from step (2) and mix it with fructose and urea at a mass ratio of 1:0.6:0.4 and ball mill it until the D50 is 30μm. Under an argon atmosphere, pre-carbonize it at 550℃ for 1h. Then add potassium hydroxide with a mass of 3 times that of the boron-containing precursor and mix it thoroughly. Under an argon atmosphere, heat it to 780℃ at a heating rate of 4℃ / min and keep it at that temperature for 4h. Let it cool naturally to room temperature. Wash it three times with 10wt% hydrochloric acid solution, then wash it thoroughly with deionized water at 80℃ until it is neutral. Dry it in a constant temperature oven at 105℃ until it reaches constant weight. (3) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (2) in deionized water at a mass ratio of 1:0.15:0.30:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0035] Comparative Example 2 (1) Pre-dry the domestic sludge with a moisture content of 80% at 105℃ to constant weight, crush it, add mixed acid at a liquid-to-solid ratio of 15mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, wash the solid with deionized water at 70℃ until the pH of the wash liquid is 5, dry it at 105℃ to constant weight and take the dry material. (2) The dry material is mixed with fructose and urea at a mass ratio of 1:0.6:0.4 and ball-milled until D50 is 30μm. Under an argon atmosphere, it is pre-carbonized at 550℃ for 1h. Then, potassium hydroxide with a mass of 3 times that of the dry material is added and mixed thoroughly. Under an argon atmosphere, the temperature is raised to 780℃ at a heating rate of 4℃ / min and held for 4h. After natural cooling to room temperature, it is washed 3 times with 10wt% hydrochloric acid solution and then thoroughly washed with 80℃ deionized water until neutral. It is then dried in a 105℃ constant temperature oven to constant weight. (3) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (2) in deionized water at a mass ratio of 1:0.15:0.30:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0036] Comparative Example 3 (1) Pre-dry the domestic sludge with a moisture content of 80% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 15mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) Take dry material and mix it with fructose, urea and boric acid in a mass ratio of 1:0.6:0.4:0.5 and ball mill until D50 is 30μm. Under argon atmosphere, pre-carbonize at 550℃ for 1h. Then add potassium hydroxide containing 3 times the mass of boron precursor and mix thoroughly. Under argon atmosphere, heat to 780℃ at a heating rate of 4℃ / min and keep at that temperature for 4h. Cool naturally to room temperature. Wash three times with 10wt% hydrochloric acid solution, then wash thoroughly with 80℃ deionized water until neutral. Dry in a 105℃ constant temperature oven to constant weight. (3) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (2) in deionized water at a mass ratio of 1:0.15:0.30:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0037] Comparative Example 4 (1) Pre-dry the domestic sludge with a moisture content of 80% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 15mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.30:0.15, and the amount of water is 12 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 160°C for 16 hours, cool, and then concentrate under reduced pressure at 80°C and dry to constant weight to obtain a boron-containing precursor. (3) Take the boron-containing precursor from step (2) and fructose at a mass ratio of 1:0.6 and ball mill until D50 is 30μm. Under an argon atmosphere, pre-carbonize at 550℃ for 1h. Then add potassium hydroxide at 3 times the mass of the boron-containing precursor and mix thoroughly. Under an argon atmosphere, heat to 780℃ at a heating rate of 4℃ / min and keep warm for 4h. Cool naturally to room temperature. Wash three times with 10wt% hydrochloric acid solution, then wash thoroughly with 80℃ deionized water until neutral. Dry in a 105℃ constant temperature oven to constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.15:0.30:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0038] Comparative Example 5 (1) Pre-dry the domestic sludge with a moisture content of 80% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 15mL / g (mixed acid: dry sludge mass), stir at 80℃ for 2h, then vacuum filter, rinse the boron-containing precursor with deionized water at 70℃ until the pH of the washing liquid is 5, dry at 105℃ to constant weight and take the dry material. (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80°C, and then mix them with dry materials. The mass ratio of dry materials, boric acid and polyvinyl alcohol is 1:0.30:0.15, and the amount of water is 8-12 times the total mass of the three. Transfer the mixture to a high-pressure reactor, with the liquid volume not exceeding 80% of the reactor volume. Heat treat at 160°C for 16 hours, cool, concentrate under reduced pressure at 80°C and dry to constant weight to obtain boron-containing precursor. (3) Take the boron-containing precursor from step (2) and urea at a mass ratio of 1:0.4 and ball mill until D50 is 30μm. Under an argon atmosphere, pre-carbonize at 550℃ for 1h. Then add potassium hydroxide with a mass of 3 times that of the boron-containing precursor and mix thoroughly. Under an argon atmosphere, heat to 780℃ at a heating rate of 4℃ / min and keep warm for 4h. Cool naturally to room temperature. Wash three times with 10wt% hydrochloric acid solution, then wash thoroughly with 80℃ deionized water until neutral. Dry in a 105℃ constant temperature oven to constant weight. (4) Disperse the carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) in deionized water at a mass ratio of 1:0.15:0.30:0.05, evacuate to -0.09 MPa and maintain for 40 min, restore to normal pressure and stir at 60℃ for 2 h, then evaporate under reduced pressure to remove water, vacuum dry at 80℃ to constant weight, raise to 280℃ at 2℃ / min under inert atmosphere and keep warm for 1 h; then raise to 680℃ at 3℃ / min and keep warm for 1.5 h, cool under inert atmosphere and wash 4 times with deionized water at 80℃.
