Cylindrical battery and electric device

CN122599551APending Publication Date: 2026-08-18CALB GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611090700.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-22
Publication Date
2026-08-18

AI Technical Summary

Technical Problem

[0005]本发明的主要目的在于提供一种圆柱电池和用电设备,以解决现有技术中圆柱电池中极片电流密度不均导致电池能量密度低的问题

Benefits of technology

[0032] Compared to other ranges, this application, by limiting a/b to the aforementioned specific range, can shorten the length of the electron flow path and suppress current density unevenness while avoiding the core hole being blocked; at the same time, it can improve the charge and discharge performance of cylindrical batteries at high rates and improve the overall performance of cylindrical batteries, such as energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122599551A_ABST
    Figure CN122599551A_ABST
Patent Text Reader

Abstract

This invention provides a cylindrical battery and an electrical device. The cylindrical battery includes a core, which includes at least one negative electrode and at least one positive electrode wound together, and a separator is provided between two adjacent positive and negative electrode sheets; a tab is provided on one side of the unfolded negative electrode sheet along its length, and the negative electrode sheet has a first tabless region, which is the area located between the starting end of the winding and the edge of the tab near the starting end of the winding; the cylindrical battery satisfies formula (I): 0.033≤a / b≤0.341 (I), where a represents the ratio of the length of the first tabless region to the unfolded length of the negative electrode sheet; b represents the ratio of the discharge capacity of the cylindrical battery at 25°C and 4C rate to the discharge capacity at 0.33C rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically, to a cylindrical battery and an electrical device. Background Technology

[0002] In the existing cylindrical battery technology field, although the tabless region design aims to avoid obstructing the ferrule holes and thus optimize the battery's internal structure, this design introduces a new challenge: it leads to uneven current distribution on the electrodes. Specifically, the presence of the tabless region causes some areas of the electrode to experience higher current densities, while other areas experience relatively lower densities. This uneven distribution of current density directly affects the insertion and extraction of lithium ions within the electrodes, thereby reducing the battery's energy density.

[0003] While the tabless design of cylindrical batteries has solved the problem of core hole obstruction, it has caused new performance bottlenecks due to uneven current density distribution. In particular, the energy density and cycle stability of the battery have become urgent problems to be solved.

[0004] Based on this, it is of great significance to research and develop a cylindrical battery with uniform current density, high energy density and excellent overall performance in the electrode. Summary of the Invention

[0005] The main objective of this invention is to provide a cylindrical battery and an electrical device to solve the problem of low battery energy density caused by uneven current density of the electrode plates in the prior art.

[0006] To achieve the above objectives, the present invention provides a cylindrical battery comprising a core, the core including at least one negative electrode and at least one positive electrode wound together, and a separator being disposed between adjacent positive and negative electrode sheets; a tab is disposed on one side of the negative electrode sheet along its length after it is unfolded, and the negative electrode sheet is provided with a first tabless region, the first tabless region being the area located between the starting end of the winding and the edge of the tab near the starting end of the winding; the cylindrical battery satisfies formula (I):

[0007] 0.033≤a / b≤0.341 (I),

[0008] Where a represents the ratio of the length of the first tabless region to the unfolded length of the negative electrode; b represents the ratio of the discharge capacity of the cylindrical battery at 25°C and 4C rate to the discharge capacity at 0.33C rate.

[0009] Furthermore, a is any value between 0.03 and 0.3; and / or b is any value between 0.8 and 1.03.

[0010] Furthermore, 0.08 ≤ a / b ≤ 0.195.

[0011] Furthermore, 0.088 ≤ a / b ≤ 0.178.

[0012] Furthermore, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer stacked together. The material of the negative electrode active material layer includes a silicon-based material, and 0.04≤a / b≤0.28.

[0013] Furthermore, the weight percentage of silicon in the negative electrode active material layer is ≥3wt%, and 0.04≤a / b≤0.23.

[0014] Furthermore, the weight percentage of silicon in the negative electrode active material layer is ≤30wt%.

[0015] Furthermore, the areal density of the negative electrode active material layer is 100–280 g / m³. 2 .

[0016] Furthermore, the thickness of the negative electrode active material layer is ≥90μm, and 0.055≤a / b≤0.26.

[0017] Furthermore, a can be any value between 0.02 and 0.28.

[0018] Furthermore, the ratio of the length of the tabless region in the positive electrode to the unfolded length of the positive electrode is 0.04 to 0.33.

[0019] Furthermore, the discharge capacity of the cylindrical battery at a 4C rate is 15–50 Ah; the discharge capacity of the cylindrical battery at a 0.33C rate is 19–55 Ah.

[0020] Furthermore, the porosity of the negative electrode sheet is 35–60%, and the compacted density is 1.2–1.7 g / cm³. 3 .

[0021] Furthermore, the positive electrode sheet includes a positive current collector and a positive active material layer stacked together. The material of the positive active material layer includes a ternary positive electrode material of lithium nickel cobalt manganese oxide, and the ratio of the length of the tabless region in the positive electrode sheet to the unfolded length of the positive electrode sheet is 0.08 to 0.33; or, the material of the positive active material layer includes lithium iron phosphate, and the ratio of the length of the tabless region in the positive electrode sheet to the unfolded length of the positive electrode sheet is 0.12 to 0.33.

[0022] Furthermore, the positive electrode sheet includes a positive current collector and a positive active material layer stacked together. The material of the positive active material layer includes lithium nickel cobalt manganese oxide ternary positive electrode material, and the Dv50 of the lithium nickel cobalt manganese oxide ternary positive electrode material is 2 to 4 μm; or, the material of the positive active material layer includes lithium iron phosphate, and the Dv50 of lithium iron phosphate is 0.4 to 2.0 μm.

[0023] Furthermore, the material of the positive electrode active material layer includes lithium nickel cobalt manganese oxide ternary cathode material, and the porosity of the cathode sheet is 12-35%, with a compaction density of 3.45-3.65 g / cm³. 3 Alternatively, the positive electrode active material layer may be made of lithium iron phosphate, and the porosity of the positive electrode sheet may be 12–35%, with a compaction density of 2.1–2.7 g / cm³. 3 .

[0024] Furthermore, along the length of the unfolded negative electrode sheet, each negative electrode sheet has multiple tabs on one side, and the width of the connection between each tab and the negative electrode sheet is 2 to 10 mm; and / or, the lead-out size of each tab is 2 to 15 mm.

[0025] Furthermore, each negative electrode sheet includes at least one second electrodeless region between the multiple tabs on one side of its unfolded length direction. The ratio of the sum of the lengths of the second electrodeless region and the first electrodeless region to the unfolded length of the negative electrode sheet is 0.05 to 0.6.

[0026] Furthermore, multiple negative electrode tabs are provided along the length direction after the negative electrode sheet is unfolded, and multiple positive electrode tabs are provided along the length direction after the positive electrode sheet is unfolded. The positive electrode tabs and negative electrode tabs are located at the same end of the winding core.

[0027] Furthermore, the core includes core holes with a diameter of 6–8 mm.

[0028] Furthermore, the core also includes an electrolyte, the electrolyte of which includes a lithium salt, the molar concentration of which is 0.6–1.6 mol / L, and the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide.

[0029] According to another aspect of the present invention, an electrical device is provided, which includes the cylindrical battery described above provided in this application.

[0030] To achieve the above objectives, another aspect of the present invention provides an electrical device comprising the cylindrical battery described in this application.

[0031] Applying the technical solution of this invention, the cylindrical battery provided in this application includes a core, including a first tabless region located at the first end after the core is unrolled. The core includes a core hole. The arrangement of the first tabless region can prevent the tabs from blocking the core hole. However, the tabs are structures that bear the current of the negative electrode. The arrangement of the first tabless region causes different current densities in different areas of the electrode, resulting in high current density in some areas and low current density in others, affecting the insertion and extraction of lithium ions, and thus affecting the battery energy density. The ratio of the battery capacity at different rates is also a key measure of the lithium ion insertion and extraction capability. By controlling the relationship between the two, the length of the first tabless region is longer. By controlling the capacity ratio at different rates, lithium ion transport is improved, and the battery energy density is increased. The capacity at different rates at a specific temperature refers to the battery's discharge capability at different rates. The smaller the ratio, the weaker the discharge capability at high rates, affecting the battery energy density. The value of a / b cannot be too large, resulting in low battery energy density; the value of a / b cannot be too small, as it will block the core hole. When 'a' is relatively large, the increased impedance necessitates a larger 'b' to achieve improved energy density and fast charging performance. Conversely, a smaller 'a' reduces electrolyte injection efficiency and limits electrolyte wetting ability, requiring a smaller 'b', which significantly degrades the battery's fast charging performance.

[0032] Compared to other ranges, this application, by limiting a / b to the aforementioned specific range, can shorten the length of the electron flow path and suppress current density unevenness while avoiding the core hole being blocked; at the same time, it can improve the charge and discharge performance of cylindrical batteries at high rates and improve the overall performance of cylindrical batteries, such as energy density. Attached Figure Description

[0033] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0034] Figure 1 A schematic diagram of the unfolded negative electrode sheet in a preferred embodiment of this application is shown.

