Method for synthesizing mg-o-based catalyst and use thereof

CN122682592APending Publication Date: 2026-09-04새틀라이트뉴머티리얼즈알앤디컴퍼니리미티드
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610936739.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-26
Publication Date
2026-09-04

AI Technical Summary

Technical Problem

[0005]1、共沉淀法中,Mg(OH)2、Ce(OH)4、La(OH)3的最佳沉淀pH差异显著,无法实现金属离子均匀共沉淀,导致催化剂组分分布不均、性能重复性差;以NaOH为沉淀剂时,Na+杂质难以通过洗涤彻底去除,残留Na+会进入反应体系影响产品纯度,增加后处理除杂成本与工艺复杂度;且高温焙烧过程中,MgO纳米颗粒易发生奥斯特瓦尔德熟化与烧结,造成晶粒显著长大、活性位点数量锐减,催化活性持续下降;

Benefits of technology

[0028]1. This invention prepares MgO-based catalysts by combining the dry gelation method with combustion decomposition. The preparation process is simple, the conditions are easy to control, and it is easy to repeat. It eliminates the need for pH adjustment, long-term aging, and repeated sodium removal washing steps required in traditional co-precipitation methods. This fundamentally avoids the problem of component inhomogeneity caused by the mismatch of pH ranges for precipitation of different metal hydroxides, and at the same time eliminates the introduction of Na by sodium hydroxide precipitant. + The risk of product contamination from residues is reduced, and the preparation cost and process difficulty are lowered, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122682592A_ABST
    Figure CN122682592A_ABST
Patent Text Reader

Abstract

The application discloses a MgO-based catalyst synthesis method and application thereof, relates to the technical field of catalyst preparation, and comprises the following steps: dissolving magnesium salt, lanthanum salt, cerium salt, calcium salt and nickel salt in deionized water, stirring uniformly to obtain a metal salt solution; adding citric acid into the metal salt solution and stirring intensively until uniform to form a mixed gel; pouring the mixed gel on a medium-speed qualitative filter paper, transferring and drying to obtain a dry gel; roasting the dry gel with the filter paper, grinding the roasted dry gel with a mortar to obtain a grinding powder; and transferring the grinding powder to a muffle furnace for calcination to obtain a uniform composite metal oxide catalyst; the MgO-based catalyst is prepared by combining the dry gel method with the combustion decomposition method, the preparation process is simple, the conditions are easy to control, the preparation process is easy to repeat, the product pollution risk caused by the introduction of sodium hydroxide precipitator is eliminated, the preparation cost and process difficulty are reduced, and the method is suitable for large-scale production. + ​
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst preparation technology, specifically relating to a method for synthesizing MgO-based catalysts and their applications. Background Technology

[0002] 2,2-Dimethyl-3-hydroxypropionic acid-2,2-dimethyl-3-carboxypropyl ester (neopentyl glycol monoester, HPN, also known as 1115 ester) is a compound with a unique molecular structure. The symmetrically distributed dimethyl quaternary carbon structure on both sides of the ester group endows this ester with excellent thermal stability, hydrolysis resistance, and antioxidant properties. At the same time, the 1115 ester molecular skeleton is highly flexible, making it a high-value diol compound widely used in the manufacture of high-performance impact-resistant and tough resins and high-quality lubricants. The synthesis of 1115 ester from 2,2-dimethyl-3-hydroxypropanal (hydroxypentanal, HPA) via catalytic disproportionation is a key reaction in the preparation of high-performance impact-resistant and tough resins, high-quality lubricants, and other high-end chemicals. This reaction has strict requirements on the basicity, active site density, structural stability, and separation and recovery of the catalyst. MgO-based solid base catalysts, due to their strong basicity, high thermal stability, and environmental friendliness, have become the most widely used catalytic system in the HPA disproportionation to HPN reaction.

