A production process for SUP13Cr stainless steel bars

CN122702820APending Publication Date: 2026-09-08AVIC SHANGDA METAL REGENERATION TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610916808.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-24
Publication Date
2026-09-08

AI Technical Summary

Technical Problem

这种残留相的存在破坏了集体组织的连续性,引发一系列性能劣化问题

Benefits of technology

本发明工艺的成分控制在Ni、Cr、Mo等元素符合标准要求的前提下,适当提高奥氏体形成元素(N元素)含量,在保证耐蚀性的前提下降低δ铁素体的形成倾向;在锭型选择中,本次试验生产的棒材规格为Φ300mm,本发明采用26吋熔炼锭,与同等规格棒材使用的30吋熔炼锭相比,小锭型钢锭在熔炼过程中的凝固速度快,可以一定程度上减轻Cr、Mo等元素的微观偏析,避免因局部成分超标而诱发δ铁素体,同时由于小锭型晶粒更细小,即使产生少量铁素体也更易在下一道工序中被消除。因此,小锭型钢锭的选用可以从源头最大程度上抑制高温铁素体的形成;对于SUP13Cr这种材料,在锻造过程中,变形量(尤其是累计的、足够大的变形量)是减少和细化高温铁素体最有效的工艺手段之一。本发明在锻造工序中,钢锭在1140±10℃保温4-5h后出炉锻造,与同等规格棒材采用的一火成型工艺不同,本发明锻造工序采用一火镦粗、二火成型的两火工艺,有效减少和细化了高温铁素体。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122702820A_ABST
    Figure CN122702820A_ABST
Patent Text Reader

Abstract

This invention discloses a production process for SUP13Cr stainless steel bars, relating to the field of metal forging technology. The process includes the following steps: electric furnace, AOD (Advanced Oxidation Discharge), LF (Frost-Reduction), VD (Vacuum-Deposition), stacking cooling, grinding, forging, and annealing. The forging process includes a single upsetting and drawing operation, followed by reheating at 1140℃±10℃ for 2-4 hours, a second drawing and rounding operation after removal from the furnace, and finally annealing at 650±10℃ for 30 hours. This invention reduces the tendency for δ-ferrite formation by controlling the nitrogen content of the SUP13Cr ingot while ensuring corrosion resistance. Simultaneously, it employs a small ingot shape with large deformation during forging, ensuring reduced microscopic segregation of Cr, Mo, and other elements while increasing the forging deformation, effectively breaking down the original cast dendritic structure and reducing and refining high-temperature ferrite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal forging technology, and in particular to a production process for SUP13Cr stainless steel bars. Background Technology

[0002] SUP13Cr (Super 13Cr) stainless steel is an ultra-low carbon martensitic stainless steel developed from traditional 13Cr martensitic stainless steel. It belongs to the high corrosion-resistant oil well pipe steel grade in the API 5CT standard, with UNS number S41426 and EN standard number 1.4415. Its core composition is designed as follows: carbon ≤0.03% (ultra-low carbon), chromium 11.5-13.5%, nickel 4.5-6.5%, molybdenum 1.5-3.0%, supplemented with trace amounts of titanium, niobium, and other elements to refine the grain and stabilize carbonitrides. This compositional optimization significantly improves the material's resistance to carbon dioxide corrosion and mechanical properties, while reducing the risk of intergranular corrosion, making it a key structural material for oil and gas extraction, especially in environments with carbon dioxide corrosion.

[0003] SUP13Cr bars are mainly used to manufacture key components such as casing, tubing, and downhole tools for oil wells. They are also widely used in corrosive environments such as chemical and marine engineering, and their service environments are mostly harsh conditions with high temperature, high pressure, and chloride ions and carbon dioxide.

[0004] The ideal microstructure of SUP13Cr is a uniform tempered martensite with a small amount of reverse-transformed austenite, achieving a balance between high strength and good toughness. However, a significant contradiction exists between its high-chromium, high-molybdenum composition design and manufacturing process, leading to the easy formation of δ-ferrite in the microstructure. This becomes a core bottleneck restricting the material's performance, directly affecting its toughness, corrosion resistance, and processing properties. Current research focuses on three main directions: precise control of composition, optimized ingot shape selection, and process optimization, to further improve the comprehensive performance of SUP13Cr bars, meet more demanding service conditions, and promote its widespread application in deep-sea oil and gas, high-temperature geothermal, and other fields.

