A rare earth doped optical fiber preform and a method for making the same

CN122748906APending Publication Date: 2026-09-15INNER MONGOLIA RARE PROD TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610891839.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-18
Publication Date
2026-09-15

Smart Images

  • Figure CN122748906A_ABST
    Figure CN122748906A_ABST
Patent Text Reader

Abstract

The application discloses a rare earth doped optical fiber preform and a preparation method thereof, and relates to the technical field of optical fiber preforms, which comprises the following steps: depositing a loose core layer on the inner wall of a quartz deposition tube by using an MCVD process, wherein the loose core layer has open pores; and contacting a doping liquid with the loose core layer at a first temperature, so that the doping liquid enters the open pores of the loose core layer, wherein the doping liquid contains rare earth ions, aluminum ions and a precipitant capable of releasing ammonia upon heating, the precipitant is urea, hexamethylenetetramine or a combination of the two, and the rare earth ions include one or both of ytterbium ions and erbium ions. The method can realize selective separation between the free liquid in the tube cavity and the effective doping liquid in the hole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optical fiber preform technology, and in particular to a rare earth-doped optical fiber preform and its preparation method. Background Technology

[0002] Rare-earth-doped silica fibers are widely used in fiber lasers, fiber amplifiers, fiber sensors, and special fiber devices. Rare-earth ions typically include Yb, Er, Tm, Ho, and Nd, while common co-doped elements include Al, P, Ge, F, and Ce. For rare-earth-doped fibers, the distribution of rare-earth elements in the core layer directly affects the fiber's pump absorption, background loss, amplification efficiency, laser efficiency, and long-term stability.

[0003] MCVD (Medium-Voltage Carbon Dioxide) combined with solution doping is a common method for preparing rare-earth-doped optical fiber preforms. This method typically involves depositing a loose core layer on the inner wall of a quartz deposition tube, wetting or immersing the loose core layer with a dopant solution containing rare-earth ions, and then drying, dehydrating, sintering, and shrinking to obtain the rare-earth-doped optical fiber preform. Existing publicly available methods include techniques for saving rare-earth solution and improving longitudinal uniformity through horizontal rotational immersion, and techniques for increasing rare-earth retention through in-situ precipitation within the tube. For example, CN102515501B discloses an MCVD doping method involving horizontally placed, rotating immersion in a deposition tube, the abstract of which states that this method can save rare-earth solution and improve longitudinal uniformity; CN115448590A discloses a method for forming a mixed solution of organosilicon and rare-earth salts and heating the solution within a quartz deposition tube to precipitate sparingly soluble organosilicon-rare-earth derivatives inside the loose core layer.

[0004] However, existing solution doping or in-situ precipitation doping methods still have an easily overlooked problem: before the precipitation reaction is triggered, it is difficult to effectively distinguish between the free-flowing dopant in the deposition tube cavity, the flowable liquid film on the inner wall of the cavity, and the liquid-rich region near the pores of the loose core layer. When precipitation is triggered, if there is still a large amount of free liquid in the cavity or near the pores, rare earth precipitation is likely to form first in the free liquid in the cavity or at the pores of the loose core layer, leading to free precipitation, pore blockage, or surface deposited shells. This phenomenon results in insufficient fixation of rare earth elements in the deep pores of the loose core layer, causing the radial distribution of rare earth elements in the core layer to deviate from the design value.

[0005] On the other hand, if a large purging pressure or a long purging time is used to avoid free liquid precipitation in the tube cavity, the effective dopant in the loose core layer pores may also be carried out, resulting in a decrease in rare earth fixation. In other words, the existing process has the following contradiction: insufficient drainage easily leads to free liquid precipitation and pore blockage, while excessive drainage will result in the loss of effective dopant in the pores.

[0006] The basic principle of capillary flow porosity measurement indicates that in porous materials saturated with wetting fluid, the liquid inside the pores will be expelled under gradually increasing gas pressure. Larger pores typically drain first at lower pressures, while smaller pores require higher pressures to drain. This principle is commonly used for pore size characterization in materials such as membranes and filter media. However, in the field of rare-earth-doped optical fiber preform fabrication, no scheme has yet been found to apply this capillary critical pressure difference principle to selectively control liquid drainage before precipitation triggering, thereby retaining capillary-retained dopant within the loose core pores while draining free liquid from the cavity, and ensuring that subsequent precipitation primarily occurs within the pores. Summary of the Invention

[0007] In view of the above problems, the present invention proposes the following technical solution.

[0008] Therefore, the present invention aims to provide a rare earth-doped optical fiber preform and its preparation method to solve the problems of insufficient rare earth fixation in the deep pores of the loose core layer and the deviation of the radial rare earth distribution in the core layer from the design value.

