An amorphous iridium-based single-layer plating layer LED lead frame
The defect problem of crystalline coating in LED lead frames was solved by using an amorphous iridium-based single-layer coating, achieving high reliability and low cost multi-functional integration to meet the needs of complex working conditions.
Patent Information
- Application Number
- CN202611090631.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-07-22
AI Technical Summary
Existing LED lead frame crystalline coatings have grain boundary and pore defects, which lead to copper atom diffusion oxidation, corrosive media penetration and erosion, and interlayer interdiffusion to form brittle compounds, affecting device reliability and cost.
An amorphous iridium-based single-layer coating is used, which, through an iridium-nickel-phosphorus alloy coating, combined with a pulse electrodeposition process and an iridium salt pre-complexing solution, forms a uniform amorphous structure without grain boundaries, blocking copper diffusion and corrosion, and enhancing the corrosion resistance and mechanical properties of the coating.
It improves the long-term reliability and stability of LED lead frames, reduces material costs, and achieves multi-functional integration with a single coating, adapting to complex working conditions and high reliability requirements.
Smart Images

Figure CN122602878B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, specifically to an LED lead frame with an amorphous iridium-based single-layer coating. Background Technology
[0002] LED lead frames are metal structural components in semiconductor packaging, used to connect the internal circuitry of the chip to external wires to achieve electrical connection. They also provide mechanical support and heat dissipation. The main material is copper alloy, including copper-iron alloys, copper-nickel-silicon alloys, and other multi-element alloys. The production methods include die stamping and chemical etching. They are suitable for high-density, ultra-thin packaging scenarios. As the chip carrier of integrated circuits, LED lead frames are key structural components for forming electrical circuits. Most semiconductor integrated circuits require the use of LED lead frames, making them an important basic material in the electronics and information industry.
[0003] Current LED lead frames generally use multi-layered crystalline metal plating. However, crystalline plating itself has a large number of grain boundary and pore defects, and there are clear material interfaces between dissimilar metal layers. Therefore, copper atoms in the copper substrate are prone to diffusion and oxidation along the grain boundaries, and external sulfur- or halogen-containing corrosive media are also prone to penetrating and eroding along the grain boundaries. At the same time, inter-layer interdiffusion during high-temperature reflow soldering will continuously generate brittle intermetallic compounds, causing silver plating systems to be prone to sulfidation and blackening, as well as failures due to weakened bonding force. Nickel-palladium-gold systems have the drawbacks of complicated processes, high risk of inter-layer peeling, and high cost of precious metals. Conventional binary amorphous plating, due to its single composition and function, cannot simultaneously meet the multiple stringent requirements of packaging for diffusion blocking, optical reflection, and bonding solderability. Ultimately, this restricts the improvement of the service life and overall cost optimization of high-reliability semiconductor devices. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides an LED lead frame with an amorphous iridium-based single-layer coating, which solves the problems mentioned in the background art.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solution: an LED lead frame with an amorphous iridium-based single-layer coating, comprising a copper substrate, wherein the surface of the copper substrate is divided into a chip die bonding area, a lead bonding area and an external pin soldering area, and each partition of the copper substrate is coated with an amorphous iridium-based coating.
[0006] The amorphous iridium-based coating is specifically a single-layer amorphous iridium-nickel-phosphorus alloy coating. The mass percentage of each component in the amorphous iridium-based coating is 3% to 8% iridium, 9% to 13% phosphorus, and 79% to 88% nickel. It also contains negligible unavoidable trace elements and impurities.
[0007] The thickness of the amorphous iridium-based coating is 0.3 μm to 1.2 μm, and it is a completely amorphous structure. Its X-ray diffraction pattern shows diffuse peaks without sharp crystalline diffraction peaks.
[0008] The specific preparation process of the plating solution for the amorphous iridium-based coating is as follows:
[0009] S1. Add nickel sulfate, boric acid, and sodium citrate to deionized water in sequence, stir until completely dissolved, and then heat to 55-65℃ to obtain the basic plating solution.