[0005] δ-ferrite is a body-centered cubic phase formed during high-temperature austenitization. Due to the high content of ferrite-forming elements such as Cr and Mo in SUP13Cr, it is difficult for it to completely transform into austenite during solidification and heating, and some δ-ferrite is retained to room temperature. The presence of this residual phase disrupts the continuity of the microstructure and causes a series of performance degradation problems. Summary of the Invention

[0006] The purpose of this invention is to provide a production process for SUP13Cr stainless steel bars. By appropriately increasing the nitrogen content of SUP13Cr steel ingots, the tendency for δ-ferrite formation is reduced while ensuring corrosion resistance. At the same time, a forging method with small ingot size and large deformation is adopted. This method reduces the microsegregation of elements such as Cr and Mo in the steel ingot while increasing the forging deformation, fully breaking down the original cast dendritic structure, and effectively reducing and refining high-temperature ferrite.

[0007] The technical solution of the present invention: A production process for SUP13Cr stainless steel bars includes the following steps: electric furnace, AOD, LF, VD, stacking cooling, grinding, forging and annealing; the forging process includes a first upsetting and drawing, followed by a furnace reheating at 1140℃±10℃ for 2-4 hours, a second drawing and rounding after exiting the furnace, and an annealing heat treatment at 650±10℃ for 30 hours after forging.

[0008] Preferably, in the electric furnace process: the composition of the electric furnace charge is controlled, the total melting temperature is >1550℃, full elemental analysis is performed by sampling, the steel content is controlled to be ≥1.5%, and the steel tapping temperature is >1650℃.

[0009] Preferred AOD process: furnace temperature ≥800℃ before steelmaking; after molten steel is added, oxide slag is formed for dephosphorization; all oxide slag is removed; ferrochrome alloy is added; oxygen is blown to raise the temperature and process the material; during decarburization, the total gas flow rate is controlled at 1100-1900 Nm³. 3 Between / h, after heating to 1700℃, oxygen and argon gradually transition, and alloying elements are added to adjust each element to the lower limit of the target composition. When the mass content C≤0.03%, the temperature is controlled at 1670-1720℃. When C≤0.015%, aluminum ingot + ferrosilicon reduction takes ≥7 minutes, slag removal ≥90%, reduction slag is added, and secondary reduction takes >5 minutes.

[0010] Preferably, in the AOD process: after the molten steel is added, the oxidation slag is formed to remove the P mass content until P ≤ 0.005%, and the oxygen-argon volume ratio is gradually transitioned from 5:1 to 3:1 to 1:1 to 1:3; The reducing slag consists of quicklime, fluorite, and aluminum granules, with the following addition amounts: quicklime 300-400 kg / t, fluorite 100-250 kg / t, and aluminum granules 2.0-2.5 kg / t.

[0011] Preferred LF process: After LF is in place, high-flow-rate argon gas is used to break the slag shell, aluminum wire is fed according to the target mass content of 0.08%, power is supplied to raise the temperature, lime and fluorite are added to adjust the slag alkalinity and fluidity, the composition is finely adjusted according to the analysis results, aluminum powder or CaSi powder is used for diffusion deoxidation, while maintaining a reducing atmosphere in the ladle, and after the slag has fully turned white or green and the temperature is ≥1560℃, samples are taken, the composition is precisely adjusted, and after the composition control meets the requirements, the white slag is maintained for ≥20 minutes, and the ladle temperature is ≥1660℃.

[0012] Preferably, in the LF process, the amount of lime added is 5-10 kg / t, the amount of fluorite added is 1-2 kg / t, and the ratio of lime to fluorite is 4:1; the slag basicity and fluidity are adjusted, and the final slag basicity is controlled at R≥3.0.

[0013] Preferred VD process: Before entering the tank, remove slag; after setting the ladle, adjust argon to prevent slag overflow; maintain vacuum degree ≤67Pa; maintain for ≥15 minutes; after breaking the vacuum, take a sample; after the composition control meets the requirements, soft blowing argon for ≥20 minutes; ladle reference temperature 1555-1565℃.