[0009] To solve the above-mentioned technical problems, the present invention provides the following technical solution: In a first aspect, the present invention provides a method for preparing a rare-earth-doped optical fiber preform, comprising: depositing a loose core layer on the inner wall of a quartz deposition tube using an MCVD process, the loose core layer having open pores; contacting a dopant solution with the loose core layer at a first temperature, allowing the dopant solution to enter the open pores of the loose core layer, wherein the dopant solution contains rare-earth ions, aluminum ions, and a precipitant that releases ammonia upon heating, the precipitant being urea, hexamethylenetetramine, or a combination thereof, and the rare-earth ions including one or two of ytterbium ions and erbium ions; before heating the quartz deposition tube to a second temperature, applying a gas venting pressure difference ΔP to both ends of the quartz deposition tube to vent any gas not contained in the open pores within the quartz deposition tube. The doping solution is held in place, and the quartz deposition tube is free of a continuous liquid column. The gas discharge pressure difference ΔP is less than the 5% liquid retention reduction critical pressure difference ΔP5. ΔP5 is the gas pressure difference corresponding to a 5% reduction in liquid retention relative to the saturated liquid retention of a loose core layer sample formed under the same doping solution and the same first temperature, saturated with the doping solution in the same batch or under the same deposition conditions. The quartz deposition tube is heated to a second temperature and held, causing the precipitant to release ammonia, thereby precipitating rare earth ions in the open pores within the loose core layer. The precipitated loose core layer is then subjected to drying, oxidative decomposition, dehydration, sintering for transparency, and melting shrinkage to obtain a rare earth-doped optical fiber preform.

[0010] In a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, the 5% liquid retention reduction critical pressure difference ΔP5 is determined by the following method: Take a quartz deposition tube sample section that has the same deposition conditions as the loose core layer in the quartz deposition tube; At the first temperature, the same doping solution is introduced into the loose core layer of the sample segment, and the loose core layer is brought to liquid saturation. After draining the free liquid from the cavity of the sample section, weigh the sample section and calculate the saturated liquid retention capacity; A gas pressure difference is applied step by step along the axial direction of the sample section, and maintained at each gas pressure difference for 60–200 s; After each stage of gas pressure difference, the sample section is weighed and the remaining liquid retention is calculated. The pressure difference ΔP5 is defined as the gas pressure difference when the remaining liquid volume decreases by 5% relative to the saturated liquid volume.

[0011] In a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, the gas discharge pressure difference ΔP is 0.40 to 0.65 times the critical pressure difference ΔP5 for reducing the liquid retention by 5%.

[0012] In a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, after applying the gas displacement pressure difference ΔP, the liquid retention in the open pores of the loose core layer decreases by no more than 10% compared to the liquid retention before applying the gas displacement pressure difference ΔP.

[0013] In a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, the first temperature is 15-35°C, the second temperature is 70-95°C, and the second temperature is maintained for 10-180 minutes.

[0014] In a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, the total concentration of rare-earth ions in the doping solution is 0.001–0.50 mol / L, the molar ratio of aluminum ions to rare-earth ions is 2–30, the concentration of urea and / or hexamethylenetetramine is 0.05–3.50 mol / L, and the molar ratio of urea and / or hexamethylenetetramine to rare-earth ions is 5–80.

[0015] In a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, the doping solution is an aqueous solution, the rare-earth ions are provided by one or more of the corresponding chlorides, nitrates, and acetates, and the aluminum ions are provided by one or more of aluminum chloride, aluminum nitrate, and aluminum acetate.

[0016] As a preferred embodiment of the method for preparing a rare-earth-doped optical fiber preform according to the present invention, the drying, oxidative decomposition, dehydration, sintering and transparentization, and melting and shrinking include: The loose core layer after precipitation was dried at 60–150℃; Oxidative decomposition treatment was carried out at 250–550°C in an oxygen-containing atmosphere. Dehydration treatment is carried out at 800–1200℃ in a dehydration atmosphere containing chlorine gas; Sintering and transparency treatment is carried out at 1450–1700℃; The quartz deposition tube is melted and shrunk to obtain a rare earth-doped optical fiber preform.

[0017] In a second aspect, the present invention provides a rare earth-doped optical fiber preform, comprising a quartz cladding and a rare earth-doped glass core layer located within the quartz cladding. In the rare earth-doped glass core layer, the content of rare earth elements, calculated as oxides, is 0.01 mol% to 2.00 mol%, and the content of Al2O3 is 0.2 mol% to 15 mol%. Among them, on the cross-section of the rare earth-doped glass core layer, the region with radius R and radius r≤0.20R is the central region, and the annular region with 0.40R≤r≤0.80R is the middle region; The ratio of the average rare earth element concentration in the central region to the average rare earth element concentration in the intermediate region is 0.80–1.20. In a preferred embodiment of the rare-earth-doped optical fiber preform of the present invention, the rare-earth element includes Yb or Er, and the molar ratio of aluminum to rare-earth element is 2 to 30. The beneficial effects of this invention are as follows: First, this invention applies a gas discharge pressure difference ΔP before precipitation triggering, and makes this gas discharge pressure difference ΔP less than 5% of the capillary retention dopant in the pores, thus reducing the critical pressure difference ΔP5. Therefore, the free-flowing dopant in the cavity can be discharged, while the capillary retention dopant in the open pores of the loose core layer can be retained, thereby achieving selective separation between the free liquid in the cavity and the effective dopant in the pores.

