Two-dimensional polyaramid composite gas separation membrane for carbon capture and preparation method thereof
By combining amino-terminated two-dimensional polyarylamide nanosheets with crosslinking agents, a stable carbon dioxide transport channel is formed, which solves the problem of the difficulty in balancing permeability and selectivity in traditional polymer membranes, improves carbon dioxide separation performance and long-term operational stability, and is suitable for the field of carbon capture.
Patent Information
- Application Number
- CN202610993493.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-06
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-07-06
AI Technical Summary
Existing polymer gas separation membranes struggle to balance permeability and selectivity, and separation membranes formed by stacking two-dimensional polyarylamide nanosheets suffer from non-selectivity defects and structural instability, affecting carbon dioxide separation performance and long-term operational stability.
A composite selective layer consisting of amino-terminated two-dimensional polyarylamide nanosheets, short-chain diepoxides, diaminopropyl-terminated polysiloxanes, and polyethylene glycol diglycidyl ether is used. The nanosheets are fixed by a cross-linking network, and the polydopamine interfacial transition layer is combined to improve the structural stability and selectivity of the membrane.
It achieves improved carbon dioxide separation performance and long-term operational stability, while taking into account both high permeability and selectivity, and is suitable for carbon dioxide separation and enrichment in flue gas and natural gas.
Smart Images

Figure CN122643909B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of gas separation membrane technology, specifically to a two-dimensional polyarylamide composite gas separation membrane for carbon capture and its preparation method. Background Technology
[0002] With the increasing carbon dioxide emissions from industrial production, the separation and enrichment of carbon dioxide from flue gas, natural gas, and other carbon dioxide-containing mixtures has become an important research direction in the field of carbon capture. Existing carbon dioxide separation methods mainly include absorption, adsorption, cryogenic separation, and membrane separation. Among these, membrane separation has advantages such as simple equipment structure, relatively low energy consumption, ease of continuous operation, and modular integration, and therefore shows promising application prospects.
[0003] Existing polymer gas separation membranes typically rely on the differences in dissolution and diffusion of different gases within the membrane material to achieve separation. However, traditional polymer membranes generally suffer from the problem of balancing permeability and selectivity. Increasing the free volume between polymer chain segments can improve the permeation rate of carbon dioxide, but it can also easily lead to the formation of large, non-selective transport channels, reducing the separation selectivity between carbon dioxide and nitrogen or methane. While increasing the density of polymer chain packing can improve molecular sieving capabilities, it can also increase gas transport resistance. Furthermore, some polymer membranes are prone to plasticization, chain rearrangement, or structural aging under high carbon dioxide partial pressures or long-term operating conditions, resulting in a decline in separation performance.
[0004] Two-dimensional polyarylamide nanosheets possess high structural stability and a large aspect ratio, enabling the formation of tortuous gas transport paths through layer-by-layer stacking, making them suitable for constructing ultrathin selective gas separation layers. However, when relying solely on stacked two-dimensional polyarylamide nanosheets to form separation membranes, two problems easily arise between adjacent nanosheets: first, excessively dense stacking of the sheets leads to increased resistance to carbon dioxide transport; second, uneven sheet arrangement creates large non-selective defects in localized areas, allowing nitrogen or methane to pass through rapidly simultaneously. Existing technologies typically employ a single crosslinking agent to immobilize the two-dimensional nanosheets, but a single crosslinking structure struggles to simultaneously achieve defect sealing, interlayer spacing regulation, and carbon dioxide affinity transport.
[0005] Therefore, it is necessary to provide a two-dimensional polyarylamide composite gas separation membrane for carbon capture. By co-regulating the interlayer structure of the two-dimensional polyarylamide nanosheets through cross-linking components of different molecular scales, a stable carbon dioxide affinity transport channel is formed while sealing non-selective defects, and the bonding stability between the selective layer and the porous support layer is improved, thereby improving the carbon dioxide separation performance and long-term operational stability of the composite gas separation membrane.
[0006] In order to overcome the shortcomings of the prior art, the present invention aims to provide a two-dimensional polyarylamide composite gas separation membrane for carbon capture and its preparation method, thereby improving the carbon dioxide separation performance and long-term operational stability of the composite gas separation membrane.