[0003] Currently, MgO-based catalysts used in the HPA-to-HPN reaction are mainly prepared by co-precipitation and traditional supported methods, with some attempts to design reverse-phase catalyst structures to improve performance. The co-precipitation method uses magnesium salts and metal promoter salts as precursors, employing strong bases such as NaOH as precipitants. By adjusting the solution pH, metal ions are simultaneously precipitated as hydroxides. After aging, washing, drying, and high-temperature calcination, a composite metal oxide catalyst is obtained. Its principle is to enhance catalytic activity through the synergistic effect of different metal oxide interfaces. Supported MgO catalysts use porous materials such as SiO2 and Al2O3 as supports. The active MgO component is dispersed on the support surface through impregnation or co-current precipitation. The porous structure and high specific surface area of ​​the support inhibit the aggregation of active components, improving catalyst stability and separability. Reverse-phase catalysts load the active MgO phase onto the surface of metal promoter oxides, actively constructing a continuous high-density active interface to further enhance catalytic efficiency.

[0004] However, MgO-based catalysts used in the HPA-to-HPN reaction have the following drawbacks:

[0005] 1. In the co-precipitation method, the optimal precipitation pH for Mg(OH)₂, Ce(OH)₄, and La(OH)₃ differs significantly, making it impossible to achieve uniform co-precipitation of metal ions. This results in uneven catalyst component distribution and poor performance repeatability. When NaOH is used as the precipitant, Na… + Impurities are difficult to remove completely by washing, leaving residual Na. +It will enter the reaction system, affecting product purity, increasing the cost of post-processing and impurity removal, and increasing process complexity; and during high-temperature calcination, MgO nanoparticles are prone to Ostwald ripening and sintering, resulting in significant grain growth, a sharp reduction in the number of active sites, and a continuous decline in catalytic activity.

[0006] 2. Traditional supported catalysts are limited by the solubility of metal salt solutions and the specific surface area of ​​the support, making it difficult to achieve high MgO loading and resulting in low overall catalytic activity. Supports such as Al2O3 tend to form a dense magnesium aluminum spinel structure with MgO, which causes the Mg active sites to be coated and completely lose their catalytic activity. At the same time, soluble base catalysts have problems such as difficult product separation and strong equipment corrosion, while ion exchange resin catalysts have defects such as swelling and short lifespan.

[0007] 3. Reversed catalyst structures generally suffer from problems such as cumbersome synthesis steps, difficult washing, and low filtration and separation efficiency, which seriously restrict the efficient and green industrial production of HPN.

[0008] Based on the above-mentioned shortcomings, there is an urgent need to provide a method for synthesizing MgO-based catalysts and their applications, so that the synthesized catalysts have good activity, are easy to prepare, and are suitable for the reaction of HPA to HPN. Summary of the Invention

[0009] The purpose of this invention is to provide a method for synthesizing MgO-based catalysts and their applications. The MgO-based catalysts prepared by this method are characterized by simple and rapid preparation and excellent activity, thereby solving the problems mentioned in the background art.

[0010] To achieve the above objectives, the present invention adopts the following technical solution:

[0011] A method for synthesizing MgO-based catalysts includes the following steps:

[0012] S1. Dissolve magnesium salt, lanthanum salt, cerium salt, calcium salt and nickel salt in deionized water and stir until homogeneous to obtain a metal salt solution;

[0013] S2. Add citric acid to the metal salt solution and stir vigorously until homogeneous to form a mixed gel;

[0014] S3. Pour the mixed gel onto medium-speed qualitative filter paper, transfer it, and then dry it to obtain a dry gel.

[0015] S4. The dry gel and filter paper are calcined, and after calcination, they are ground in a mortar and pestle to obtain a powder.

[0016] S5. Transfer the ground powder to a muffle furnace for calcination to obtain a uniform composite metal oxide catalyst.