[0010] S2. Iridium sulfate and ethylenediaminetetramethylenephosphonic acid are mixed separately at a mass ratio of 1:2 to 1:3 until completely dissolved to obtain an iridium salt pre-complexed solution. The iridium salt pre-complexed solution is slowly added dropwise to the base plating solution under continuous stirring, and the solution is kept warm and stirred for 30 to 40 minutes to complete in-situ complexation.
[0011] S3. Add sodium hypophosphite to the base plating solution, stir to dissolve, adjust the pH value to 4.2-4.8, let it stand for 20-30 minutes to obtain the finished plating solution.
[0012] Preferably, the amorphous iridium-based coating exhibits a continuous gradient distribution of iridium elements along the thickness direction;
[0013] From the inner side of the copper substrate to the outer surface of the amorphous iridium-based coating, the mass fraction of iridium gradually increases from 2% to 3% to 9% to 11%, while the mass fraction of phosphorus remains stable at 9% to 13%.
[0014] Preferably, the surface region of the amorphous iridium-based coating contains in-situ precipitated pure iridium nanocrystal particles;
[0015] The iridium nanocrystals have a grain size of 5nm to 15nm and account for 6% to 10% of the volume in the surface region;
[0016] The depth of the surface region ranges from 0.1 μm to 0.2 μm, and the remaining main regions of the amorphous iridium-based coating still maintain a completely amorphous structure.
[0017] Preferably, an ultrathin amorphous nickel-phosphorus transition layer and an iridium-based amorphous coating are disposed between the copper substrate and the amorphous iridium-based coating.
[0018] The thickness of the nickel-phosphorus transition layer is 0.03 μm to 0.08 μm, and the mass fraction of phosphorus is 10% to 14%. The overall structure is completely amorphous. The nickel-phosphorus transition layer and the upper iridium-based amorphous coating layer form a homogeneous, grain boundary-free interface.
[0019] The functional surface of the copper substrate is provided with uniformly distributed nano-pits, and the nickel-phosphorus transition layer is embedded in the nano-pits to form a mechanically interlocked bonding interface with the copper substrate.
[0020] Preferably, the functional surface of the copper substrate is provided with uniformly distributed nano-pits;
[0021] The depth of the nano-pits is 20nm to 50nm, the diameter is 80nm to 150nm, and the surface roughness Ra of the copper substrate after texturing is ≤5nm.
[0022] Preferably, the method for manufacturing the LED lead frame includes the following steps:
[0023] A1. The copper substrate is subjected to chemical degreasing, electrolytic degreasing, acid pickling activation and water washing in sequence to remove surface oil and oxide layer and obtain a clean substrate.
[0024] A2. The plating solution is deposited on the surface of a clean substrate using a pulsed electrodeposition process to obtain the amorphous iridium-based coating, and the thickness of the amorphous iridium-based coating is controlled to be 0.3 μm to 1.2 μm.
[0025] A3. The copper substrate after the amorphous iridium-based coating has been deposited is sequentially washed with pure water, sealed with hot pure water, and dried to obtain the finished LED lead frame.
[0026] Preferably, in step S1, before the acid pickling and activation process, the copper substrate is first subjected to pulse electrochemical micro-etching treatment to form uniformly distributed nano-pits on the functional surface of the copper substrate in situ, and then the subsequent acid pickling, activation and water washing processes are carried out.
[0027] Preferably, before step S2, an ultrathin amorphous nickel-phosphorus transition layer is pulse-electrodeposited on the surface of the activated copper substrate, and the thickness of the nickel-phosphorus transition layer is controlled to be 0.03 μm to 0.08 μm before proceeding with the subsequent main plating deposition process.
[0028] Preferably, during the pulse electrodeposition process in step S2, the concentration of iridium salt and the peak pulse current density in the plating solution are gradually increased to form an amorphous plating layer in situ with iridium elements distributed along the thickness direction.