[0035] The above figures include the following reference numerals:

[0036] 10. Negative electrode plate; 20. Electrode tab; 30. First electrodeless zone; 40. Second electrodeless zone. Detailed Implementation

[0037] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0038] As described in the background art, existing cylindrical batteries suffer from low energy density due to uneven current density on the electrodes. To address this technical problem, one aspect of this application provides a cylindrical battery comprising a core, the core including at least one negative electrode 10 and at least one positive electrode 10 wound together, with a separator between adjacent positive and negative electrode 10s; characterized in that a tab 20 is provided on one side of the negative electrode 10 along its length after unfolding, and the negative electrode 10 has a first tabless-free region 30, the first tabless-free region 30 being the area between the starting end of winding and the edge of the tab 20 near the starting end of winding; the cylindrical battery satisfies formula (I):

[0039] 0.033≤a / b≤0.341 (I),

[0040] Where a represents the ratio of the length of the first tabless region 30 to the unfolded length of the negative electrode 10; b represents the ratio of the discharge capacity of the cylindrical battery at 25°C and 4C rate to the discharge capacity at 0.33C rate.

[0041] This application reveals that battery capacity performance at different charge / discharge rates is also a key indicator for evaluating battery performance. At high rates, the battery must be able to quickly respond to high current demands to ensure good charge / discharge performance. However, when a battery operates at high rates, the rapid transport and storage of lithium ions are often hindered, especially when the tabless region has a high proportion of length. This hindering effect is more pronounced, resulting in a significantly lower capacity at high rates compared to low rates, thus impacting the battery's overall performance and application range.

[0042] The arrangement of the first tabless region 30 in the core of this application can avoid obstructing the core hole. However, the arrangement of the first tabless region 30 will cause different current densities in different areas of the negative electrode 10, resulting in some areas of the negative electrode 10 having high current density and others having low current density, affecting the insertion and extraction of lithium ions, and thus affecting the energy density of the cylindrical battery. Specifically, the larger the value of 'a', the larger the proportion of the first tabless region 30 in the unfolded length of the negative electrode 10, the longer the electron flow path, resulting in greater impedance and affecting the energy density of the cylindrical battery; the smaller the value of 'a', the smaller the proportion of the first tabless region 30 in the unfolded length of the negative electrode 10, which will cause obstruction of the core hole, reduce the electrolyte injection efficiency, limit the electrolyte wetting ability, and cause concentration polarization in the short term, resulting in poor battery transport dynamics.

[0043] The ratio of the discharge capacity of a cylindrical battery at different rates can measure its lithium-ion intercalation / deintercalation capability. Generally, the discharge capacity of a battery at high rates is lower than that at low rates. In this application, the ratio under specific temperature (25°C) and discharge rate (4C and 0.33C) conditions is defined as b. The closer b is to 1, the smaller the difference between the battery's capacity at 4C high-rate discharge and 0.33C low-rate discharge; that is, the battery's high-rate and low-rate discharge performances are very similar. This means the battery has good rate characteristics and can maintain high energy output without significantly sacrificing capacity under high-current rapid charging and discharging. A larger b indicates severe heat generation under 4C high-rate discharge, significantly increasing the internal temperature and causing the gain in active material and ion diffusion capability to exceed polarization losses. Low-resistance, high-power cell designs are more likely to exceed 1. A closer b is to 0 indicates a significant decrease in battery performance at high-rate charging and discharging, lower lithium-ion intercalation / deintercalation efficiency, and worse overall battery performance.

[0044] The cylindrical battery provided in this application includes a core and a first tabless region 30, which is located at the first end of the core after it is unrolled. The core includes a core hole. The arrangement of the first tabless region 30 can prevent the tabs 20 from blocking the core hole. However, the tabs 20 are structures that bear the current of the negative electrode 10. The arrangement of the first tabless region 30 causes different current densities in different areas of the electrode, resulting in high current density in some areas and low current density in others, which affects the insertion and extraction of lithium ions and thus affects the battery energy density. The ratio of the battery capacity at different rates is also a key measure of the lithium ion insertion and extraction capability. By controlling the relationship between the two, the length of the first tabless region 30 is longer. By controlling the capacity ratio at different rates, lithium ion transport is improved and the battery energy density is increased. The capacity at different rates at a specific temperature refers to the battery's discharge capability at different rates. The smaller the ratio, the weaker the discharge capability at high rates, which affects the battery energy density. The value of a / b cannot be too large, resulting in low battery energy density; the value of a / b cannot be too small, as it will block the core hole. When 'a' is relatively large, the increased impedance necessitates a larger 'b' to achieve improved energy density and fast charging performance. Conversely, a smaller 'a' reduces electrolyte injection efficiency and limits electrolyte wetting ability, requiring a smaller 'b', which significantly degrades the battery's fast charging performance.

[0045] Compared to other ranges, this application, by limiting a / b to the aforementioned specific range, can shorten the length of the electron flow path and suppress current density unevenness while avoiding the core hole being blocked; at the same time, it can improve the charge and discharge performance of cylindrical batteries at high rates and improve the overall performance of cylindrical batteries, such as energy density.

[0046] In a preferred embodiment, 'a' is any value from 0.03 to 0.3. Compared to other ranges, limiting the value of 'a' to the above range is beneficial for improving the uniformity of current density; it also helps to improve the battery's charge-discharge performance at high rates, and enhance the battery's overall performance, such as energy density. Specifically, 'a' can be 0.03, 0.05, 0.07, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18, 0.2, 0.22, 0.24, 0.26, 0.28, or 0.3.

[0047] In a preferred embodiment, b is any value from 0.8 to 1.03. Compared to other ranges, limiting the value of b to the above range is beneficial to improving the uniformity of current density; it also helps to improve the charge-discharge performance of the battery at high rates, and improve the overall performance of the battery, such as energy density. Specifically, b can be 0.8, 0.82, 0.84, 0.86, 0.88, 0.9, 0.92, 0.94, 0.96, 0.98, 1.0, 1.01, 1.02, or 1.03. In order to shorten the length of the electron current path and suppress the unevenness of current density; and at the same time improve the charge-discharge performance of the cylindrical battery at high rates, and improve the overall performance of the cylindrical battery, such as energy density, preferably, 0.08 ≤ a / b ≤ 0.195.

[0048] In order to shorten the length of the electron flow path and suppress the unevenness of current density, while improving the overall performance of the cylindrical battery such as charge and discharge performance at high rates and energy density, more preferably, 0.088≤a / b≤0.178.

[0049] It should be noted that the negative electrode active material layer is disposed on one or both surfaces of the negative electrode current collector. When disposed on one surface, the negative electrode active material layer is disposed on the surface of the negative electrode current collector closest to the separator; when the negative electrode sheet 10 and the negative electrode sheet 10 are wound together (e.g., in a cylindrical battery), the negative electrode active material layer is disposed on both surfaces of the negative electrode current collector.

[0050] A cylindrical battery core typically includes a wound negative electrode 10, a positive electrode, and a separator between the negative electrode 10 and the positive electrode. In a preferred embodiment, the negative electrode 10 includes a stacked negative current collector and a negative active material layer, wherein the negative current collector includes, but is not limited to, copper foil. Compared to other types, using the above-mentioned type of negative current collector is beneficial to improving conductivity, thereby increasing the energy density of the cylindrical battery.

[0051] Silicon-based materials have a significantly higher lithium storage capacity than traditional graphite anode materials. In a preferred embodiment, the anode active material layer comprises a silicon-based material, and 0.04 ≤ a / b ≤ 0.28. Using silicon-based materials as a component of the anode active material layer is beneficial for improving the theoretical capacity of cylindrical batteries. When the anode active material layer comprises silicon-based materials, limiting the a / b ratio within the aforementioned range helps to balance the energy density of the cylindrical battery, allowing the battery to maintain a good energy output level even under high-rate charge-discharge conditions. Specifically, the silicon-based material can be elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys, with one or more of elemental silicon embedded within porous carbon; the shape of the silicon-based material includes one or more of spherical, near-spherical, sheet-like, and linear shapes.

[0052] In a preferred embodiment, the weight percentage of silicon in the negative electrode active material layer is ≥3 wt%, and 0.04 ≤ a / b ≤ 0.23. The weight percentage of silicon in the negative electrode active material layer includes, but is not limited to, the above range. Limiting it to the above range, and simultaneously limiting the a / b ratio to the above range, is beneficial for balancing the energy density of the cylindrical battery, enabling the battery to maintain a good energy output level even under high-rate charge-discharge conditions.

[0053] In a preferred embodiment, the weight percentage of silicon in the negative electrode active material layer is ≤30 wt%. The weight percentage of silicon in the negative electrode active material layer includes, but is not limited to, the above range; limiting it to this range is beneficial for further improving the energy density of the cylindrical battery. Specifically, the weight percentage of silicon in the negative electrode active material layer can be 3 wt%, 5 wt%, 7 wt%, 9 wt%, 11 wt%, 13 wt%, 15 wt%, 17 wt%, 19 wt%, 21 wt%, 23 wt%, 25 wt%, 27 wt%, 29 wt%, 30 wt%, or any two of the above values.