[0014] Preferably, the composition of the electric furnace charge, LF process, and VD process is controlled within the following mass content range: C≤0.02%, Mn: 0.3-0.4%, Si: 0.2-0.4%, S≤0.001%, P≤0.018%, Ni: 5.4-5.6%, Cr: 11.65-11.75%, Mo: 1.55-1.60%, V≤0.15%, Cu≤0.15%, Ti: 0.02-0.03%, N: 450-550ppm, H≤2ppm, O≤40ppm.

[0015] Preferably, the forging process is as follows: according to the process curve, the furnace temperature is ≤600℃ for waiting for materials. After the steel ingot is loaded into the furnace, it is left to sit for ≥2 hours. Then, the temperature is increased to 800℃±10℃ at a rate of ≤100℃ / h and held for 2-3 hours. After the intermediate section is held, the temperature is increased to 1140℃±10℃ at a rate of ≤100℃ / h and held for 4-5 hours. After heating is completed, the ingot is taken out of the furnace for forging.

[0016] Preferably, the production process uses 26-inch molten ingots to be freely forged into bars with a diameter of φ300mm.

[0017] The beneficial effects of this invention are: The composition of this invention is controlled to meet the standard requirements for elements such as Ni, Cr, and Mo, while appropriately increasing the content of austenite-forming elements (N) to reduce the tendency for δ-ferrite formation while ensuring corrosion resistance. Regarding ingot selection, the bars produced in this experiment are Φ300mm in diameter. This invention uses 26-inch smelting ingots. Compared to 30-inch smelting ingots used for bars of the same size, smaller ingots solidify faster during smelting, which can reduce the micro-segregation of elements such as Cr and Mo to a certain extent, avoiding the induction of δ-ferrite due to localized excessive composition. Furthermore, because the grains of smaller ingots are finer, even if a small amount of ferrite is formed, it is easier to eliminate in the next process. Therefore, the selection of smaller ingots can suppress the formation of high-temperature ferrite to the greatest extent possible from the source. For materials like SUP13Cr, during forging, the amount of deformation (especially cumulative and sufficiently large deformation) is one of the most effective process methods to reduce and refine high-temperature ferrite. In the forging process of this invention, the steel ingot is held at 1140±10℃ for 4-5 hours before being forged. Unlike the one-fire forming process used for bars of the same specifications, the forging process of this invention adopts a two-fire process of one-fire upsetting and two-fire forming, which effectively reduces and refines the high-temperature ferrite. Attached Figure Description

[0018] Figure 1 Metallographic structure at half the radius of the head of a SUP13Cr bar prepared in Example 1 of this invention; Figure 2 Metallographic structure diagram of the tail half radius of the SUP13Cr bar prepared in Example 1 of the present invention; Figure 3 The metallographic structure of the SUP13Cr bar at half the radius of the head is shown in Comparative Example 1 of this invention. Figure 4 The metallographic structure of the tail half radius of the SUP13Cr bar prepared for Comparative Example 1 of this invention is shown in the figure. Detailed Implementation

[0019] A production process for SUP13Cr stainless steel bars, which uses 26-inch molten ingots to forge bars with a diameter of φ300mm, includes the following steps: electric furnace, AOD, LF, VD, stack cooling, grinding, forging and annealing. Electric furnace process: The total melting temperature of the electric furnace charge is >1550℃. The composition is initially adjusted to prepare for subsequent refining. At the same time, samples are taken for full element analysis to control the steel content C ≥1.5% and the tapping temperature >1650℃.

[0020] AOD process: Before steelmaking, the furnace temperature is ≥800℃. After the molten steel is poured in, oxide slag is formed for decarburization. All oxide slag is removed, ferrochrome alloy is added, oxygen is blown to raise the temperature and process the material. During decarburization, the total gas flow rate is controlled at 1100-1900 Nm³.3 Between / h, after heating to 1700℃, oxygen and argon gradually transition, and alloying elements are added to adjust each element to the lower limit of the target composition. When the mass content C≤0.03%, the temperature is controlled at 1670-1720℃. When C≤0.015%, aluminum ingot + ferrosilicon reduction takes ≥7 minutes, slag removal ≥90%, reduction slag is added, and secondary reduction takes >5 minutes.