[0029] Preferably, at the end of the deposition stage of step S2, the pulse parameters are adjusted to reduce the pulse frequency and increase the duty cycle, so as to induce the in-situ precipitation of diffusely distributed iridium nanocrystal particles on the surface of the amorphous iridium-based coating, before proceeding to the post-processing step.
[0030] This invention provides an LED lead frame with an amorphous iridium-based single-layer coating. It offers the following advantages:
[0031] (1) By using a single-layer amorphous iridium-based alloy coating to replace the traditional multi-layer crystalline metal stacked coating, the inherent grain boundary and pore defects of the crystalline coating are eliminated from the structure. There is also no clear material interface between the heterogeneous metal layers. This can block the outward diffusion and oxidation of copper atoms along the grain boundary, and also prevent the inward penetration and erosion of external sulfur-containing and halogen-containing corrosive media. Furthermore, it avoids the generation of brittle intermetallic compounds through interlayer diffusion during high-temperature reflow soldering, thereby reducing the risk of sulfidation blackening, bonding performance decay and coating peeling, improving the long-term reliability of LED lead frames under complex working conditions, and ensuring the service life and operational stability of semiconductor devices.
[0032] (2) Iridium is introduced into the amorphous nickel-phosphorus matrix to form a nickel-phosphorus-iridium alloy. The size difference between iridium atoms and nickel atoms increases the randomness of atomic arrangement, thereby improving the amorphous formation ability of the alloy and ensuring that the coating forms a complete and uniform amorphous structure. At the same time, the high chemical inertness and solid solution strengthening effect of iridium itself are utilized to improve the corrosion protection ability and mechanical properties of the coating. This allows a single coating to have multiple functions such as diffusion blocking, environmental corrosion resistance, optical reflection and bonding solderability. This breaks through the limitation of the single function of conventional binary amorphous coatings. The performance requirements of the entire packaging area can be met without additional stacking of functional coatings, realizing the multi-functional integration of a single coating.
[0033] (3) The LED lead frame adopts a single-layer plating design, combined with a stable plating solution prepared by iridium salt pre-complexation and pulse electrodeposition process. Only a single main plating process is needed to complete the preparation of the functional plating layer. There is no need to carry out multiple electroplating processes of different materials in steps, which reduces the yield loss and wastewater discharge caused by multi-step processes. At the same time, the precious metal iridium is added in small amounts in the form of alloy, which does not require the use of a large amount of expensive precious metals, effectively simplifying the production process and improving production efficiency. At the same time, it reduces material costs and environmental treatment costs, and optimizes the overall cost while improving the overall performance of the device, which is convenient for large-scale mass production and promotion. Attached Figure Description
[0034] Figure 1 This is a flowchart illustrating the process steps for preparing the coating solution of the amorphous iridium-based coating of the present invention.
[0035] Figure 2 This is a flowchart illustrating the process steps of manufacturing the LED lead frame of the present invention. Detailed Implementation
[0036] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0037] Example 1
[0038] Reference Figure 1-2 Preparation of plating solution: Add 220 g / L nickel sulfate, 40 g / L boric acid and 60 g / L sodium citrate to deionized water in sequence, stir until completely dissolved, add water to make up to 1 L, and then heat to 65℃ to obtain the basic plating solution.
[0039] 6g of iridium sulfate and 18g of ethylenediaminetetramethylenephosphonic acid were mixed separately at a mass ratio of 1:3 and stirred until completely dissolved to obtain a pre-complexed solution of iridium salt.
[0040] Under continuous uniform stirring, the pre-complexing solution was slowly added dropwise to the base plating solution, and the in-situ complexing was completed by stirring at a constant temperature for 40 minutes.
[0041] Add 35 g / L of sodium hypophosphite to the base plating solution, stir to dissolve, adjust the pH value to 4.8 with dilute sulfuric acid, and let it stand for 30 minutes to obtain the finished plating solution.
[0042] Pulse electrodeposition: Employs a pulse electroplating process with an average current density of 3.0 A / dm³. 2 The pulse frequency was 2000Hz, the duty cycle was 40%, the deposition time was 16min, and the coating thickness was controlled to be 1.2μm.
