Polymers for photoresists, block copolymers for photoresists, and methods of making and using the same

By employing iodine transfer polymerization and sulfur-free reversible addition-fragmentation chain transfer polymerization methods, the problem of non-uniformity in the polymer structure of photoresists in existing technologies has been solved, enabling precise control of polymer molecular weight and improvement of photolithography performance, making it suitable for the preparation of high-performance photoresists.

CN122647652BActive Publication Date: 2026-11-24SUZHOU LABORATORY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611163950.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-03
Publication Date
2026-11-24
Estimated Expiration
2046-08-03

AI Technical Summary

Technical Problem

In existing photoresist polymerization methods, RAFT and ATRP technologies suffer from problems with thioester terminal groups and metal ion catalysts, leading to a decline in photolithography performance and making it difficult to meet the stringent requirements of high-performance photoresists for polymer structure uniformity.

Method used

By employing iodine transfer polymerization and sulfur-free reversible addition-fragmentation chain transfer polymerization methods, the use of metal catalysts and sulfur residues is avoided, enabling precise control of the number-average molecular weight of polymers in the range of 3000~30000 g/mol and a narrow molecular weight distribution.

Benefits of technology

It significantly reduces the adverse effects of residual terminal groups and metal impurities on photolithography performance, improves the exposure sensitivity of photoresist and reduces line edge roughness, making it suitable for high-performance photolithography applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122647652B_ABST
    Figure CN122647652B_ABST
Patent Text Reader

Abstract

This invention provides a polymer for photoresists, a block copolymer for photoresists, its preparation method, and its applications. The preparation method is based on iodine transfer polymerization or sulfur-free reversible addition-fragmentation chain transfer polymerization, which has the advantages of no metal catalysis, no sulfur residue, and high polymerization controllability. It can achieve precise control of the polymer's number-average molecular weight within the range of 3000~30000 g / mol, and the polymer molecular weight distribution is relatively narrow. The preparation method provided by this invention effectively avoids the photolithographic performance degradation problem caused by existing RAFT and ATRP polymerizations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer synthesis and semiconductor photolithography technology, specifically relating to a polymer for photoresist, a block copolymer for photoresist, and their preparation methods and applications. Background Technology

[0002] Line edge roughness (LER) and line width roughness (LWR) are key challenges in the current advanced integrated circuit miniaturization process. Especially in EUV lithography, these roughnesses have a significant impact on device performance and production yield. Pattern roughness not only causes fluctuations in electrical performance, such as threshold voltage drift, current leakage, and reduced device speed, but it is also amplified in subsequent etching or deposition processes, thus affecting the structural consistency and reliability of the final device. Among the many factors affecting pattern roughness, the molecular structure characteristics of the polymer resin in the photoresist play a crucial role. In particular, the sequence distribution of monomers in the polymer chain and the overall molecular weight distribution (MWD) significantly affect the phase separation behavior, acid diffusion characteristics, and dissolution interface stability during development. These microstructural heterogeneities easily lead to irregularities at the pattern edges, resulting in high LER / LWR. Therefore, preparing polymer systems with a more uniform molecular weight distribution can effectively reduce compositional fluctuations within the material, improve the spatial uniformity of the photo-induced acid reaction, and enhance the stability of the interface response of the photoresist during exposure, post-baking (PEB), and development. This will help achieve higher resolution, steeper edges, and lower roughness during imaging, thereby improving the performance and reliability of the photolithography process.

[0003] In the preparation of photoresist matrix resins, the use of reversible-deactivation radical polymerization (RDRP) technology to precisely control the molecular weight and distribution of polymers has become an important research direction of interest in the industry. For example, among existing technologies, DuPont has developed a method for synthesizing photoresist resins suitable for 193nm wavelengths using reversible addition-fragmentation chain transfer polymerization (RAFT); Milan Mari The research group applied nitroxide-mediated polymerization (NMP) technology to the controllable synthesis of photoresist resins; meanwhile, atom transfer radical polymerization (ATRP) has also been widely studied and applied in this field.

[0004] However, the NMP method exhibits poor polymerization controllability when polymerizing methyl methacrylate monomers. It is usually difficult to achieve a narrow molecular weight distribution (e.g.) ≤1.3), with a distribution range generally between 1.3 and 1.5, which cannot meet the stringent requirements of high-performance photoresists for polymer structure uniformity. Although RAFT and ATRP technologies can achieve higher molecular weight control precision (e.g., by using thioester chain transfer agents and copper-based catalysts, respectively) While the specific concentrations (≤1.25) are relatively low, their inherent defects also limit the final material properties. Specifically, the thioester terminal groups introduced in RAFT polymerization tend to have strong absorption characteristics at deep ultraviolet wavelengths, causing unexpected light attenuation and thus increasing LER. Similarly, the residual metal ion catalyst in the ATRP polymerization system can also reduce exposure sensitivity and may adversely affect the device structure.

[0005] Therefore, developing a polymerization method with low residue, weak side reactivity, and suitability for high-performance photolithography applications is an important way to realize the industrial production and performance improvement of this type of functional polymer material. Summary of the Invention

[0006] To solve all or part of the above-mentioned technical problems, the present invention provides the following technical solutions: A first aspect of the present invention provides a method for preparing a polymer for photoresist, the method being based on iodine transfer polymerization or sulfur-free reversible addition-fragmentation chain transfer polymerization; The preparation method based on iodine transfer polymerization includes: subjecting a first mixed reaction system containing a first monomer, an iodine transfer agent, and a free radical thermal initiator to an iodine transfer polymerization reaction to obtain a polymer for photoresist; The preparation method based on sulfur-free reversible addition-fragmentation chain transfer polymerization includes: subjecting a second mixed reaction system containing a first monomer, a sulfur-free RAFT chain transfer agent, and a free radical thermal initiator to a sulfur-free reversible addition-fragmentation chain transfer polymerization reaction to obtain a photoresist matrix resin; The first monomer includes one or a combination of styrene monomers, (meth)acrylate monomers, (meth)acrylamide monomers, and fluorine-containing functional monomers.