[0021] In the AOD process: after the molten steel is added, the oxidation slag is made to remove the phosphorus content until the phosphorus content is ≤0.005%, and the oxygen-argon ratio is gradually transitioned from 5:1 to 3:1 to 1:1 to 1:3; the reducing slag includes quicklime, fluorite and aluminum granules, and the addition amounts of the three are quicklime 300-400 kg / t, fluorite 100-250 kg / t, and aluminum granules 2.0-2.5 kg / t.

[0022] LF process: After the LF process is completed, high-flow-rate argon gas is used to break the slag shell, aluminum wire is fed according to the target mass content of 0.08%, power is supplied to raise the temperature, and lime and fluorite are added to adjust the slag basicity and fluidity. In the LF process, the amount of lime added is 5-10 kg / t, and the amount of fluorite added is 1-2 kg / t, with a lime-fluorite ratio of 4:1. The overall slag basicity and fluidity are adjusted, and the final slag basicity is controlled at R≥3.0. The composition is fine-tuned according to the analysis results, and aluminum powder or CaSi powder is used for diffusion deoxidation while maintaining a reducing atmosphere inside the ladle. After the slag has fully turned white or green and the temperature is ≥1560℃, samples are taken, and the composition is precisely adjusted according to the internal control target. The white slag is maintained for ≥20 minutes, and the ladle temperature is ≥1660℃.

[0023] In the LF process, the amount of lime added is 5-10 kg / t, and the amount of fluorite added is 1-2 kg / t, with a lime-to-fluorite ratio of 4:1. Adjust the slag basicity and fluidity, and control the final slag basicity to R≥3.0.

[0024] The chemical composition control requirements are shown in Table 1 (%): Table 1

[0025] VD process: Before entering the tank, remove slag; after setting the ladle, adjust the argon flow to prevent slag overflow; maintain a vacuum of ≤67Pa for ≥15 minutes; after breaking the vacuum, take a sample; after the composition control meets the internal control requirements, soft blow argon for ≥20 minutes; the ladle reference temperature is 1555-1565℃.

[0026] Forging process: According to the process curve, the furnace temperature is ≤600℃ for waiting for materials. After the steel ingot is loaded into the furnace, it is left to sit for ≥2 hours. Then, the temperature is raised to 800℃±10℃ at a rate of ≤100℃ / h and held for 2-3 hours. After the intermediate holding is completed, the temperature is raised to 1140℃±10℃ at a rate of ≤100℃ / h and held for 4-5 hours. After heating is completed, it is taken out of the furnace for forging. The forging process includes one upsetting and drawing. After forging, it is returned to the furnace and held at 1140℃±10℃ for 2-4 hours. After taking it out of the furnace, it is drawn and rounded in a second upsetting. After forging, it is annealed at 650±10℃ for 30 hours.

[0027] The following examples illustrate the specific process parameters of Examples 1-3 and the comparative examples.

[0028] Example 1

[0029] This invention provides a manufacturing process for SUP13Cr stainless steel bars, the steps of which are as follows: 1. Main smelting: Electric furnace process: The total melting temperature of the electric furnace charge is 1555℃. All elements are sampled and analyzed. The carbon content of the tapped steel is controlled at 1.5%, and the tapping temperature is 1655℃.

[0030] AOD process: The furnace temperature before steelmaking is 800℃. After the molten steel is added, oxide slag is formed to remove phosphorus (P) to 0.005%. All oxide slag is removed, ferrochrome alloy is added, oxygen is blown to raise the temperature and carburize the material. During decarburization, the total gas flow rate is controlled at 1500 Nm³. 3 / h, based on the dynamic segmented control of C content in the molten steel, the flow rate is high in the initial stage and gradually decreases in the later stage. After heating to 1700℃, the oxygen-argon volume ratio is gradually transitioned according to 5:1→3:1→1:1→1:3. Alloying elements are added to adjust each element to the lower limit of the target composition. When C is 0.03%, the temperature is controlled at 1700℃. When C is 0.015%, aluminum ingot + ferrosilicon is reduced for 7 minutes, 90% of the slag is removed, and reducing slag (lime, fluorite, aluminum granules) is added. The amount added is 350kg of lime, 150kg of fluorite, and 2.3kg / t of aluminum granules for secondary reduction for 6 minutes.