[0043] Post-processing: Wash three times with pure water, then seal with 80℃ hot pure water, and finally dry with clean hot air to obtain the finished amorphous iridium-based single-layer coated LED lead frame.
[0044] Example 2
[0045] Preparation of plating solution: 200 g / L nickel sulfate, 35 g / L boric acid and 50 g / L sodium citrate were added to deionized water in sequence and stirred until completely dissolved. After adding water to make up to 1 L, the temperature was raised to 60℃ to obtain the basic plating solution.
[0046] Weigh 4g of iridium sulfate and 10g of ethylenediaminetetramethylenephosphonic acid, with a mass ratio of 1:2.5, and mix them separately until completely dissolved to obtain an iridium salt pre-complexed solution.
[0047] Under continuous uniform stirring, the pre-complexing solution was slowly added dropwise to the base plating solution, and the in-situ complexing was completed by stirring at a constant temperature for 35 minutes.
[0048] Add 30 g / L of sodium hypophosphite to the base plating solution, stir to dissolve, adjust the pH value to 4.5 with dilute sulfuric acid, and let it stand for 25 minutes to obtain the finished plating solution.
[0049] Pulse electrodeposition: Employs a pulse electroplating process with an average current density of 2.0 A / dm³. 2The pulse frequency was 1000Hz, the duty cycle was 30%, the deposition time was 10min, and the coating thickness was controlled to be 0.75μm.
[0050] Post-processing: Wash three times with pure water, then seal with 80℃ hot pure water, and finally dry with clean hot air to obtain the finished amorphous iridium-based single-layer coated LED lead frame.
[0051] Example 3
[0052] Preparation of plating solution: 180g nickel sulfate, 30g boric acid and 40g sodium citrate were added to deionized water in sequence and stirred until completely dissolved. Water was added to make up to 1L and then the temperature was raised to 55℃ to obtain the base plating solution.
[0053] Weigh 2g of iridium sulfate and 4g of ethylenediaminetetramethylenephosphonic acid in a mass ratio of 1:2. Mix them separately and stir until completely dissolved to obtain an iridium salt pre-complexing solution. Under continuous uniform stirring, slowly add the pre-complexing solution to the base plating solution and keep it warm and stirred for 30 minutes to complete in-situ complexation.
[0054] Add 25g of sodium hypophosphite to the base plating solution, stir to dissolve, adjust the pH value to 4.2, and let it stand for 20 minutes to obtain the finished plating solution.
[0055] Pulse electrodeposition: Average current density 1.5 A / dm³ 2 The pulse frequency was 500Hz, the duty cycle was 20%, the deposition time was 4min, and the coating thickness was controlled to be 0.3μm.
[0056] Post-processing: Wash three times with pure water, then seal with 80℃ hot pure water, and finally dry with clean hot air to obtain the finished amorphous iridium-based single-layer coated LED lead frame.
[0057] Comparative Example 1
[0058] The silver-plated lead frame was prepared using the industry-standard cyanide silver plating process, with a silver plating layer thickness of 0.8 μm. The substrate and pretreatment process are existing technologies.
[0059] Comparative Example 2
[0060] A multilayer coating was prepared using a conventional pre-plating framework process. The structure consisted of a 1.0 μm crystalline nickel layer, a 0.05 μm crystalline palladium layer, and a 0.03 μm crystalline gold layer. The substrate and pretreatment process were based on existing technologies.
[0061] Comparative Example 3
[0062] The plating solution does not contain iridium sulfate or ethylenediaminetetramethylenephosphonic acid. The rest of the plating solution preparation, deposition process and post-treatment are completely consistent with those in Example 2, and it is a completely amorphous structure.
[0063] Comparative Example 4
[0064] The target composition of the coating is the same as in Example 2. The plating solution is fed in a single batch, with 4g of iridium sulfate added directly to the base plating solution per liter of plating solution for mixing and dissolution. The separate iridium salt pre-complexation step is omitted. The remaining plating solution components, deposition process and post-treatment are completely the same as in Example 2.