[0054] In a preferred embodiment, the areal density of the negative electrode active material layer is 100–280 g / m³. 2 The areal density of the negative electrode active material layer includes, but is not limited to, the range mentioned above. Limiting it to the range is beneficial for improving lithium-ion transport efficiency, increasing conductivity, and reducing impedance, thereby improving the overall performance of the cylindrical battery, such as energy density.

[0055] In a preferred embodiment, the thickness of the negative electrode active material layer is ≥90 μm, and 0.055 ≤ a / b ≤ 0.26. The thickness of the negative electrode active material layer includes, but is not limited to, the above range. Limiting it to the above range and limiting the a / b ratio to the above range is beneficial to improving conductivity, reducing internal resistance, and thus improving the overall performance of the cylindrical battery, such as energy density.

[0056] To further improve the uniformity of current density, reduce battery internal resistance, suppress battery temperature rise, and further improve the battery's charge and discharge performance at high rates, preferably, a is any value between 0.02 and 0.28.

[0057] To further improve the uniformity of current density, reduce battery internal resistance, suppress battery temperature rise, and further improve the battery's charge and discharge performance at high rates, preferably, a is any value from 0.08 to 0.17; b is any value from 0.87 to 0.98.

[0058] After unwinding the core of the cylindrical battery, the positive electrode sheet and the negative electrode sheet 10 are unfolded along the length direction. The distance between the winding start end and the positive electrode tab or the negative electrode tab is measured. The unfolded length of the positive electrode sheet and the unfolded length of the negative electrode sheet 10 are measured. Finally, the ratio of the length of the tabless region in the positive electrode sheet to the unfolded length of the positive electrode sheet and the ratio of the length of the first tabless region 30 in the negative electrode sheet 10 to the unfolded length of the negative electrode sheet 10 are calculated.

[0059] In this application, the ratio b of the discharge capacity of the cylindrical battery at 25°C and 4C rate to that at 0.33C rate can be adjusted by adjusting the pressure inside the classifier during the preparation of the negative electrode sheet 10 (500-1800Pa); the main frequency of the roller mill or impact mill during powder preparation (25-50Hz); the pressure of the roller during the negative electrode preparation process (6-28T); and the axial extension size of the tab (5-15mm).

[0060] The discharge capacity test at a charging rate of 0.33C includes the following steps: (1) stand at 25℃ for 2 hours to achieve thermal equilibrium; (2) discharge at 0.33C to the cutoff voltage of 2.5V; (3) stand for 30 minutes; (4) charge at 0.33C with constant current to the upper limit voltage, and then charge at constant voltage to the cutoff current of 0.05C; (5) stand for 30 minutes; (6) discharge at 0.33C to the cutoff voltage of 2.5V; (7) repeat steps (3) to (6) for 3 cycles; (8) stand for 30 minutes, charge at 0.33C with constant current to the upper limit voltage, and then charge at constant voltage to the cutoff current of 0.05C; (9) stand for 30 minutes, discharge at 0.33C to the cutoff voltage of 2.5V; stand for 30 minutes; charge at 0.33C for 10 minutes, stand for 30 minutes, discharge at 0.33C to 2.5V, and obtain the discharge capacity at a charging rate of 0.33C, which is recorded as b1.

[0061] Discharge capacity test at 4C charging rate: (1) Let stand at 25℃ for 2 hours to achieve thermal equilibrium; (2) Discharge at 0.33C to cutoff voltage of 2.5V; (3) Let stand for 30 minutes; (4) Charge at 0.33C constant current to the upper limit voltage, and then charge at constant voltage to the cutoff current of 0.05C; (5) Let stand for 30 minutes; (6) Discharge at 0.33C to the cutoff voltage of 2.5V; (7) Repeat steps (3) to (6) for 3 cycles; (8) Let stand for 30 minutes, charge at 0.33C constant current to the upper limit voltage, and then charge at constant voltage to the cutoff current of 0.05C; (9) Let stand for 30 minutes, discharge at 0.33C to the cutoff voltage of 2.5V; let stand for 30 minutes; charge at 0.33C for 10 minutes, let stand for 30 minutes, discharge at 4C to 2.5V, and obtain the discharge capacity at 4C charging rate, which is recorded as b2.

[0062] It should be noted that the upper and lower voltage limits need to be adjusted accordingly for discharge capacity testing of different battery systems: the upper limit voltage for LFP is 3.65V, and the lower limit voltage is 2.5V; the upper limit voltage for NCM is 4.25V, and the lower limit voltage is 2.5V. Calculate b = b2 / b1.

[0063] In a preferred embodiment, the ratio of the length of the tabless region in the positive electrode to the unfolded length of the positive electrode is 0.04 to 0.33. Compared to other ranges, limiting the ratio to the above range is beneficial to improving the overall electrochemical performance of the cylindrical battery, such as its energy density.

[0064] In a preferred embodiment, the cylindrical battery has a discharge capacity of 15–50 Ah at a 4C rate and a discharge capacity of 19–55 Ah at a 0.33C rate. The discharge capacity of the cylindrical battery under the aforementioned specific rate conditions includes, but is not limited to, the ranges described above. Limiting it to these ranges is beneficial for improving the electrochemical performance of the cylindrical battery. Specifically, the discharge capacity of cylindrical batteries under 4C rate conditions can be 15Ah, 16Ah, 17Ah, 18Ah, 19Ah, 20Ah, 25Ah, 30Ah, 35Ah, 40Ah, 45Ah, or 50Ah; the discharge capacity of cylindrical batteries under 0.33C rate conditions can be 19Ah, 20Ah, 21Ah, 22Ah, 23Ah, 24Ah, 25Ah, 30Ah, 35Ah, 40Ah, 45Ah, 50Ah, 51Ah, 52Ah, 53Ah, 54Ah, or 55Ah.

[0065] In a preferred embodiment, the negative electrode 10 has a porosity of 35-60% and a compaction density of 1.2-1.7 g / cm³. 3The porosity and compaction density of the negative electrode 10 include, but are not limited to, the ranges mentioned above. Limiting them to the ranges is beneficial for improving lithium-ion transport efficiency, increasing conductivity, reducing impedance, and thus improving the overall performance of the cylindrical battery, such as energy density.

[0066] In a preferred embodiment, the positive electrode sheet includes a positive current collector and a positive active material layer stacked together. The positive current collector includes, but is not limited to, aluminum foil. Compared to other types, using the above-mentioned type of positive current collector is beneficial for improving conductivity, while also providing suitable strength and flexibility for the positive electrode sheet, facilitating winding.

[0067] It should be noted that the positive electrode active material layer is disposed on one or both surfaces of the positive electrode current collector. When disposed on one surface, the positive electrode active material layer is disposed on the surface of the positive electrode current collector closest to the separator; when the positive electrode sheet and the positive electrode sheet are wound together (e.g., in a cylindrical battery), the positive electrode active material layer is disposed on both surfaces of the positive electrode current collector.

[0068] The a / b ratio varies depending on the cathode material. In a preferred embodiment, the cathode active material layer comprises a lithium nickel cobalt manganese oxide ternary cathode material, and the ratio of the length of the tabless region in the cathode sheet to the unfolded length of the cathode sheet is 0.08 to 0.33; or, the cathode active material layer comprises lithium iron phosphate, and the ratio of the length of the tabless region in the cathode sheet to the unfolded length of the cathode sheet is 0.12 to 0.33. When the material in the cathode active material layer is a lithium nickel cobalt manganese oxide ternary cathode material or lithium iron phosphate, the ratio of the length of the tabless region in the cathode sheet to the unfolded length of the cathode sheet includes, but is not limited to, the above range. Limiting it within the above range is beneficial for shortening the length of the electron flow path while avoiding the core hole being blocked, suppressing the unevenness of current density; at the same time, it improves the charge and discharge performance of the battery at high rates, and improves the overall performance of the battery, such as energy density.

[0069] In a preferred embodiment, the positive electrode active material layer comprises a lithium nickel cobalt manganese oxide ternary cathode material, wherein the Dv50 of the lithium nickel cobalt manganese oxide ternary cathode material is 2–4 μm. The Dv50 of the lithium nickel cobalt manganese oxide ternary cathode material includes, but is not limited to, the above-mentioned range. Limiting it to this range is beneficial for promoting lithium-ion insertion / extraction and for increasing the material's compaction density, thereby improving the energy density of the cylindrical battery. Specifically, the Dv50 of the lithium nickel cobalt manganese oxide ternary cathode material can be 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, or any two of the above values.

[0070] In a preferred embodiment, the positive electrode active material layer comprises lithium iron phosphate, and the Dv50 of lithium iron phosphate is 0.4–2.0 μm. The Dv50 of lithium iron phosphate includes, but is not limited to, the above range. Limiting it to this range is beneficial for promoting lithium-ion insertion / extraction and for increasing the compaction density of the material, thereby improving the energy density of the cylindrical battery. Specifically, the Dv50 of lithium iron phosphate can be 0.4 μm, 0.8 μm, 1.0 μm, 1.2 μm, 1.4 μm, 1.6 μm, 2.0 μm, or any two of the above values.