[0031] LF process: After the LF is in place, high-flow-rate argon gas is used to break the slag shell, aluminum wire is fed according to the target of 0.08%, power is supplied to raise the temperature, and appropriate amounts of lime and fluorite are added to adjust the slag basicity and fluidity. The amount of lime added is 8 kg / T, and the amount of fluorite added is 2 kg / T, with a lime-fluorite ratio of 4:1. The final slag basicity is controlled at R=3.0. The composition is finely adjusted according to the analysis results, and aluminum powder or CaSi powder is used for diffusion deoxidation while maintaining a reducing atmosphere inside the ladle. After the slag has fully turned white or green and the temperature reaches 1560℃, samples are taken, and the composition is precisely adjusted according to the internal control target. The white slag is maintained for 20 minutes, and the ladle temperature is 1660℃.

[0032] VD process: Before entering the tank, remove slag; after setting the ladle, adjust argon to prevent slag overflow; maintain a vacuum of 65 Pa for 15 minutes; after breaking the vacuum, take a sample; if the composition meets the internal control requirements, gently blow argon for 25 minutes; the ladle reference temperature is 1560℃; finally, pour 26-inch molten steel ingots.

[0033] 2. Steel ingot preparation: According to the process curve, the furnace is heated to 600℃ for material preparation. After the steel ingot is loaded into the furnace, it is left to stand for 2 hours. Then, the temperature is increased to 800℃ at a rate of 100℃ / h and held for 2.5 hours. After the intermediate holding is completed, the temperature is increased to 1140℃ at a rate of 100℃ / h and held for 4.5 hours. After heating is completed, the ingot is taken out of the furnace for forging.

[0034] 3. Main body forging: The main body forging process involves two heat treatments. The first heat treatment involves upsetting and drawing, while the second heat treatment involves only drawing and rounding. The single hammer reduction for each heat treatment is 80-150mm, and the single hammer feed is 200-250mm.

[0035] First fire: Upsetting: Control the upsetting speed to 7mm / s, and the diameter after upsetting is Φ985mm; Lengthening: Lengthen to a 500mm square shape, lengthening time 7.5min; After forging, the metal is reheated to 1140℃ and held for 3 hours.

[0036] Second fire: Stretch and round: Stretch and round to a length of 310mm, stretch for 10 minutes.

[0037] 3. Gloss finishing: The Φ310mm bar is machined to remove surface oxide scale and minor defects, resulting in a Φ300mm finished bar.

[0038] High-temperature ferrite testing: Ferrite content was tested at half the transverse radius of bars 1-1 and 1-2. Figure 1 and Figure 2 As can be seen, they are levels 0.9 and 0.2 respectively.

[0039] Example 2

[0040] This invention provides a manufacturing process for SUP13Cr stainless steel bars, the steps of which are as follows: 1. Main smelting: Electric furnace process: The total melting temperature of the electric furnace charge is 1560℃. All elements are sampled and analyzed. The carbon content of the tapped steel is controlled at 1.5%, and the tapping temperature is 1660℃.

[0041] AOD process: Before steelmaking, the furnace temperature is 800℃. After the molten steel is added, oxide slag is formed to reduce phosphorus content to 0.004%. All oxide slag is removed, ferrochrome alloy is added, and oxygen is blown to raise the temperature and process the material. During decarburization, the total gas flow rate is controlled at 1100 Nm³. 3 / h, based on the dynamic segmented control of C content in the molten steel, with high flow rate initially and decreasing later. After heating to 1700℃, the oxygen-argon ratio is gradually transitioned at 5:1→3:1→1:1→1:3. Alloying elements are added to adjust each element to the lower limit of the target composition. When C is 0.03%, the temperature is controlled at 1700℃. When C is 0.015%, aluminum ingot + ferrosilicon is reduced for 7 minutes, 90% of the slag is removed, and reducing slag (lime, fluorite, aluminum granules) is added at a rate of 350kg lime, 150kg fluorite, and 2.3kg / t aluminum granules. Secondary reduction is carried out for 7 minutes.

