Multifunctional gel electrolyte and preparation method and application thereof

CN122659335APending Publication Date: 2026-08-28BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610848501.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-12
Publication Date
2026-08-28

AI Technical Summary

Technical Problem

[0006]为了克服现有凝胶电解质离子电导率低、界面稳定性差、锌枝晶抑制能力不足以及与传统电极制造工艺适配性差等问题,提供一种复合凝胶电解质、用于三维打印锌金属电池的电极浆料、三维打印柔性锌金属电池及其制备方法和应用

Benefits of technology

(1)本发明在聚合物凝胶基体中引入ZnHA填料,ZnHA内部独特的离子传输通道能够加速Zn²+的传导,其表面丰富的羟基基团可有效吸附溶剂分子并调控Zn²+的溶剂化结构,显著提升Zn²+的传输效率与界面稳定性,从材料层面抑制锌枝晶生长。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present application relates to the technical field of zinc metal battery, in particular to a multifunctional composite gel electrolyte, its preparation method and application. The present application provides a composite gel electrolyte, which comprises a polymer gel matrix, a zinc salt and a ZnHA filler; wherein the ZnHA filler is a hydroxyapatite material doped with zinc ions. The electrolyte is prepared by polymer dissolution, zinc salt addition, ZnHA dispersion, three-dimensional printing forming, low-temperature gelation and zinc salt solution activation, and has good shear thinning characteristics, self-supporting property and printability. Further, a three-dimensional printed interdigital structure electrode is constructed, and the electrolyte is covered to form an ion transmission channel, and a flexible zinc metal battery is assembled; multiple monomers can be connected in series to increase the output voltage. The flexible battery has excellent ion transmission, cycle stability, flexibility and safety, and can be used in the fields of flexible electronics, wearable devices and intelligent sensing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to a multifunctional composite gel electrolyte, a three-dimensional printed flexible zinc metal battery, its preparation method, and its application. Background Technology

[0002] With the rapid development of flexible electronic devices, wearable devices, intelligent sensing systems, and health monitoring equipment, there is an urgent need for energy storage devices that combine high safety, high flexibility, and high energy density. Zinc metal batteries, due to their high theoretical capacity (zinc anode specific capacity reaches 820 mAh / g), abundant resources, low cost, and environmental friendliness, have become a strong candidate to replace lithium-ion batteries. In particular, aqueous zinc metal batteries, using water-based electrolytes, fundamentally avoid the safety risks of flammability and explosion associated with organic electrolytes.

[0003] However, traditional aqueous liquid electrolytes suffer from problems such as hydrogen evolution reaction, zinc dendrite growth, and electrode side reactions, which severely limit the cycle life and coulombic efficiency of zinc metal batteries. To alleviate these problems, gel electrolytes have emerged. Gel electrolytes immobilize water molecules through a polymer network, effectively suppressing water activity, reducing side reactions, and providing a certain mechanical barrier to inhibit zinc dendrite formation. However, existing gel electrolytes still generally have the following problems: first, low ionic conductivity and slow zinc ion transport kinetics; second, poor contact with the zinc anode interface, which easily leads to interface peeling during repeated charge and discharge, resulting in increased impedance; and third, a lack of effective control over the zinc ion solvation structure, resulting in uneven zinc ion deposition and persistent dendrite problems.

[0004] On the other hand, the positive and negative electrodes of traditional zinc metal batteries are typically fabricated using coating or pressing processes, resulting in simple electrode structures and poor interfacial compatibility with gel electrolytes. This is particularly challenging when constructing miniaturized, planar flexible batteries, where conformal coverage and integrated assembly of the electrodes and electrolytes present significant challenges. In recent years, 3D printing technology has offered new avenues for the development of high-performance flexible zinc metal batteries due to its unique advantages in complex structure forming, precise material distribution, and integrated manufacturing. However, currently, gel electrolyte ink systems suitable for 3D printing are scarce, and systematic solutions for co-designing with electrode materials are lacking.

[0005] Therefore, developing a composite gel electrolyte that combines high ionic conductivity, excellent interfacial stability, and good adaptability to 3D printing, and using it as a basis to construct an integrated, structurally controllable flexible zinc metal battery, is of great significance for promoting the development of wearable electronic devices. Summary of the Invention

[0006] To overcome the problems of low ionic conductivity, poor interface stability, insufficient zinc dendrite suppression ability, and poor compatibility with traditional electrode manufacturing processes in existing gel electrolytes, this paper provides a composite gel electrolyte, an electrode slurry for 3D printed zinc metal batteries, a 3D printed flexible zinc metal battery, its preparation method, and its application.

[0007] To achieve the above objectives, the present invention provides the following technical solution.

[0008] The first aspect of the present invention provides a composite gel electrolyte, the composite gel electrolyte comprising a polymer gel matrix, a zinc salt and a ZnHA filler; The ZnHA filler is a hydroxyapatite material doped with zinc ions, and the content of ZnHA filler accounts for 0.1wt% to 30wt% of the total mass of the composite gel electrolyte.

[0009] In one embodiment, the zinc ions account for 0.1 to 20 wt% of the ZnHA filler mass, preferably 0.5 to 10 wt%, based on zinc element content.

[0010] In one embodiment, the content of the ZnHA filler accounts for 0.5 wt%-20 wt% of the total mass of the composite gel electrolyte, preferably 1 wt%-10 wt%.

[0011] In this invention, the zinc-doped hydroxyapatite material is prepared by ion exchange between hydroxyapatite and a zinc-containing salt solution. The ZnHA filler is dispersed in a polymer gel matrix to form an ion transport network, and its internal channels are used to promote Zn²⁺ transport. + Migration occurs when the hydroxyl groups on the surface of hydroxyapatite adsorb solvent molecules, thereby modulating the Zn²⁺ migration. + Solvation structure, thereby improving Zn² + Improves transmission efficiency and enhances the stability of the zinc anode interface.