[0007] The preparation method provided by this invention, based on iodine transfer polymerization or sulfur-free reversible addition-fragmentation chain transfer polymerization, has the advantages of requiring no metal catalyst, having no sulfur residue, and high polymerization controllability. It can achieve precise control of the polymer's number-average molecular weight within the range of 3000~30000 g / mol, with a narrow molecular weight distribution. This preparation method avoids the use of sulfur-based chain transfer agents in existing RAFT polymerization and metal catalysts in ATRP polymerization systems, significantly reducing the adverse effects of residual terminal groups and metal impurities on photolithography performance (especially exposure sensitivity and line edge roughness).

[0008] In some embodiments, the total concentration of the first monomer in the first mixed reaction system is 2.5-3.5 mol / L.

[0009] In some embodiments, the total concentration of the first monomer in the second mixed reaction system is 2.5-3.5 mol / L.

[0010] In some embodiments, the molar ratio of the first monomer to the iodine transfer agent is determined according to the target degree of polymerization formula. The regulation is defined as follows: n represents the degree of polymerization, [M0] represents the initial molar concentration of the first monomer, [CTA0] represents the initial molar concentration of the iodine transfer agent, and C represents the monomer conversion rate, which satisfies 0.90. <C<0.99。

[0011] In some embodiments, the molar ratio of the first monomer to the sulfur-free RAFT chain transfer agent is determined according to the target degree of polymerization formula. The regulation is defined as follows: n represents the degree of polymerization, [M0] represents the initial molar concentration of the first monomer, [CTA0] represents the initial molar concentration of the sulfur-free RAFT chain transfer agent, and C represents the monomer conversion rate, which satisfies 0.90. <C<0.99。

[0012] In some embodiments, the molar ratio of the iodine transfer agent to the free radical thermal initiator is 2:1 to 10:1.

[0013] In some embodiments, the molar ratio of the sulfur-free RAFT chain transfer agent to the free radical thermal initiator is 2:1 to 10:1.

[0014] In some embodiments, the temperature of the iodine transfer polymerization reaction is 60-110°C.

[0015] In some embodiments, the reaction time of the iodine transfer polymerization reaction is 12h to 24h.

[0016] In some embodiments, the iodine transfer polymerization reaction is carried out under light-protected and inert atmosphere conditions after the first mixed reaction system is deoxygenated.

[0017] In some embodiments, the temperature of the sulfur-free reversible addition-fragmentation chain transfer polymerization reaction is 60-110°C.

[0018] In some embodiments, the reaction time of the sulfur-free reversible addition-fragmentation chain transfer polymerization reaction is 12 h to 24 h.

[0019] In some embodiments, the second mixed reaction system is deoxygenated and then subjected to the sulfur-free reversible addition-fragmentation chain transfer polymerization reaction under an inert atmosphere.

[0020] In some embodiments, the iodine transfer agent has the general formula R1-I or Z-R2-I; wherein R1 is selected from C1-C 20 Any one of alkyl, acyl, aryl, polymer chain, iodine atom, or HI2C group; Z is selected from any one of alkoxy, ester, carboxyl, or isocyanate group; R2 is selected from C1-C. 12 Alkylene or aryleneene. In the general formula Z-R2-I, Z can be considered as a functional group, and R2 can be considered as a stabilizing group.

[0021] In some embodiments, the iodine transfer agent satisfying general formula R1-I includes one or a combination of iodoform, iodooctane, and (1-iodoethyl)benzene.

[0022] In some embodiments, the iodine transfer agent satisfying the general formula Z-R2-I includes one or a combination of more of ethyl 4-iodobutyrate, ethyl 2-iodopropionate, and 2-iodo-2-methylpropionitrile.

[0023] In some embodiments, the sulfur-free RAFT chain transfer agent satisfies formula A:

[0024] Formula A R3 represents the leaving group, selected from any one of isobutyryloxy, propionyloxy, N-methylisobutyramido, N-methylpropionamido, cyano, phenyl, and p-methoxyphenyl; Y represents the stationary group, selected from any one of isobutyryloxy, phenyl, p-methylphenyl, and p-methoxyphenyl.

[0025] In some embodiments, the sulfur-free RAFT chain transfer agent includes one or more of the compounds shown in A1 to A6; .

[0026] In some embodiments, the styrene monomers include, but are not limited to, one or a combination of p-acetoxystyrene, styrene, tert-butyl 4-vinylphenyl carbonate, and p-methylstyrene. The styrene monomers can provide an aromatic backbone for the polymer resin used in photoresists, improving its film-forming properties.

[0027] In some embodiments, the (meth)acrylate monomers include, but are not limited to, one or more combinations of tert-butyl acrylate, n-butyl acrylate, methyl methacrylate, isobornyl methacrylate, hydroxyethyl methacrylate, 1-methylcyclopentyl methacrylate, 2-methyl-2-adamantyl methacrylate, and 3-methacrylate-4-butyrolactone. The (meth)acrylate monomers can incorporate photosensitive protective groups and modify material properties.

[0028] In some embodiments, the (meth)acrylamide monomers include, but are not limited to, one or a combination of acrylamide, N-methylacrylamide, and N,N-dimethylacrylamide. The (meth)acrylamide monomers can improve the hydrophilicity, adhesion, and development behavior of photoresist polymer resins.

[0029] In some embodiments, the fluorinated functional monomers include, but are not limited to, one or more combinations of tridecylfluorooctyl methacrylate, perfluoroalkyl methacrylate, and fluorostyrene derivatives. The fluorinated functional monomers can reduce the surface energy of the polymer and improve its hydrophobicity.

[0030] In some embodiments, the free radical thermal initiator includes at least one of azo initiators and peroxide initiators. The free radical thermal initiator can decompose at a certain temperature to generate free radicals, initiating the polymerization reaction.

[0031] In some embodiments, the azo initiator includes one or more of azobisisobutyronitrile (AIBN), azobisisoheptanenitrile (AIPH), and dimethyl azobisisobutyrate (MMAIBN), but is not limited thereto.

[0032] In some embodiments, the peroxide initiator includes one or more of benzoyl peroxide (BPO) and dicumyl peroxide (DCP), but is not limited thereto.

[0033] In some embodiments, the first mixed reaction system and the second mixed reaction system further include a solvent.