[0017] Preferably, in step S1, the metal salt solution comprises the following raw materials by molar percentage: 50%-100% magnesium salt, 0%-50% lanthanum salt, 0%-50% cerium salt, 0%-20% calcium salt, and 0%-10% nickel salt, and the amount of deionized water used is 25 times the total amount of magnesium salt, lanthanum salt, cerium salt, calcium salt, and nickel salt.

[0018] Preferably, the magnesium salt is one or more of magnesium nitrate hexahydrate and magnesium sulfate heptahydrate, and the lanthanum salt is one or more of lanthanum nitrate hexahydrate and lanthanum sulfate octahydrate.

[0019] Preferably, the cerium salt is one or more of cerium nitrate hexahydrate and cerium ammonium sulfate.

[0020] Preferably, the calcium salt is one or more of calcium nitrate tetrahydrate and calcium nitrite; the nickel salt is nickel nitrate hexahydrate.

[0021] Preferably, in step S2, the citric acid is anhydrous citric acid or citric acid monohydrate, and the amount of citric acid added is 0.2 times the total metal salt solution.

[0022] Preferably, in step S3, the mixed gel and medium-speed qualitative filter paper are dried in an oven at 90°C for 12 hours.

[0023] Preferably, in step S4, the dry gel and filter paper are calcined at a temperature of 200℃-250℃ for 4-5 hours, and then ground in a mortar to obtain a powder with particles smaller than 60 mesh.

[0024] Preferably, in step S5, the calcination temperature in the muffle furnace is 700℃-800℃, and the calcination time is 5-6 hours.

[0025] A composite metal oxide catalyst, prepared by the above-described MgO-based catalyst synthesis method, comprises the following raw materials in molar percentage: MgO 50%-100%, La2O3 0-25%, CeO2 0-50%, CaO 0-20%, NiO 0-10%, and the sum of the molar percentages of each component is 100%.

[0026] An application of an MgO-based catalyst, including a composite metal oxide catalyst, is disclosed in the HPA conversion process for 1115 ester.

[0027] The present invention provides a method for synthesizing MgO-based catalysts and their applications, which have the following advantages compared with existing technologies:

[0028] 1. This invention prepares MgO-based catalysts by combining the dry gelation method with combustion decomposition. The preparation process is simple, the conditions are easy to control, and it is easy to repeat. It eliminates the need for pH adjustment, long-term aging, and repeated sodium removal washing steps required in traditional co-precipitation methods. This fundamentally avoids the problem of component inhomogeneity caused by the mismatch of pH ranges for precipitation of different metal hydroxides, and at the same time eliminates the introduction of Na by sodium hydroxide precipitant. + The risk of product contamination from residues is reduced, and the preparation cost and process difficulty are lowered, making it suitable for large-scale production.

[0029] 2. This invention constructs a reverse-phase catalyst by introducing magnesium salt, lanthanum salt, cerium salt, calcium salt and nickel salt metal promoters, which can form a continuous and high-density metal oxide-active site interface. Combined with citric acid calcination to create pores, it improves the specific surface area and the dispersion of active sites, inhibits the migration, sintering and Ostwald ripening of MgO particles at high temperature, and makes the catalyst structure more stable, improves catalytic activity and service life, and does not generate inert phases such as magnesium aluminum spinel, ensuring highly efficient active sites.

[0030] 3. The composite metal oxide catalyst prepared by this invention can be used directly without activation and applied to the HPA conversion of 1115 ester process. At the same time, the composite metal oxide catalyst is a solid powder that is easy to separate and recover, which improves the overall catalytic activity, reaction efficiency and industrial applicability. Attached Figure Description

[0031] Figure 1 This is a flowchart of the present invention;

[0032] Figure 2 This is an XRD test result diagram of catalyst A of the present invention;

[0033] Figure 3 This is a graph showing the XRD test results of the C catalyst of this invention;

[0034] Figure 4 This is a graph showing the XRD test results of the D catalyst of this invention;

[0035] Figure 5 The image shows the XRD test results of the comparative F catalyst.