[0012] In one embodiment, the zinc salt is selected from one or more of zinc sulfate, zinc trifluoromethanesulfonate, zinc chloride, zinc acetate, and zinc gluconate, preferably zinc chloride or zinc sulfate.

[0013] In one embodiment, the concentration of the zinc salt in the composite gel electrolyte is 0.1–10 mol / L, preferably 1–5 mol / L.

[0014] Zinc salts (e.g., zinc chloride) are added to the composite gel electrolyte of this invention. Due to their high water solubility and ion dissociation ability, zinc salts can provide a high concentration of migratable zinc ions to the gel electrolyte. These ions can act as ion carriers in the electrolyte and participate in the construction of ion transport channels in the gel network, thereby promoting the uniform migration of zinc ions and inhibiting the occurrence of side reactions. This also helps to improve the ionic conductivity and electrochemical reaction kinetics of the electrolyte.

[0015] In one embodiment, the polymer in the polymer gel matrix is ​​selected from natural polymers and their modified derivatives or synthetic polymers.

[0016] Preferably, the natural polymer and its modified derivatives are selected from one or more of gelatin, sodium alginate, chitosan, carboxymethyl cellulose, and collagen; Preferably, the synthetic polymer is selected from one or more of polyvinyl alcohol, polyacrylamide, polyethylene glycol, polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyurethane, and polyacrylonitrile.

[0017] In a preferred embodiment, the polymer gel matrix may be made using any of the above-mentioned materials alone, or may be made by combining two or more materials to form an interpenetrating network structure, a blended network structure, or a composite gel network structure.

[0018] Preferably, the polymer gel matrix is ​​a compound system of gelatin and polyvinyl alcohol, a compound system of gelatin and polyacrylamide, or a compound system of gelatin and polyvinylidene fluoride-hexafluoropropylene copolymer. More preferably, the polymer in the polymer gel matrix is ​​gelatin.

[0019] In one embodiment, the content of the polymer gel matrix in the composite gel electrolyte is 10 wt%-99.9 wt%, preferably 30 wt%-95 wt%, and more preferably 50 wt%-90 wt%.

[0020] The composite gel electrolyte described in this invention has shear-thinning properties, self-supporting properties, and extrudable rheological properties. It can be formed by direct writing printing, extrusion printing, inkjet printing, or digital light processing printing, preferably by direct writing three-dimensional printing.

[0021] A second aspect of the present invention provides a method for preparing a composite gel electrolyte, comprising the following steps: (1) Add the polymer gel matrix to the solvent and heat and stir until completely dissolved; (2) Add zinc salt to the system of step (1) and continue stirring to form a homogeneous solution; (3) Add ZnHA filler to the system of step (1) to form a uniformly dispersed slurry; (4) Use a three-dimensional printing device to print the slurry obtained in step (3) into a preset structure at a printing temperature of 20-80℃; (5) Place the printed sample from step (4) in an environment of -10 to 10℃ for gelation treatment; (6) The gelled sample from step (5) is immersed in zinc salt solution for activation treatment to obtain composite gel electrolyte.

[0022] In one embodiment, the solvent is deionized water, an organic solvent, or a mixture thereof; preferably, it is deionized water.

[0023] In one embodiment, the mass-to-volume ratio of the polymer gel matrix to the solvent is 0.05-0.3 g / mL.

[0024] In one embodiment, in step (2), the amount of ZnHA filler added is 0.1 wt%-30 wt% of the polymer gel mass, preferably 0.5 wt%~20 wt%.

[0025] In one embodiment, the gelation treatment time in step (5) is 0.1-24 h.

[0026] In one embodiment, in step (6), the concentration of the zinc salt solution is 0.5-5 mol / L.

[0027] In step (3) of this invention, the material can be uniformly dispersed by mechanical stirring, ultrasonic dispersion, or a combination of both to obtain a printing slurry with good rheological properties. ZnHA can act as a functional filler, uniformly distributed in the slurry system, providing ion transport channels and structural reinforcement for the subsequent gel electrolyte.

[0028] In step (4) of this invention, the printing conditions can be adjusted according to requirements. By performing layer-by-layer deposition printing according to preset model parameters, a gel electrolyte precursor with a specific shape, size, and internal structure can be prepared. During the printing process, parameters such as nozzle diameter, printing speed, extrusion pressure, and layer thickness can be adjusted to obtain a stable molding effect.

[0029] In step (5) of this invention, gelation treatment is performed at a low temperature, which can cause physical or chemical cross-linking of polymer chain segments, thereby forming a gel skeleton with a three-dimensional network structure. The preferred low temperature treatment temperature is 0~10 ℃, and the preferred treatment time is 0.2~8 h.

[0030] In step (6) of this invention, the activation treatment allows zinc ions to further penetrate into the gel network and reach a sufficient equilibrium, while simultaneously improving the ionic conductivity and electrochemical stability of the gel electrolyte. After activation, the sample is removed, and the residual solution on the surface is removed to obtain the composite gel electrolyte.

[0031] A third aspect of the present invention provides a composite gel electrolyte prepared by the preparation method described in the second aspect.

[0032] A fourth aspect of the present invention provides a three-dimensional printed flexible zinc metal battery, comprising a composite gel electrolyte as described in the first or third aspect, and an electrode slurry for three-dimensional printing the zinc metal battery.

[0033] In one embodiment, the active material, conductive agent, binder, and solvent are mentioned.

[0034] In one embodiment, the active material is selected from at least one of the positive electrode active material and the negative electrode active material.

[0035] Preferably, the positive electrode active material is selected from one or more of ammonium vanadate, vanadium pentoxide, and manganese dioxide.

[0036] The preferred cathode material of this invention is ammonium vanadate, which has a layered structure that is beneficial for Zn²⁺. + The ammonium vanadate exhibits reversible insertion / extraction and has a high specific capacity (theoretical capacity of approximately 300 mAh / g). More preferably, the ammonium vanadate is an ammonium vanadate nanoribbon induced by polyvinylpyrrolidone (PVP) synthesis, which has a higher specific surface area and structural stability.