[0018] Second, this invention confines the precipitation triggering space within the pores of the loose core layer. Since there is essentially no continuous liquid column or a large amount of free-flowing dopant liquid in the cavity when precipitation is triggered by heating, rare earth precipitates are less likely to be generated in large quantities in the free liquid of the cavity, and are less likely to form a continuous deposition shell at the pore opening of the loose core layer, thereby reducing the risk of pore blockage.

[0019] Third, this invention does not reduce free liquid precipitation through excessive purging, but rather drains the liquid under conditions where the critical pressure difference ΔP5 is reduced to below 5% of the liquid retention. Therefore, while reducing free liquid precipitation in the lumen, it can prevent a large amount of effective dopant from being carried out of the porous core layer, thereby maintaining a high rare earth fixation level.

[0020] Fourth, the 5% liquid retention reduction critical pressure difference ΔP5 in this invention can be predetermined by the same batch of sample sections, sample sections with the same process conditions, or ineffective sections of the deposition tube, so that the selective liquid drainage process is transformed from empirical purging to a calibrable and repeatable pressure window control process, which is beneficial to improving the process consistency of different batches of rare earth doped optical fiber preforms.

[0021] Fifth, this invention is compatible with existing MCVD process lines. Except for the addition of low-temperature circulating permeation, selective drainage, and low-temperature precipitation triggering steps, the subsequent drying, oxidative decomposition, chlorine-containing dehydration, sintering and transparentization, and melting and shrinkage steps can still be completed using conventional MCVD preform post-processing equipment, thus demonstrating good industrial feasibility. Attached Figure Description

[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 A scatter plot of ΔP / ΔP5 versus the mass of free precipitate in the lumen and the rate of decrease in liquid retention; Figure 2 A scatter plot of ΔP / ΔP5 and the average content of Yb2O3; Figure 3 A scatter plot of ΔP / ΔP5 versus the radial concentration variation coefficient of Yb; Figure 4 This is a schematic diagram of the ΔP5 measurement curve and linear interpolation in Example 1; Figure 5 This is a schematic diagram of the ΔP5 values ​​for Examples 1 to 6; Figure 6 This is a schematic diagram comparing the mass of free precipitate in the lumen of Example 1 and Comparative Examples 1-3; Figure 7 This is a schematic diagram comparing the 1200nm background loss of Example 1 with Comparative Examples 1-3; Figure 8 This is a schematic diagram of the normalized Yb radial distribution of Example 1, Comparative Example 1, and Comparative Example 3; Figure 9 This is a schematic diagram of the normalized radial distribution of Al in Example 1, Comparative Example 1, and Comparative Example 3; Figure 10 This is a schematic diagram showing the rare earth concentration ratio of the central / intermediate region in Examples 1-6; Figure 11 This is a schematic diagram showing the variation of the absorption coefficient of the 976nm small signal core along the axial position of the preform in Example 1 and Comparative Example 3. Figure 12 A scatter plot of the sample showing the rate of decrease in liquid retention versus the amount of free precipitate in the lumen. Detailed Implementation

[0024] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0025] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0026] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0027] In this embodiment, the "loose core layer" refers to a silica-based loose layer with an open porous structure that is not fully vitrified and deposited on the inner wall of a quartz deposition tube using the MCVD process. This loose core layer may contain SiO2, and may further contain precursors or oxides of co-doped components such as Al, P, Ge, F, and Ce. The "free-flowing dopant" refers to a dopant located within the cavity of the quartz deposition tube that can form a continuous flow under gravity or low gas pressure, including continuous liquid columns, liquid pools, flowable liquid films, and larger movable droplets. The "capillary-retained dopant" refers to a dopant that, after being discharged from the free-flowing dopant, remains within the open pores of the loose core layer due to capillary action.

[0028] "5% reduction in liquid retention capacity reduces critical pressure difference ΔP5" refers to the gas pressure difference corresponding to a 5% reduction in liquid retention capacity relative to the saturated liquid retention capacity of a loose core layer sample from the same batch or under the same conditions as the actual liquid discharge, including the same dopant solution, first temperature, gas type, and pressure difference holding time.

[0029] When determining ΔP5, the following method can be used: Take a loose core sample with a length of 40-80 mm, prepared under the same batch or deposition conditions as the quartz deposition tube to be prepared; dry the sample at 100-120℃ for 1-2 hours, and weigh the dry weight m0 after cooling to the first temperature; immerse the sample in a doping solution identical to that used in the actual process until saturated, drain the free liquid from the tube cavity and remove any movable surface droplets, and weigh the saturated weight m1; then apply nitrogen pressure differentials in stages along the axial direction of the sample at the first temperature, maintaining each stage for 90 seconds, and weigh the sample weight m1.i According to η i =(m1-m i The liquid retention reduction rate is calculated as (m1 - m0) × 100%. When the η value corresponding to two adjacent pressure levels crosses by 5%, ΔP5 is obtained through linear interpolation.