[0065] Comparative Example 5
[0066] The target composition of the coating is the same as in Example 2, and it is prepared using a DC electroplating process with a current density of 2.0 A / dm³. 2 The deposition time was adjusted to control the coating thickness to 0.75 μm. The remaining pretreatment and posttreatment were the same as in Example 2, and the coating structure was a crystalline iridium-nickel-phosphorus alloy.
[0067] Comparative Example 6
[0068] The amount of iridium sulfate added to the plating solution was reduced by adding 1.2g of iridium sulfate and 3g of ethylenediaminetetramethylenephosphonic acid per liter of plating solution for pre-complexation. The target coating iridium content was 1.5wt%. The rest of the plating solution preparation, deposition process and post-treatment were completely consistent with Example 2, and the coating was a partially amorphous structure.
[0069] Comparative Example 7
[0070] The amount of iridium sulfate added to the plating solution was increased by adding 9g of iridium sulfate and 27g of ethylenediaminetetramethylenephosphonic acid per liter of plating solution for pre-complexation. The target coating iridium content was 12wt%. The rest of the plating solution preparation, deposition process and post-treatment were completely consistent with those in Example 2, and the coating was a partially crystalline structure.
[0071] Comparative Example 8
[0072] The amount of sodium hypophosphite added to the plating solution was reduced to 15 g / L, the target coating phosphorus content was 6 wt%, and the rest of the plating solution preparation, deposition process and post-treatment were completely consistent with Example 2, with the crystalline structure being the main feature.
[0073] Comparative Example 9 (Coating thickness below the lower limit)
[0074] The deposition time was shortened and the coating thickness was controlled to 0.15 μm. The rest of the plating solution preparation, deposition process and post-treatment were completely consistent with those in Example 2.
[0075] Test case
[0076] Test items and methods
[0077] Sulfur resistance: The sample was placed in a sealed container with a saturated hydrogen sulfide atmosphere and left to stand at room temperature. The time it took for the surface to show obvious discoloration was recorded visually.
[0078] Copper diffusion barrier performance: The sample was stored in a constant temperature oven at 150℃, and the time it took for copper oxide brown spots to appear on the surface was recorded; the rate of increase in pin contact resistance after 1000 hours was tested (based on the initial resistance).
[0079] Coating adhesion: Rating is performed according to GB / T9286 cross-cut test; then, the coating is subjected to 500 cycles of thermal shock from -40℃ to 125℃ to observe whether the coating blisters or peels off.
[0080] Table 1 shows the test results of the coating's basic protective properties and interface bonding performance:
[0081] Group Sulfurization resistance time (h) Time (h) for brown spots to appear on copper diffusion at 150℃ 1000h contact resistance rise rate (%) 100-point test level Example 1 120 showed no obvious color change >1800 1.5 Level 0 Example 2 84 showed no obvious color change 1300 2.7 Level 0 Example 3 52 No obvious color change 850 4.9 Level 0 Comparative Example 1 2 Completely black 400 38.2 Level 0 Comparative Example 2 24 slight discoloration 900 8.5 Level 0 Comparative Example 3 12 changed color 600 12.3 Level 0 Comparative Example 4 36 changed color 700 7.6 Level 0 Comparative Example 5 18 changed color 500 18.7 Level 0 Comparative Example 6 16 changed color 550 15.2 Level 0 Comparative Example 7 60 changed color 850 6.3 Level 1 Comparative Example 8 15 changed color 480 21.4 Level 0 Comparative Example 9 20 changed color 350 25.8 Level 1
[0082] Visible reflectance: The specular reflectance at a wavelength of 550 nm was measured using a UV-Vis spectrophotometer.
[0083] Gold wire bonding performance: Thermo-ultrasonic bonding with φ25μm gold wire was used, and the average thrust at the bonding point was tested.