[0037] Preferably, the negative electrode active material is selected from spherical zinc powder (particle size 1~10 μm) or zinc alloy powder (such as Zn-Cu, Zn-Al alloy), and more preferably spherical zinc powder. Zinc powder has a high specific surface area and good electronic conductivity, making it suitable for 3D printing to prepare thick electrodes.

[0038] Preferably, the conductive agent is selected from one or more of carbon nanotubes, graphene, and carbon black (such as Ketjenblack, Super P), with carbon nanotubes being the most preferred. The selection of carbon nanotubes as the conductive agent is based on their high aspect ratio (>1000) and excellent conductivity, enabling them to form a three-dimensional conductive network while enhancing the mechanical flexibility of the electrode.

[0039] Preferably, the adhesive is selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylic acid (PAA), and carboxymethyl cellulose, and is preferably polyvinylidene fluoride.

[0040] Preferably, the solvent is N-methyl-2-pyrrolidone (NMP) or deionized water.

[0041] When the adhesive is PVDF, the solvent is NMP.

[0042] In one embodiment, the electrode slurry for 3D printing zinc metal batteries is prepared by ball milling: active material, conductive agent and binder are mixed in a ball mill jar in a solvent.

[0043] Preferably, the mixing speed in the ball mill jar is 100-1000 rpm.

[0044] Preferably, the mixing time in the ball mill jar is 1-24 h (e.g., 6 h).

[0045] The purpose of mixing in the ball mill jar is to obtain electrode ink that is uniformly dispersed and has suitable rheological properties for direct-write 3D printing.

[0046] In one embodiment, when the electrode slurry used for 3D printing zinc metal batteries is a positive electrode slurry, the mass ratio of the positive electrode active material, the conductive agent, and the binder is (6-9):(0.5-2):(0.5-2), preferably 8:1:1.

[0047] In one embodiment, when the electrode slurry used for 3D printing zinc metal batteries is a negative electrode slurry, the mass ratio of the negative electrode active material (e.g., zinc powder), the conductive agent, and the binder is (7-9):(0.5-1.5):(0.5-1.5), preferably 9:0.5:0.5.

[0048] In one embodiment, the structure of the three-dimensional printed flexible zinc metal battery is as follows: a positive electrode structure and a negative electrode structure formed on the same plane by three-dimensional printing, and a composite gel electrolyte as described in the first or third aspect of the present invention covering the surfaces of the positive electrode structure and the negative electrode structure.

[0049] In a preferred embodiment, the positive electrode structure and the negative electrode structure are arranged alternately on the same substrate surface, and the composite gel electrolyte covers the surfaces of the positive electrode structure and the negative electrode structure and fills the gaps between them to form an ion transport pathway.

[0050] Preferably, the positive and negative electrode structures are arranged in an interdigitated pattern, with adjacent positive and negative electrodes nested together to form a planar interdigitated structure; both the positive and negative electrode structures are fabricated using 3D printing.

[0051] Preferably, the positive electrode structure is an ammonium vanadate electrode, and the negative electrode structure is a zinc powder electrode.

[0052] Preferably, after the composite gel electrolyte is printed and gelled, it is immersed in a zinc salt solution for activation, and then covers the surfaces of the interdigitated positive and negative electrodes to form an electrochemical circuit.

[0053] Preferably, the activation solution is a 2 mol / L zinc sulfate solution.

[0054] The three-dimensional printed flexible zinc metal battery of the present invention comprises two or more interdigitated cells; wherein, the two or more interdigitated cells are connected in series through a conductive connection structure to form a flexible battery pack to improve the output voltage. After being encapsulated with a flexible encapsulation material, the flexible battery pack can maintain normal operation under bending, folding, twisting, compression, or puncture conditions; and the battery or battery pack is integrated with flexible sensors, flexible circuits, wireless communication modules, or wearable electronic devices to form a flexible power supply system.

[0055] The fifth aspect of the present invention provides a flexible power supply system comprising a three-dimensionally printed flexible zinc metal battery as described in the fourth aspect.

[0056] The sixth aspect of the present invention provides a flexible wearable electronic device, including a three-dimensional printed flexible zinc metal battery as described in the fourth aspect or a flexible power supply system as described in the fifth aspect, and functional devices integrated on the same flexible substrate.

[0057] In one embodiment, the functional device is selected from one or more of flexible sensors, flexible switches, flexible circuits, flexible LEDs, and health monitoring sensors.

[0058] The functional components and the battery are electrically connected via 3D-printed conductive lines. All components (battery, functional components, circuits) are integrated onto the same PDMS flexible substrate via 3D printing, achieving true "integrated" manufacturing.

[0059] In a preferred embodiment, the flexible wearable electronic device is a self-powered flexible sensing system. A 3D-printed flexible zinc metal battery provides power to functional devices, which respond to external stimuli (such as pressure, deformation, temperature, etc.) and generate signals or perform actions. For example, by co-designing an interdigital battery with a flexible pressure / deformation switch, printing the entire assembly on a flexible PDMS substrate, and attaching it to a human joint, the stretching deformation generated by joint bending can drive the flexible switch to close, thereby achieving self-powering and signal regulation of sensor devices or indicating devices (such as LEDs). This system can still function normally after 1000 repeated bends and can still operate stably under partial puncture or severe torsion conditions.

[0060] The seventh aspect of the present invention provides the application of composite gel electrolytes as described in the first or third aspect, or three-dimensional printed flexible zinc metal batteries as described in the fourth aspect, or flexible power supply systems as described in the fifth aspect, or flexible wearable electronic devices as described in the sixth aspect, in energy storage devices, flexible electronic devices, wearable devices, health monitoring devices, human-computer interaction devices, and intelligent sensing systems.