[0071] In a preferred embodiment, the positive electrode active material layer comprises a lithium nickel cobalt manganese oxide ternary positive electrode material, the porosity of the positive electrode sheet is 12-35%, and the compaction density is 3.45-3.65 g / cm³. 3 Alternatively, the positive electrode active material layer may be made of lithium iron phosphate, and the porosity of the positive electrode sheet may be 12–35%, with a compaction density of 2.1–2.7 g / cm³. 3 For different types of positive electrode active materials, the porosity and compaction density of the positive electrode sheet are independently within the ranges mentioned above. Limiting them to the above ranges is beneficial to improving lithium-ion transport efficiency, thereby improving the overall performance of cylindrical batteries, such as energy density.

[0072] In a preferred embodiment, the thickness of the positive electrode active material layer is 100–140 μm, and the thickness of the positive electrode current collector is 11–13 μm. The areal density of the positive electrode active material layer includes, but is not limited to, the above range. Limiting it to the above range is beneficial to improving lithium-ion transport efficiency, thereby improving the overall performance of the cylindrical battery, such as energy density.

[0073] In a preferred embodiment, along the length of the unfolded negative electrode 10, each negative electrode 10 has multiple tabs 20 on one side. The width of the connection between each tab 20 and the negative electrode 10 is 2–10 mm, and / or the lead-out dimension of each tab 20 is 2–15 mm. Compared to a single tab 20, the arrangement of multiple tabs 20 is beneficial for improving the electron conduction path and reducing the local current density, thereby helping to reduce heat generation and improve the safety and energy density of the cylindrical battery.

[0074] In a preferred embodiment, such as Figure 1As shown, each negative electrode 10, when unfolded, includes at least one second tabless region 40 between multiple tabs 20 on one side along its length. The ratio of the sum of the lengths of the second tabless region 40 and the first tabless region 30 to the unfolded length of the negative electrode 10 is 0.05 to 0.6. The arrangement of the second tabless region 40 helps to avoid direct contact between the multiple tabs 20, reducing the risk of short circuits. Simultaneously, it helps to further optimize the current distribution within the negative electrode 10 and the battery, improving lithium-ion transport efficiency and thus enhancing the overall performance of the cylindrical battery, enabling it to achieve both high energy density and high rate performance.

[0075] In a preferred embodiment, multiple negative electrode tabs are provided along the length of the unfolded negative electrode sheet 10, and multiple positive electrode tabs are provided along the length of the unfolded positive electrode sheet. The positive and negative electrode tabs are located at the same end of the core edge. Compared to a single tab 20, the arrangement of multiple tabs 20 is beneficial to improving the electron conduction path and reducing the local current density, thereby helping to reduce heat generation and improve the safety and energy density of the cylindrical battery.

[0076] In a preferred embodiment, the winding core includes a winding core hole with a diameter of 6-8 mm. The diameter of the winding core hole includes, but is not limited to, the above range. Limiting it to the above range is beneficial for the dissipation of heat inside the cylindrical battery, for the discharge of gas generated during the cycling process of the cylindrical battery, and for reducing internal pressure, thereby improving the cycle stability and safety of the cylindrical battery.

[0077] The electrolyte acts as a conductor of ions between the positive and negative electrodes. In a preferred embodiment, the core further includes an electrolyte comprising a lithium salt, including but not limited to one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI); and a solvent including but not limited to one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The types of lithium salts and solvents in the electrolyte are not limited to those described above. Limiting them to these ranges is beneficial for improving conductivity and promoting the formation of the SEI film, thereby improving the energy density and rate performance of the cylindrical battery.

[0078] To further improve conductivity and increase the energy density of cylindrical batteries, preferably, the molar concentration of lithium salt in the electrolyte is 0.6–1.6 mol / L.

[0079] In a preferred embodiment, the diaphragm includes, but is not limited to, one of polypropylene (PP), polyethylene (PE), and PP / PF; the diaphragm may also be a structure in which a coating is provided on the surface of a base membrane, wherein the base membrane coating includes, but is not limited to, one of PP, PE, and PP / PF, and the coating is an inorganic coating and / or an organic coating. The inorganic coating includes, but is not limited to, one or more of alumina, silicon oxide, titanium oxide, magnesium oxide, zirconium oxide, and boehmite, and the organic coating includes, but is not limited to, one or more of polyvinylidene fluoride (PVDF) and aramid.

[0080] Another aspect of this application provides a method for preparing a cylindrical battery, the method comprising: step S1, preparing a negative electrode sheet 10 with tabs 20 and a separator; step S2, alternately stacking and winding the negative electrode sheet 10 and the separator to obtain a bare cell; step S3, placing the bare cell in an outer packaging shell, drying it, and then injecting electrolyte to obtain a cylindrical battery; wherein, a tab 20 is provided on one side of the unfolded length direction of each negative electrode sheet 10, and the area between the tab 20 and the winding start end is a first tabless region 30, the ratio of the length of the first tabless region 30 to the unfolded length of the negative electrode sheet 10 is a, and the discharge capacity of the cylindrical battery under 4C rate and 0.33C rate conditions at 25°C is measured respectively, the ratio of the two is b, and a and b have the same definition as in the preceding text.

[0081] The method for preparing the cylindrical battery provided in this application, by limiting a / b within the aforementioned specific range, can shorten the length of the electron flow path and suppress the unevenness of current density while avoiding the blockage of the core hole; at the same time, it can improve the charge and discharge performance of the cylindrical battery at high rates and improve the overall performance of the cylindrical battery, such as energy density.

[0082] Moreover, the above-mentioned cylindrical battery preparation method ensures the stability of the internal structure of the battery and the smooth flow of lithium-ion channels by controlling the stacking or winding of the positive electrode, negative electrode 10 and separator, which can improve the lithium-ion transport efficiency; the electrolyte injection in a dry environment avoids side reactions caused by moisture, enhances the quality of SEI film formation, and ensures the electrochemical performance and cycle life of the cylindrical battery.

[0083] In a preferred embodiment, the method for preparing the positive electrode sheet includes: mixing a positive electrode active material, a positive electrode conductive agent, a positive electrode binder, and a first solvent to obtain a positive electrode slurry; coating the positive electrode slurry onto both sides of a positive electrode current collector; drying, and then cold pressing and slitting to obtain the positive electrode sheet. This preparation method, through the uniform mixing and double-sided coating of the positive electrode active material, combined with the subsequent cold pressing treatment, effectively improves the density of the positive electrode sheet and the utilization rate of the positive electrode active material, and has a direct promoting effect on the improvement of cylindrical battery performance.

[0084] To improve the dispersibility of the positive electrode active material and the coatability of the positive electrode slurry, preferably, the positive electrode slurry comprises, by weight percentage, 94.5–98.5 wt% of the positive electrode active material, 1.3–2.2 wt% of the positive electrode binder, 0.5–1.5 wt% of the positive electrode conductive agent, and 0.05–2 wt% of the first solvent.

[0085] This application does not impose any particular restrictions on the type of positive electrode active material for the positive electrode sheet. As an example, the positive electrode active materials in this application include binary positive electrode materials such as lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), and lithium nickel oxide (LiNiO2), or ternary positive electrode materials such as lithium nickel cobalt manganese oxide.

[0086] In this application, the positive electrode binder is used to improve the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. This application does not have any particular restrictions on the type of positive electrode binder for the positive electrode sheet; the positive electrode binder can be a conventional choice in the battery field. Specifically, the positive electrode binder can be at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyacrylonitrile (PAN), polyimide (PI), polyacrylic acid (PAA), polyacrylate, polyolefin, sodium carboxymethyl cellulose (CMC), or sodium alginate.

[0087] Positive conductive agents include, but are not limited to, at least one of superconducting carbon (SP), acetylene black, carbon black, Ketjen black, nanotubes (CNT), graphene, and carbon nanofibers.

[0088] The first solvent includes, but is not limited to, N-methylpyrrolidone (NMP).

[0089] In a preferred embodiment, the method for preparing the negative electrode sheet 10 includes: mixing a negative electrode active material, a negative electrode conductive agent, a negative electrode binder, and a second solvent to obtain a negative electrode slurry; coating the negative electrode slurry onto both sides of a negative electrode current collector; drying the slurry; and then rolling and cutting it to obtain the negative electrode sheet 10. This preparation method, through uniform mixing and double-sided coating, combined with rolling technology, ensures the loading of the negative electrode active material on the surface of the negative electrode current collector, which significantly contributes to improving the overall performance of the cylindrical battery.

[0090] To improve the dispersibility of the negative electrode active material and the coatability of the negative electrode slurry, preferably, the negative electrode slurry comprises, by weight percentage, 95-96.5 wt% of the negative electrode active material, 0.6-1.1 wt% of the negative electrode conductive agent, and 2.8-5 wt% of the negative electrode binder.

[0091] In a preferred embodiment, the negative electrode active material includes, but is not limited to, silicon-carbon (SiC), natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon, soft carbon, silicon, SiOx, and Li4Ti5O. 12 One or more of the following are acceptable: The negative electrode conductive agent includes, but is not limited to, one or more of superconducting carbon (SP), acetylene black, carbon black, Ketjen black, carbon nanotubes, conductive graphite, and graphene; the negative electrode binder includes, but is not limited to, one or more of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, and tetrafluoroethylene-hexafluoropropylene copolymer. Using the above-mentioned types of negative electrode active materials is beneficial for improving the energy density of cylindrical batteries, and also for reducing volume expansion and contraction during charging and discharging. Using the above-mentioned types of negative electrode conductive agents is beneficial for improving conductivity, thereby improving the energy density of cylindrical batteries. Using the above-mentioned types of negative electrode binders is beneficial for improving the bonding force between the negative electrode active material layer and the negative electrode current collector, reducing the peeling of the negative electrode active material, and thus reducing self-discharge.