[0030] In this invention, the gas discharge pressure difference ΔP is 0.40 to 0.65 times ΔP5, preferably 0.40 to 0.55 times. If ΔP is too small, the free-flowing dopant, flowable liquid film, or movable droplets in the cavity may not be discharged sufficiently; if ΔP is close to or exceeds ΔP5, the effective capillary retention of dopant in the loose core layer pores may be carried out, resulting in a reduction in the rare earth fixation amount.

[0031] The doping solution may include rare earth salts, aluminum salts, a thermally slow-release precipitant, and a solvent. The rare earth salt is a nitrate or chloride of Yb, or a combination of nitrates of Yb and Er. The aluminum salt is aluminum nitrate or aluminum chloride. The thermally slow-release precipitant may be urea, hexamethylenetetramine, or a combination thereof. The solvent may be water, a mixture of water and ethanol, or other solvents capable of dissolving the above components and compatible with the MCVD quartz deposition tube.

[0032] The thermally slow-release precipitant preferably does not release precipitate components sufficient to induce rare earth ion precipitation at a first temperature, but releases precipitate components at a second temperature. The first temperature can be 10–45°C, preferably 20–35°C; the second temperature can be 60–105°C, preferably 75–95°C.

[0033] In one embodiment, after the low-temperature cyclic permeation is completed, a gas discharge pressure difference ΔP is first established between the inlet and outlet ends of the deposition tube and maintained for 80–100 s to discharge the free-flowing dopant until no continuous liquid column, flowable liquid film, or movable droplets remain in the tube cavity. Subsequently, the temperature is raised to a second temperature in a closed atmosphere, a slightly positive pressure inert atmosphere, or an inert atmosphere containing water vapor to prevent the capillary-retained dopant in the pores from evaporating too quickly before the precipitation reaction is fully completed.

[0034] The loose core layer after precipitation and fixation can be subjected to low-temperature drying, oxidative decomposition, chlorine-containing dehydration, sintering and transparentization, and melting and shrinkage in sequence. The low-temperature drying temperature can be 60-150℃; the oxidative decomposition temperature can be 250-550℃; the dehydration temperature can be 800-1200℃, and the dehydration atmosphere can contain He, O2, and Cl2; the sintering and transparentization temperature can be 1450-1700℃; the melting and shrinkage temperature can be selected according to the size of the quartz deposition tube and equipment conditions, and is generally 1900-2300℃.

[0035] It should be noted that the mass of free precipitate in the lumen was determined using a uniform method: after precipitation and cooling, the lumen of the deposition tube was rinsed with 3 × 30 mL of deionized water, and the washings were combined and filtered through a pre-weighed 0.22 μm polyethersulfone filter membrane; the filter membrane was washed with 20 mL of deionized water and dried at 105 °C until the difference between two adjacent weighings was less than 0.2 mg. The mass of free precipitate in the lumen was obtained after deducting the weight gain of the blank filter membrane.

[0036] The average contents of Yb₂O₃, Er₂O₃, and Al₂O₃ in the glass core layer were calculated from the EPMA-WDS surface scanning results, and cross-checked using inductively coupled plasma atomic emission spectrometry (ICP-AES) on the micro-drilling sampling results of the preform core layer. Three axial sections were tested for each sample, with at least three regions per section, and the average values ​​were reported. The final Al / total rare earth molar ratio was calculated based on the final glass core layer composition and was not replaced by the dopant feed ratio.

[0037] All samples were drawn under consistent conditions, with a fiber core diameter of 12.0±0.2μm, a cladding diameter of 125±1μm, and a numerical aperture of 0.12±0.01. Background loss at 1200nm was measured using the 100m to 10m cutoff method with a fiber winding radius of 100mm. Small-signal core absorption at 976nm was measured using a narrow-linewidth 976nm light source and a power meter, employing the 40mm to 10mm cutoff method; samples were drawn at corresponding preform axial lengths of 50, 125, 200, 275, 350, 425, 500, and 550mm.

[0038] Example 1: A high-purity quartz deposition tube with an outer diameter of 25 mm, an inner diameter of 19 mm, and a length of 600 mm was selected. A SiO2 barrier layer was deposited on the inner wall of the quartz deposition tube using the MCVD process, followed by the deposition of a SiO2-based loose core layer inside the barrier layer. The deposition temperature of the loose core layer was controlled at 1320–1380 °C, and deposition was performed in 9 passes. Measurements of samples from the same batch showed that the thickness of the loose core layer was 126 μm, and the open porosity was 42.7%.

[0039] Prepare the doping solution. The concentration of Yb(NO3)3 in the doping solution is 0.110 mol / L, the concentration of Al(NO3)3 is 0.680 mol / L, the concentration of urea is 2.30 mol / L, the solvent is deionized water, and the pH is adjusted to 2.7 with dilute nitric acid.