[0061] The present invention, through the above technical solution, has the following beneficial effects: (1) In this invention, ZnHA filler is introduced into the polymer gel matrix. The unique ion transport channels inside ZnHA can accelerate the Zn²⁺ transport. + The abundant hydroxyl groups on its surface can effectively adsorb solvent molecules and regulate Zn²⁺ conduction. + The solvation structure significantly improves Zn² + The transmission efficiency and interface stability are improved, and zinc dendrite growth is suppressed at the material level.

[0062] (2) Excellent biocompatibility: Due to the use of biomass-derived materials such as gelatin and hydroxyapatite, this composite gel electrolyte exhibits excellent biocompatibility. Co-culture experiments with human umbilical vein endothelial cells (HUVEC) confirmed that the electrolyte of this invention has almost no cytotoxicity to cells (cell survival rate >95%) and extremely low levels of reactive oxygen species (ROS), which are far superior to traditional organic electrolytes (cell survival rate <5%), making it an ideal power source for wearable electronic devices that can be directly attached to human skin.

[0063] (3) Integrated 3D Printing Manufacturing for Flexible Electronics: The composite gel electrolyte and electrode slurry provided by this invention both possess excellent shear-thinning properties and printable rheological properties, perfectly adapting to direct-write 3D printing technology. Through layer-by-layer printing, the designed interdigitated positive and negative electrode structures can be constructed in one go with high precision, and the electrolyte layer can be printed directly on them, achieving integrated and seamless integration of the electrode / electrolyte interface. The interdigitated structure effectively shortens the Zn²... + The reduced transport path (from millimeters to micrometers) lowers the interface impedance (EIS tests show that the interface impedance of interdigitated cells is significantly lower than that of traditional button cells). This process avoids the reliance on separators and encapsulation shells in traditional battery manufacturing, providing a new paradigm for developing flexible batteries with arbitrary shapes and customized structures.

[0064] (4) System-level flexible wearable applications: This invention further demonstrates system integration capabilities. By integrating a 3D-printed flexible zinc metal battery with flexible switches, circuits, and sensors also manufactured using 3D printing, a self-powered flexible wearable sensing system was successfully constructed. This system can be attached to human skin and can respond to physiological activities such as joint bending, achieving stable power supply and signal interaction (such as lighting up an LED), fully demonstrating the enormous application potential and practical value of the technology of this invention in cutting-edge fields such as smart wearables, health monitoring, and human-computer interaction.

[0065] (5) Simple process and low cost: The ZnHA filler used in this invention is simple to prepare (one-step ion exchange method) and can be mass-produced; the main matrix material gelatin is widely available and low in cost; the 3D printing manufacturing process is carried out at room temperature or low temperature, without the need for expensive cleanrooms or photolithography equipment, with low energy consumption and high material utilization (>95%), which is very suitable for large-scale, low-cost manufacturing and has good prospects for industrial application. Attached Figure Description

[0066] Figure 1 The images are scanning electron microscope (SEM) images of the ZnHA packing materials prepared in Examples 1 and 5-7 of this invention. Figure 2 The ionic conductivity diagram is shown for the gel electrolyte prepared in Example 1 of this invention. Figure 3 The puncture performance of the gel electrolytes prepared in Example 1 and Comparative Example 1 of this invention; Figure 4 The tensile properties of the gel electrolytes prepared in Example 1 and Comparative Example 1 of this invention; Figure 5 The cycling performance diagram shows the half-cells assembled with the gel electrolytes prepared in Application Example 1 and Comparative Example 1 of this invention. Figure 6 The cycling performance diagram shows the symmetrical battery assembled with the gel electrolytes prepared in Application Example 1 and Comparative Example 1 of this invention. Figure 7 The rate performance of the assembled full cells using the gel electrolytes prepared in Application Example 1 and Comparative Example 1 of this invention is shown in the diagram. Figure 8 The cycling performance of the full cells assembled with the gel electrolytes prepared in Application Example 1 and Comparative Example 1 of this invention is shown in the figure. Figure 9 This is an optical photograph of the flexible electronic device prepared in Application Example 1 of the present invention during its operation. Figure 10 Photographs of the flexible battery prepared in Application Example 1 of the present invention under extreme conditions.

[0067] The present invention will be described in detail below through embodiments.

[0068] Unless otherwise specified in the following examples and comparative examples, all conditions were performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments used, unless otherwise specified, are all commercially available products.

[0069] Test methods used in the embodiments In the context of this invention, including the following embodiments, the ionic conductivity is determined by an alternating current impedance method. The alternating current impedance method can characterize various resistance information within a battery, and can also be used to calculate the lithium-ion conductivity of the solid polymer electrolyte. The electrochemical workstation used for the alternating current impedance test is a Shanghai Chenhua CHI660E, with a frequency range of 0.01~106Hz and an amplitude of 10mV. A solid polymer electrolyte sheet with a diameter of 12mm is sandwiched between two stainless steel sheets, and the ionic conductivity (σ) is calculated using the following formula:

[0070] Where L is the thickness of the electrolyte sheet (cm), R is the impedance of the electrolyte sheet (ohms), and S is the area of ​​the electrolyte sheet (cm²). 2 ).

[0071] In the context of this specification, including the following embodiments, the lithium-ion transference number (t) Zn 2+ The measurements were performed at room temperature using AC impedance and DC polarization techniques on a Shanghai Chenhua CHI660E. Before testing, the button cell was first tested at 0.1 mA. cm - ² and 0.1 mAh cm - Cycling under 20°C conditions for 20 h allowed a stable SEI interface layer to form between the elastic polymer solid electrolyte and the electrode. Tests were performed before and after polarization. Zn 2+ Calculate using the following formula:

[0072] Where Io and Iss are the initial and steady-state current values, respectively, ΔV is the polarization potential (10 mV), and R b o and R b s These are the initial and steady-state values ​​of the body resistance, respectively.