[0039] Comparative Example 6 The sewage sludge was dried to a moisture content of <5%, then mixed with fructose, urea, and boric acid in a mass ratio of 1:0.6:0.4:0.5 and ball-milled until the D50 was 30 μm. Then, potassium hydroxide with a solid mass of 3 times was added and mixed thoroughly. Under an argon atmosphere, the mixture was heated to 780°C at a heating rate of 4°C / min and held at that temperature for 4 hours. After naturally cooling to room temperature, the sludge was washed three times with a 10wt% hydrochloric acid solution, then thoroughly washed with deionized water at 80°C until neutral, and finally dried in a constant temperature oven at 105°C until constant weight.
[0040] Comparative Example 7 Boric acid, fructose, and urea were mixed in a mass ratio of 0.5:0.6:0.4 and ball-milled until D50 was 30 μm. The mixture was pre-carbonized at 550 °C for 1 h under an argon atmosphere. Then, potassium hydroxide with a mass of 3 times that of fructose was added and thoroughly mixed. The mixture was then heated to 780 °C at a heating rate of 4 °C / min under an argon atmosphere and held at that temperature for 4 h. After naturally cooling to room temperature, the mixture was washed three times with a 10 wt% hydrochloric acid solution and then thoroughly washed with deionized water at 80 °C until neutral. Finally, it was dried in a constant temperature oven at 105 °C until constant weight.
[0041] Performance testing: (1) Nitrogen adsorption-desorption tests were conducted at 77 K using a McMeter spectrometer. The specific surface area was calculated using the BET formula, and the results are shown in Table 1. The micropore size distribution was calculated from the adsorption branch data using the quench solid density function theory (QSDFT) and based on the slit-shaped pore model.
[0042] (2) Conductivity test method: The Mitsubishi Chemical MCP-PD51 powder conductivity tester was used. The activated carbon powder was placed in the sample tank and the conductivity was tested at a pressure of 63.66 MPa.
[0043] (3) The capacitance performance of the activated carbon in the sulfuric acid-based capacitor of this application was evaluated using a symmetrical dual-electrode system. The process was as follows: Activated carbon, Super P conductive agent, and polytetrafluoroethylene binder were accurately weighed, with a mass ratio of approximately 80:15:5. A certain amount of isopropanol was added, and the mixture was stirred evenly to form a slurry. The slurry was then rolled to a thickness of approximately 100 μm, and micropores were punched to form electrode discs with a diameter of 13 mm. The electrode discs were then vacuum-dried at 120 °C for at least 12 hours. After weighing, the mass of the active material on a single electrode was approximately 3 ± 0.3 mg / cm³. -2 The dried and weighed electrode sheet was pressed onto the current collector (titanium mesh). Two symmetrical current collectors / electrodes were separated by two layers of microporous fiber film. The current collector / electrode was then immersed in 1M H2SO4 solution and wrapped with parafilm sealing film. The immersion time was more than 5 hours. The test was performed using a CHI660D electrochemical workstation.
[0044] Test methods for specific capacity, overall specific capacity, and rate retention: At 0.25 A·g -1 The specific capacitance (Cm) of a capacitor was tested under constant current charge-discharge conditions of 0V to 0.9V. A 20A·g test was used. -1 Test its rate capability. The specific capacitance (Cm) of the capacitor is calculated using the following formula based on the constant current discharge curve:
[0045] Where I is the constant current (A), m represents the total mass of the two electrodes (g), and dV / dt (V / s) is the slope of the voltage-time fitting curve of the discharge curve, taken as its absolute value in the calculation. The current density is 0.25 A·g. -1 C m This represents the capacitance-to-mass ratio of a capacitor.