[0040] At 25°C, the dopant solution was brought into contact with the porous core layer and circulated at a flow rate of 38 mL / min. The quartz deposition tube rotated at 18 rpm for 55 min. At the end of the circulation, the Yb in the inlet and outlet dopant solutions was... 3+ The concentration difference is 3.7% of the inlet concentration.

[0041] The dry weight m0 of the 60mm sample section was 27.3618g, the saturated weight m1 was 27.5764g, and the saturated liquid retention was 0.2146g. After evaporation blank correction, the liquid retention reduction rates at 40kPa and 45kPa were 4.63% and 5.06%, respectively, with a linear interpolation value of ΔP5 = 44.3kPa. The liquid retention reduction rate at the drainage pressure of 21.5kPa in the example was 3.60%.

[0042] After draining the liquid, the quartz deposition tube is placed in a slightly positive pressure humid nitrogen atmosphere and heated to 90°C. It is kept at this temperature for 55 minutes to allow the urea to release ammonia upon heating, thereby causing the Yb / Al precursor in the open pores to precipitate in the loose core layer.

[0043] The following post-processing steps were then performed: drying at 110℃ for 70 min; oxidative decomposition at 380℃ in an oxygen atmosphere for 60 min; dehydration at 980℃ in a He / O2 / Cl2 mixed atmosphere for 45 min; sintering and transparentization at 1580–1640℃; and melting and shrinking at 2050–2160℃ to obtain the Yb / Al co-doped optical fiber preform.

[0044] The test results showed that the average Yb₂O₃ content in the rare-earth-doped glass core layer was 0.21 mol%, and the average Al₂O₃ content was 1.43 mol%; the ratio of the average Yb concentration in the central region to that in the middle region was 1.05; and the coefficient of variation of Yb radial concentration was 5.8%. After drawing, the background loss at 1200 nm was 17.6 dB / km, and the absorption at 976 nm fluctuated by ±4.1% along the length direction.

[0045] Example 2 is based on Example 1, except that the thickness of the loose core layer is 112 μm and the open porosity is 38.9%; the concentration of Yb(NO3)3 in the doping solution is 0.085 mol / L, the concentration of Al(NO3)3 is 0.510 mol / L, the concentration of urea is 1.70 mol / L, and the pH is 2.8.

[0046] The initial temperature was 24℃, the circulation time was 60 min, and the circulation flow rate was 34 mL / min. The measured ΔP5 was 41.6 kPa. The applied nitrogen displacement pressure difference ΔP was 16.7 kPa, approximately 0.40ΔP5, and the displacement time was 100 s. After displacement, there was no continuous liquid column in the tube, and very thin wetting traces were visible in some locations; the liquid retention reduction rate of the same batch of samples was measured to be 2.8%.

[0047] The second temperature was 88°C, and the temperature was maintained for 70 minutes. The post-treatment conditions were the same as in Example 1.

[0048] The test results showed that the average content of Yb₂O₃ in the core layer was 0.17 mol%, and the average content of Al₂O₃ was 1.05 mol%; the ratio of the average Yb concentration in the central region to that in the middle region was 1.10; and the coefficient of variation of Yb radial concentration was 7.2%. After drawing, the background loss at 1200 nm was 18.9 dB / km, and the absorption at 976 nm fluctuated by ±5.0% along the length direction.

[0049] Example 3 is based on Example 1, except that the thickness of the loose core layer is 135 μm and the open porosity is 45.2%; the concentration of Yb(NO3)3 in the doping solution is 0.140 mol / L, the concentration of Al(NO3)3 is 0.840 mol / L, the concentration of urea is 2.60 mol / L, and the pH is 2.6.

[0050] The sample was circulated at 25℃ for 50 min at a flow rate of 42 mL / min. The measured ΔP5 was 47.8 kPa. The applied nitrogen displacement pressure difference ΔP was 25.3 kPa, approximately 0.53ΔP5, and the displacement time was 80 s. After displacement, no continuous liquid column or flowing liquid film was observed in the lumen; the liquid retention reduction rate for the same batch of samples was 4.6%.

[0051] The second temperature was 92℃, and the temperature was maintained for 50 minutes. The post-treatment conditions were the same as in Example 1.

[0052] The test results showed that the average content of Yb₂O₃ in the core layer was 0.26 mol%, and the average content of Al₂O₃ was 1.67 mol%; the ratio of the average Yb concentration in the central region to that in the middle region was 0.98; and the coefficient of variation of Yb radial concentration was 5.5%. After drawing, the background loss at 1200 nm was 19.8 dB / km, and the absorption at 976 nm fluctuated by ±3.8% along the length direction.

[0053] Example 4 uses a quartz deposition tube of the same specifications as in Example 1. A SiO2 barrier layer and a SiO2-based porous core layer are deposited using the MCVD process. The porous core layer has a thickness of 118 μm and an open porosity of 39.5%.