[0007] To achieve the above objectives, the present invention provides the following technical solution: a two-dimensional polyarylamide composite gas separation membrane for carbon capture, comprising a porous support layer, an interface transition layer disposed on the surface of the porous support layer, and a composite selective layer disposed on the surface of the interface transition layer;
[0008] The composite selective layer comprises amino-terminated two-dimensional polyarylamide nanosheets, short-chain diepoxides, diaminopropyl-terminated polysiloxanes, and polyethylene glycol diglycidyl ether.
[0009] Furthermore, the amino-terminated two-dimensional polyarylamide nanosheets are prepared by polycondensation reaction of melamine and trimesoyl chloride, wherein the molar ratio of melamine to trimesoyl chloride is 1.05-1.20:1.
[0010] Furthermore, the short-chain diepoxide is one of ethylene glycol diglycidyl ether and 1,4-butanediol diglycidyl ether; the number average molecular weight of the polyethylene glycol diglycidyl ether is 500-1000.
[0011] Furthermore, based on 100 parts by weight of amino-terminated two-dimensional polyarylamide nanosheets, the amount of the short-chain diester compound is 6-10 parts by weight, the amount of the diaminopropyl-terminated polysiloxane is 2-4 parts by weight, and the amount of the polyethylene glycol diglycidyl ether is 5-8 parts by weight.
[0012] Furthermore, the porous support layer is a polyacrylonitrile porous membrane; the interface transition layer is a polydopamine layer.
[0013] Furthermore, the preparation method of the two-dimensional polyarylamide composite gas separation membrane for carbon capture includes the following steps:
[0014] S1. Melamine and pyromellitic methyl chloride were added to an organic reaction medium to carry out a polycondensation reaction. After the reaction was completed, the mixture was washed, dispersed and exfoliated to obtain a dispersion of amino-terminated two-dimensional polyarylamide nanosheets.
[0015] S2. The porous support membrane is placed in a dopamine buffer solution to carry out a self-polymerization reaction, and an interface transition layer is formed on the surface of the porous support membrane to obtain a modified porous support membrane.
[0016] S3. Add a short-chain dieoxy compound and a diaminopropyl-terminated polysiloxane to the amino-terminated two-dimensional polyarylamide nanosheet dispersion, and stir for 20-40 min; then add polyethylene glycol diglycidyl ether, continue stirring for 20-40 min, and ultrasonically disperse for 10-30 min to obtain a composite selective layer film-forming solution.
[0017] S4. The composite selective layer film-forming solution is deposited on the surface of the interface transition layer of the modified porous support membrane, and then dried and heat-treated in sequence to allow the short-chain diepoxy compound and polyethylene glycol diglycidyl ether to undergo crosslinking reaction with the amino-terminated two-dimensional polyarylamide nanosheets, respectively, to obtain the two-dimensional polyarylamide composite gas separation membrane for carbon capture.
[0018] Further, in step S1, the organic reaction medium includes N-methylpyrrolidone and pyridine, and the volume ratio of N-methylpyrrolidone to pyridine is 5-15:1; the polycondensation reaction temperature is 20-35℃ and the time is 12-20h; the exfoliation treatment is ultrasonic exfoliation or high-speed shear exfoliation.
[0019] Further, in step S2, the dopamine-containing buffer solution is a Tris buffer solution, wherein the concentration of dopamine is 3-5 mg / mL, the pH value is 8.0-9.0, and the self-polymerization reaction time is 8-10 h.
[0020] Furthermore, in step S4, the deposition method is vacuum filtration deposition, the heat treatment temperature is 55-65℃, and the heat treatment time is 5-8h.
[0021] Compared with the prior art, the present invention has the following beneficial technical effects:
[0022] (1) In this invention, two-dimensional polyarylamide nanosheets with terminal amino groups are used as the main body of the composite selective layer. The orderly stacking of two-dimensional nanosheets forms a tortuous gas transport path with molecular sieving function. At the same time, short-chain diepoxy compounds can cross-link with the terminal amino groups on the surface of the nanosheets to connect and fix adjacent nanosheets at close range, thereby reducing non-selective defects such as pores and cracks formed during the layer arrangement process and improving the structural integrity and gas sieving capacity of the composite selective layer.
[0023] (2) This invention employs short-chain diepoxy compounds, diaminopropyl-terminated polysiloxanes, and polyethylene glycol diglycidyl ether to jointly regulate the interlayer structure of two-dimensional polyarylamide nanosheets. The short-chain diepoxy compounds form a relatively dense cross-linked structure, suppressing excessively large non-selective channels; the flexible segments of the diaminopropyl-terminated polysiloxanes alleviate the excessively tight packing of the two-dimensional rigid sheets, reducing gas transport resistance; and the polyethylene glycol diglycidyl ether further participates in cross-linking while introducing polyether segments with an affinity for carbon dioxide. The components work together in defect sealing, interlayer spacing regulation, and carbon dioxide affinity transport, which is beneficial for balancing carbon dioxide permeability and separation selectivity.