[0036] Figure 6 The image shows the XRD test results of the comparative H catalyst.

[0037] Figure 7 The image shows the XRD test results of catalyst J in the comparative example. Detailed Implementation

[0038] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The specific embodiments described herein are merely used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0039] This invention provides, for example Figure 1 The method for synthesizing an MgO-based catalyst, as shown, includes the following steps:

[0040] S1. Dissolve magnesium salt, lanthanum salt, cerium salt, calcium salt, and nickel salt in deionized water and stir until homogeneous to obtain a metal salt solution; wherein, by molar percentage, the metal salt solution contains the following raw materials: 50%-100% magnesium salt, 0%-50% lanthanum salt, 0%-50% cerium salt, 0%-20% calcium salt, and 0%-10% nickel salt, the sum of the molar percentages of each component is 100%, and the amount of deionized water used is 25 times the total amount of magnesium salt, lanthanum salt, cerium salt, calcium salt, and nickel salt;

[0041] Specifically, the magnesium salt is one or more of magnesium nitrate hexahydrate and magnesium sulfate heptahydrate; the lanthanum salt is one or more of lanthanum nitrate hexahydrate and lanthanum sulfate octahydrate; the cerium salt is one or more of cerium nitrate hexahydrate and cerium ammonium sulfate; the calcium salt is one or more of calcium nitrate tetrahydrate and calcium nitrite; and the nickel salt is nickel nitrate hexahydrate.

[0042] S2. Add citric acid to the metal salt solution and stir vigorously until homogeneous to form a mixed gel;

[0043] Wherein, the citric acid is anhydrous citric acid or citric acid monohydrate, and the amount of citric acid added is 0.2 times the total metal salt solution;

[0044] S3. Pour the mixed gel onto medium-speed qualitative filter paper, transfer it, and then dry it to obtain a dry gel; wherein, the mixed gel and the medium-speed qualitative filter paper are dried in an oven at 90°C for 12 hours.

[0045] S4. The dry gel and filter paper are calcined, and after calcination, they are ground in a mortar to obtain a powder. The calcination temperature of the dry gel and filter paper is 200℃-250℃, the calcination time is 4-5 hours, and the powder obtained after grinding in the mortar is less than 60 mesh.

[0046] S5. The ground powder is transferred to a muffle furnace for calcination to obtain a uniform composite metal oxide catalyst; the calcination temperature in the muffle furnace is 700℃-800℃, and the calcination time is 5-6 hours.

[0047] The preparation of MgO-based catalysts by combining the dry gelation method and combustion decomposition method is simple, with easily controllable and reproducible conditions. It eliminates the need for pH adjustment, long-term aging, and repeated sodium removal washing steps required in traditional co-precipitation methods, fundamentally avoiding the component inhomogeneity problem caused by the mismatch in pH ranges of different metal hydroxide precipitation. Simultaneously, it eliminates the introduction of Na+ by the sodium hydroxide precipitant. + The risk of product contamination from residues is reduced, and the preparation cost and process difficulty are lowered, making it suitable for large-scale production.

[0048] By introducing magnesium salt, lanthanum salt, cerium salt, calcium salt and nickel salt metal promoters to construct a reverse-phase catalyst, a continuous and high-density metal oxide-active site interface can be formed. Combined with citric acid calcination to create pores, the specific surface area and active site dispersion are improved, and the migration, sintering and Ostwald ripening of MgO particles at high temperature are suppressed. The catalyst structure is more stable, the catalytic activity and service life are improved, and no inert phases such as magnesium aluminum spinel are generated, ensuring highly efficient active sites.

[0049] A composite metal oxide catalyst, prepared by the above-described MgO-based catalyst synthesis method, comprises the following raw materials in molar percentage: MgO 50%-100%, La2O3 0-25%, CeO2 0-50%, CaO 0-20%, NiO 0-10%, and the sum of the molar percentages of each component is 100%.