[0034] In some embodiments, the solvent includes one or more of tetrahydrofuran (THF), methyl ethyl ketone (MEK), propylene glycol monomethyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), hexafluoroisopropanol (HFIP), dimethyl carbonate (DMC), diethyl carbonate (DEC), toluene, and xylene.

[0035] In some embodiments, the first and second mixed reaction systems further include a regulator, which includes, but is not limited to, one or more of tetrabutylammonium iodide, tetrapropylammonium iodide, tetrahexylammonium iodide, sodium iodide, and potassium iodide. The regulator can be used to control the polymerization activity of various free radicals when there are significant differences, thereby further reducing the polymer molecular weight distribution.

[0036] In some embodiments, the amount of the regulator added is 0.1-1 molar equivalent of the iodine transfer agent or the sulfur-free RAFT chain transfer agent.

[0037] In some embodiments, the preparation method further includes separating the obtained polymer using a precipitant after the reaction is complete. The precipitant may include, for example, methanol, ethanol, diethyl ether, n-hexane, cyclohexane, water, etc.

[0038] For example, the method for preparing the polymer for photoresist includes the following steps: (1) Construction of reaction system: Dissolve the first monomer in a solvent and add a free radical thermal initiator, an iodine transfer agent or a sulfur-free RAFT chain transfer agent to obtain a mixed reaction system; (2) Polymerization reaction: After the mixed reaction system is deoxygenated by three cycles of liquid nitrogen freezing-vacuuming-thawing, a living polymerization reaction is carried out at 60~110℃ for 12~24 hours under an inert atmosphere (iodine transfer polymerization also requires protection from light). The polymerization is stopped when the monomer conversion is complete (monomer conversion rate is greater than 90%). 1 H-NMR monitoring); (3) Product purification: The reaction liquid is added dropwise to the precipitant, and after repeated dissolution and precipitation, it is filtered, washed and dried to obtain the polymer for photoresist.

[0039] A second aspect of the present invention provides a polymer for photoresist, which is prepared by any of the above-described methods for preparing a polymer for photoresist.

[0040] In some embodiments, the number-average molecular weight of the polymer used for the photoresist is 3000~30000 g / mol.

[0041] In some embodiments, the molecular weight distribution of the polymer used for the photoresist ( The value is below 1.25.

[0042] A third aspect of the present invention provides a method for preparing a block copolymer for photoresist, comprising: A polymer for photoresist is prepared by any of the above preparation methods and used as a macromolecular chain transfer agent; A third mixed reaction system containing the aforementioned photoresist polymer and the second monomer is subjected to a polymerization reaction to obtain a block copolymer for photoresist; The second monomer includes one or more of styrene monomers, (meth)acrylate monomers, (meth)acrylamide monomers, and fluorine-containing functional monomers, and the second monomer may be the same as or different from the first monomer.

[0043] Further selection of the styrene monomers, (meth)acrylate monomers, (meth)acrylamide monomers, and fluorine-containing functional monomers has been described in detail in the first aspect of the present invention, and will not be repeated here.

[0044] In some embodiments, the preparation method specifically includes: introducing the second monomer in batches into a solution containing the polymer for photoresist under an inert atmosphere, wherein the amount of the second monomer added is 2-6 times the molar amount of the polymer for photoresist, and the reaction continues for a preset time after the second monomer is completely added.

[0045] In some embodiments, the polymerization reaction temperature is 60°C to 110°C.

[0046] In some embodiments, the preset time is 20h~25h.

[0047] For example, the method for preparing the block copolymer for photoresist includes the following steps: (1) A polymer for photoresist is prepared by the preparation method described in any one of the technical solutions of the first aspect of the present invention; (2) Dissolve the photoresist polymer in a solvent, maintain a reaction temperature of 60°C to 110°C, and add the second monomer in 3 to 5 gradients under nitrogen protection; each addition is 25 to 35 minutes apart, and the total amount of the second monomer added is 2 to 6 times the molar amount of the polymer obtained in step (1); after the addition is complete, continue the reaction for 20 to 25 hours, and stop when the second monomer is completely converted (monomer conversion rate is greater than 90%). 1 H-NMR monitoring); (3) The reaction solution was added dropwise to the precipitant, filtered, washed, and dried to obtain the molecular weight distribution (Molecular weight distribution). Block copolymers with a strength of 1.25 or less.

[0048] A fourth aspect of the present invention provides a block copolymer for photoresist, which is prepared by the method for preparing a block copolymer for photoresist as described in any of the technical solutions.

[0049] In some embodiments, the number-average molecular weight of the block copolymer used for photoresist is 3000~30000 g / mol.

[0050] In some embodiments, the molecular weight distribution of the block copolymer used in the photoresist ( The value is below 1.25.

[0051] The fifth aspect of the present invention provides the use of the polymer for photoresist or the block copolymer for photoresist described in any of the technical solutions in the preparation of photoresist.

[0052] In some embodiments, the application includes: formulating a photoresist composition using the aforementioned photoresist polymer and / or its derivatives, and / or the photoresist block copolymer and / or its derivatives, wherein the derivatives include the photoresist polymer and hydrolysis products of the photoresist block copolymer.

[0053] A sixth aspect of the present invention provides a photoresist composition comprising a base resin, said base resin comprising a photoresist polymer and / or its derivatives as described in any of the technical solutions, and / or a photoresist block copolymer and / or its derivatives, said derivatives comprising the photoresist polymer and hydrolysis products of the photoresist block copolymer.

[0054] In some embodiments, the photoresist composition further includes a photoacid generator, a quencher, and a solvent.