[0024] (3) The present invention provides a polydopamine interface transition layer between the porous support layer and the composite selective layer. The active functional groups on the surface of polydopamine are used to improve the wettability and interfacial effect of the support membrane surface, so that the composite selective layer can be deposited more uniformly and firmly attached to the surface of the porous support layer, reducing membrane peeling and local defects, and improving the interfacial stability of the composite membrane.
[0025] (4) The present invention fixes two-dimensional polyarylamide nanosheets through a cross-linking network, which can suppress sheet slip, chain rearrangement and structural relaxation during high carbon dioxide partial pressure or long-term operation, reduce the degree of separation performance decline with the use time, thereby improving the structural stability and long-term operation stability of the composite gas separation membrane, and is suitable for the separation and enrichment of flue gas, natural gas and other mixed gases containing carbon dioxide. Attached Figure Description
[0026] Figure 1 TEM image of the amino-terminated two-dimensional polyarylamide nanosheets prepared in Example 1.
[0027] Figure 2 SEM image of the cross-section of the composite gas separation membrane prepared in Example 1. Detailed Implementation
[0028] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] Unless otherwise specified, the melamine, trimesoyl chloride, N-methylpyrrolidone, pyridine, dopamine hydrochloride, tris(hydroxymethyl)aminomethane (Tris), ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, and tetramethylammonium hydroxide used in this invention were all purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; polyethylene glycol diglycidyl ether was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., and the specifications with Mn of 500, 750, and 1000 were selected according to the nominal number average molecular weight; the polyacrylonitrile porous membrane was a PZ type polyacrylonitrile flat sheet porous membrane manufactured by Synder Filtration.
[0030] The preparation method of diaminopropyl-terminated polysiloxane is as follows: 19.6 g of octamethylcyclotetrasiloxane, 18.4 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 1.30 g of tetramethylammonium hydroxide are added to a reaction flask, and the mixture is stirred and heated to 84 °C under nitrogen protection for 2 h; then the temperature is raised to 130 °C and the reaction is continued for 1.5 h; after the reaction is completed, low-boiling substances are removed under reduced pressure and vacuum distillation is performed to obtain diaminopropyl-terminated polysiloxane.
[0031] Example 1
[0032] This embodiment provides a two-dimensional polyarylamide composite gas separation membrane for carbon capture, the preparation method of which includes the following steps:
[0033] S1. Preparation of amino-terminated two-dimensional polyarylamide nanosheets: 80 mL of N-methylpyrrolidone and 20 mL of pyridine were added to a reaction flask, followed by melamine. The mixture was stirred and dispersed evenly. Tristyroyl chloride was dissolved in 20 mL of N-methylpyrrolidone and slowly added to the above reaction solution. The molar ratio of melamine to tristyroyl chloride was 1.05:1. The reaction was carried out at 20 °C for 12 h. After the reaction was completed, the nanosheets were centrifuged and washed with N-methylpyrrolidone and anhydrous ethanol. The nanosheets were then redispersed in N-methylpyrrolidone and ultrasonically exfoliated for 1 h to obtain an amino-terminated two-dimensional polyarylamide nanosheet dispersion.
[0034] S2. Preparation of modified porous support membrane: The polyacrylonitrile porous membrane was placed in a dopamine Tris buffer solution with a concentration of 3 mg / mL and a pH of 8.0 and subjected to self-polymerization reaction at room temperature for 8 h; after removal, it was rinsed with deionized water and dried to obtain the modified porous support membrane.
[0035] S3. Preparation of composite selective layer film-forming solution: Take a dispersion containing 1.00 g of amino-terminated two-dimensional polyarylamide nanosheets, add 0.06 g of ethylene glycol diglycidyl ether and 0.02 g of diaminopropyl-terminated polysiloxane, and stir for 20 min; then add 0.05 g of polyethylene glycol diglycidyl ether with a number average molecular weight of 500, continue stirring for 20 min, and ultrasonically disperse for 10 min to obtain the composite selective layer film-forming solution.