[0050] The composite metal oxide catalyst prepared by the above synthesis method can be used directly without activation. It is applied in the HPA conversion of 1115 ester. Furthermore, this composite metal oxide catalyst is a solid powder, making it easy to separate and recover, thus improving overall catalytic activity, reaction efficiency, and industrial applicability.

[0051] To verify the effectiveness of the MgO-based catalyst prepared by the above synthesis method, the present invention provides the following specific examples and comparative examples:

[0052] Example 1

[0053] The catalyst composition is 90% mol% MgO and 10% mol% La2O3. 0.16 mol magnesium nitrate hexahydrate and 0.04 mol lanthanum nitrate nonahydrate were added to 60 g of deionized water and stirred at room temperature to dissolve. After uniform dissolution, 0.04 mol anhydrous citric acid was added and stirred until completely dissolved. The resulting gel solution was then transferred to a glass container with filter paper for adsorption. After adsorption, the catalyst was transferred to a 90°C oven for drying. The dried filter paper and solid were crushed and calcined at 220°C for 5 h. The solid from the calcined crucible was then removed and calcined at 750°C for 5 h to obtain catalyst A.

[0054] Example 2

[0055] The catalyst composition is 75% mol% MgO and 25% mol% La2O3. 0.15 mol magnesium nitrate hexahydrate and 0.05 mol lanthanum nitrate nonahydrate were added to 60 g of deionized water and stirred at room temperature. After the metal salts were completely dissolved, 0.04 mol anhydrous citric acid was slowly added. After the anhydrous citric acid was completely dissolved, the resulting gel solution was transferred to a glass container, and filter paper was added for adsorption. The solution was dried overnight in an oven at 90 °C. The resulting filter paper catalyst solid was divided and calcined at 220 °C for 5 h. The calcined catalyst solid was then ground, and the resulting powder was calcined at 750 °C for 5 h to obtain catalyst B.

[0056] Example 3

[0057] The catalyst composition is 80% mol% MgO and 20% mol% CeO2. 0.16 mol magnesium nitrate and 0.04 mol cerium nitrate were added to 60 g of deionized water and stirred at room temperature to dissolve, yielding a clear metal precursor solution. 0.04 mol anhydrous citric acid was added to the metal solution and stirred vigorously until the anhydrous citric acid was completely dissolved, resulting in a catalyst gel. The gel was transferred to a glass container and filtered with filter paper for adsorption. It was then dried overnight in a 90°C oven to convert the gel into a dry gel. The dried filter paper and solid were separated and calcined at 250°C for 4 h. The catalyst was then removed, ground, and transferred to a muffle furnace for calcination at 750°C for 6 h to obtain the final catalyst C.

[0058] Example 4

[0059] The catalyst composition is 80% mol% MgO and 20% mol% CaO. 0.16 mol magnesium nitrate and 0.04 mol calcium nitrate were added to 60 g of deionized water and stirred thoroughly to dissolve, yielding a colorless metal solution. 0.04 mol anhydrous citric acid was added to the above mixed solution, and stirring continued until the anhydrous citric acid dissolved. The resulting gel was transferred to a glass container and lined with filter paper to allow complete adsorption. The entire mixture was then dried overnight in a 90°C oven to obtain a dry gel. The dry gel was decomposed and calcined at 250°C for 5 h, followed by grinding and calcination at 750°C for 6 h to obtain catalyst D.

[0060] Example 5

[0061] The catalyst composition is 70% mol% MgO, 20% mol% CeO2, and 10% mol% NiO. 0.14 mol magnesium nitrate, 0.04 mol cerium nitrate, and 0.02 mol nickel nitrate were added to 60 g of deionized water and stirred thoroughly to dissolve, yielding a pale green metal precursor solution. 0.04 mol anhydrous citric acid was added to the pale green metal precursor solution, and stirring continued until the anhydrous citric acid dissolved. The resulting gel was transferred to a glass container and lined with filter paper to adsorb the gel. The wet gel was transferred to a 90°C oven and dried overnight to obtain a dry gel. The dry gel was decomposed and calcined at 220°C for 5 h, then ground and calcined at 750°C for 6 h to obtain catalyst E.