[0092] The preparation method of the silicon-carbon composite material in this application includes the following steps: porous carbon material is used as the carbon matrix, sieved, and then added to a rotary kiln. Nitrogen gas is introduced to remove oxygen at a flow rate of 10–20 L / min. The calcination heating rate is 5–10 °C / min, the temperature is 480–540 °C, and the rotary kiln rotation speed is 0.5–3 rpm. While maintaining the calcination temperature, a mixed gas is introduced. The mixed gas includes nitrogen and silane in a volume ratio of 1:(1–4), and the flow rate of the mixed gas is 0.2–0.6 L / min. The gas flow time is 50–170 min; after the reaction is complete, the silane gas is turned off and only nitrogen gas is introduced. The silicon-carbon composite material is calcined in a nitrogen atmosphere at a temperature of 550–600℃ for 60–180 min. When the temperature fluctuation gradually stabilizes, acetylene gas is introduced to carry out the reaction. The acetylene gas flow rate is set to 1–3 L / min. The deposition temperature is 500–600℃ and the deposition time is 10–18 h. After the reaction is complete, the gas is turned off and the material is allowed to cool naturally in a nitrogen atmosphere. After the temperature has completely cooled, the material is demagnetized to obtain the silicon-carbon composite material.

[0093] Before the above step of "adding it to the rotary kiln and purging with nitrogen to remove oxygen", sieving is performed first. In this application, sieving can be carried out by an air classifier. During the sieving process, the pressure inside the classifier is controlled within the range of 500 to 1800 Pa. The higher the pressure, the larger b is.

[0094] The preparation method of the negative electrode active material (graphite) in this application includes the following steps: (1) Powdering: Petroleum coke, needle coke or pitch coke is crushed to the set specifications through coarse crushing, fine crushing, spheroidizing and grading processes. After testing and meeting the process data standards, it can be transferred to the next process; Powder is obtained by roller mill or impact mill, wherein the powder specifications are adjusted by adjusting the main frequency, internal grading frequency, induced draft frequency and feeding frequency; the main frequency is 25-50Hz; the internal grading frequency is 30-70Hz; the induced draft frequency is 30-50Hz; the feeding frequency is 10-30Hz; (2) Mixing: The auxiliary material pitch is mixed with the powder to obtain the first mixture; wherein the amount of pitch added is 1-15%, the mixing speed is 30-60rpm, and the time is 30-50min; (3) Granulation: The above first mixture is transferred to a high temperature furnace for high temperature re-granulation. Combined, the target specifications of the material are obtained by adjusting the temperature of the granulation equipment and the speed of the main machine; preferably, the temperature in this process is 500-700℃; the speed of the main machine is 25-50Hz; (4) Graphitization: the above material is filled into a graphite crucible and transferred to a graphitization furnace for graphitization; control the power supply, furnace exit time and temperature (≤400℃); in this process, carbon atoms rearrange into a three-dimensional ordered graphite crystal structure at high temperature; (5) Modification (coating): the auxiliary material asphalt is mixed with the grinding powder to obtain a second mixture, which is then loaded into a carbonization crucible; preferably, the amount of asphalt added is 1-15%, the speed is 30-60rpm, and the time is 30-50min; (6) Carbonization: the asphalt is carbonized and coated on the surface of the graphite particles; the carbonization time is controlled to be 15-22h and the temperature is 1000-1300℃, and the flow rate of inert gas (such as nitrogen) is 50-80m 3 / h; (7) Finished product mixing: Single particles and secondary particles are mixed in proportion, and then screened, demagnetized, sieved and tested in sequence, and finally packaged, weighed and shipped; During this process, the frequency of the mixer is controlled at 10-30Hz, the magnetic field strength is ≥3000GS, and the mesh size of the sieve is 200-400 mesh. By adjusting the frequency of the main machine of the powder making, the higher the main machine frequency range is within 25-50Hz, the larger b is.

[0095] Vacuum sealing eliminates residual air inside the bare cell, reducing oxidation side reactions; standing allows for more thorough wetting of the active material, stabilizing the cell structure; the formation process promotes the formation of the SEI film, thus protecting the negative electrode; and the shaping process facilitates subsequent assembly and improves space utilization, thereby enhancing the overall performance of the cylindrical battery. In a preferred embodiment, step S3, after electrolyte injection, further includes sequential vacuum sealing, standing, formation, and shaping processes to obtain a cylindrical battery.

[0096] In this application, the tabs 20 in the negative electrode sheet 10 can be connected to the current collector by welding or by slitting, ensuring that the area on the current collector surface that serves as the tab region is not coated before slitting. In a preferred embodiment, step S1 includes welding the positive electrode tab to one side of the unfolded length direction of the positive electrode sheet, and welding the negative electrode tab to one side of the unfolded length direction of the negative electrode sheet 10, thereby obtaining a negative electrode sheet 10 with tabs 20. During welding, the ratio of the length of the first tabless region 30 to the unfolded length of the negative electrode sheet 10 is controlled as 'a', thereby obtaining the desired negative electrode sheet 10 with tabs 20. In another preferred embodiment, step S1 includes protecting the tab region when coating the positive current collector with positive electrode slurry, or protecting the tab region when coating the negative current collector with negative electrode slurry, to ensure that the material of the tab region is only the positive or negative current collector.

[0097] In another aspect, this application provides an electrical device that includes the cylindrical battery described above. The cylindrical battery provided by this application possesses advantages such as high energy density, low self-discharge rate, and high safety performance. Applying this cylindrical battery to electrical devices (such as electric vehicles, electronic communication equipment, computers, etc.) can improve their overall performance and market competitiveness.

[0098] It should be noted that the test methods for various performance aspects in this application are as follows:

[0099] (1) Discharge energy density of cylindrical batteries:

[0100] A higher discharge energy density indicates that a cylindrical battery can store more energy for the same mass, which is an important indicator for evaluating battery storage capacity.

[0101] The specific test method is as follows: Weigh the battery and record the weight as m; place the battery in the fixture, apply a force of 3000N, charge it to the upper limit voltage with a constant current of 0.33C, let it rest for 30 minutes, discharge it to the lower limit voltage with a constant current of 0.33C, let it rest for 30 minutes, and repeat the cycle 3 times; obtain the discharge capacity (in Ah) and energy E (average of three cycles), and calculate the discharge energy density using the following formula: Discharge energy density = E / m (in Wh / kg).

[0102] For different systems, the upper and lower limit voltages need to be adjusted accordingly: the upper limit voltage for LFP is 3.65V and the lower limit voltage is 2.5V; the upper limit voltage for NCM is 4.25V and the lower limit voltage is 2.5V.

[0103] (2) Electrolyte filling efficiency of cylindrical batteries: In an environment of 25±1℃, dew point ≤-45℃, oxygen ≤10ppm (glove box / low humidity workshop), cylindrical bare cells (unformed, unsealed) were used as test samples, with ≥5 parallel samples in each group. They were vacuum dried at 85℃ for 24h to remove residual moisture, cooled and weighed: M0 (empty shell + electrode group weight), -96±0.2kPa, pressure held for 30s (air removal from electrode group) pre-vacuum, electrolyte filling for 20min, isobaric immersion at 50kPa and 45℃: pressure held for 10min, free liquid was removed by secondary vacuum, and after standing for 1min, the filling port was wiped clean and weighed immediately M2. The electrolyte filling efficiency was calculated using the following formula: electrolyte filling efficiency = (M2-M0) / [total pore volume of electrode group × electrolyte density].

[0104] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0105] Example 1

[0106] (1) Preparation of the positive electrode:

[0107] LiNi, a positive electrode active material with a Dv50 of 3 μm, was mixed at a mass ratio of 98:0.9:1.1. 0.92 Co 0.06 Mn 0.02 O2 is mixed with acetylene black (positive electrode conductive agent) and polyvinylidene fluoride (PVDF) (positive electrode binder), and N-methylpyrrolidone (NMP) (solvent) is added to obtain a mixed system. The mixed system is stirred until homogeneous to obtain a positive electrode slurry; the solid content of the positive electrode slurry is 98.5 wt%.

[0108] The above-mentioned positive electrode slurry was uniformly coated on both sides of an aluminum foil with a thickness of 12 μm, and the coating amount of the positive electrode slurry was 405 g / m. 2 After being air-dried at room temperature, the material is transferred to an oven for further drying, and then subjected to cold pressing and slitting to obtain a positive electrode sheet. This positive electrode sheet comprises stacked aluminum foil and a layer of positive electrode active material. The porosity of this positive electrode sheet is 15%, and its compaction density is 3.55 g / cm³. 3 The thickness of the positive electrode active material layer is 116 μm; the ratio 'a' of the length of the tabless region to the unfolded length of the positive electrode sheet is 0.1.