[0036] S4. Preparation of composite gas separation membrane: The composite selective layer film-forming solution obtained in step S3 is deposited on the surface of the interface transition layer of the modified porous support membrane obtained in step S2 by vacuum filtration; then dried at 40℃ for 2h, and then heat-treated at 55℃ for 5h to obtain a two-dimensional polyarylamide composite gas separation membrane for carbon capture.
[0037] Depend on Figure 1 As can be seen, the amino-terminated two-dimensional polyarylamide prepared in Example 1 exhibits a distinct two-dimensional sheet structure. The nanosheets are relatively thin overall, have high electron permeability, clear edge contours, and exhibit certain wrinkles and curling on the sheet surface. Some nanosheets overlap and merge, but no obvious agglomeration of large particles was observed, indicating that the obtained two-dimensional polyarylamide can be well dispersed to form a sheet structure.
[0038] The morphology described above indicates that the interfacial polymerization process effectively restricts the growth of polyarylamide along the thickness direction, allowing it to preferentially expand along the planar direction to form two-dimensional nanosheets. The wrinkled structure on the surface of the nanosheets can increase the effective specific surface area, while its terminal amino groups can provide active sites for subsequent crosslinking reactions with ethylene glycol diglycidyl ether, which is beneficial for constructing a continuous and dense two-dimensional selective separation layer on the surface of the porous support membrane.
[0039] Depend on Figure 2 It can be seen that the composite gas separation membrane prepared in Example 1 has a relatively clear layered cross-sectional structure, with a selective layer, a transition layer, and a porous support layer visible from top to bottom. The surface selective layer is continuous and relatively dense, and no obvious macroscopic defects such as through-holes or cracks were observed, indicating that the two-dimensional polyarylamide nanosheets can form a relatively complete gas selective separation structure after filtration deposition and subsequent cross-linking treatment.
[0040] The transition layer beneath the selective layer possesses a rich microporous structure and forms a continuous connection with the underlying porous support layer. This structure reduces the mass transfer resistance caused by the dense selective layer directly blocking the macropores of the support membrane, and also improves the bonding stability between the selective and support layers. Cross-sectional morphology shows that the layers are tightly bonded, with no obvious delamination or interface separation, indicating that the composite selective layer can be stably loaded onto the surface of the modified porous support membrane.
[0041] Example 2
[0042] This embodiment provides a two-dimensional polyarylamide composite gas separation membrane for carbon capture, the preparation method of which includes the following steps:
[0043] S1. Preparation of amino-terminated two-dimensional polyarylamide nanosheets: 90 mL of N-methylpyrrolidone and 10 mL of pyridine were added to a reaction flask, followed by melamine, and the mixture was stirred and dispersed evenly. Tristyrene chloride was dissolved in 10 mL of N-methylpyrrolidone and slowly added to the above reaction solution, wherein the molar ratio of melamine to tristyrene chloride was 1.125:1. The reaction was carried out at 28 °C for 15 h. After the reaction was completed, the nanosheets were centrifuged and washed with N-methylpyrrolidone and anhydrous ethanol. The nanosheets were then redispersed in N-methylpyrrolidone and ultrasonically exfoliated for 1.5 h to obtain an amino-terminated two-dimensional polyarylamide nanosheet dispersion.
[0044] S2. Preparation of modified porous support membrane: The polyacrylonitrile porous membrane was placed in a dopamine Tris buffer solution with a concentration of 4 mg / mL and a pH of 8.5 and subjected to self-polymerization reaction at room temperature for 9 h; after removal, it was rinsed with deionized water and dried to obtain the modified porous support membrane.
[0045] S3. Preparation of composite selective layer film-forming solution: Take a dispersion containing 1.00 g of amino-terminated two-dimensional polyarylamide nanosheets, add 0.08 g of 1,4-butanediol diglycidyl ether and 0.03 g of diaminopropyl-terminated polysiloxane, and stir for 30 min; then add 0.065 g of polyethylene glycol diglycidyl ether with a number average molecular weight of 750, continue stirring for 30 min, and ultrasonically disperse for 20 min to obtain the composite selective layer film-forming solution.
[0046] S4. Preparation of composite gas separation membrane: The composite selective layer film-forming solution obtained in step S3 is deposited on the surface of the interface transition layer of the modified porous support membrane obtained in step S2 by vacuum filtration. Then, it is dried at 45°C for 2 hours and then heat-treated at 60°C for 6.5 hours to obtain a two-dimensional polyarylamide composite gas separation membrane for carbon capture.