[0054] Prepare the doping solution. The concentrations of Yb(NO3)3 in the doping solution are 0.075 mol / L, Er(NO3)3 is 0.008 mol / L, Al(NO3)3 is 0.460 mol / L, urea is 1.90 mol / L, deionized water is used as the solvent, and the pH is adjusted to 2.8 with dilute nitric acid.

[0055] The solution was circulated at 25°C for 60 min at a flow rate of 34 mL / min and a deposition tube rotation speed of 20 rpm. At the end of the circulation, the Yb concentration in the inlet and outlet dopant solutions was [data missing]. 3+ The concentration difference is 4.5%.

[0056] The measured ΔP5 was 39.1 kPa. The applied nitrogen venting pressure difference ΔP was 18.4 kPa, approximately 0.47ΔP5, and the venting time was 100 s. After venting, there was no continuous liquid column in the tube, and the liquid retention reduction rate of the same batch of samples was measured to be 3.9%.

[0057] The quartz deposition tube was then heated to 88°C and held for 60 min to allow urea to release ammonia and induce the precipitation of Yb / Er / Al precursors within the pores. Subsequently, it was dried at 105°C for 80 min, oxidized and decomposed at 360°C for 70 min, dehydrated at 960°C in a He / O2 / Cl2 mixed atmosphere for 50 min, sintered for transparency at 1570–1630°C, and then shrunk at 2050–2160°C.

[0058] The test results showed that the average content of Yb₂O₃ in the core layer was 0.15 mol%, the average content of Er₂O₃ was 0.018 mol%, and the average content of Al₂O₃ was 1.18 mol%. The ratio of the average Yb concentration in the central region to that in the middle region was 1.08, and the ratio of the average Er concentration in the central region to that in the middle region was 1.10. The radial concentration variation coefficient of Yb was 6.6%, and the radial concentration variation coefficient of Er was 7.3%. After drawing, the background loss at 1200 nm was 21.4 dB / km.

[0059] Example 5 is based on Example 1, except that the concentration of Yb(NO3)3 in the doping solution is 0.095 mol / L, the concentration of Al(NO3)3 is 0.570 mol / L, the concentration of hexamethylenetetramine is 1.10 mol / L, no urea is added, and the pH is 2.9.

[0060] The porous core layer has a thickness of 121 μm and an open porosity of 41.1%. After circulation at 23℃ for 65 min, ΔP5 was measured to be 43.5 kPa. Applying nitrogen to displace the liquid resulted in a pressure difference ΔP of 22.8 kPa, approximately 0.52ΔP5, with a displacement time of 100 s. After displacement, no continuous liquid column remained in the tube, and the liquid retention reduction rate for the same batch of samples was measured to be 4.4%.

[0061] The quartz deposition tube was heated to 85°C and held at that temperature for 90 minutes. Since hexamethylenetetramine releases ammonia at a slightly slower rate than the urea system, the holding time was extended accordingly. Subsequently, drying, oxidative decomposition, dehydration, sintering for transparency, and melting were performed, with the process temperatures identical to those in Example 1.

[0062] The test results showed that the average Yb₂O₃ content in the core layer was 0.18 mol%, and the average Al₂O₃ content was 1.12 mol%; the ratio of the average Yb concentration in the central region to that in the middle region was 1.03; and the coefficient of variation of Yb radial concentration was 6.1%. After drawing, the background loss at 1200 nm was 18.4 dB / km, and the absorption at 976 nm fluctuated by ±4.4% along the length direction.

[0063] Example 6 uses a high-purity quartz deposition tube with an outer diameter of 25 mm, an inner diameter of 19 mm, and a length of 600 mm. An SiO2 barrier layer and a SiO2-based porous core layer are formed using the MCVD process. The porous core layer has a thickness of 130 μm and an open porosity of 43.8%.

[0064] Prepare a water-soluble doping solution. The doping solution contains 0.070 mol / L YbCl3, 0.420 mol / L AlCl3, and 1.50 mol / L urea, with an initial pH of 2.5. To reduce potential localized hydrolysis caused by the chloride system, the solution is filtered through a 0.45 μm filter membrane after preparation and allowed to stand for 15 min to remove bubbles before use.

[0065] The sample was circulated at 22℃ for 70 min at a flow rate of 32 mL / min. The measured ΔP5 was 46.2 kPa. Applying nitrogen to displace the liquid resulted in a pressure difference ΔP of 25.4 kPa, approximately 0.55ΔP5, with a displacement time of 90 s. After displacement, no continuous liquid column remained in the tube, and the liquid retention reduction rate for the same batch of samples was 4.9%.

[0066] The temperature was then raised to 90℃ and held for 65 min to allow urea to release ammonia and induce the precipitation of Yb / Al precursors within the open pores of the porous core layer. Post-treatment included: drying at 100℃ for 80 min; oxygen treatment at 420℃ for 80 min; dehydration at 1020℃ in a He / O2 / Cl2 atmosphere for 60 min; sintering at 1600–1660℃ for transparency; and subsequent melting and shrinkage.