[0109] (2) Preparation of negative electrode 10:

[0110] (2.1) Preparation of graphite:

[0111] (1) Powdering: The asphalt coke is crushed to the set specifications through coarse crushing, fine crushing, spheroidizing and grading processes. After testing and meeting the process data standards, it can be transferred to the next process. The powder is obtained by roller mill, wherein the main frequency is 40Hz; the internal grading frequency is 50Hz; the induced draft frequency is 40Hz; and the feeding frequency is 20Hz. (2) Mixing: The auxiliary material asphalt is mixed with the powder to obtain the first mixture. The amount of asphalt added is 8%, the mixing speed is 45rpm, and the time is 40min. (3) Granulation: The first mixture is transferred to a high-temperature furnace for high-temperature compounding. The medium temperature is 600℃; the main machine speed is 40Hz; (4) Graphitization: The above materials are filled into a graphite crucible and transferred to a graphitization furnace for graphitization; control the power supply, furnace exit time and temperature (≤400℃); during this process, carbon atoms rearrange into a three-dimensional ordered graphite crystal structure at high temperature; (5) Modification (coating): The auxiliary material asphalt is mixed with the grinding powder to obtain a second mixture, which is then loaded into a carbonization crucible; the amount of asphalt added is 10%, the speed is 50rpm, and the time is 40min; (6) Carbonization: Carbonization is carried out at 1200℃ for 18h, and the nitrogen flow rate is controlled at 65m 3 / h, carbonize the asphalt and coat it on the surface of the graphite particles; (7) Finished product mixing: single particles and secondary particles are mixed in proportion, and then screened, demagnetized, sieved and tested in sequence, and finally packaged, weighed and shipped; during this process, the mixer frequency is controlled at 20Hz, the magnetic field strength is ≥3000GS, and the screen mesh is 300 mesh.

[0112] (2.2) Preparation of silicon-carbon composite materials:

[0113] Porous carbon material was used as the carbon matrix and sieved using an air classifier. During sieving, the pressure inside the classifier was controlled at 896 Pa. The material was then added to a rotary kiln, with nitrogen gas introduced to purge oxygen at a flow rate of 15 L / min. The calcination heating rate was 8 °C / min, the temperature was 500 °C, and the rotary kiln rotation speed was 2 rpm. While maintaining a constant calcination temperature, a mixed gas consisting of nitrogen and silane in a 1:4 volume ratio was introduced at a flow rate of 0.4 L / min for 100 min. After the reaction was complete, the silane gas was shut off, and only nitrogen gas was introduced. The silicon-carbon composite material was calcined in a nitrogen atmosphere at 580 °C for 120 min. When the temperature fluctuation gradually stabilized, acetylene gas was introduced for the reaction at a flow rate of 2 L / min. The deposition temperature was 550 °C, and the deposition time was 14 h. After the reaction was complete, the gas was shut off, and the material was allowed to cool naturally in a nitrogen atmosphere. After complete cooling, the material was demagnetized to obtain the silicon-carbon composite material.

[0114] (2.3) Preparation of negative electrode slurry:

[0115] Graphite, silicon-carbon composite material, single-walled carbon nanotubes (SWCNTs), superconducting carbon (SP), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) binder were mixed in a mass ratio of 92.4:4:0.05:0.95:1:1.6. Deionized water was added and the mixture was stirred until it became homogeneous to obtain the negative electrode slurry. The solid content of the negative electrode slurry was 58 wt%.

[0116] (2.4) Preparation of negative electrode 10:

[0117] The aforementioned negative electrode slurry is coated on both sides of a 6μm thick copper foil, and then sequentially rolled and slit at 21.3T to obtain a negative electrode sheet 10. Tabs 20 are welded onto the negative electrode sheet 10, and the length of the tabs 20 and their welding positions on the negative electrode sheet 10 are controlled so that the ratio 'a' of the length of the first tabless region 30 to the unfolded length of the negative electrode sheet 10 is 0.1; the ratio of the length of the second tabless region 40 to the unfolded length of the negative electrode sheet 10 is also 0.1. The negative electrode sheet 10 comprises stacked copper foil and a negative electrode active material layer, wherein the silicon content in the negative electrode active material layer is 5wt%; the porosity of the negative electrode sheet 10 is 38%, and the compaction density is 1.5g / cm³. 3 The areal density of the negative electrode active material layer is 160 g / m³. 2 The thickness of the negative electrode active material layer is 112.7 μm.

[0118] (3) Preparation of electrolyte:

[0119] EC, EMC and DEC were mixed in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, fully dried LiPF6 was dissolved in the above mixed solvent to prepare an electrolyte with a molar concentration of 1 mol / L.

[0120] (4) Preparation of the diaphragm:

[0121] A polyethylene film base with a thickness of 8 μm is selected, and a ceramic layer with a thickness of 3 μm is coated on both sides of the base film as a separator for later use;

[0122] (5) Preparation of cylindrical batteries:

[0123] The positive electrode sheet obtained in step (1), the separator prepared in step (4), and the negative electrode sheet 10 obtained in step (2) are stacked sequentially, with the positive electrode tab and the negative electrode tab located at the same end of the winding core, and the separator placed between the positive electrode sheet and the negative electrode sheet 10. Then, the electrode is wound to obtain a bare battery cell. During the winding process, the winding tension of the electrode sheet is 800g and the winding tension of the separator is 250g.

[0124] The bare cell was placed in the outer packaging shell, dried, and then injected with the electrolyte prepared in step (3). The cell was then subjected to vacuum sealing, settling, formation, volume adjustment, and shaping processes to obtain a cylindrical battery.

[0125] The formation process is as follows: After resting at 25°C for 24 hours, the glass is placed in a glass fixture with a pressure of 0.5 MPa; it is left to stand for 10 minutes; then charged at a rate of 0.02C to the cutoff voltage of 3.2V; it is left to stand for 10 minutes, then charged at a rate of 0.05C to the cutoff voltage of 3.4V; it is left to stand for 10 minutes; then charged at a rate of 0.08C to the cutoff voltage of 3.75V; after resting at 25°C for 24 hours, the glass is placed in a glass fixture with a pressure of 0.5 MPa; it is left to stand for 10 minutes; then charged at a rate of 0.02C to the cutoff voltage of 3.2V; it is left to stand for 10 minutes, then charged at a rate of 0.05C to the cutoff voltage of 3.4V; it is left to stand for 10 minutes, then charged at a rate of 0.08C to the cutoff voltage of 3.75V, thus completing the formation process.

[0126] The converted battery should be calibrated according to the following steps:

[0127] 1) Let the battery rest for 10 minutes; 2) Charge the battery with a constant current (0.33C) to the upper voltage limit of 4.25V, and then charge the battery with a constant voltage of 4.25V until the cutoff current is less than or equal to 0.05C; 3) Let the battery rest for 10 minutes; 4) Discharge the battery with a constant current (0.33C) to the lower voltage limit of 2.5V; 5) Repeat steps 2) to 4) three times; 6) Use the discharge capacity of the third discharge as the fixed capacity.

[0128] The cylindrical battery has a bottom diameter of 46 mm and a height of 95 mm; the diameter of the winding hole is 6 mm; and the axial extension dimension of the tab 20 is 11.7 mm. The measured discharge capacity of this cylindrical battery at 25℃ under 4C rate is 51.5 Ah, and the discharge capacity at 0.33C rate is 59.1 Ah, with a ratio b of 0.87.

[0129] Example 2

[0130] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.17 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1517 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 10.8 T, and the axial extension dimension of the tab 20 is 7.7 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 49.5 Ah and the discharge capacity at 0.33C rate is 50.6 Ah. The remaining steps are the same as in Example 1.

[0131] Example 3

[0132] The difference from Example 1 is that: in step (2), the ratio of the length of the first tabless region 30 in the negative electrode sheet to the unfolded length of the negative electrode sheet 10 is 0.08; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1122 Pa, the pressure of the roller pressing during the preparation of the negative electrode sheet 10 is 17.5 T, and the axial extension dimension of the tab 20 is 9.3 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 52.8 Ah and the discharge capacity at 0.33C rate is 58.0 Ah. The remaining steps are the same as in Example 1.

[0133] Example 4

[0134] The difference from Example 1 is that: in step (2), the ratio of the length of the first tabless region 30 in the negative electrode sheet to the unfolded length of the negative electrode sheet 10 is 0.16; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1065 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 18.4 T, and the axial extension dimension of the tab 20 is 10.1 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 49.4 Ah and the discharge capacity at 0.33C rate is 54.9 Ah. The remaining steps are the same as in Example 1.

[0135] Example 5

[0136] The difference from Example 1 is that in step (1), LiNi is used. 0.63 Co 0.07 Mn 0.3 O2 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.12 to the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1348 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 13.7 T, and the axial extension dimension of the tab 20 is 8.5 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 23.5 Ah and the discharge capacity at 0.33C rate is 24.7 Ah. The remaining steps are the same as in Example 1.