[0055] Compared with existing technologies, the present invention has some or all of the following beneficial effects: The preparation method based on iodine transfer polymerization or sulfur-free reversible addition-fragmentation chain transfer polymerization provided by the present invention has the advantages of no metal catalysis, no sulfur residue, and high controllability of polymerization. It can achieve precise control of the polymer number-average molecular weight within a certain range (e.g., precise control within the range of 3000~30000 g / mol), and a narrow molecular weight distribution (in some preferred embodiments, the molecular weight distribution is no greater than 1.25). The preparation method provided by the present invention is suitable for preparing photoresist matrix resins required for deep ultraviolet lithography processes, providing a good solution for preparing high-purity, low-absorption, and narrow molecular weight distribution photoresist resins, and avoiding the photolithographic performance degradation problems caused by existing RAFT and ATRP polymerizations. Attached Figure Description

[0056] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0057] Figure 1 This is the GPC curve of the polymer obtained in Example 1; Figure 2 It is the polymer obtained in Example 1. 1 H-NMR spectrum; Figure 3This is the GPC curve of the polymer obtained in Example 2; Figure 4 It is the polymer obtained in Example 2. 1 H-NMR spectrum; Figure 5 This is the GPC curve of the polymer obtained in Example 3; Figure 6 It is the polymer obtained in Example 3. 1 H-NMR spectrum; Figure 7 This is the GPC curve of the polymer obtained in Example 4; Figure 8 It is the polymer obtained in Example 4. 1 H-NMR spectrum; Figure 9 This is the GPC curve of the polymer obtained in Example 5; Figure 10 It is the polymer obtained in Example 5. 1 H-NMR spectrum; Figure 11 This is the GPC curve of the polymer obtained in Example 6; Figure 12 This is the GPC curve of the polymer obtained in Example 7; Figure 13 This is the GPC curve of the polymer obtained in Example 8; Figure 14 This is the GPC curve of the polymer obtained in Example 9; Figure 15 This is the ¹H-NMR spectrum of the polymer synthesized in Example 9; Figure 16 This is the DOSY-NMR spectrum of the polymer synthesized in Example 9; Figure 17 This is the ¹H-NMR spectrum of the polymer synthesized in Example 9 after hydrolysis; Figure 18 This is the DOSY-NMR spectrum of the polymer synthesized in Example 9 after hydrolysis; Figure 19 A schematic diagram showing the exposure dose gradient setting for spin-coating a photoresist composition based on the polymer of Example 9 onto a silicon wafer for exposure. Figure 20 This is a thickness mapping diagram of the thin film prepared based on the polymer photoresist composition of Example 9; Figure 21 The contrast curve is based on the polymer photoresist composition of Example 9. Detailed Implementation

[0058] The invention will be more fully understood through the following detailed description of its embodiments. The detailed embodiments disclosed herein are merely illustrative, and the invention may be embodied in various forms. Therefore, the specific functional details disclosed herein should not be construed as limiting, but rather as the basis for the claims.

[0059] In addition, unless otherwise specified, all raw materials used in the following embodiments can be purchased from the market or other sources, and all production and testing equipment used are known in the art, as are the testing methods used.

[0060] This invention develops a synthesis method suitable for photoresist matrix resins based on two controllable free radical polymerization methods: iodine transfer polymerization (ITP) and sulfur-free reversible addition-fragmentation chain transfer polymerization (RAFT Polymerization). Both polymerization methods do not require metal catalysts, possess an active / controllable polymerization mechanism, and have good process compatibility. They allow for precise control of the polymer's number-average molecular weight (Mn) within the range of 3000–30000 g / mol, and precise control of the molecular weight distribution (Mn). The narrower ray retardation path is achieved through this synthetic route, avoiding the use of sulfide chain transfer agents in existing RAFT polymerization and metal catalysts in ATRP polymerization systems. This significantly reduces the adverse effects of residual terminal groups and metal impurities on photolithography performance (especially exposure sensitivity and line edge roughness), providing a new solution for preparing high-purity, low-light-absorption, and uniformly molecular weight photoresist matrix resins. It also exhibits good process adaptability and industrial application potential.

[0061] The principle of iodine transfer polymerization is as follows:

[0062] The principle of sulfur-free reversible addition-fragmentation chain transfer polymerization is as follows: .

[0063] Example 1 This embodiment provides a method for the controlled synthesis of binary random copolymers based on 4-acetoxystyrene (4-AST) and 4-vinylphenyl tert-butyl carbonate (tBVPC) using iodine transfer polymerization, comprising the following steps: In a Schlenk flask, 0.4232 g (2.610 mmol) of 4-AST, 0.5751 g (2.6100 mmol) of tBVPC, 0.0043 g (0.0261 mmol) of azobisisobutyronitrile (AIBN), and 0.0119 g (0.0522 mmol) of ethyl 2-iodopropionate were added and dissolved in 2 mL of DMF to obtain a mixed reaction system. This mixed reaction system was degassed three times by freeze-drying cycles and then reacted at 70 °C in the dark for 16 hours until the monomers were completely consumed. After the reaction was complete, it was quenched by freezing in air (the reaction progress was confirmed by 1H-NMR). The resulting polymer was precipitated with methanol, and the polymer was repeatedly dissolved and precipitated with DMF and methanol, followed by washing with a large amount of methanol. Finally, it was dried under vacuum to obtain 0.8973 g of a white solid binary random copolymer, with a yield of 89.91%.

[0064] Figure 1 This is the GPC curve of the polymer obtained in Example 1. Figure 2 This is the 1H-NMR spectrum of the polymer obtained in Example 1.

[0065] Example 2 This embodiment provides a method for the controlled synthesis of a terpolymer based on p-acetoxystyrene (4-AST), tert-butyl acrylate (TBA), and styrene (St) using iodine transfer polymerization, comprising the following steps: In a Schlenk flask, 0.4100 g (2.53 mmol) of 4-AST, 0.2642 g (2.53 mmol) of TBA, 0.3241 g (2.53 mmol) of St, 0.0062 g (0.0379 mmol) of AIBN, and 0.05977 g (0.1518 mmol) of iodoform were added, and the mixture was dissolved in 3 mL of DMF to obtain a mixed reaction system. This mixed reaction system was degassed three times by freeze-drying cycles and then reacted at 70 °C in the dark for 16 hours until the monomers were completely consumed. After the reaction was complete, it was quenched by exposure to air (the reaction progress was confirmed by 1H-NMR). The resulting polymer was precipitated with methanol, and the polymer was repeatedly dissolved and precipitated using DMF and methanol, followed by washing with a large amount of methanol. Finally, it was dried under vacuum to obtain 0.9120 g of a pale yellow powdery ternary random copolymer, with a yield of 91.20%.

[0066] Figure 3 This is the GPC curve of the polymer obtained in Example 2. Figure 4 This is the 1H-NMR spectrum of the polymer obtained in Example 2.