[0067] The test results showed that the average content of Yb₂O₃ in the core layer was 0.13 mol%, and the average content of Al₂O₃ was 0.86 mol%; the ratio of the average Yb concentration in the central region to that in the middle region was 1.07; and the coefficient of variation of Yb radial concentration was 7.0%. After drawing, the background loss at 1200 nm was 22.7 dB / km, and the absorption at 976 nm fluctuated by ±5.6% along the length direction.

[0068] In this embodiment, the background loss is slightly higher than that of the nitrate system, mainly due to the hydrolysis of the chloride system and subsequent dehydration control, but it is still within an acceptable range.

[0069] Comparative Example 1 is based on Example 1, except that after the low-temperature cyclic permeation is completed, the gas discharge pressure difference ΔP is not applied, but the quartz deposition tube is directly heated to 90°C and kept at that temperature for 55 minutes.

[0070] After the temperature rise and precipitation were completed, obvious flocculent precipitate was observed in the lumen of the quartz deposition tube. The free precipitate in the lumen was collected and dried, with a mass of 0.63 g.

[0071] The test results showed that the average content of Yb2O3 in the core layer was 0.24 mol%, and the average content of Al2O3 was 1.49 mol%; the average Yb concentration ratio in the central region / middle region was 1.57, and the radial concentration variation coefficient of Yb was 19.6%; a rich precipitate layer of about 6-14 μm was formed near the original lumen; the background loss at 1200 nm was 31.8 dB / km; the average small signal core absorption coefficient at 976 nm was about 480 dB / m, but the radial distribution was obviously uneven.

[0072] Comparative Example 2 is based on Example 1, except that after the low-temperature cyclic permeation was completed, ΔP5 was not measured, and the drainage was not controlled according to ΔP / ΔP5. Instead, a nitrogen pressure difference of 6.0 kPa was used to purge for 90 seconds.

[0073] After purging, intermittent liquid films and localized droplets were still visible on the inner wall of the quartz deposition tube. After heating and precipitation, the mass of free precipitate collected from the tube was 0.18 g.

[0074] The test results showed that the average content of Yb2O3 in the core layer was 0.22 mol%, and the average content of Al2O3 was 1.37 mol%; the average Yb concentration ratio in the central region to the middle region was 1.29, and the radial concentration variation coefficient of Yb was 12.4%; the background loss at 1200 nm was 24.6 dB / km; and the average small signal core absorption coefficient at 976 nm was approximately 440 dB / m.

[0075] Comparative Example 3 is based on Example 1, except that after the low-temperature cyclic permeation was completed, a nitrogen pressure difference of 53.0 kPa was used to drain the liquid for 90 seconds. This pressure difference is 1.20 times that of ΔP5 (44.3 kPa) under the same conditions.

[0076] After drainage, no continuous liquid column was observed in the tube, and the mass of free precipitate in the tube after heating and sedimentation was only 0.014 g. However, the liquid retention reduction rate of the same batch of samples was measured to be 21.1%.

[0077] The test results showed that the average content of Yb2O3 in the core layer was 0.14 mol%, and the average content of Al2O3 was 0.93 mol%; the average Yb concentration ratio in the central region / middle region was 0.98, and the radial concentration variation coefficient of Yb was 6.4%; the background loss at 1200 nm was 18.2 dB / km; the average small signal core absorption coefficient at 976 nm was 280 dB / m, which was 33.3% lower than the 420 dB / m in Example 1, and the maximum axial relative deviation was 4.0%.

[0078] Table 1 Data Comparison As shown in Table 1, all of Examples 1 to 6 used a drainage pressure of 0.40 to 0.55ΔP5, the liquid retention reduction rate of the sample section did not exceed 5%, the mass of free precipitate in the lumen was 0.011 to 0.043 g, and the average rare earth concentration ratio of the central region to the intermediate region was 0.98 to 1.10.

[0079] Comparative Example 1 shows that when there is no drainage, the free liquid in the tube will form more free precipitates and cause central enrichment; Comparative Example 2 shows that purging at too low a pressure and without ΔP5 calibration cannot stably remove liquid film and droplets; Comparative Example 3 shows that although pressure exceeding ΔP5 reduces free precipitates, it will cause a significant decrease in the amount of doped liquid and rare earth fixed in the pore.

[0080] Therefore, under the conditions of the above embodiments, controlling ΔP to 0.40 to 0.55 times ΔP5 and controlling the liquid retention reduction rate to within 5% can take into account the free liquid discharge in the cavity, the liquid retention in the pores and the final rare earth fixation amount, and is beneficial to improving the radial doping uniformity.