[0042] LF process: After the LF is in place, high-flow-rate argon gas is used to break the slag shell, aluminum wire is fed according to the target of 0.08%, power is supplied to raise the temperature, and appropriate amounts of lime and fluorite are added to adjust the slag basicity and fluidity. The amount of lime added is 8 kg / ton, and the amount of fluorite added is 2 kg / ton, with a lime-fluorite ratio of 4:1. The final slag basicity is controlled at R=3.0. The composition is finely adjusted according to the analysis results, and aluminum powder or CaSi powder is used for diffusion deoxidation while maintaining a reducing atmosphere inside the ladle. After the slag has fully turned white or green and the temperature reaches 1560℃, samples are taken, and the composition is precisely adjusted according to the internal control target. The white slag is maintained for 20 minutes, and the ladle temperature is 1660℃.

[0043] VD process: Before entering the tank, remove slag; after setting the argon pack, adjust the argon pressure to prevent slag overflow; maintain a vacuum of 66 Pa for 16 minutes; after breaking the vacuum, take a sample; if the composition meets the internal control requirements, gently blow argon for 26 minutes; the reference temperature for the argon pack is 1560℃.

[0044] Finally, 26-inch molten steel ingots were poured.

[0045] Steel ingot preparation: According to the process curve, the furnace is heated to 600℃ for material waiting. After the steel ingot is loaded into the furnace, it is left to sit for 2 hours. Then, the temperature is increased to 790℃ at a rate of 100℃ / h and held for 2 hours. After the intermediate holding is completed, the temperature is increased to 1130℃ at a rate of 100℃ / h and held for 4 hours. After heating is completed, the ingot is taken out of the furnace for forging.

[0046] 3. Main body forging: The main body forging process involves two heat treatments. The first heat treatment involves upsetting and drawing, while the second heat treatment involves only drawing and rounding. The single hammer reduction for each heat treatment is 80-150mm, and the single hammer feed is 200-250mm.

[0047] First fire: Upsetting: Control the upsetting speed to 7mm / s, and the diameter after upsetting is Φ985mm; Lengthening: Lengthen to a 500mm square shape, lengthen for 7 minutes; After forging, the metal is reheated to 1140℃ and held for 3 hours.

[0048] Second fire: Stretch and round: Stretch and round to a length of 310mm, stretching time is 9.5min.

[0049] 3. Gloss finishing: The Φ310mm bar is machined to remove surface oxide scale and minor defects, resulting in a Φ300mm finished bar.

[0050] High-temperature ferrite testing: Ferrite levels of 0.5 and 1.2 were found at half the transverse radius of bars 1-1 and 1-2, respectively.

[0051] Example 3

[0052] This invention provides a manufacturing process for SUP13Cr stainless steel bars, the steps of which are as follows: 1. Main smelting: Electric furnace process: The total melting temperature of the electric furnace charge is 1565℃. All elements are sampled and analyzed. The carbon content of the tapped steel is controlled to be ≥1.5%, and the tapping temperature is 1665℃.

[0053] AOD process: Before steelmaking, the furnace temperature is 800℃. After the molten steel is added, oxide slag is formed to remove phosphorus (P) to 0.005%. All oxide slag is removed, ferrochrome alloy is added, and oxygen is blown to raise the temperature and process the material. During decarburization, the total gas flow rate is controlled at 1900 Nm³. 3 / h, based on the dynamic segmented control of C content in molten steel, with high flow rate in the initial stage and decreasing flow rate in the later stage.

[0054] After heating to 1700℃, the oxygen-argon ratio was gradually transitioned from 5:1 to 3:1 to 1:1 to 1:3. Alloying elements were added to adjust each element to the lower limit of the target composition. When C was 0.03%, the temperature was controlled at 1700℃. When C was 0.015%, aluminum ingots were reduced with ferrosilicon for 7 minutes. 90% of the slag was removed, and reducing slag (lime, fluorite, and aluminum granules) was added. The amount added was 350 kg of lime, 150 kg of fluorite, and 2.3 kg / t of aluminum granules. The secondary reduction lasted for 8 minutes.

[0055] LF process: After the LF is in place, high-flow-rate argon gas is used to break the slag shell, aluminum wire is fed according to the target of 0.08%, power is supplied to raise the temperature, and appropriate amounts of lime and fluorite are added to adjust the slag basicity and fluidity. The amount of lime added is 8 kg / T, and the amount of fluorite added is 2 kg / T, with a lime-fluorite ratio of 4:1. The final slag basicity is controlled at R=3.0. The composition is finely adjusted according to the analysis results, and aluminum powder or CaSi powder is used for diffusion deoxidation while maintaining a reducing atmosphere inside the ladle. After the slag has fully turned white or green and the temperature reaches 1560℃, samples are taken, and the composition is precisely adjusted according to the internal control target. The white slag is maintained for 20 minutes, and the ladle temperature is 1660℃.