[0062] Comparative Example 1

[0063] The synthesis of the catalyst MgO particles is based on Clean Techn Environ Policy 20, 1219-1231 (2018);

[0064] Add magnesium nitrate to 100 mL of deionized water to make Mg 2+ The concentration of 0.1M was used to prepare a Mg salt solution after vigorous stirring. Simultaneously, a 0.1M NaOH solution was prepared and vigorously stirred until dissolved, yielding a precipitant solution. The NaOH aqueous solution was slowly added dropwise to the Mg salt solution using a reverse addition method, with thorough stirring, until the pH reached 12-13. The addition of the precipitant was then stopped, resulting in a white turbid liquid. This liquid was then aged with continuous stirring for 12 hours. After aging, the solid in the solution was Mg(OH)₂. The solution was transferred to a Buchner funnel for filtration. Since NaOH was used as the precipitant, the Na₂O₃ in the solution was filtered. + It can only be removed in the filtration step, otherwise it will remain in the catalyst and gradually dissolve in the reaction solution during the reaction process, thus affecting the product quality. The filtration step must ensure that the conductivity of the filtrate is <30μs / cm. After washing, it is dried in an oven at 60℃, ground, and then calcined in a muffle furnace at 700℃ for 5h to obtain catalyst F.

[0065] Comparative Example 2:

[0066] The catalyst composition is 100% MgO. 0.2 mol magnesium nitrate was added to 60 g of deionized water and stirred thoroughly to dissolve. 0.04 mol citric acid monohydrate was added to the above mixed solution and stirred continuously until completely dissolved. The resulting gel was transferred to a glass container and lined with filter paper to allow the gel to be fully adsorbed. The entire mixture was then transferred to a 90°C oven and dried overnight to obtain a dry gel. The dry gel was decomposed and calcined at 220°C for 5 h. Subsequently, it was removed, ground, and calcined at 700°C for 6 h to obtain catalyst G.

[0067] Comparative Example 3:

[0068] The catalyst in Comparative Example 3 was referenced from an article published in the Journal of Qingdao University of Science and Technology on the synthesis of neopentyl glycol monoester of hydroxypentyl acid catalyzed by supported MgO / SiO2.

[0069] In a constant temperature water bath at 40℃, 0.5 mol of Mg(NO3)2 aqueous solution and 0.5 mol of NaOH aqueous solution were added dropwise to a beaker while stirring. The dropwise flow rate was 1:2 for metal salt and precipitant. The solution temperature was maintained at 35℃-40℃ during the titration process. The target amount of alkaline silica gel was added dropwise to the above mixed solution to make the molar percentage of MgO in the final solid 80%. After titration, the temperature was raised to 80℃ for aging for 12 hours. After aging, the solution was transferred to a Buchner funnel for filtration. After the conductivity of the filtrate was <30 μs / cm, it was dried at 90℃. After grinding, it was calcined at 500℃ for 12 hours to obtain the supported catalyst H.

[0070] Comparative Example 4:

[0071] The catalyst composition is 80% mol% MgO and 20% mol% SiO2. Following the Mg to Si molar ratio in Comparative Example 3, 0.08 mol of magnesium nitrate was added to 30 g of deionized water and stirred at room temperature for 30 min. Then, 0.02 mol of tetraethyl orthosilicate was added, and stirring continued for another 30 min. After stirring, 0.02 mol of citric acid monohydrate was added and stirred vigorously until the solution was homogeneous and free of solid residue. The solution was then transferred to a glass container and adsorbed onto filter paper. The container and filter paper were then dried overnight in a 90°C oven to convert the gel to a dry gel. The dried filter paper and solid were separated and calcined at 250°C for 4 h. The catalyst was then removed, ground, and transferred to a muffle furnace for calcination at 700°C for 8 h to obtain the final catalyst I.