[0073] In the context of this invention, including the following embodiments, the nucleation overpotential is measured using a constant current deposition method with a LAND (Blue Electric) battery system. A constant current is applied to simulate the actual charging process, and the change in potential over time is recorded. After a sudden drop in potential in the initial stage, a stable nucleation plateau appears. The plateau potential is the nucleation potential, and the difference between it and the equilibrium potential is the nucleation overpotential.

[0074] In the context of this invention specification, including the following embodiments, the elastic modulus and elongation at break are tested using an AI-7000-NGD type electronic universal testing machine. The test machine is prepared into a dumbbell shape of 100 mm × 50 mm that conforms to national standards. The test machine is stretched at a speed of 100 mm / min, and the average value is taken after three measurements. The elongation at break and stress-strain curve are then obtained.

[0075] In the context of this specification, including the following embodiments, the morphology of the electrolyte and negative electrode was characterized using a scanning electron microscope (SEM, JEOL, JSM-6701-F).

[0076] In this embodiment of the invention, unless otherwise specified, the low-temperature drying is a drying method well known to those skilled in the art, without any special operation, as long as the material can be dried without denaturation.

[0077] Example 1 (1) Preparation of zinc-doped apatite filler 4 g of HA was dissolved in 50 ml of zinc chloride aqueous solution (2 mol / L) and stirred for 5 h. ZnHA was then obtained by vacuum filtration. The filtered ZnHA was dried at 60 °C for 24 h to obtain ZnHA (with excess zinc salt added).

[0078] (2) Preparation of gel electrolytes At 60 °C, 1 g of gelatin was dissolved in 10 mL of deionized water. Then, 1.79 g of zinc sulfate monohydrate was added to the mixture, and the mixture was stirred until a clear solution was obtained. Next, 50 mg of ZnHA was added to the mixture, and the mixture was stirred for 5 h. The electrolyte solution was then printed and extruded using a printer. The printed surface was then transferred to a low-temperature chamber and allowed to stand at 3 °C for 0.5 h. After the electrolyte gelled, it was removed from the substrate surface and immersed in a 2 mol / L ZnSO4 aqueous solution for one day to obtain the ZnHA / Gel electrolyte (i.e., the composite gel electrolyte).

[0079] (3) The printed electrode ink was prepared using traditional ball milling technology. This method uses ammonium vanadate (NH4V4O) as the ink. 10NVO4 powder and zinc powder (Zn-P) were used as the active materials for the positive and negative electrodes, respectively. To prepare the positive electrode ink, 0.12 g of NVO4 was dispersed in 0.5 ml of N-methyl-2-pyrrolidone, which contained 3 wt% PVDF solution, and 0.015 g of carbon nanotubes were added. The mixed precursor solution was placed in a ball mill jar and milled to prepare a uniformly mixed positive electrode printing slurry. Similarly, the negative electrode ink was prepared by using 0.54 g of Zn-P in the same manner. After preparation, the electrode slurries were allowed to stand for 6 h. Subsequently, the positive and negative electrode inks were loaded into syringes and dried at low temperature for storage.

[0080] Example 2 The method of Example 1 is followed, except that in step (2), 50 mg of ZnHA is replaced with 20 mg of ZnHA, and the other conditions are the same as in Example 1, to obtain a composite gel electrolyte.

[0081] Example 3 The method of Example 1 is followed, except that in step (2), 50 mg of ZnHA is replaced with 100 mg of ZnHA, and the other conditions are the same as in Example 1, to obtain a composite gel electrolyte.

[0082] Example 4 The method of Example 1 is followed, except that in step (2), 50 mg of ZnHA is replaced with 200 mg of ZnHA, and the other conditions are the same as in Example 1, to obtain a composite gel electrolyte.

[0083] Example 5 The method of Example 1 is different in that, in step (1), 50 ml of zinc chloride aqueous solution (2 mol / L) is replaced with 50 ml of zinc sulfate aqueous solution (2 mol / L), and the other conditions are the same as in Example 1, to obtain zinc-doped apatite, and composite gel electrolyte is prepared using the zinc-doped apatite.

[0084] Example 6 The method of Example 1 is different in that, in step (1), 50 ml of zinc chloride aqueous solution (2 mol / L) is replaced with 50 ml of zinc acetate aqueous solution (2 mol / L), and the other conditions are the same as in Example 1, to obtain zinc-doped apatite, and composite gel electrolyte is prepared using this zinc-doped apatite.

[0085] Example 7 The method of Example 1 is different in that, in step (1), 50 ml of zinc chloride aqueous solution (2 mol / L) is replaced with 50 ml of zinc gluconate aqueous solution (2 mol / L), and the other conditions are the same as in Example 1, to obtain zinc-doped apatite, and composite gel electrolyte is prepared using this zinc-doped apatite.

[0086] Example 8 The method of Example 1 was followed, except that in step (2), gelatin was replaced with acrylamide. 2 g of acrylamide was dissolved in 10 mL of deionized water at room temperature and stirred until completely dissolved to form a homogeneous and transparent solution. Then, 1.79 g of zinc sulfate monohydrate was added and stirred continuously until a transparent and homogeneous electrolyte precursor solution was obtained. Next, 50 mg of ZnHA was added to the system and stirred for 5 h to ensure complete dispersion. Then, 10 mg of N,N'-methylenebisacrylamide and 10 mg of ammonium persulfate were added and mixed thoroughly to obtain the printing slurry. The slurry was then loaded into the barrel of a 3D printer for printing and extrusion molding. The printed sample was placed at 60 ℃ for 4 h to complete polymerization and crosslinking, forming a stable gel network. After gel formation, it was removed from the substrate surface and immersed in a 2 mol / L ZnSO4 aqueous solution for one day to finally obtain the ZnHA / PAM composite gel electrolyte.

[0087] Example 9 The method was followed according to Example 1, except that in step (2), gelatin was replaced with cellulose. At room temperature, 50 mg of ZnHA was added to 5 g of cellulose nanofibers (CNF), and a uniform dispersion was obtained by high-speed stirring and ultrasonic treatment, resulting in a printing slurry with good rheological properties. The slurry was then extruded using a 3D printer. The printed sample was left to stand at room temperature for 24 h to allow the cellulose nanofibers to form a three-dimensional network structure through hydrogen bonding. After the gel stabilized, it was immersed in a 2 mol / L ZnSO4 aqueous solution for 24 h to activate it, ultimately obtaining a ZnHA / CNF composite gel electrolyte.