[0056] VD process: Before entering the tank, remove slag; after setting the argon pack, adjust the argon pressure to prevent slag overflow; maintain a vacuum of 67 Pa for 17 minutes; after breaking the vacuum, take a sample; if the composition meets the internal control requirements, gently blow argon for 25 minutes; the reference temperature for the argon pack is 1560℃.

[0057] Finally, 26-inch molten steel ingots were poured.

[0058] 2. Steel ingot preparation: According to the process curve, the furnace is heated to 600℃ for material preparation. After the steel ingot is loaded into the furnace, it is left to stand for 2 hours. Then, the temperature is increased to 810℃ at a rate of 100℃ / h and held for 3 hours. After the intermediate holding is completed, the temperature is increased to 1150℃ at a rate of 100℃ / h and held for 5 hours. After heating is completed, the ingot is taken out of the furnace for forging.

[0059] 3. Main body forging: The main body forging process involves two heat treatments. The first heat treatment involves upsetting and drawing, while the second heat treatment involves only drawing and rounding. The single hammer reduction for each heat treatment is 80-150mm, and the single hammer feed is 200-250mm.

[0060] First fire: Upsetting: Control the upsetting speed to 7mm / s, and the diameter after upsetting is Φ985mm; Lengthening: Lengthen to a 500mm square shape, lengthening time 6.5min; After forging, the metal is reheated to 1140℃ and held for 3 hours.

[0061] Second fire: Stretch and round: Stretch and round to a length of 310mm, stretch for 9 minutes.

[0062] 3. Gloss finishing: The Φ310mm bar is machined to remove surface oxide scale and minor defects, resulting in a Φ300mm finished bar.

[0063] High-temperature ferrite testing: Ferrite levels of 0.1 and 0.3 were found at half the transverse radius of bars 1-1 and 1-2, respectively.

[0064] Comparative Example 1 This invention provides a comparative example of a production process for SUP13Cr stainless steel bars, which differs from Example 1 as follows: Smelting process: The nitrogen content in the steel is 150-250 ppm (the nitrogen content in the steel in Example 1 is 450-550 ppm), and the final cast steel ingot size is 30 inches (Example 1 cast 26-inch steel ingot). Forging process: The material is formed by one-fire forging and rounding, directly drawing and rounding it to a Φ310mm round bar, which is different from the two-fire forging process of one-fire forging and one-fire forging and rounding in Example 1.

[0065] The remaining process parameters of this comparative example are exactly the same as those of Example 1, and will not be repeated here.

[0066] The bars prepared in Comparative Example 1 were tested. Ferrite was examined at half the transverse radius of bars 1-1 and 1-2. Figure 3 and Figure 4 As can be seen, they are levels 4.9 and 4.4 respectively.

[0067] The specific chemical composition control requirements for the examples and comparative examples are shown in Table 2 (%): Table 2

[0068] This process uses a 26-inch ingot, first forging to reduce the ingot body by half, then drawing it to 500 mm, followed by a second forging and rounding process to form the finished product, with a total forging ratio of 11.6. The comparative process uses a 30-inch ingot, first forging and rounding it, with a total forging ratio of 7.36. The high-temperature ferrite results are shown in Table 3 below. Table 3

[0069] By comparing Examples 1-3 and Comparative Example 1, it can be concluded that the adjustments to the forming elements, ingot shape, and forging process in Examples 1-3 have a significant effect on improving the high-temperature ferrite of the bar stock.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A manufacturing process for SUP13Cr stainless steel bars, characterized in that, The process includes the following steps: electric furnace, AOD, LF, VD, stacking cooling, grinding, forging and annealing; the forging process includes one upsetting and drawing, after forging, it is returned to the furnace and held at 1140℃±10℃ for 2-4 hours, after exiting the furnace, it is drawn and rounded in a second upsetting, and after forging, it is annealed at 650±10℃ for 30 hours.