[0084] Salt spray resistance: Perform neutral salt spray test according to GB / T10125 and record the time when the first corrosion point appears on the surface;
[0085] Plating solution stability: The plating solution was sealed and left to stand at 60℃ for 30 days. Observe whether precipitation occurs and test the deviation rate of iridium content in the plating layer before and after standing.
[0086] Table 2 shows the test results of coating reliability and process compatibility:
[0087] Group Post-thermal shock state 550nm reflectance (%) Average thrust (gf) of gold wire bonding Time to corrosion from neutral salt spray (h) 30-day iridium content deviation rate of plating solution (%) Example 1 No abnormalities 76 13.1 520 3.5 Example 2 No abnormalities 78 12.4 380 2.6 Example 3 No abnormalities 79 11.7 260 2.9 Comparative Example 1 No abnormalities 92 13.5 48 - Comparative Example 2 Interlayer microcracks 65 12 168 - Comparative Example 3 No abnormalities 77 11.5 120 - Comparative Example 4 No abnormalities 77 11.7 200 18.6 (precipitate appears after 10 days) Comparative Example 5 No abnormalities 75 11.2 96 - Comparative Example 6 No abnormalities 78 11.6 108 - Comparative Example 7 Edge microbubbles 74 11.9 280 - Comparative Example 8 No abnormalities 75 11 84 - Comparative Example 9 Localized blistering 72 10.5 72 -
[0088] As can be seen from Tables 1 and 2 above, the three embodiments of the present invention have significantly better sulfur resistance, copper diffusion blocking performance, and salt spray resistance than the existing mainstream solutions. In particular, Embodiment 1 is the best. The sulfur resistance without discoloration of Embodiment 1 is more than 60 times that of the traditional silver plating solution, and the copper diffusion blocking time is more than twice that of the nickel-palladium-gold solution. This effect is due to the homogeneous structure of the amorphous coating without grain boundaries and pores, which completely blocks the natural channels for corrosive media to penetrate inward and copper atoms to diffuse outward. Combined with the high chemical inertness and surface passivation effect of iridium, the industry pain points of sulfur blackening and copper migration oxidation that are common in traditional crystalline coatings are solved from the material essence. It is fully suitable for long-term use in harsh working conditions such as outdoor and automotive applications.
[0089] The results of thermal shock and adhesion tests show that the adhesion of the coatings in all embodiments of this invention reaches level 0 in the cross-cut adhesion test. After 500 thermal shocks, there is no blistering, peeling, or cracking. In contrast, the traditional nickel-palladium-gold multilayer solution exhibits interlayer micro-cracks after the same test. The results verify the structural advantages of the single-layer integrated coating.
[0090] This invention eliminates the material interface between heterogeneous metal layers, preventing interlayer interdiffusion and the formation of brittle intermetallic compounds during high-temperature service and temperature cycling. Structurally, it eliminates the risk of interface failure such as coating delamination, peeling, and embrittlement. Compared to the existing multi-layer stacked coating technology that "relies on the number of layers to add functionality and sacrifices reliability by relying on interfaces," the single-layer multi-functional design of this invention has an essential advantage in structural reliability.
[0091] Optical and bonding performance tests show that the visible light reflectance and gold wire bonding push of the coating of this invention meet the application standards of LED packaging. It can simultaneously cover the performance requirements of the entire area of chip die bonding, wire bonding, and external pin soldering without the need to prepare different coatings in separate areas. Compared with the shortcomings of conventional binary amorphous coatings, which have single functions and cannot take into account both protection and packaging adaptability, this invention, through the ternary alloy composition of iridium-nickel-phosphorus, takes into account both optical reflection characteristics and bonding solderability while ensuring amorphous structure and protective performance. It truly achieves multi-functionality in one layer and reduces the application limitations of amorphous coatings, which can only be used in anti-corrosion and wear-resistant scenarios. Although the initial specular reflectance is slightly lower than that of pure silver coating, combined with the huge advantage of sulfur resistance, its light efficiency retention rate throughout the entire life cycle is much higher than that of silver plating solution, and its overall optical performance in long-term use is better.