[0088] Example 10 The method was followed according to Example 1, except that in step (2), gelatin was replaced with sodium alginate. 1 g of sodium alginate was dissolved in 10 mL of deionized water at room temperature and stirred continuously until a homogeneous and transparent solution was formed. Then, 1.79 g of zinc sulfate monohydrate was added to the solution and stirred until completely dissolved. Next, 50 mg of ZnHA was added to the mixed solution and stirred continuously for 5 h to ensure complete dispersion of ZnHA in the system. The resulting electrolyte slurry was then printed and extruded using a printer. After printing, the printed sample was immersed in a 2 mol / L ZnSO4 aqueous solution and left to stand for one day to allow Zn²⁺ to dissolve.+ The electrolyte undergoes ionic cross-linking with the carboxyl groups on the sodium alginate molecular chain to form a stable gel network structure. After gelation is complete, the sample is removed from the substrate surface, and residual electrolyte is removed to obtain the ZnHA / SA composite gel electrolyte.

[0089] Comparative Example 1 (1) Preparation of gel electrolytes At 60 ºC, 1 g of gelatin was dissolved in 10 ml of deionized water. Then, 1.79 g of zinc sulfate monohydrate was added to the mixture, and the mixture was stirred until a clear solution was obtained. The electrolyte solution was then printed and extruded using a printer. The printed surface was then transferred to a low-temperature chamber and allowed to stand at 3 ºC for 0.5 h. After the electrolyte gelled, it was removed from the substrate surface and immersed in a zinc sulfate aqueous solution (2 mol / L) for one day to obtain the ZnHA / Gel electrolyte.

[0090] (2) The printed electrode ink was prepared using traditional ball milling technology. This method uses ammonium vanadate (NH4V4O) as the ink. 10 NVO4 powder and zinc powder (Zn-P) were used as the active materials for the positive and negative electrodes, respectively. To prepare the positive electrode ink, 0.12 g of NVO4 was dispersed in 0.5 ml of N-methyl-2-pyrrolidone, which contained 3 wt% PVDF solution, and 0.015 g of carbon nanotubes were added. The mixed precursor solution was placed in a ball mill jar and milled to prepare a uniformly mixed positive electrode printing slurry. Similarly, the negative electrode ink was prepared by using 0.54 g of Zn-P in the same manner. After preparation, the electrode slurries were allowed to stand for 6 h. Subsequently, the positive and negative electrode inks were loaded into syringes and dried at low temperature for storage.

[0091] Comparative Example 2 The method of Example 1 is followed, except that in step (2), 50 mg ZnHA is replaced with 50 mg HA, and the other conditions are the same as in Example 1, to obtain gel electrolyte.

[0092] Comparative Example 3 The method of Example 1 is different in that, in step (2), the method of preparing electrolyte by 3D printing is replaced by solution casting.

[0093] Test case (1) Basic characterization and electrochemical evaluation tests Basic characterization was performed on the hydroxyapatite fillers prepared in the examples and comparative examples. Basic mechanical and electrochemical tests were conducted on the gel electrolytes prepared in the examples and comparative examples. SEM images of the ZnHA fillers prepared in Examples 1 and 5-7 are shown below. Figure 1As shown; the ionic conductivity of the gel electrolyte prepared in Example 1 is as follows: Figure 2 As shown in the figure; the experimental results are shown in Table 1.

[0094] Table 1. Basic test data of gel electrolytes prepared in the examples and comparative examples.

[0095] (2) Mechanical property testing To verify the enhancing effect of ZnHA on the mechanical properties of the gel electrolyte, the ZnHA / Gel electrolyte prepared in Example 1 and the Gel electrolyte prepared in Comparative Example 1 were cut into samples of the same size and subjected to puncture and tensile tests at room temperature. For the puncture test, a cylindrical probe was perpendicularly pressed into the electrolyte membrane at a constant rate until the sample ruptured, and the force-displacement curve was recorded. For the tensile test, a universal testing machine was used to determine the stress-strain curve of the sample. The test results are as follows: Figure 3 and Figure 4 As shown.

[0096] Depend on Figure 3 It can be seen that the maximum puncture force of ZnHA / Gel electrolyte reaches 0.75 N, while that of Gel electrolyte is only 0.31 N, representing an increase in puncture strength of approximately 141.9%. Furthermore, ZnHA / Gel exhibits greater deformation displacement before rupture, indicating superior puncture resistance and structural stability.

[0097] Depend on Figure 4 It can be seen that the maximum tensile stress of ZnHA / Gel electrolyte reaches 0.91 MPa, which is significantly higher than that of Gel electrolyte (0.30 MPa), representing an increase of approximately 203%. In addition, ZnHA / Gel still maintains an elongation at break of approximately 180%, indicating that it achieves high strength while maintaining good flexibility.

[0098] The above results demonstrate that the introduction of ZnHA significantly improves the mechanical properties of the gel electrolyte. This is mainly attributed to the abundant hydroxyl and phosphate functional groups on the ZnHA surface, which can form a stable hydrogen bond network and interfacial interactions with the gelatin molecular chains, increasing the interfacial bonding strength between the filler and the polymer matrix and promoting uniform stress transmission in the composite system. Simultaneously, ZnHA, as a rigid inorganic framework, effectively enhances the gel network structure and suppresses local stress concentration, thereby improving the tensile strength and puncture resistance of the electrolyte. The enhanced electrolyte helps resist dendrite puncture generated during zinc anode cycling, providing a reliable guarantee for the interfacial stability and long cycle life of zinc metal batteries.