[0072] Comparative Example 5:

[0073] The catalyst composition is 90% MgO and 10% Al₂O₃. 0.16 mol magnesium nitrate hexahydrate and 0.04 mol aluminum nitrate nonahydrate were added to 60 g of deionized water and dissolved by stirring at room temperature. After stirring for 30 min, 0.04 mol anhydrous citric acid was added and the mixture was stirred vigorously. The resulting solution was transferred to a glass container, filtered using filter paper, and then dried in a 90 °C oven. The dried solid was divided and calcined at 250 °C for 4 h. After calcination, the remaining solid was ground and then calcined in a muffle furnace at 750 °C for 5 h to obtain catalyst J.

[0074] The catalysts prepared in Examples 1 to 5 and the catalysts prepared in Comparative Examples 1 to 5 were evaluated respectively, and the evaluation conditions were as follows:

[0075] (1) The test was conducted in a batch reactor. The reaction temperature was 90℃, the stirring speed was 600rpm, and the gas was air. No additional gas was added during the reaction.

[0076] (2) The default reaction materials are: HPA 6g, H2O 4g, catalyst 0.2g, reaction time 3h, and the catalyst used is the solid powder obtained by calcination in the last step of the example and comparative example. Any changes in conditions will be explained in the table.

[0077] The test results are shown in Table 1:

[0078] Table 1

[0079]

[0080] In Table 1, * indicates that the reaction used 0.2g of catalyst, and the contents of HPA and H2O were doubled to 12g and 8g respectively.

[0081] The data in Table 1 show that the HPA conversion rates of Examples 1-5 are 74%-96%, which is significantly higher than the 15%-73% in Comparative Examples 1-5. This further demonstrates that the catalysts synthesized in Examples 1-5 have significantly improved activity compared to Comparative Examples 1-5.

[0082] Among them, such as Figure 2 The figure shows the XRD test results of catalyst A. In the figure, Mg element in catalyst A exists in the form of MgO, and La element in the catalyst exists in the form of LaOOH and La2O3. The XRD diffraction peak signal attributable to MgO becomes weaker and wider, indicating that under the action of various oxides formed after the introduction of La element, the MgO particle crystals become smaller and the dispersion becomes higher, and no special dense structure is formed, which greatly improves its activity.

[0083] like Figure 3 The figure shows the XRD test results of the C catalyst. The figure shows that the C catalyst introduces 20% molar fraction of Ce element. The XRD results show two phases, CeO2 and MgO. The XRD diffraction peak of MgO becomes wider, indicating that a small amount of CeO2 exists on the surface, which allows MgO to be well dispersed. This helps HPA to be adsorbed onto the Mg2+ active site and further promotes the disproportionation reaction.

[0084] like Figure 4The figure shows the XRD test results of catalyst D. The figure shows that the catalyst surface consists of three phases: Ca(OH)2, CaO, and MgO. Although the diffraction peak at around 43° belonging to MgO is strong and sharp, representing larger MgO particles, the presence of CaO and Ca(OH)2 species means that they also act as active centers and react, and may also have a synergistic effect with MgO. This gives the catalyst described in Example 5 extremely high catalytic activity, enabling it to achieve a better conversion rate in a shorter time.

[0085] like Figure 5 The figure shows the XRD test results of the F catalyst solid powder. After the preparation process of Comparative Example 1, the obtained catalyst is a homogeneous MgO, which confirms that the catalyst is MgO powder.