[0137] Example 6

[0138] The difference from Example 1 is as follows: in step (1), LiFePO4 is used as the positive electrode active material; in step (2), graphite is used as the negative electrode active material; in step (2), the ratio of the length of the first tabless region 30 in the negative electrode sheet to the unfolded length of the negative electrode sheet is 0.14; in step (2), the host frequency during graphite preparation is 35Hz, the rolling pressure during negative electrode sheet 10 preparation is 19.4T, and the axial extension dimension of the tab 20 is 10.9mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 16.8Ah, and the discharge capacity at 0.33C rate is 18.9Ah. The remaining steps are the same as in Example 1.

[0139] Example 7

[0140] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.19 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 531 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 28.1 T, and the axial extension dimension of the tab 20 is 14.7 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 48.3 Ah, and the discharge capacity at 0.33C rate is 60.3 Ah. The remaining steps are the same as in Example 1.

[0141] Example 8

[0142] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.18 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1703 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 7.1 T, and the axial extension dimension of the tab 20 is 5.6 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 48.4 Ah and the discharge capacity at 0.33C rate is 47.5 Ah. The remaining steps are the same as in Example 1.

[0143] Example 9

[0144] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.075 to the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 547 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 27.1 T, and the axial extension dimension of the tab 20 is 14.6 mm, so that the discharge capacity of the cylindrical battery at 4C rate in an environment of 25°C is 48.9 Ah and the discharge capacity at 0.33C rate is 60.4 Ah. The remaining steps are the same as in Example 1.

[0145] Example 10

[0146] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.081 to the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1557 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 11.6 T, and the axial extension dimension of the tab 20 is 7.4 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 44.7 Ah and the discharge capacity at 0.33C rate is 45.7 Ah. The remaining steps are the same as in Example 1.

[0147] Example 11

[0148] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.169 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 952 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 20.3 T, and the axial extension dimension of the tab 20 is 11.7 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 45.5 Ah and the discharge capacity at 0.33C rate is 52.2 Ah. The remaining steps are the same as in Example 1.

[0149] Example 12

[0150] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.03 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 529 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 27.5 T, and the axial extension dimension of the tab 20 is 14.9 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 34.2 Ah and the discharge capacity at 0.33C rate is 42.7 Ah. The remaining steps are the same as in Example 1.

[0151] Example 13

[0152] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.033 to the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1621 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 8.5 T, and the axial extension dimension of the tab 20 is 7.3 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 39.2 Ah, and the discharge capacity at 0.33C rate is 39.2 Ah. The remaining steps are the same as in Example 1.

[0153] Example 14

[0154] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.3 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1744 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 6.1 T, and the axial extension dimension of the tab 20 is 5.5 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 31.9 Ah and the discharge capacity at 0.33C rate is 31.0 Ah. The remaining steps are the same as in Example 1.

[0155] Example 15

[0156] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.28 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1631 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 8.9 T, and the axial extension dimension of the tab 20 is 7.1 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 41.2 Ah, and the discharge capacity at 0.33C rate is 41.2 Ah. The remaining steps are the same as in Example 1.

[0157] Example 16

[0158] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.29 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 783 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 23.2 T, and the axial extension dimension of the tab 20 is 13.3 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 28.5 Ah and the discharge capacity at 0.33C rate is 33.5 Ah. The remaining steps are the same as in Example 1.

[0159] Example 17

[0160] The difference from Example 1 is that in step (1), LiNi is used. 0.63 Co 0.07 Mn 0.3O2 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.034 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1761 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 6.6 T, and the axial extension dimension of the tab 20 is 5.0 mm, so that the discharge capacity of the cylindrical battery at 4C rate in an environment of 25℃ is 23.2 Ah, and the discharge capacity at 0.33C rate is 22.6 Ah. The remaining steps are the same as in Example 1.

[0161] Example 18

[0162] The difference from Example 1 is that in step (1), LiNi is used. 0.63 Co 0.07 Mn 0.3 O2 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.273 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 497 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 27.9 T, and the axial extension dimension of the tab 20 is 15.0 mm, so that the discharge capacity of the cylindrical battery at 4C rate in an environment of 25℃ is 20.3 Ah, and the discharge capacity at 0.33C rate is 25.3 Ah. The remaining steps are the same as in Example 1.

[0163] Example 19

[0164] The difference from Example 1 is as follows: In step (1), LiFePO4 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.033 of the unfolded length of the negative electrode sheet 10; in step (2), the host frequency during graphite preparation is 48Hz, the rolling pressure during negative electrode sheet 10 preparation is 7.9T, and the axial extension dimension of the tab 20 is 6.1mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 16.2Ah, and the discharge capacity at 0.33C rate is 16.0Ah. The remaining steps are the same as in Example 1.

[0165] Example 20

[0166] The difference from Example 1 is as follows: In step (1), LiFePO4 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.283 times the unfolded length of the negative electrode sheet 10; in step (2), the host frequency during graphite preparation is 29Hz, the rolling pressure during negative electrode sheet 10 preparation is 25.3T, and the axial extension dimension of the tab 20 is 14.1mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 15Ah, and the discharge capacity at 0.33C rate is 18.1Ah. The remaining steps are the same as in Example 1.

[0167] Example 21

[0168] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.24 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1653 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 9.2 T, and the axial extension dimension of the tab 20 is 6.9 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 43 Ah, and the discharge capacity at 0.33C rate is 43 Ah. The remaining steps are the same as in Example 1.

[0169] Example 22

[0170] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.18 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 839 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 22.3 T, and the axial extension dimension of the tab 20 is 12.5 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 44 Ah, and the discharge capacity at 0.33C rate is 51.2 Ah. The remaining steps are the same as in Example 1.

[0171] Example 23

[0172] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.26 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 671 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 25.1 T, and the axial extension dimension of the tab 20 is 14.3 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 29.6 Ah, and the discharge capacity at 0.33C rate is 35.7 Ah. The remaining steps are the same as in Example 1.

[0173] Example 24

[0174] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.025 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 501 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 26.3 T, and the axial extension dimension of the tab 20 is 15.9 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 26.1 Ah, and the discharge capacity at 0.33C rate is 35.8 Ah. The remaining steps are the same as in Example 1.

[0175] Example 25

[0176] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.35 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1817 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 5.7 T, and the axial extension dimension of the tab 20 is 4.9 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 24 Ah, and the discharge capacity at 0.33C rate is 23.1 Ah. The remaining steps are the same as in Example 1.

[0177] Comparative Example 1

[0178] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.03 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1772 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 6.9 T, and the axial extension dimension of the tab 20 is 5.3 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 22.4 Ah, and the discharge capacity at 0.33C rate is 21.8 Ah. The remaining steps are the same as in Example 1.

[0179] Comparative Example 2

[0180] The difference from Example 1 is that: in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.33 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 488 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 28.7 T, and the axial extension dimension of the tab 20 is 15.3 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 18.5 Ah and the discharge capacity at 0.33C rate is 23.7 Ah. The remaining steps are the same as in Example 1.

[0181] Comparative Example 3

[0182] The difference from Example 1 is that in step (1), LiNi is used. 0.63 Co 0.07 Mn 0.3 O2 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.023 to the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 1835 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 5.8 T, and the axial extension dimension of the tab 20 is 4.7 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 17.1 Ah and the discharge capacity at 0.33C rate is 16.3 Ah. The remaining steps are the same as in Example 1.

[0183] Comparative Example 4

[0184] The difference from Example 1 is that in step (1), LiNi is used. 0.63 Co 0.07 Mn 0.3 O2 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.31 times the unfolded length of the negative electrode sheet 10; in step (2), the pressure inside the classifier during the preparation of the silicon-carbon composite material is 469 Pa, the rolling pressure during the preparation of the negative electrode sheet 10 is 29.9 T, and the axial extension dimension of the tab 20 is 15.7 mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25°C environment is 16.5 Ah and the discharge capacity at 0.33C rate is 22.0 Ah. The remaining steps are the same as in Example 1.

[0185] Comparative Example 5

[0186] The difference from Example 1 is as follows: In step (1), LiFePO4 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.35 times the unfolded length of the negative electrode sheet 10; in step (2), the host frequency during graphite preparation is 23Hz, the rolling pressure during negative electrode sheet 10 preparation is 29.5T, and the axial extension dimension of the tab 20 is 15.5mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 11.8Ah, and the discharge capacity at 0.33C rate is 15.5Ah. The remaining steps are the same as in Example 1.

[0187] Comparative Example 6

[0188] The difference from Example 1 is as follows: In step (1), LiFePO4 is used as the positive electrode active material; in step (2), the length of the first tabless region 30 in the negative electrode sheet is 0.021 times the unfolded length of the negative electrode sheet 10; in step (2), the host frequency during graphite preparation is 52Hz, the rolling pressure during negative electrode sheet 10 preparation is 5.9T, and the axial extension dimension of the tab 20 is 4.8mm, so that the discharge capacity of the cylindrical battery at 4C rate in a 25℃ environment is 13.3Ah, and the discharge capacity at 0.33C rate is 12.8Ah. The remaining steps are the same as in Example 1.

[0189] Table 1 shows the types of positive electrode active materials and negative electrode active materials used in all the above embodiments and comparative examples.

[0190] Table 2 shows the discharge capacity of cylindrical batteries at 4C rate and 0.33C rate in an environment of 25°C for all the above embodiments and comparative examples, as well as the energy density and electrolyte injection efficiency of the cylindrical batteries (a, b, a / b ...