[0099] (3) Performance test of zinc metal half cell To evaluate the improvement effect of ZnHA on the reversibility of zinc anode deposition / stripping, the ZnHA / Gel electrolyte prepared in Example 1 and the Gel electrolyte prepared in Comparative Example 1 were assembled into Zn / / Cu half-cells. The zinc anode was a 10 mm diameter zinc sheet, the copper current collector was a 10 mm diameter copper foil, and the coin cell model was CR2032. The above Zn / / Cu half-cells were subjected to a 5 mA cm⁻¹ temperature. - ² Current density and 2.5 mAh cm⁻¹ - The test was conducted under the condition of ²area capacity, and the results are as follows: Figure 5 As shown, the ZnHA / Gel system can still cycle stably for about 500 cycles with a coulombic efficiency of around 99.5%; while the Gel system fails within tens of cycles. These results demonstrate that the ZnHA / Gel electrolyte can maintain excellent Zn²⁺ efficiencies even under high current density and high deposition capacity conditions. + Good transport capacity and deposition stability are beneficial for achieving uniform zinc deposition behavior.

[0100] (4) Performance testing of zinc metal symmetrical button cell To further verify the effect of ZnHA on improving the stability of the zinc metal anode interface, the electrolytes prepared in Examples 1, 5, and Comparative Example 1 were assembled into Zn / / Zn symmetric cells. Both electrodes used 15mm diameter zinc sheets, and the button cell model was CR2032. At 1 mA cm⁻¹ - ² Current density and 1 mAh cm⁻¹ - Long-term cyclic testing was conducted under the condition of ² areal capacity, and the test results are as follows: Figure 6 As shown in the figure, the Zn / / Zn symmetric cell assembled with ZnHA / Gel electrolyte can cycle stably for more than 2800 h, and the polarization voltage remains stable during the cycle; while the Gel system shows a significant increase in polarization and eventually short-circuits after several hundred hours. The results indicate that the introduction of ZnHA can effectively improve the stability of the zinc anode / electrolyte interface and suppress zinc dendrite growth and interfacial side reactions.

[0101] The results clearly demonstrate that the introduction of ZnHA as a functional inorganic filler into the gelatin gel electrolyte significantly improves the electrolyte's mechanical properties, electrochemical performance, and interfacial stability. Mechanical property testing and COMSOL mechanical simulations show that ZnHA effectively enhances the gel electrolyte network structure, improving the material's load transfer capacity and deformation resistance. Compared to pure gel electrolyte, ZnHA / Gel exhibits higher tensile strength and puncture resistance. During long-term deposition / stripping of the zinc anode, the enhanced gel electrolyte effectively resists the mechanical penetration of zinc dendrites, maintaining the electrolyte structural integrity and thus improving the battery's cycle stability and safety.

[0102] In terms of ion transport, the abundant hydroxyl groups, phosphate groups, and zinc active sites of ZnHA can promote the dissociation of Zn salts, thus facilitating Zn²⁺ ion transport. + Provides additional ion migration channels while reducing Zn² + The solvation energy barrier is removed. Therefore, ZnHA / Gel exhibits excellent ionic conductivity and high Zn²⁺. + Transfer number. Further analysis using molecular dynamics simulations and density functional theory calculations revealed that ZnHA has a strong effect on water molecules and Zn²⁺. + Both gelatin molecular chains and other components exhibit strong adsorption properties, which not only improves the interfacial compatibility between the filler and the polymer matrix but also effectively regulates Zn²⁺. + Solvation of the structure reduces the amount of coordinated water and decreases the occurrence of interfacial side reactions.

[0103] Electrochemical test results fully demonstrate the above mechanism. The Zn / / Cu half-cell exhibits a coulombic efficiency as high as 99.5%; the Zn / / Zn symmetric cell achieves a efficiency of 1 mA cm⁻¹. - Under certain conditions, it can cycle stably for over 2800 h while maintaining a low polarization voltage; the assembled Zn / / NVO full cell can cycle at 5 A g. - ¹After 1000 stable cycles at the current density, it still maintains 89% capacity retention. Meanwhile, the pouch cell can stably cycle for 300 cycles, demonstrating good potential for practical applications. The above half-cell, symmetrical cell, and full-cell test results fully demonstrate that ZnHA / Gel improves the stability of the zinc anode interface, suppresses dendrite growth, and promotes Zn²⁺… + Significant advantages in fast transmission.

[0104] Furthermore, cell compatibility experiments verified the excellent biocompatibility of ZnHA / Gel. Based on this electrolyte system, interdigitated flexible zinc metal batteries were fabricated using 3D printing technology, and wearable flexible electronic devices were successfully constructed. The devices can operate stably under conditions such as bending, skin adhesion, and gesture actuation, enabling normal power supply for electronic devices and demonstrating good performance in flexible applications.

[0105] In summary, ZnHA possesses multiple functions, including ion conduction, interface regulation, and mechanical enhancement, which can significantly improve the overall performance of gel electrolytes. Combining 3D printing manufacturing technology with a highly biocompatible gel system, the constructed ZnHA / Gel flexible energy storage device shows broad application prospects in flexible electronics, wearable devices, and bioelectronics, providing important ideas and technical pathways for the design of high-performance flexible zinc metal batteries and novel gel electrolytes.

Claims

1. A composite gel electrolyte, characterized in that, The composite gel electrolyte comprises a polymer gel matrix, zinc salt, and ZnHA filler. The ZnHA filler is a hydroxyapatite material doped with zinc ions, and the content of ZnHA filler accounts for 0.1wt% to 30wt% of the total mass of the composite gel electrolyte.