[0047] Example 3
[0048] This embodiment provides a two-dimensional polyarylamide composite gas separation membrane for carbon capture, the preparation method of which includes the following steps:
[0049] S1. Preparation of amino-terminated two-dimensional polyarylamide nanosheets: 90 mL of N-methylpyrrolidone and 7 mL of pyridine were added to a reaction flask, followed by melamine. The mixture was stirred and dispersed evenly. Tristyroyl chloride was dissolved in 15 mL of N-methylpyrrolidone and slowly added to the above reaction solution. The molar ratio of melamine to tristyroyl chloride was 1.20:1. The reaction was carried out at 35 °C for 20 h. After the reaction was completed, the nanosheets were centrifuged and washed with N-methylpyrrolidone and anhydrous ethanol. The nanosheets were then redispersed in N-methylpyrrolidone and subjected to high-speed shearing and exfoliation for 2 h to obtain an amino-terminated two-dimensional polyarylamide nanosheet dispersion.
[0050] S2. Preparation of modified porous support membrane: The polyacrylonitrile porous membrane was placed in a dopamine Tris buffer solution with a concentration of 5 mg / mL and a pH of 9.0 and subjected to self-polymerization reaction at room temperature for 10 h; after removal, it was rinsed with deionized water and dried to obtain the modified porous support membrane.
[0051] S3. Preparation of composite selective layer film-forming solution: Take a dispersion containing 1.00 g of amino-terminated two-dimensional polyarylamide nanosheets, add 0.10 g of ethylene glycol diglycidyl ether and 0.04 g of diaminopropyl-terminated polysiloxane, and stir for 40 min; then add 0.08 g of polyethylene glycol diglycidyl ether with a number average molecular weight of 1000, continue stirring for 40 min, and ultrasonically disperse for 30 min to obtain the composite selective layer film-forming solution.
[0052] S4. Preparation of composite gas separation membrane: The composite selective layer film-forming solution obtained in step S3 is deposited on the surface of the interface transition layer of the modified porous support membrane obtained in step S2 by vacuum filtration. Then, it is dried at 50°C for 2 hours and then heat-treated at 65°C for 8 hours to obtain a two-dimensional polyarylamide composite gas separation membrane for carbon capture.
[0053] Comparative Example 1
[0054] The difference between this comparative example and Example 3 is that ethylene glycol diglycidyl ether is not added in step S3, while the amounts of other raw materials and preparation steps are the same as in Example 3.
[0055] Comparative Example 2
[0056] The difference between this comparative example and Example 3 is that diaminopropyl-terminated polysiloxane is not added in step S3, while the amounts of other raw materials and preparation steps are the same as in Example 3.
[0057] Comparative Example 3
[0058] The difference between this comparative example and Example 3 is that the dopamine self-polymerization treatment in step S2 is not performed. Instead, a polyacrylonitrile porous membrane is used directly as the support membrane, and the composite selective layer film-forming solution obtained in step S3 is deposited on the surface of the polyacrylonitrile porous membrane. The remaining raw material amounts and preparation steps are the same as in Example 3.
[0059] 1. Gas separation performance test
[0060] The test was conducted according to GB / T40260-2021 "Test Method for Gas Permeability Performance of Polymer Membrane Materials". The membrane to be tested was vacuum dried at 40℃ for 12h, and then fixed in the gas permeability test cell. The effective test area of the membrane was 12.56cm². The test temperature was 25±1℃, the feed-side pressure was 0.30MPa, and CO2, N2 and CH4 with a purity of not less than 99.99% were introduced respectively.
[0061] After the gas permeation reaches a steady state, the gas permeability of CO2, N2, and CH4 is measured, and the ideal selectivity is calculated according to the following formula:
[0062] αCO2 / N2 = JCO2 / JN2;
[0063] αCO2 / CH4=JCO2 / JCH4.
[0064] In the formula, JCO2, JN2, and JCH4 are the gas permeability of CO2, N2, and CH4, respectively.
[0065] In addition, a CO2 / N2 mixture with a volume ratio of 15:85 was used for actual separation performance testing. The test temperature was 25±1℃, and the feed-side pressure was 0.50MPa. After the operation stabilized, the gas composition on the feed side and the permeate side was determined using gas chromatography, and the separation factor of the CO2 / N2 mixture was calculated.
[0066] 2. Long-term operational stability test
[0067] A CO2 / N2 mixture with a volume ratio of 15:85 was used for continuous operation testing. The test temperature was 25±1℃, the feed-side pressure was 0.50MPa, and the continuous operation lasted for 168 hours.