[0067] Example 3 This embodiment provides a method for the controlled synthesis of terpolymers based on 1-methylcyclopentyl methacrylate (MCPMA), 2-methyl-2-adamantyl methacrylate (MAdMA), and 3-methacrylate-4-butyrolactone (GBLMA) using iodine transfer polymerization, comprising the following steps: In a Schlenk flask, 0.9310 g (5.4800 mmol) of GBLMA, 0.6970 g (2.9700 mmol) of MAdMA, 0.1941 g (1.1500 mmol) of MCPMA, 0.0331 mg (0.2000 mmol) of AIBN, and 0.1571 g (0.4000 mmol) of iodoform were added. Then, 3.5 mL of methyl ethyl ketone was added to dissolve the mixture, yielding a mixed reaction system. This mixed reaction system was degassed through three freeze cycles and then reacted at 70°C in the dark for 20 hours until the monomers were completely consumed. After the reaction was complete, it was quenched by freezing in air (the reaction process was confirmed by 1H-NMR). Subsequently, the polymer was precipitated with methanol, repeatedly dissolved and precipitated with DMF and methanol, and washed with a large amount of methanol. Finally, it was dried under vacuum to obtain 1.5710 g of a pale yellow powdery ternary random copolymer, with a yield of 86.22%.

[0068] Figure 5 This is the GPC curve of the polymer obtained in Example 3. Figure 6 This is the 1H-NMR spectrum of the polymer obtained in Example 3.

[0069] Example 4 Example 4 provides a method for synthesizing poly(FMA-13)-bo-poly(GBLMA-rad-MAdMA-rad-MCPMA) block copolymers, comprising the following steps: (1) Preparation of macromolecular chain transfer agent poly(GBLMA-rad-MAdMA-rad-MCPMA): The steps included adding 1.8620 g (10.9600 mmol) of GBLMA, 1.3940 g (5.8400 mmol) of MAdMA, 0.3882 g (2.3000 mmol) of MCPMA, 0.0413 mg (0.2500 mmol) of AIBN and 0.1969 g (0.5000 mmol) of iodoform to a Schlenk flask, and then adding 7.0 mL of methyl ethyl ketone to dissolve the mixture to obtain a mixed reaction system; after degassing the mixed reaction system through three freeze cycles, it was placed at 70 °C and reacted in the dark for 20 hours until the monomer was completely consumed. After the reaction was completed, it was quenched by freezing in the air (the reaction process was confirmed by 1H-NMR). Subsequently, the polymer was precipitated with methanol, repeatedly dissolved and precipitated with DMF and methanol, and washed with a large amount of methanol. Finally, the product was dried in a vacuum to obtain 2.9780 g of a pale yellow powdery ternary random copolymer with a yield of 81.97%. The number average molecular weight of the obtained macromolecular chain transfer agent was 7100 g / mol, and the molecular weight distribution was 1.14.

[0070] (2) 2.1000 g of the macromolecular chain transfer agent prepared above was added to a three-necked flask, along with 0.0331 g (0.2000 mmol) of AIBN and 7 mL of THF to dissolve the mixture, obtaining a reaction system. After degassing with nitrogen for 40 minutes, the reaction system was placed under reflux at 70 °C in the dark. Next, 0.3890 g (0.900 mmol) of tridecyl methacrylate (FMA-13) was dissolved in 1.5 mL of THF and degassed with nitrogen for 30 minutes. Under nitrogen protection, 0.4000 g of the THF solution of tridecyl methacrylate was added to the reaction system every 30 minutes, and the addition was completed within two hours. Then, the mixture was stirred under reflux at 70 °C in the dark for 24 hours to obtain a block copolymer. After the monomer was completely consumed, the reaction was quenched by freezing in the air (the reaction progress was confirmed by 1H-NMR). Subsequently, the polymer was precipitated in methanol, and the block copolymer was repeatedly dissolved and precipitated with DMF and methanol, followed by washing with a large amount of methanol. Finally, it was dried under vacuum to obtain 2.0800 g of pale yellow powdered block copolymer, with a yield of 83.60%.

[0071] Figure 7 This is the GPC curve of the polymer obtained in Example 4. Figure 8 This is the 1H-NMR spectrum of the polymer obtained in Example 4.

[0072] Example 5 Example 5 provides a method for the controlled synthesis of terpolymers based on 3-hydroxy-1-adamantyl methacrylate (HAdMA), 2-methyl-2-adamantyl methacrylate (MAdMA), and 2-carboxy-6-norbornolactone-5-methacrylate (NLM) using a sulfur-free reversible addition-fragmentation chain transfer polymerization method, comprising the following steps: In a Schlenk flask, 0.0709 g (0.3000 mmol) of HAdMA, 0.1875 g (0.8000 mmol) of MAdMA, 0.2000 g (0.9000 mmol) of NLM, 0.0033 g (0.0200 mmol) of AIBN, and 0.0300 g (0.1000 mmol) of methyl methacrylate trimer (compound A2, as a sulfur-free RAFT chain transfer agent) were added, and the mixture was dissolved in 1 mL of LDM to obtain a mixed reaction system. This mixed reaction system was degassed three times by a freeze cycle and then reacted at 70 °C for 16 hours until the monomers were completely consumed. After the reaction was complete, it was quenched by freezing in air (the reaction progress was confirmed by 1H-NMR). The resulting polymer was precipitated with methanol, and the polymer was repeatedly dissolved and precipitated with MEK and methanol, followed by washing with a large amount of methanol. Finally, the product was dried in a vacuum to obtain 0.4045 g of a white powdery ternary random copolymer, with a yield of 88.41%.

[0073] Figure 9 This is the GPC curve of the polymer obtained in Example 5. Figure 10 This is the 1H-NMR spectrum of the polymer obtained in Example 5.