[0086] like Figure 6 As shown, the solid XRD test results of the H catalyst are shown. The catalyst surface is present with substances such as MgO and MgSiO3 (SiO2). The relevant XRD diffraction peaks are very weak, that is, the SiO2 species present on the surface are extremely low. The MgO participating in the reaction on the catalyst surface is almost similar to the MgO dispersion form. Therefore, the catalyst activity is only slightly improved.

[0087] like Figure 7 The image shows the XRD results of catalyst powder J. The catalyst surface exists entirely in the form of MgAl2O4 (magnesium aluminum spinel), and the peaks attributed to MgO have completely disappeared. The MgAl2O4 surface is dense, and Mg atoms are entirely contained within the framework. It is often used as a support with excellent stability, but it often lacks catalytic activity. Therefore, using Al2O3 as a support or as a metal additive is not suitable in the HPA-to-1115 ester production system.

[0088] In summary, magnesium salt and metal additive salt solutions are converted into gels by citric acid or citric acid monohydrate, the gels are dried to form dry gels, and then calcined to obtain a homogeneous reverse MgO-based catalyst containing metal additives. During the calcination process, citric acid decomposes upon heating, thereby generating some pores inside the catalyst, increasing the specific surface area of ​​the catalyst, and thus improving the catalyst activity.

[0089] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for synthesizing an MgO-based catalyst, characterized in that: Includes the following steps: S1. Dissolve magnesium salt, lanthanum salt, cerium salt, calcium salt and nickel salt in deionized water and stir until homogeneous to obtain a metal salt solution; S2. Add citric acid to the metal salt solution and stir vigorously until homogeneous to form a mixed gel; S3. Pour the mixed gel onto medium-speed qualitative filter paper, transfer it, and then dry it to obtain a dry gel. S4. The dry gel and filter paper are calcined, and after calcination, they are ground in a mortar and pestle to obtain a powder. S5. Transfer the ground powder to a muffle furnace for calcination to obtain a uniform composite metal oxide catalyst.

2. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: In step S1, the metal salt solution contains the following raw materials by molar percentage: 50%-100% magnesium salt, 0%-50% lanthanum salt, 0%-50% cerium salt, 0%-20% calcium salt, and 0%-10% nickel salt. The amount of deionized water used is 25 times the total amount of magnesium salt, lanthanum salt, cerium salt, calcium salt, and nickel salt.

3. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: The magnesium salt is one or more of magnesium nitrate hexahydrate and magnesium sulfate heptahydrate, and the lanthanum salt is one or more of lanthanum nitrate hexahydrate and lanthanum sulfate octahydrate.

4. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: The cerium salt is one or more of cerium nitrate hexahydrate and cerium ammonium sulfate; the calcium salt is one or more of calcium nitrate tetrahydrate and calcium nitrite; and the nickel salt is nickel nitrate hexahydrate.

5. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: In step S2, the citric acid is anhydrous citric acid or citric acid monohydrate, and the amount of citric acid added is 0.2 times the total metal salt solution.

6. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: In step S3, the mixed gel and medium-speed qualitative filter paper are dried in an oven at 90°C for 12 hours.

7. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: In step S4, the dry gel and filter paper are calcined at a temperature of 200℃-250℃ for 4-5 hours, and then ground in a mortar to obtain a powder with particles smaller than 60 mesh.

8. The method for synthesizing an MgO-based catalyst according to claim 1, characterized in that: In step S5, the calcination temperature in the muffle furnace is 700℃-800℃, and the calcination time is 5-6 hours.

9. A composite metal oxide catalyst, prepared using the synthesis method of an MgO-based catalyst according to any one of claims 1-8, characterized in that: The product contains the following raw materials by molar percentage: MgO 50%-100%, La2O3 0-25%, CeO2 0-50%, CaO 0-20%, NiO 0-10%, and the sum of the molar percentages of each component is 100%.

10. An application of an MgO-based catalyst, comprising the composite metal oxide catalyst of claim 9, characterized in that: The composite metal oxide catalyst is used in the HPA conversion process of 1115 ester.