2. The production process of SUP13Cr stainless steel bars according to claim 1, characterized in that, Electric furnace process: control the composition of the electric furnace charge, with a full melting temperature >1550℃, take samples for full element analysis, control the steel quality content C ≥1.5%, and the steel tapping temperature >1650℃.

3. The production process of SUP13Cr stainless steel bars according to claim 1, characterized in that, AOD process: Before steelmaking, the furnace temperature is ≥800℃. After the molten steel is poured in, oxide slag is formed for decarburization. All oxide slag is removed, ferrochrome alloy is added, oxygen is blown to raise the temperature and process the material. During decarburization, the total gas flow rate is controlled at 1100-1900 Nm³. 3 Between / h, after heating to 1700℃, oxygen and argon gradually transition, and alloying elements are added to adjust each element to the lower limit of the target composition. When the mass content C≤0.03%, the temperature is controlled at 1670-1720℃. When C≤0.015%, aluminum ingot + ferrosilicon reduction takes ≥7 minutes, slag removal ≥90%, reduction slag is added, and secondary reduction takes >5 minutes.

4. The production process of SUP13Cr stainless steel bars according to claim 3, characterized in that, In the AOD process: after the molten steel is added, the oxidation slag is made to remove the P content until P ≤ 0.005%, and the oxygen-argon volume ratio is gradually transitioned from 5:1 to 3:1 to 1:1 to 1:

3. The reducing slag consists of quicklime, fluorite, and aluminum granules, with the following addition amounts: quicklime 300-400 kg / t, fluorite 100-250 kg / t, and aluminum granules 2.0-2.5 kg / t.

5. The production process of SUP13Cr stainless steel bars according to claim 2, characterized in that, LF process: After the LF is in place, high-flow-rate argon gas is used to break the slag shell, aluminum wire is fed according to the target mass content of 0.08%, power is supplied to raise the temperature, lime and fluorite are added to adjust the slag alkalinity and fluidity, the composition is finely adjusted according to the analysis results, aluminum powder or CaSi powder is used for diffusion deoxidation, while maintaining a reducing atmosphere in the ladle, and after the slag has fully turned white or green and the temperature is ≥1560℃, samples are taken, the composition is precisely adjusted, and after the composition control meets the requirements, the white slag is maintained for ≥20 minutes, and the ladle temperature is ≥1660℃.

6. The production process of SUP13Cr stainless steel bars according to claim 5, characterized in that, In the LF process, the amount of lime added is 5-10 kg / t, the amount of fluorite added is 1-2 kg / t, and the ratio of lime to fluorite is 4:1; adjust the slag basicity and fluidity, and control the final slag basicity according to R≥3.

0.

7. The production process for SUP13Cr stainless steel bars according to claim 5, characterized in that VD Procedure: Before entering the tank, remove slag; after setting the ladle, adjust the argon flow to prevent slag overflow; maintain a vacuum of ≤67Pa for ≥15 minutes; after breaking the vacuum, take a sample; after the composition control meets the requirements, perform soft argon blowing for ≥20 minutes; the ladle reference temperature is 1555-1565℃.

8. The production process of SUP13Cr stainless steel bars according to claim 7, characterized in that, The composition of the electric furnace charge, LF process, and VD process shall be controlled within the following mass content range: C≤0.02%, Mn: 0.3-0.4%, Si: 0.2-0.4%, S≤0.001%, P≤0.018%, Ni: 5.4-5.6%, Cr: 11.65-11.75%, Mo: 1.55-1.60%, V≤0.15%, Cu≤0.15%, Ti: 0.02-0.03%, N: 450-550ppm, H≤2ppm, O≤40ppm.

9. The production process of SUP13Cr stainless steel bars according to claim 1, characterized in that, Forging process: According to the process curve, the furnace temperature is ≤600℃ for waiting for materials. After the steel ingot is loaded into the furnace, it is left to sit for ≥2 hours. Then, the temperature is raised to 800℃±10℃ at a rate of ≤100℃ / h and held for 2-3 hours. After the intermediate section is held, the temperature is raised to 1140℃±10℃ at a rate of ≤100℃ / h and held for 4-5 hours. After heating is completed, the ingot is taken out of the furnace for forging.

10. A production process for SUP13Cr stainless steel bars according to any one of claims 1-9, characterized in that, The production process uses 26-inch molten ingots to be freely forged into bars with a diameter of φ300mm.