[0074] Example 6 Example 6 provides a method for the controlled synthesis of a terpolymer based on p-acetoxystyrene (4-AST), tert-butyl acrylate (TBA), and styrene (St) using a sulfur-free reversible addition-fragmentation chain transfer polymerization method, comprising the following steps: In a Schlenk flask, 0.8200 g (5.06 mmol) of 4-AST, 0.5284 g (5.06 mmol) of TBA, 0.6482 g (5.06 mmol) of St, 0.0124 g (0.0758 mmol) of azobisisobutyronitrile (AIBN), and 0.1058 g (0.3036 mmol) of dimethyl-2-[2-(4-methoxyphenyl)enyl]-2,4,4-trimethylglutarate (A6, as a sulfur-free RAFT chain transfer agent) were added, and the mixture was dissolved in 7 mL of DMF to obtain a mixed reaction system. This mixed reaction system was degassed three times by freeze-drying cycles and then reacted at 70 °C in the dark for 16 hours until the monomers were completely consumed. After the reaction was complete, it was quenched by freezing in air (the reaction progress was confirmed by 1H-NMR). The resulting polymer was precipitated with methanol by repeatedly dissolving and precipitating the polymer with DMF and methanol, and then washing with a large amount of methanol. Finally, the product was dried in a vacuum to obtain 1.8340 g of a pale yellow powdery ternary random copolymer, with a yield of 91.84%.

[0075] Figure 11 This is the GPC curve of the polymer obtained in Example 6.

[0076] Example 7 Example 7 provides a method for the controlled synthesis of terpolymers based on methylcyclopentyl methacrylate (MCPMA), 2-methyl-2-adamantyl methacrylate (MAdMA), and 3-methacrylate-4-butyrolactone (GBLMA) using a sulfur-free reversible addition-fragmentation chain transfer polymerization method, comprising the following steps: 0.5420 g (3.1800 mmol) of GBLMA, 0.4060 g (1.7400 mmol) of MAdMA, 0.1120 g (0.6800 mmol) of MCPMA, 0.0164 g (0.1000 mmol) of AIBN, and 0.1052 g (0.3500 mmol) of methyl methacrylate trimer (compound A2, as a sulfur-free RAFT chain transfer agent) were added to a Schlenk flask, and the mixture was dissolved in 2 mL of MEK to obtain a mixed reaction system. This mixed reaction system was degassed three times by freeze-drying cycles and then reacted at 70 °C in the dark for 16 hours until the monomers were completely consumed. After the reaction was complete, it was quenched by freezing in air (the reaction progress was confirmed by 1H-NMR). The resulting polymer was precipitated with methanol by repeatedly dissolving and precipitating the polymer with MEK and methanol, and then washed with a large amount of methanol. Finally, the product was dried in a vacuum to obtain 0.9620 g of a pale yellow powdery ternary random copolymer, with a yield of 90.75%.

[0077] Figure 12 This is the GPC curve of the polymer obtained in Example 7.

[0078] Example 8 Example 8 provides a method for synthesizing poly(FMA-13)-bo-poly(GBLMA-rad-MAdMA-rad-MCPMA) block copolymers, comprising the following steps: (1) Add 1.1400g (6.7000mmol) GBLMA and 0.8520g (3.6400mmol) GBLMA to the Schlenk flask. The following mixture was prepared: 0.2400 g (1.4200 mmol) of MAdMA, 0.0164 mg (0.1000 mmol) of azobisisobutyronitrile (AIBN), and 0.1052 mg (0.3500 mmol) of methyl methacrylate trimer (compound A2, used as a sulfur-free RAFT chain transfer agent). 5 mL of MEK was added to dissolve the mixture, yielding the reaction system. This system was degassed through three freeze cycles and then reacted at 70°C in the dark for 20 hours. After the reaction was complete, a preliminary polymer was obtained by precipitation in methanol and then dried.

[0079] (2) Subsequently, the dried preliminary polymer obtained in step (1) was redissolved in 3 mL of MEK, and 0.0246 g (0.1500 mmol) of AIBN and 1 mL of MEK solution were added. The resulting reaction system was subjected to three more freeze-drying cycles for degassing and stirred at 70 °C in the dark. Next, 0.4760 g (1.1000 mmol) of tridecyl methacrylate (FMA-13) was dissolved in 2 mL of MEK and degassed with nitrogen for 20 minutes. Then, under nitrogen protection, 0.6000 g of MEK solution of tridecyl methacrylate was added to the reaction system every 30 minutes, and the addition was completed within two hours. The reaction was continued to be stirred at 70 °C in the dark for 24 hours. After the monomer was completely consumed, the reaction was quenched by freezing in the air (the reaction progress was confirmed by 1H-NMR). Finally, by precipitating the block copolymer in methanol, repeatedly dissolving and precipitating it with methyl ethyl ketone and methanol, washing it with a large amount of methanol, and drying it under vacuum, 2.0410 g of white powdered block copolymer was obtained, with a yield of 75.37%.

[0080] Figure 13 This is the GPC curve of the polymer obtained in Example 8.

[0081] Example 9 Example 9 provides a method for the controlled synthesis of a terpolymer based on tert-butyl acrylate (TBA), p-acetoxystyrene (4-AST), and styrene (St) using iodine transfer polymerization, specifically including the following steps: In a Schlenk flask, 1.9463 g (12.0000 mmol) of 4-acetoxystyrene (AST), 0.7680 g (6.0000 mmol) of tert-butyl acrylate (TBA), 0.2082 g (2.0000 mmol) of styrene (St), 0.0069 mg (0.0426 mmol) of azobisisobutyronitrile (AIBN), 0.0390 mg (0.1710 mmol) of ethyl 2-iodopropionate, and 0.0252 mg (0.0684 mmol) of tetrabutylammonium iodide were added as regulators. Then, 5 mL of DMF was added to dissolve the mixture, yielding the reaction system. This system was degassed through three freeze cycles and then reacted at 70 °C in the dark for 16 hours. After the reaction was complete, the DMF solvent was removed under reduced pressure, and the crude product was redissolved in dichloromethane and purified by precipitation with n-hexane. The dichloromethane dissolution and n-hexane precipitation operations were repeated several times, and the precipitate was washed with a large amount of n-hexane. Finally, the product was dried under vacuum to obtain 2.3105 g of pale yellow solid powder ternary random polymer with a yield of 79.13%.