[0081] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method of producing a rare earth-doped optical fiber preform, characterized by, Includes the following steps: A porous core layer with open pores is deposited on the inner wall of a quartz deposition tube using the MCVD process. At a first temperature, the dopant solution is brought into contact with the porous core layer, allowing the dopant solution to enter the open pores of the porous core layer. The dopant solution contains rare earth ions, aluminum ions, and a precipitant that releases ammonia upon heating. The precipitant is urea, hexamethylenetetramine, or a combination of both. The rare earth ions include one or two of ytterbium ions and erbium ions. Before heating the quartz deposition tube to the second temperature, a gas discharge pressure difference ΔP is applied to both ends of the quartz deposition tube to discharge the dopant liquid that is not retained by the open pores in the inner cavity of the quartz deposition tube, and to ensure that there is no continuous liquid column in the inner cavity of the quartz deposition tube. Wherein, the gas discharge pressure difference ΔP is less than the critical pressure difference ΔP5 for a 5% reduction in liquid retention. The critical pressure difference ΔP5 for a 5% reduction in liquid retention is the gas pressure difference corresponding to a 5% reduction in liquid retention relative to the saturated liquid retention of a loose core layer sample formed under the same doping solution and the same first temperature and saturated with the doping solution in the same batch or under the same deposition conditions. The quartz deposition tube is heated to a second temperature and kept at that temperature, causing the precipitant to release ammonia, thereby causing rare earth ions in the open pores to precipitate in the loose core layer. The loose core layer after precipitation is successively dried, oxidized and decomposed, dehydrated, sintered and transparentized, and melted and shrunk to obtain rare earth-doped optical fiber preforms.

2. The production method according to claim 1, characterized by: The 5% reduction in liquid retention capacity lowers the critical pressure difference ΔP5 by the following method: Take a quartz deposition tube sample section that has the same deposition conditions as the loose core layer in the quartz deposition tube; At the first temperature, the same doping solution is introduced into the loose core layer of the sample segment, and the loose core layer is brought to liquid saturation. After draining the free liquid from the cavity of the sample section, weigh the sample section and calculate the saturated liquid retention capacity; A gas pressure difference is applied step by step along the axial direction of the sample section, and maintained at each gas pressure difference for 60–200 s; After each stage of gas pressure difference, the sample section is weighed and the remaining liquid retention is calculated. The pressure difference ΔP5 is defined as the gas pressure difference when the remaining liquid volume decreases by 5% relative to the saturated liquid volume.

3. The production method according to claim 1 or 2, characterized by: The gas discharge pressure difference ΔP is 0.40 to 0.65 times the critical pressure difference ΔP5 for the 5% liquid retention reduction.

4. The production method according to claim 3, characterized by: After applying the gas discharge pressure difference ΔP, the liquid retention in the open pores of the loose core layer decreases by no more than 10% compared to the liquid retention before applying the gas discharge pressure difference ΔP.

5. The production method according to claim 4, characterized by: The first temperature is 15–35°C, the second temperature is 70–95°C, and the temperature is maintained at the second temperature for 10–180 minutes.

6. The production method according to claim 5, characterized by: The total concentration of rare earth ions in the doping solution is 0.001–0.50 mol / L, the molar ratio of aluminum ions to rare earth ions is 2–30, the concentration of urea and / or hexamethylenetetramine is 0.05–3.50 mol / L, and the molar ratio of urea and / or hexamethylenetetramine to rare earth ions is 5–80.

7. The method of any one of claims 4 to 6, wherein: The doping solution is an aqueous solution, the rare earth ions are provided by one or more of the corresponding chlorides, nitrates, and acetates, and the aluminum ions are provided by one or more of aluminum chloride, aluminum nitrate, and aluminum acetate.

8. The method of any one of claims 4 to 6, wherein: The drying, oxidative decomposition, dehydration, sintering and transparentization, and melting and shrinkage processes include: The loose core layer after precipitation was dried at 60–150℃; Oxidative decomposition treatment was carried out at 250–550°C in an oxygen-containing atmosphere. Dehydration treatment is carried out at 800–1200℃ in a dehydration atmosphere containing chlorine gas; Sintering and transparency treatment is carried out at 1450–1700℃; The quartz deposition tube is melted and shrunk to obtain a rare earth-doped optical fiber preform.

9. A rare earth-doped optical fiber preform produced by the method of any one of claims 1 to 8, characterized in that: It includes a quartz cladding and a rare-earth-doped glass core layer located within the quartz cladding; In the rare earth-doped glass core layer, the content of rare earth elements, calculated as oxides, is 0.01 mol% to 2.00 mol%, and the content of Al2O3 is 0.2 mol% to 15 mol%. Among them, on the cross-section of the rare earth-doped glass core layer, the region with radius R and radius r≤0.20R is the central region, and the annular region with 0.40R≤r≤0.80R is the middle region; The ratio of the average rare earth element concentration in the central region to the average rare earth element concentration in the intermediate region is 0.80 to 1.

20.

10. The rare earth-doped optical fiber preform of claim 9, wherein: The rare earth elements include Yb or Er, and the molar ratio of aluminum to rare earth elements is 2 to 30.

Citation Information

Patent Citations

  • Method for manufacturing doped optical fibre preform by MCVD (modified chemical vapour deposition)

    CN102515501B

  • Method for preparing rare earth doped optical fiber preform by in-tube method

    CN115448590A