2. The composite gel electrolyte according to claim 1, characterized in that, The zinc ions, based on elemental zinc, constitute 0.1–20 wt% of the ZnHA filler mass, preferably 0.5–10 wt%. And / or, the content of the ZnHA filler accounts for 0.5 wt%-20 wt% of the total mass of the composite gel electrolyte, preferably 1 wt%-10 wt%; And / or, the zinc salt is selected from one or more of zinc sulfate, zinc trifluoromethanesulfonate, zinc chloride, zinc acetate and zinc gluconate, preferably zinc chloride or zinc sulfate; And / or, the concentration of the zinc salt in the composite gel electrolyte is 0.1–10 mol / L, preferably 1–5 mol / L; And / or, the polymer in the polymer gel matrix is ​​selected from natural polymers and their modified derivatives or synthetic polymers; Preferably, the natural polymer and its modified derivatives are selected from one or more of gelatin, sodium alginate, chitosan, carboxymethyl cellulose, and collagen; Preferably, the synthetic polymer is selected from one or more of polyvinyl alcohol, polyacrylamide, polyethylene glycol, polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyurethane, and polyacrylonitrile; Preferably, the polymer gel matrix is ​​a compound system of gelatin and polyvinyl alcohol, a compound system of gelatin and polyacrylamide, or a compound system of gelatin and polyvinylidene fluoride-hexafluoropropylene copolymer; more preferably, the polymer in the polymer gel matrix is ​​gelatin. And / or, the content of the polymer gel matrix in the composite gel electrolyte is 10 wt%-99.9 wt%, preferably 30 wt%-95 wt%, more preferably 50 wt%-90 wt%.

3. A method for preparing the composite gel electrolyte as described in claim 1 or 2, comprising the following steps: (1) Add the polymer gel matrix to the solvent and heat and stir until completely dissolved; (2) Add zinc salt to the system of step (1) and continue stirring to form a homogeneous solution; (3) Add ZnHA filler to the system of step (2) to form a uniformly dispersed slurry; (4) Use a three-dimensional printing device to print the slurry obtained in step (3) into a preset structure at a printing temperature of 20-80℃; (5) Place the printed sample from step (4) in an environment of -10 to 10℃ for gelation treatment; (6) The gelled sample from step (5) is immersed in zinc salt solution for activation treatment to obtain composite gel electrolyte.

4. The preparation method according to claim 3, characterized in that, The solvent is deionized water, an organic solvent, or a mixture thereof; preferably deionized water. And / or, the mass-to-volume ratio of the polymer gel matrix to the solvent is 0.05-0.3 g / mL; And / or, in step (2), the amount of ZnHA filler added is 0.1 wt%-30 wt% of the polymer gel mass, preferably 0.5 wt%~20 wt%; And / or, in step (5), the gelation treatment time is 0.2-8 h; And / or, in step (6), the concentration of the zinc salt solution is 0.5-5 mol / L.

5. A composite gel electrolyte prepared by the preparation method as described in claim 3 or 4.

6. A three-dimensional printed flexible zinc metal battery, comprising a composite gel electrolyte as described in any one of claims 1, 2 and 5, and an electrode slurry for three-dimensional printing the zinc metal battery.

7. The three-dimensional printed flexible zinc metal battery according to claim 6, characterized in that, The active substance, conductive agent, binder, and solvent; Preferably, the active material is selected from at least one of the positive electrode active material and the negative electrode active material; Preferably, the positive electrode active material is selected from one or more of ammonium vanadate, vanadium pentoxide, and manganese dioxide; ammonium vanadate is preferred. Preferably, the negative electrode active material is selected from spherical zinc powder or zinc alloy powder, and more preferably spherical zinc powder; Preferably, the conductive agent is selected from one or more of carbon nanotubes, graphene, and carbon black, with carbon nanotubes being the most preferred. Preferably, the adhesive is selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylic acid and carboxymethyl cellulose, and is preferably polyvinylidene fluoride; Preferably, the solvent is N-methyl-2-pyrrolidone (NMP) or deionized water; Preferably, when the adhesive is PVDF, the solvent is NMP; Preferably, when the electrode slurry used for 3D printing zinc metal batteries is a positive electrode slurry, the mass ratio of the positive electrode active material, the conductive agent and the binder is (6-9):(0.5-2):(0.5-2), preferably 18:1:1; Preferably, when the electrode slurry used for 3D printing zinc metal batteries is a negative electrode slurry, the mass ratio of the negative electrode active material (e.g., zinc powder), the conductive agent, and the binder is (7-9):(0.5-1.5):(0.5-1.5), preferably 9:0.5:0.5; Preferably, the structure of the three-dimensional printed flexible zinc metal battery is: a positive electrode structure and a negative electrode structure formed on the same plane by three-dimensional printing, and the composite gel electrolyte covering the surfaces of the positive electrode structure and the negative electrode structure; Preferably, the positive electrode structure and the negative electrode structure are arranged alternately on the same substrate surface, and the composite gel electrolyte covers the surfaces of the positive electrode structure and the negative electrode structure and fills the gap between them; Preferably, the positive and negative electrode structures are arranged in an interdigitated pattern, with adjacent positive and negative electrodes nested together to form a planar interdigitated structure; both the positive and negative electrode structures are fabricated using 3D printing. Preferably, the positive electrode structure is an electrode structure composed of ammonium vanadate, and the negative electrode structure is an electrode structure composed of zinc powder.

8. A flexible power supply system comprising the three-dimensional printed flexible zinc metal battery as described in claim 7.

9. A flexible wearable electronic device, comprising a three-dimensional printed flexible zinc metal battery as described in claim 7 or a flexible power supply system as described in claim 8, and functional devices integrated on the same flexible substrate; Preferably, the functional device is selected from one or more of flexible sensors, flexible switches, flexible circuits, flexible LEDs, and health monitoring sensors; Preferably, the functional device and the three-dimensional printed flexible zinc metal battery are electrically connected through 3D-printed conductive lines.

10. The application of a composite gel electrolyte as described in any one of claims 1, 2 and 5, or a three-dimensional printed flexible zinc metal battery as described in claim 7, or a flexible power supply system as described in claim 8, or a flexible wearable electronic device as described in claim 9 in energy storage devices, flexible electronic devices, wearable devices, health monitoring devices, human-computer interaction devices and intelligent sensing systems.