[0082] The synthetic route of Example 9 is shown below:

[0083] The above-mentioned ternary random polymer is further hydrolyzed via the following reaction route:

[0084] The hydrolysis method included: adding methanol (3 times the polymer mass) and ammonia (2.5 times the polymer mass) to the ternary random polymer prepared above to prepare a mixed solution, and purging with nitrogen for 30 min to replace the oxygen in the system. The reaction was then refluxed at 80 °C for 16 h. After the reaction was complete, the reaction system was added to a 10% acetic acid aqueous solution for precipitation separation. The obtained precipitate was redissolved in N,N-dimethylformamide (DMF), and repeated dissolution-precipitation purification was performed using DMF and a 10% acetic acid aqueous solution, repeated three times. The precipitate was then thoroughly washed with a large amount of deionized water. Finally, the obtained product was dried under vacuum to obtain a yellow solid powder (hereinafter referred to as the hydrolyzed polymer).

[0085] Figure 14 This is the GPC curve of the polymer obtained in Example 9.

[0086] The number-average molecular weight and molecular weight distribution of the polymers prepared in the above examples were analyzed by gel permeation chromatography (GPC) in the THF phase. The test results are summarized in Table 1.

[0087] Table 1. Number-average molecular weight, molecular weight distribution, and monomers used for the polymers synthesized in Examples 1-9.

[0088] The polymer prepared by the method provided in this invention has a molecular weight close to the theoretical value and a narrow molecular weight distribution.

[0089] Using deuterated chloroform (CDCl3) as a solvent, the ternary random polymer prepared in Example 9 was subjected to 1H NMR and DOSY NMR spectroscopy. Figure 15 This is the ¹H-NMR spectrum of the ternary random polymer (unhydrolyzed) synthesized in Example 9. Figure 16 This is the DOSY-NMR spectrum of the ternary random polymer (unhydrolyzed) synthesized in Example 9. The hydrolyzed polymer from Example 9 was subjected to ¹H-NMR and DOSY-NMR tests using deuterated dimethyl sulfoxide (DMSO-d6) as the solvent. Figure 17 This is the ¹H-NMR spectrum of the polymer after hydrolysis. Figure 18 This is the DOSY-NMR spectrum of the polymer after hydrolysis.

[0090] according to Figure 15 The molar ratios of the monomer units in the ternary random polymer before hydrolysis were calculated, and the molar ratios of the monomer units were x:y:z = 18.6:67.8:13.6. Based on... Figure 16 DOSY-NMR results showed that the obtained product was a terpolymer system, and no obvious homopolymer signal was observed, indicating that there were no significant homopolymer byproducts. (Comparison) Figure 17 The ¹H-NMR spectrum of the polymer after hydrolysis shows that the characteristic peak at 2.29 ppm disappeared, while a new characteristic peak appeared at approximately 9.00 ppm, indicating a structural transformation. Combined with spectral analysis, this suggests that the p-acetoxystyrene (4-AST) monomer unit underwent a hydrolysis reaction and transformed into p-hydroxystyrene (PHS), while the remaining monomer structural units remained largely unchanged. Figure 18 The DOSY-NMR results of the hydrolyzed polymer further showed that the polymer diffusion coefficient distribution remained consistent and no obvious low molecular weight fragment signals appeared, indicating that the polymer main chain structure remained stable during the hydrolysis process and no side reactions such as chain breakage occurred.

[0091] KrF (248nm) photoresist composition was prepared using the hydrolyzed polymer of the ternary random polymer obtained in Example 9 as the photoresist matrix resin: the solid content of the photoresist matrix resin was 15wt%; triphenylthioperfluorobutanesulfonate (TPS-NF) was used as the photoacid generator (PAG), and the amount of the photoacid generator added accounted for 11wt% of the solid content of the resin; trioctylamine (TOA) was used as the quencher, and the amount of the quencher added was 5wt% of the solid content of the photoacid generator; propylene glycol monomethyl ether acetate (PGMEA) was selected as the main solvent of the photoresist.

[0092] The prepared photoresist composition was spin-coated onto a silicon substrate and pre-baked at 110°C for 60 seconds to remove most of the solvent, forming a dense solid photoresist film on the silicon substrate surface. Open exposure experiments were conducted using a 248nm KrF exposure light source with an exposure area of ​​5mm × 5mm and an exposure dose gradient set to 1-25mJ / cm². 2 (Exposure machine LTJ-VUVES4700i); After exposure, the film was baked at 120℃ for 90s, followed by static wetting and development at 23℃ for 60s using a 2.38wt% tetramethylammonium hydroxide (TMAH) aqueous solution as the developer; immediately after development, the film was rinsed with ultrapure deionized water for 30s and then purged with nitrogen to dry. The film thickness was measured and characterized by imaging after development.

[0093] Figure 19 This is a schematic diagram of the exposure dose gradient setting. Figure 20 This is a film thickness mapping diagram based on KLA Filmetrics F50-UVX measurements. Figure 21 The contrast curves are for the photoresist composition using the ternary random polymer as the matrix resin in Example 9. It can be seen that, after exposure imaging mapping tests on the developed film, the minimum exposure dose of this KrF photoresist was measured to be approximately 11 mJ / cm². 2 Contrast ratio γ = 2.72.

[0094] Furthermore, referring to Example 1 above, this invention also obtained binary random copolymers based on 4-acetoxystyrene (4-AST) and 4-vinylphenyl tert-butyl carbonate (tBVPC) by varying the temperature of the iodine transfer polymerization reaction to 60°C and 110°C, and by varying the reaction time to 12 h and 24 h. Referring to Example 5 above, this invention also obtained ternary random copolymers based on 3-hydroxy-1-adamantyl methacrylate (HAdMA), 2-methyl-2-adamantyl methacrylate (MAdMA), and 2-carboxy-6-norbornolactone-5-methacrylate (NLM) by varying the temperature of the sulfur-free reversible addition-fragmentation chain transfer polymerization reaction to 60°C and 110°C, and by varying the reaction time to 12 h and 24 h. In addition, this invention also conducted experiments using other raw materials, process operations, and process conditions described in the specification, and obtained relatively ideal results in all cases.

[0095] All aspects, embodiments, features, and examples of this invention should be considered illustrative and used to explain and illustrate the invention, but not to limit it. The scope of the invention is defined only by the claims.

[0096] Although the invention has been described with reference to the above embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that substantially equivalents can be substituted for elements in the described embodiments. Therefore, the invention is not intended to be limited to the specific embodiments disclosed, but rather to encompass all embodiments falling within the scope defined by the claims.