[0068] The CO2 permeability and CO2 / N2 mixture separation factor were measured before and after 168 hours of operation, and the performance retention rate was calculated according to the following formula:
[0069] CO2 transmission rate retention rate = CO2 transmission rate after 168 hours of operation / initial CO2 transmission rate × 100%; Separation factor retention rate = CO2 / N2 separation factor after 168 hours of operation / initial CO2 / N2 separation factor × 100%.
[0070] 3. Pressure Cyclic Stability Test
[0071] A CO2 / N2 mixture with a volume ratio of 15:85 was used as the test gas, and a pressure cycling test was conducted at 25±1℃.
[0072] The feed-side pressure is increased from 0.10 MPa to 1.0 MPa, held for 30 minutes, then decreased to 0.10 MPa and held for 30 minutes. This is one cycle, and a total of 20 pressure cycles are performed.
[0073] After the cycle was completed, the separation factor of the CO2 / N2 mixture was re-measured under 0.50 MPa conditions, and the retention rate of the separation factor after pressure cycling was calculated.
[0074] Table 1: Gas separation performance tests of each embodiment and comparative example
[0075] Group <![CDATA[CO₂ Permeance Rate / GPU]]> <![CDATA[CO2 / N2 ideal selectivity]]> <![CDATA[CO2 / CH4 ideal selectivity]]> <![CDATA[CO₂ / N₂ mixture separation factor]]> Example 1 1092 58.7 44.3 52.5 Example 2 1115 60.1 45.5 53.8 Example 3 1104 59.4 44.9 53.1 Comparative Example 1 1258 34.6 30.5 30.2 Comparative Example 2 762 49.8 38.7 43.9 Comparative Example 3 1015 40.8 32.6 35.4
[0076] Table 2: Operational stability performance tests of each embodiment and comparative example
[0077] Group <![CDATA[CO2 transmittance retention rate after 168h / %]]> Separation factor retention rate after 168 hours / % Separation factor retention rate after 20 pressure cycles / % Example 1 97.3 97.5 96.8 Example 2 98.2 98.5 98.0 Example 3 97.7 98.0 97.4 Comparative Example 1 86.2 83.8 82.5 Comparative Example 2 91.1 91.5 89.7 Comparative Example 3 79.6 78.5 75.9
[0078] As shown in Table 1, the CO2 permeability, ideal CO2 / N2 selectivity, ideal CO2 / CH4 selectivity, and CO2 / N2 mixed gas separation factor of Examples 1-3 all remained at a high level, indicating that the composite selective layer structure used in this invention has good stability and repeatability. In contrast, each comparative example showed varying degrees of decrease in gas permeability or separation selectivity, indicating that the short-chain diepoxide, diaminopropyl-terminated polysiloxane, and polydopamine interfacial transition layer each have irreplaceable roles.
[0079] Comparative Example 1, without the addition of ethylene glycol diglycidyl ether, showed an increased CO2 permeability of 1258 GPU, higher than the 1104 GPU of Example 3. However, the ideal CO2 / N2 selectivity decreased from 59.4 to 34.6, the ideal CO2 / CH4 selectivity decreased from 44.9 to 30.5, and the CO2 / N2 mixed gas separation factor decreased from 53.1 to 30.2. This is because the short molecular chain of ethylene glycol diglycidyl ether allows it to cross-link with the amino groups on the surface of the amino-terminated two-dimensional polyarylamide nanosheets, enabling close-range connection and fixation of adjacent nanosheets and sealing larger pores and cracks between the layers. Without this component, the constraint between the two-dimensional nanosheets weakens, the interlayer free space increases, and the gas transport resistance decreases, thus improving the CO2 permeability. However, at the same time, some larger non-selective transport channels were not effectively sealed, and N2 and CH4 could more easily pass through the membrane, resulting in a significant decrease in gas separation selectivity. Therefore, Comparative Example 1 shows that short-chain diepoxides mainly play the role of fixing the lamellar structure and sealing non-selective defects, and their absence will result in "increased transmittance and significantly decreased selectivity".