[0092] The plating solution stability test results show that the plating solution prepared using the pre-complexing process of this invention has an iridium content deviation rate of less than 4% after 30 days of high-temperature standing, and no precipitation is generated.
[0093] In contrast, in Comparative Example 4, where pre-complexation was omitted, iridium salt hydrolysis precipitation occurred in the plating solution after 10 days, with an iridium content deviation rate approaching 20%. This directly led to uneven coating composition and decreased protective performance. The results validated the technical value of the stepwise feeding process for iridium salt pre-complexation.
[0094] By forming a stable complex with iridium ions in advance, the technical problem of easy hydrolysis and precipitation of high-valent iridium salts in weakly acidic plating solutions is completely solved. This not only ensures the uniformity of the coating composition and the integrity of the amorphous structure, but also significantly improves the service life and batch stability of the plating solution, providing process assurance for the industrial mass production of the solution.
[0095] Comparative verification using Examples 6-9 shows that when the iridium content, phosphorus content, and thickness of the coating deviate from the limits specified in this invention, significant performance degradation occurs.
[0096] When the iridium content is below the lower limit, the amorphous forming ability is insufficient, and the corrosion resistance and diffusion barrier properties are significantly reduced.
[0097] If the iridium content exceeds the upper limit, partial crystallization of the coating will occur, and the increased internal stress will lead to a decrease in adhesion.
[0098] If the phosphorus content is below the lower limit, a completely amorphous structure cannot be formed, and the protective performance is significantly reduced.
[0099] If the coating thickness is below the lower limit, pinhole defects are likely to occur, and a complete and dense barrier layer cannot be formed;
[0100] This proves that the parameter range of 3%-8% iridium, 9%-13% phosphorus, and 0.3μm-1.2μm coating thickness specified in this invention is the optimal range for ensuring the coating has a completely amorphous structure and achieving the best overall performance in terms of protection, mechanical properties, and process cost, and has clear technical support and verification basis.
[0101] In summary, this invention, through the material structure of an amorphous iridium-based monolayer coating and the preparation process of iridium salt pre-complexation, systematically solves the technical problems of rapid sulfidation failure, severe copper diffusion, poor interlayer reliability, and high process cost of existing LED lead frame coatings. It achieves performance improvement over existing technologies while taking into account mass production feasibility and cost advantages. It has outstanding substantive features and significant technological progress, and has good industrial application value and market promotion prospects.
[0102] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. An LED lead frame with an amorphous iridium-based single-layer coating, comprising a copper substrate, wherein the surface of the copper substrate is divided into a die-bonding region, a wire bonding region, and an external lead soldering region, characterized in that: Each section of the copper substrate is coated with an amorphous iridium-based coating. The amorphous iridium-based coating is specifically a single-layer amorphous iridium-nickel-phosphorus alloy coating, wherein the mass percentages of each component in the amorphous iridium-based coating are 3%–8% iridium, 9%–13% phosphorus, and 79%–88% nickel; The thickness of the amorphous iridium-based coating is 0.3 μm to 1.2 μm, and it is a completely amorphous structure. Its X-ray diffraction pattern shows diffuse peaks without sharp crystalline diffraction peaks. The specific preparation process of the plating solution for the amorphous iridium-based coating is as follows: S1. Add nickel sulfate, boric acid, and sodium citrate to deionized water in sequence, stir until completely dissolved, and then heat to 55-65℃ to obtain the basic plating solution. S2. Iridium sulfate and ethylenediaminetetramethylenephosphonic acid are mixed separately at a mass ratio of 1:2 to 1:3 until completely dissolved to obtain an iridium salt pre-complexed solution. The iridium salt pre-complexed solution is slowly added dropwise to the base plating solution under continuous stirring, and the solution is kept warm and stirred for 30 to 40 minutes to complete in-situ complexation. S3. Add sodium hypophosphite to the base plating solution, stir to dissolve, adjust the pH value to 4.2-4.8, let it stand for 20-30 minutes to obtain the finished plating solution.
2. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 1, characterized in that: The amorphous iridium-based coating exhibits a continuous gradient distribution of iridium elements along the thickness direction. From the inner side of the copper substrate to the outer surface of the amorphous iridium-based coating, the mass fraction of iridium gradually increases from 2% to 3% to 9% to 11%, while the mass fraction of phosphorus remains stable at 9% to 13%.
3. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 1, characterized in that: The surface region of the amorphous iridium-based coating contains in-situ precipitated pure iridium nanocrystal particles. The iridium nanocrystals have a grain size of 5nm to 15nm and account for 6% to 10% of the volume in the surface region; The depth of the surface region ranges from 0.1 μm to 0.2 μm, and the remaining main regions of the amorphous iridium-based coating still maintain a completely amorphous structure.
4. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 1, characterized in that: An ultrathin amorphous nickel-phosphorus transition layer and an iridium-based amorphous coating are disposed between the copper substrate and the amorphous iridium-based coating. The thickness of the nickel-phosphorus transition layer is 0.03 μm to 0.08 μm, and the mass fraction of phosphorus is 10% to 14%. The overall structure is completely amorphous. The nickel-phosphorus transition layer and the upper iridium-based amorphous coating layer form a homogeneous, grain boundary-free interface. The functional surface of the copper substrate is provided with uniformly distributed nano-pits, and the nickel-phosphorus transition layer is embedded in the nano-pits to form a mechanically interlocked bonding interface with the copper substrate.
5. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 4, characterized in that: The functional surface of the copper substrate is provided with uniformly distributed nano-pits. The depth of the nano-pits is 20nm to 50nm, the diameter is 80nm to 150nm, and the surface roughness Ra of the copper substrate after texturing is ≤5nm.
6. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 1, characterized in that: The method for manufacturing the LED lead frame includes the following steps: A1. The copper substrate is subjected to chemical degreasing, electrolytic degreasing, acid pickling activation and water washing in sequence to remove surface oil and oxide layer and obtain a clean substrate. A2. The plating solution is deposited on the surface of a clean substrate using a pulsed electrodeposition process to obtain the amorphous iridium-based coating, and the thickness of the amorphous iridium-based coating is controlled to be 0.3 μm to 1.2 μm. A3. The copper substrate after the amorphous iridium-based coating has been deposited is sequentially washed with pure water, sealed with hot pure water, and dried to obtain the finished LED lead frame.
7. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 6, characterized in that: In step S1, before the acid pickling and activation process, the copper substrate is first subjected to pulsed electrochemical micro-etching treatment to form uniformly distributed nano-pits on the functional surface of the copper substrate in situ, and then the subsequent acid pickling, activation and water washing processes are carried out.
8. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 6, characterized in that: Before step S2, an ultrathin amorphous nickel-phosphorus transition layer is pulse-electrodeposited on the surface of the activated copper substrate, and the thickness of the nickel-phosphorus transition layer is controlled to be 0.03μm to 0.08μm before proceeding with the subsequent main plating deposition process.
9. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 6, characterized in that: During the pulse electrodeposition process in step S2, the concentration of iridium salt and the peak pulse current density in the plating solution are gradually increased to form an amorphous plating layer in situ with iridium elements distributed along the thickness direction.
10. The LED lead frame with an amorphous iridium-based single-layer coating according to claim 6, characterized in that: At the end of the deposition stage in step S2, the pulse parameters are adjusted to reduce the pulse frequency and increase the duty cycle, inducing the in-situ precipitation of diffusely distributed iridium nanocrystal particles on the surface of the amorphous iridium-based coating, before proceeding to the post-processing step.
Citation Information
Patent Citations
Process for preparing optically active carboxylic acids
CA2234983A1
Chemical plating preparation process of Ni-Cu-P amorphous alloy plating layer serving as electronic packaging brazing interface diffusion barrier layer
CN117286480A