Claims

1. A method for preparing a polymer for photoresist, characterized in that, The preparation method is based on iodine transfer polymerization or sulfur-free reversible addition-fragmentation chain transfer polymerization; The preparation method based on iodine transfer polymerization includes: subjecting a first mixed reaction system containing a first monomer, an iodine transfer agent, and a free radical thermal initiator to an iodine transfer polymerization reaction at 60℃-110℃ for a reaction time of 12h-24h to obtain a polymer for photoresist; The preparation method based on sulfur-free reversible addition-fragmentation chain transfer polymerization includes: subjecting a second mixed reaction system containing a first monomer, a sulfur-free RAFT chain transfer agent, and a free radical thermal initiator to a sulfur-free reversible addition-fragmentation chain transfer polymerization reaction at 60℃-110℃ for a reaction time of 12-24 h to obtain a photoresist matrix resin. The first monomer includes one or a combination of styrene monomers, (meth)acrylate monomers, (meth)acrylamide monomers, and fluorine-containing functional monomers; wherein the molar ratio of the first monomer to the iodine transfer agent or sulfur-free RAFT chain transfer agent is determined according to the target degree of polymerization formula wherein n represents the degree of polymerization, [M0] represents the initial molar concentration of the first monomer, [CTA0] represents the initial molar concentration of the iodine transfer agent or sulfur-free RAFT chain transfer agent, C represents the monomer conversion rate, and 0.90<C<0.99; the molar ratio of the iodine transfer agent or sulfur-free RAFT chain transfer agent to the free radical thermal initiator is 2:1 to 10:1; The iodine transfer agent has the general formula R1-I or Z-R2-I; wherein R1 is selected from C1-C 20 Any one of alkyl, acyl, aryl, polymer chain, iodine atom, or HI2C group; Z is selected from any one of alkoxy, ester, carboxyl, or isocyanate group; R2 is selected from C1-C. 12 alkylene or arylene; The sulfur-free RAFT chain transfer agent satisfies formula A: ; R3 represents the leaving group, selected from any one of isobutyryloxy, propionyloxy, N-methylisobutyramido, N-methylpropionamido, cyano, phenyl, and p-methoxyphenyl; Y represents the stationary group, selected from any one of isobutyryloxy, phenyl, p-methylphenyl, and p-methoxyphenyl.

2. The preparation method according to claim 1, characterized in that, The total concentration of the first monomer in the first mixed reaction system and the second mixed reaction system is 2.5-3.5 mol / L.

3. The preparation method according to claim 1, characterized in that, After the first mixed reaction system is deoxygenated, the iodine transfer polymerization reaction is carried out under light-protected and inert atmosphere conditions.

4. The preparation method according to claim 1, characterized in that, After the second mixed reaction system is deoxygenated, the sulfur-free reversible addition-fragmentation chain transfer polymerization reaction is carried out under an inert atmosphere.

5. The preparation method according to claim 1, characterized in that, Iodine transfer agents satisfying general formula R1-I include one or more combinations of iodoform, iodooctane, and (1-iodoethyl)benzene, and iodine transfer agents satisfying general formula Z-R2-I include one or more combinations of ethyl 4-iodobutyrate, ethyl 2-iodopropionate, and 2-iodo-2-methylpropionitrile.

6. The preparation method according to claim 1, characterized in that, The sulfur-free RAFT chain transfer agent includes one or more of the compounds shown in A1 to A6; 。 7. The preparation method according to claim 1, characterized in that, The styrene monomers include one or a combination of p-acetoxystyrene, styrene, 4-vinylphenyl tert-butyl carbonate, and p-methylstyrene.

8. The preparation method according to claim 1, characterized in that, The (meth)acrylate monomers include one or more of the following: tert-butyl acrylate, n-butyl acrylate, methyl methacrylate, isobornyl methacrylate, hydroxyethyl methacrylate, 1-methylcyclopentyl methacrylate, 2-methyl-2-adamantyl methacrylate, and 3-methacrylate-4-butyrolactone.

9. The preparation method according to claim 1, characterized in that, The (meth)acrylamide monomers include one or a combination of acrylamide, N-methylacrylamide, and N,N-dimethylacrylamide.

10. The preparation method according to claim 1, characterized in that, The fluorinated functional monomers include one or a combination of multiple of tridecylfluorooctyl methacrylate, perfluoroalkyl methacrylate, and fluorostyrene derivatives.

11. The preparation method according to claim 1, characterized in that, The free radical thermal initiator includes at least one of azo initiators and peroxide initiators.

12. The preparation method according to claim 1, characterized in that, The first and second mixed reaction systems further include solvents, which include one or more of the following: tetrahydrofuran, methyl ethyl ketone, propylene glycol monomethyl ether acetate, N,N-dimethylformamide, hexafluoroisopropanol, dimethyl carbonate, diethyl carbonate, toluene, and xylene.

13. A polymer for photoresist, characterized in that, It is prepared by the preparation method according to any one of claims 1-12.

14. A method for preparing a block copolymer for photoresist, characterized in that, include: A polymer for photoresist is prepared by the preparation method according to any one of claims 1-12 and used as a macromolecular chain transfer agent; A third mixed reaction system containing the aforementioned photoresist polymer and the second monomer is subjected to a polymerization reaction to obtain a block copolymer for photoresist; The second monomer includes one or more of styrene monomers, (meth)acrylate monomers, (meth)acrylamide monomers, and fluorine-containing functional monomers, and the second monomer may be the same as or different from the first monomer.

15. The preparation method according to claim 14, characterized in that, Specifically, it includes: Under inert atmosphere conditions, the second monomer is introduced in batches into a solution containing the polymer for photoresist, and the amount of the second monomer added is 2-6 times the molar amount of the polymer for photoresist. After the second monomer is completely added, the reaction continues for a preset time.

16. A block copolymer for photoresist, characterized in that, It is prepared by the preparation method according to any one of claims 14-15.

17. The use of the polymer for photoresist according to claim 13 or the block copolymer for photoresist according to claim 16 in the preparation of photoresist.

Citation Information

Patent Citations

  • Star-shaped polymer photoresist film-forming resin as well as preparation method and application thereof

    CN119613600A

  • Iodine transfer polymerization method and compositions therefrom

    US20220106423A1