[0191] Table 1

[0192]

[0193] Table 2

[0194]

[0195] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:

[0196] The type of material used in the positive electrode active layer of a battery affects its energy density. When lithium iron phosphate (LiFePO4) is used as the positive electrode active material, the battery has the lowest energy density (120–190 Wh / kg); when a medium-nickel ternary cathode material (LiNi) is used, the energy density is significantly higher. 0.63 Co 0.07 Mn 0.3 The energy density of the battery is second only to that of O2 (200-250 Wh / kg); when the positive electrode active material is a high-nickel ternary positive electrode material (LiNi 0.92 Co 0.06 Mn 0.02 The battery has the optimal energy density (260-370Wh / kg) when O2 is present.

[0197] The electrolyte injection efficiency of a battery is mainly related to the risk of the core hole being blocked. The smaller the length ratio of the first tabless region 30, the lower the electrolyte injection efficiency. Furthermore, the type of material in the positive electrode active material layer affects the electrolyte injection efficiency. The wettability of the electrolyte to the positive electrode sheet is affected by the positive electrode active material. Specifically, the electrolyte has good wettability to lithium iron phosphate but poor wettability to lithium nickel cobalt manganese oxide ternary materials. When the positive electrode active material is a high-nickel ternary positive electrode material (LiNi... 0.92 Co 0.06 Mn 0.02 When O2 is present, the battery's electrolyte injection efficiency is lowest (82%–92%); when the positive electrode active material is a medium-nickel ternary positive electrode material (LiNi), the efficiency is even lower. 0.63 Co 0.07 Mn 0.3 The battery's liquid injection efficiency is second best when O2 is used (82%–92%); when lithium iron phosphate (LiFePO4) is used as the positive electrode active material, the battery's liquid injection efficiency is best (90%–97%).

[0198] The cylindrical battery provided in this application includes a core and a first tabless region 30, which is located at the first end of the core after it is unrolled. The core includes a core hole. The arrangement of the first tabless region 30 can prevent the tabs 20 from blocking the core hole. However, the tabs 20 are structures that bear the current of the negative electrode 10. The arrangement of the first tabless region 30 causes different current densities in different areas of the electrode, resulting in high current density in some areas and low current density in others, which affects the insertion and extraction of lithium ions and thus affects the battery energy density. The ratio of the battery capacity at different rates is also a key measure of the lithium ion insertion and extraction capability. By controlling the relationship between the two, the length of the first tabless region 30 is longer. By controlling the capacity ratio at different rates, lithium ion transport is improved and the battery energy density is increased. The capacity at different rates at a specific temperature refers to the battery's discharge capability at different rates. The smaller the ratio, the weaker the discharge capability at high rates, which affects the battery energy density. The value of a / b cannot be too large, resulting in low battery energy density; the value of a / b cannot be too small, as it will block the core hole. When 'a' is relatively large, the increased impedance necessitates a larger 'b' to achieve improved energy density and fast charging performance. Conversely, a smaller 'a' reduces electrolyte injection efficiency and limits electrolyte wetting ability, requiring a smaller 'b', which significantly degrades the battery's fast charging performance.

[0199] Compared to other ranges, this application, by limiting a / b to the aforementioned specific range, can shorten the length of the electron flow path and suppress current density unevenness while avoiding the core hole being blocked; at the same time, it can improve the charge and discharge performance of cylindrical batteries at high rates and improve the overall performance of cylindrical batteries, such as energy density.

[0200] It should be noted that the terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such terms can be used interchangeably where appropriate so that the embodiments of this application described herein can be implemented, for example, in a sequence other than those described herein.

[0201] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A cylindrical battery, the cylindrical battery comprising a core, the core comprising at least one negative electrode (10) and at least one positive electrode wound together, and a separator being disposed between two adjacent positive electrode sheets and the negative electrode sheet (10); characterized in that, The negative electrode sheet (10) has a tab (20) on one side of its length direction after being unfolded, and the negative electrode sheet (10) has a first tabless region (30), which is located between the winding start end and the edge of the tab (20) near the winding start end; the cylindrical battery satisfies formula (I): 0.033≤a / b≤0.341 (I), Wherein, a represents the ratio of the length of the first tabless region (30) to the unfolded length of the negative electrode (10); b represents the ratio of the discharge capacity of the cylindrical battery at 25°C and 4C rate to the discharge capacity at 0.33C rate.

2. The cylindrical battery according to claim 1, characterized in that, The value of a is any value between 0.03 and 0.3; and / or the value of b is any value between 0.8 and 1.

03.

3. The cylindrical battery according to claim 1, characterized in that, 0.08≤a / b≤0.

195.

4. The cylindrical battery according to claim 1, characterized in that, 0.088≤a / b≤0.

178.

5. The cylindrical battery according to claim 1, characterized in that, The negative electrode sheet (10) includes a negative electrode current collector and a negative electrode active material layer stacked together. The material of the negative electrode active material layer includes silicon-based material, and 0.04≤a / b≤0.

28.

6. The cylindrical battery according to claim 5, characterized in that, The silicon content in the negative electrode active material layer is ≥3wt%, and 0.04≤a / b≤0.

23.

7. The cylindrical battery according to claim 6, characterized in that, The weight percentage of silicon in the negative electrode active material layer is ≤30wt%.

8. The cylindrical battery according to claim 7, characterized in that, The face density of the negative active material layer is 100 to 280 g / m 2 .

9. The cylindrical battery according to claim 7, characterized in that, The thickness of the negative electrode active material layer is ≥90μm, and 0.055≤a / b≤0.

26.

10. The cylindrical battery according to claim 1, characterized in that, The value of 'a' is any value between 0.02 and 0.

28.

11. The cylindrical battery according to claim 1, characterized in that, The ratio of the length of the tabless region in the positive electrode to the unfolded length of the positive electrode is 0.04 to 0.

33.

12. The cylindrical battery according to any one of claims 1 to 5, characterized in that, The cylindrical battery has a discharge capacity of 15-50 Ah at a 4C rate; the cylindrical battery has a discharge capacity of 19-55 Ah at a 0.33C rate.

13. The cylindrical battery according to claim 1, characterized in that, The porosity of the negative electrode sheet (10) is 35 to 60%, and the compacted density is 1.2 to 1.7 g / cm 3 .

14. The cylindrical battery according to claim 11, characterized in that, The positive electrode sheet includes a positive current collector and a positive active material layer stacked together. The material of the positive active material layer includes lithium nickel cobalt manganese oxide ternary positive electrode material, and the ratio of the length of the tabless region in the positive electrode sheet to the unfolded length of the positive electrode sheet is 0.08 to 0.33; or, the material of the positive active material layer includes lithium iron phosphate, and the ratio of the length of the tabless region in the positive electrode sheet to the unfolded length of the positive electrode sheet is 0.12 to 0.

33.

15. The cylindrical battery according to claim 11, characterized in that, The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer stacked together. The material of the positive electrode active material layer includes a lithium nickel cobalt manganese oxide ternary positive electrode material, and the Dv50 of the lithium nickel cobalt manganese oxide ternary positive electrode material is 2-4 μm; or... The material of the positive electrode active material layer includes lithium iron phosphate, and the Dv50 of the lithium iron phosphate is 0.4 to 2.0 μm.

16. The cylindrical battery according to claim 15, characterized in that, The material of the positive electrode active material layer comprises a lithium nickel cobalt manganese oxide ternary positive electrode material, and the porosity of the positive electrode sheet is 12-35%, and the compaction density is 3.45-3.65 g / cm 3 ; or, The positive electrode active material layer is made of lithium iron phosphate, and the porosity of the positive electrode sheet is 12-35%, with a compaction density of 2.1-2.7 g / cm³. 3 .

17. The cylindrical battery according to claim 1, characterized in that, Along the length direction of the unfolded negative electrode sheet (10), each negative electrode sheet (10) has a plurality of tabs (20) on one side, and the width of the connection between each tab (20) and the negative electrode sheet (10) is 2 to 10 mm; and / or, the lead-out size of each tab (20) is 2 to 15 mm.

18. The cylindrical battery according to claim 17, characterized in that, Each negative electrode (10) includes at least one second electrodeless region (40) between the multiple tabs (20) provided on one side of its unfolded length direction. The ratio of the sum of the length of the second electrodeless region (40) and the length of the first electrodeless region (30) to the unfolded length of the negative electrode (10) is 0.05 to 0.

6.

19. The cylindrical battery according to claim 1, characterized in that, Multiple negative electrode tabs are provided along the length direction of the unfolded negative electrode sheet (10), and multiple positive electrode tabs are provided along the length direction of the unfolded positive electrode sheet. The positive electrode tabs and the negative electrode tabs are located at the same end of the winding core.

20. The cylindrical battery according to claim 1, characterized in that, The core includes a core hole with a diameter of 6-8 mm.

21. The cylindrical battery according to claim 1, characterized in that, The winding core also includes an electrolyte, wherein the electrolyte comprises a lithium salt, and the molar concentration of the lithium salt in the electrolyte is 0.6 to 1.6 mol / L. The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide.

22. An electrical appliance, characterized in that, The electrical device includes the cylindrical battery according to any one of claims 1 to 21.