[0080] Comparative Example 2, without the addition of diaminopropyl-terminated polysiloxane, showed a CO2 permeability of 762 GPU, the lowest among all groups. Simultaneously, the ideal selectivity for CO2 / N2, CO2 / CH4, and the separation factor for the CO2 / N2 mixture decreased to 49.8, 38.7, and 43.9, respectively. The diaminopropyl-terminated polysiloxane possesses flexible siloxane segments that can be inserted between rigid two-dimensional polyarylamide nanosheets, adjusting the interlayer spacing and mitigating excessively dense packing of the two-dimensional nanosheets during drying and heat treatment. Without this component, the two-dimensional nanosheets are more prone to close packing under the cross-linking effect of short-chain diepoxides, leading to a reduction in effective interlayer channels and an increase in CO2 diffusion resistance, thus significantly reducing CO2 permeability. Furthermore, due to the lack of buffering and stress-regulating effects from the flexible segments, the membrane layer is prone to uneven local shrinkage during drying, heat treatment, and operation, resulting in excessive density in some areas and the formation of micro-defects in others, reducing the uniformity of the membrane structure and consequently decreasing the separation selectivity to some extent. The results indicate that diaminopropyl-terminated polysiloxanes mainly play a role in adjusting interlayer spacing, maintaining effective gas transport channels, and improving film flexibility.
[0081] Comparative Example 3, without the polydopamine interfacial transition layer, had a CO2 permeability of 10¹⁵ GPU, slightly lower than Example 3, but its ideal CO2 / N₂ selectivity, ideal CO₂ / CH₄ selectivity, and CO₂ / N₂ mixed gas separation factor decreased to 40.8, 32.6, and 35.4, respectively. The polydopamine interfacial transition layer improves the wettability of the polyacrylonitrile porous support membrane surface, enhances the spreading and deposition uniformity of the composite selective layer film-forming solution on the support membrane surface, and strengthens the interfacial bonding between the selective layer and the support layer. Without the polydopamine layer, the composite selective layer is prone to uneven local deposition on the polyacrylonitrile support membrane surface. Some film-forming components may enter the support membrane pores, causing local blockage and reducing the effective CO₂ permeation area. On the other hand, some areas are prone to forming pores, cracks, or interfacial defects, leading to non-selective permeation of N₂ and CH₄. Therefore, its CO₂ permeability decreased slightly, while the separation selectivity significantly decreased. This demonstrates that the polydopamine interfacial transition layer plays an important role in improving film uniformity, reducing interfacial defects, and stabilizing the composite film structure.
[0082] As shown in Table 2, after 168 hours of continuous operation and 20 pressure cycles, the CO2 permeability retention rate and separation factor retention rate of Examples 1-3 remained at a high level, indicating that the composite gas separation membrane prepared by the present invention has good long-term operational stability and resistance to pressure fluctuations.
[0083] After 168 hours, the CO2 permeability retention rate, separation factor retention rate, and separation factor retention rate after pressure cycling in Comparative Example 1 decreased to 86.2%, 83.8%, and 82.5%, respectively. This is because the lack of short-chain dieoxy compounds reduced the number of close-range crosslinking points between the two-dimensional polyarylamide nanosheets, resulting in insufficient sheet fixation. Under continuous airflow impact and pressure changes, the sheets are more prone to slippage, rearrangement, and interlayer spacing changes, further amplifying existing defects and thus significantly reducing long-term stability.
[0084] The retention rates of the above three items in Comparative Example 2 were 91.1%, 91.5%, and 89.7%, respectively. Although these were lower than those in Example 3, they were still superior to those in Comparative Examples 1 and 3. This is because the cross-linked structure formed by ethylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether still exists in its system, and the film layer still has a certain degree of structural stability. However, due to the lack of flexible polysiloxane segments, the film layer's ability to resist internal stress and pressure changes is reduced. During long-term operation, it is prone to local densification, structural shrinkage, or the propagation of micro-defects, thus resulting in a decrease in performance retention.
[0085] Comparative Example 3 exhibited the worst long-term stability, with CO2 permeability retention, separation factor retention, and separation factor retention after pressure cycling remaining at only 79.6%, 78.5%, and 75.9%, respectively. This is attributed to the lack of a polydopamine interfacial transition layer, resulting in insufficient bonding strength between the composite selective layer and the polyacrylonitrile support membrane. During continuous operation and repeated pressure changes, relative displacement, local delamination, or interfacial defect propagation easily occur between the selective and support layers, leading to a continuous decline in gas separation performance. These results further demonstrate that the polydopamine interfacial transition layer plays a significant role in improving the interfacial stability between the selective and support layers.