[0046] 20A·g -1 Rate retention was tested under the following conditions: 0.25 A·g -1 Its specific capacity was tested under the specified conditions.
[0047] Comprehensive specific capacity (C) 综合 The formula for calculating C is: 综合 =C m / (1 + absorbance value) The overall specific capacitance reflects the combined capacity performance of the electrolyte and activated carbon, and is directly related to the energy density of the actual capacitor.
[0048] (4) Self-discharge retention rate test method: The circuit is charged to a working voltage of 0.9V using a constant current and held at a constant voltage for 120 minutes. Then the circuit is opened, and the open-circuit voltage-time relationship is obtained. The self-discharge retention rate is the ratio of the voltage value U(V) after 30 hours of opening to the initial voltage of 0.9(V).
[0049] Table 1. Main Technical Parameters of Boron-Nitrogen Co-doped Carbon Materials for Capacitors
[0050] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.
Claims
1. A method for preparing a boron-nitrogen co-doped carbon material for capacitors, characterized in that, The preparation steps include the following: (1) Pre-dry domestic sludge with a moisture content of 75%~85% at 105℃ to constant weight, crush it, add mixed acid at a liquid-solid ratio of 10~15mL / g, wherein the mixed acid includes 0.5-1.5M hydrochloric acid, 0.1-0.5M citric acid, 0.1-0.3M oxalic acid, and the remainder is water, stir at 60-100℃ for 1-3h, then vacuum filter, wash the solid with deionized water at 60~70℃ until the pH of the washing liquid is ≥4.5, dry at 105℃ to constant weight and take dry material; (2) First, dissolve boric acid and polyvinyl alcohol in deionized water at 80-90℃, then mix them with dry materials, transfer them to a high-pressure reactor, and fill the reactor with liquid at no more than 80% of its volume. Heat treatment is then carried out, and after cooling, the mixture is concentrated under reduced pressure at 60-80℃ and dried to obtain a boron-containing precursor. (3) Take the boron-containing precursor from step (2) and mix it with the additives and urea. Ball mill until the D50 is 30-50 μm. Pre-carbonize at 450-550℃ for 1-2 hours under an inert atmosphere. Then add potassium hydroxide and mix thoroughly. Under a nitrogen or argon atmosphere, heat to 700-800℃ at a heating rate of 1-5℃ / min and keep warm for 4 hours. Cool naturally to room temperature. Wash three times with 10wt% hydrochloric acid solution, then wash thoroughly with 80℃ deionized water until neutral. Dry in a 105℃ constant temperature oven to constant weight. (4) The carbon material obtained in step (3) is subjected to secondary heat treatment.
2. The method for preparing a boron-nitrogen co-doped carbon material for capacitors according to claim 1, characterized in that, In step (2), the mass ratio of dry material, boric acid and polyvinyl alcohol is 1:0.15-0.30:0.05-0.15, and the amount of water used is 8-12 times the total mass of dry material, boric acid and polyvinyl alcohol.
3. The method for preparing a boron-nitrogen co-doped carbon material for capacitors according to claim 1, characterized in that, In step (2), the heat treatment temperature is 140-160℃ and the heat treatment time is 12-18h.
4. The method for preparing a boron-nitrogen co-doped carbon material for capacitors according to claim 1, characterized in that, The adjuvant in step (3) is one of starch, cellulose, lignin, sucrose, glucose and fructose.
5. The method for preparing a boron-nitrogen co-doped carbon material for capacitors according to claim 1, characterized in that, The mass ratio of the boron-containing precursor to the auxiliaries and urea in step (3) is 1:0.2-0.8:0.1-0.
5.
6. The method for preparing a boron-nitrogen co-doped carbon material for capacitors according to claim 1, characterized in that, In step (3), the amount of potassium hydroxide used is 1-4 times the mass of the boron-containing precursor.
7. The method for preparing a boron-nitrogen co-doped carbon material for capacitors according to claim 1, characterized in that, The specific steps of the secondary heat treatment in step (4) are as follows: The carbon material, boric acid, urea and polyvinyl alcohol obtained in step (3) are dispersed in deionized water at a mass ratio of 1:0.05-0.15:0.10-0.30:0.02-0.
05. Vacuum is drawn and maintained for 30-60 minutes. After restoring normal pressure, the mixture is stirred for a period of time. Then, the water is removed by vacuum evaporation, and the mixture is dried. The mixture is then subjected to segmented heat treatment under an inert atmosphere.
Citation Information
Patent Citations
Magnetic activated carbon and methods for preparing and regenerating such materials
CN104703689A
Nitrogen-containing carbon material for supercapacitor as well as preparation method and application thereof
CN111422865A