[0086] As shown in Tables 1 and 2, the short-chain diepoxide compound is mainly used to seal non-selective defects and fix two-dimensional nanosheets; the diaminopropyl-terminated polysiloxane is mainly used to adjust the interlayer spacing, reduce excessive dense packing, and alleviate internal stress in the membrane; the polydopamine interfacial transition layer is mainly used to improve the deposition uniformity of the selective layer and the interfacial bonding stability. The components work together to enable the composite gas separation membrane to simultaneously maintain high CO2 permeability, good gas separation selectivity, and good long-term operational and pressure cycling stability.
[0087] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0088] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
[0089] Those skilled in the art should understand that the above descriptions are merely several specific embodiments of the present invention, and not all embodiments.
Claims
1. A two-dimensional polyarylamide composite gas separation membrane for carbon capture, characterized in that, It includes a porous support layer, an interface transition layer disposed on the surface of the porous support layer, and a composite selective layer disposed on the surface of the interface transition layer; The composite selective layer comprises amino-terminated two-dimensional polyarylamide nanosheets, short-chain diesters, diaminopropyl-terminated polysiloxanes, and polyethylene glycol diglycidyl ether. The amino-terminated two-dimensional polyarylamide nanosheets are prepared by polycondensation reaction of melamine and trimesoyl chloride, wherein the molar ratio of melamine to trimesoyl chloride is 1.05-1.20:
1. The short-chain diepoxide compound is one of ethylene glycol diglycidyl ether and 1,4-butanediol diglycidyl ether; the number average molecular weight of the polyethylene glycol diglycidyl ether is 500-1000.
2. The two-dimensional polyarylamide composite gas separation membrane for carbon capture according to claim 1, characterized in that, Based on 100 parts by weight of amino-terminated two-dimensional polyarylamide nanosheets, the amount of the short-chain diester compound is 6-10 parts by weight, the amount of the diaminopropyl-terminated polysiloxane is 2-4 parts by weight, and the amount of the polyethylene glycol diglycidyl ether is 5-8 parts by weight.
3. The two-dimensional polyarylamide composite gas separation membrane for carbon capture according to claim 1, characterized in that, The porous support layer is a polyacrylonitrile porous membrane; the interface transition layer is a polydopamine layer.
4. A method for preparing a two-dimensional polyarylamide composite gas separation membrane for carbon capture as described in any one of claims 1-3, characterized in that, Includes the following steps: S1. Melamine and pyromellitic methyl chloride were added to an organic reaction medium to carry out a polycondensation reaction. After the reaction was completed, the mixture was washed, dispersed and exfoliated to obtain a dispersion of amino-terminated two-dimensional polyarylamide nanosheets. S2. The porous support membrane is placed in a dopamine buffer solution to carry out a self-polymerization reaction, and an interface transition layer is formed on the surface of the porous support membrane to obtain a modified porous support membrane. S3. Add a short-chain dieoxy compound and a diaminopropyl-terminated polysiloxane to the amino-terminated two-dimensional polyarylamide nanosheet dispersion, and stir for 20-40 min; then add polyethylene glycol diglycidyl ether, continue stirring for 20-40 min, and ultrasonically disperse for 10-30 min to obtain a composite selective layer film-forming solution. S4. The composite selective layer film-forming solution is deposited on the surface of the interface transition layer of the modified porous support membrane, and then dried and heat-treated sequentially to obtain the two-dimensional polyarylamide composite gas separation membrane for carbon capture.
5. The method for preparing the two-dimensional polyarylamide composite gas separation membrane for carbon capture according to claim 4, characterized in that, In step S1, the organic reaction medium includes N-methylpyrrolidone and pyridine, and the volume ratio of N-methylpyrrolidone to pyridine is 5-15:1; the polycondensation reaction temperature is 20-35℃ and the time is 12-20h; the exfoliation treatment is ultrasonic exfoliation or high-speed shear exfoliation.
6. The method for preparing a two-dimensional polyarylamide composite gas separation membrane for carbon capture according to claim 4, characterized in that, In step S2, the dopamine buffer solution is a Tris buffer solution, wherein the concentration of dopamine is 3-5 mg / mL, the pH value is 8.0-9.0, and the self-polymerization reaction time is 8-10 h.
7. The method for preparing the two-dimensional polyarylamide composite gas separation membrane for carbon capture according to claim 4, characterized in that, In step S4, the deposition method is vacuum filtration deposition, the heat treatment temperature is 55-65℃, and the heat treatment time is 5-8h.
Citation Information
Patent Citations
CO2 gas separation membrane and preparation method thereof
CN116571095A