Preparation method of copper-cobalt secondary battery with long cycle life and battery
Patent Information
- Application Number
- CN202611181245.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-09-15
Smart Images

Figure CN122762864A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical energy storage technology, specifically to a method for preparing a copper-cobalt secondary battery with a long cycle life and the battery itself. Background Technology
[0002] Zinc-cobalt batteries and other aqueous secondary batteries have broad application prospects in large-scale energy storage, backup power, and portable electronic devices due to their advantages such as high safety, low cost, environmental friendliness, and high electrolyte ionic conductivity. As the requirements for cycle life and operational stability of energy storage systems continue to increase, how to further improve the cycle performance of aqueous secondary batteries has become a research hotspot in this field.
[0003] Currently, zinc-cobalt batteries and similar aqueous secondary batteries typically use metallic zinc as the negative electrode active material. During repeated charge and discharge cycles, the deposition and dissolution of zinc ions on the negative electrode surface can easily lead to uneven local current density distribution and uneven zinc deposition, resulting in the gradual formation of dendritic structures on the negative electrode surface. As the number of charge and discharge cycles increases, the zinc dendrites continue to grow, which not only easily puncture the separator, causing internal short circuits and reducing battery safety, but also leads to reduced utilization of the negative electrode active material, increased interfacial side reactions, and intensified electrode polarization. Ultimately, this results in rapid capacity decay and a significantly shortened cycle life, severely restricting the practical application of zinc-cobalt batteries and similar aqueous secondary batteries.
[0004] Therefore, this invention proposes a method for preparing a copper-cobalt secondary battery with a long cycle life and the battery itself. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing a copper-cobalt secondary battery with a long cycle life and the battery itself, so as to solve the technical problems of short cycle life and poor safety of existing zinc-cobalt batteries and similar aqueous secondary batteries due to dendrite growth on the negative electrode, and to achieve ultra-long cycle charge and discharge performance.
[0006] According to a first aspect of the present invention, in order to achieve the above-mentioned objective, the present invention provides the following technical solution: a method for preparing a copper-cobalt secondary battery with a long cycle life, comprising the following steps: S1. Pre-treat the nickel foam to obtain a nickel foam matrix that meets the requirements for electrode preparation; S2. Using the nickel foam substrate obtained in step S1 as the negative electrode current collector, copper active material is deposited in situ onto the surface of the nickel foam by electrodeposition to prepare a copper negative electrode. S3. Using the nickel foam substrate obtained in step S1 as the positive electrode current collector, a cobalt-based oxide active material is loaded onto the surface of the nickel foam by electrodeposition or hydrothermal method to prepare a cobalt positive electrode. S4. Prepare an alkaline electrolyte and wet the diaphragm with the alkaline electrolyte, and place the treated diaphragm between the copper negative electrode and the cobalt positive electrode. S5. The copper negative electrode prepared in step S2, the separator treated in step S4, and the cobalt positive electrode prepared in step S3 are stacked and assembled in sequence, and the alkaline electrolyte is added to obtain a copper-cobalt secondary battery. In this embodiment, both the copper negative electrode and the cobalt positive electrode use nickel foam as the current collector, and the copper active material and the cobalt-based oxide active material are respectively loaded on the surface of the corresponding nickel foam substrate to form the electrode.
[0007] Furthermore, in step S1, the nickel foam is pretreated as follows: S11. Select a thickness of 0.2–1.0 mm and a surface density of 200–500 g / m³. 2 Nickel foam with a porosity of 90%–98% and a pore size of 100–500 μm; S12. Place the nickel foam in an organic solvent in sequence for ultrasonic degreasing; S13. Use pickling solution to remove the oxide layer on the surface of the foamed nickel; S14. Rinse repeatedly with deionized water until neutral; S15. After rinsing with anhydrous ethanol, the material is dried to obtain a clean and activated nickel foam matrix.
[0008] Furthermore, the organic solvent is acetone; The pickling solution is a hydrochloric acid solution; The drying process is either natural drying or oven drying.
[0009] Further, in step S2, copper active material is deposited in situ onto the surface of nickel foam by electrodeposition to prepare a copper anode, as detailed below: S21. Using the nickel foam obtained in step S1 as the cathode and the copper plate as the anode, the copper plate is placed in a copper electrodeposition electrolyte for constant current electrodeposition, so that copper grains are uniformly deposited along the surface of the nickel foam to form a copper active layer covering the surface of the nickel foam. S22. After electroplating, the foamed nickel is removed by rinsing with deionized water and drying, and a copper negative electrode is obtained. The copper electrodeposition electrolyte includes copper sulfate with a concentration of 0.5–2 mol / L and sulfuric acid with a concentration of 0.3–1 mol / L; the current density is 10–50 mA / cm²; and the deposition time is 10–60 min.
[0010] Furthermore, in step S3, a cobalt-based oxide active material is loaded onto the surface of nickel foam by electrodeposition to prepare a cobalt cathode, as detailed below: Using nickel foam as the cathode and platinum or graphite as the anode, constant current electrodeposition is performed in a cobalt electroplating solution, followed by heat treatment to form a cobalt-based oxide active layer. The cobalt electroplating solution comprises 0.1–0.5 mol / L cobalt sulfate and 0.5–1.0 mol / L sulfuric acid, with a current density of 10–50 mA / cm². 2 The electrodeposition time is 10 to 60 minutes.
[0011] Furthermore, in step S3, a cobalt cathode is prepared by loading a cobalt-based oxide active material onto the surface of nickel foam using a hydrothermal method, as detailed below: Prepare a hydrothermal reaction precursor solution, which includes cobalt nitrate, urea, and ammonium chloride, wherein the concentration of cobalt nitrate is 0.01–0.1 mol / L, the concentration of urea is 0.05–0.5 mol / L, and the concentration of ammonium chloride is 0.05–0.5 mol / L. The nickel foam is immersed in a hydrothermal reactor containing the hydrothermal reaction precursor solution at a hydrothermal temperature of 120–180°C for 4–12 hours. The hydrothermally treated nickel foam is removed, washed with deionized water, vacuum dried at 60–100°C, and then heat-treated in air at 300–500°C for 1–4 hours to obtain a cobalt cathode with nickel foam loaded with cobalt-based oxide.
[0012] Furthermore, the alkaline electrolyte comprises potassium hydroxide and zinc salt, wherein the zinc salt is zinc oxide and / or zinc acetate, wherein the concentration of potassium hydroxide is 1–6 mol / L and the concentration of zinc salt is 0.1–0.5 mol / L; The separator is made of glass fiber, cellulose, or hydrophilic polyolefin and is used for battery assembly after being completely immersed in the alkaline electrolyte.
[0013] According to a second aspect of the present invention, the present invention provides a copper-cobalt secondary battery, which is prepared by a method for preparing a copper-cobalt secondary battery with a long cycle life as described in the first aspect. The battery uses nickel foam as a common current collector for both the negative and positive electrodes, uses metallic copper electroplated on nickel foam as the negative electrode active material, and uses cobalt-based oxide electroplated or hydrothermally deposited on nickel foam as the positive electrode active material. A membrane impregnated with electrolyte is provided between the positive and negative electrodes.
[0014] Furthermore, the diaphragm is made of glass fiber, cellulose, or hydrophilic polyolefin, with a thickness of 100–300 μm and a pore size of 0.1–5 μm.
[0015] Furthermore, the cobalt-based oxide is Co3O4, which is directly loaded on the surface of the nickel foam skeleton and forms a tightly bonded positive electrode structure with the nickel foam current collector.
[0016] The present invention has at least the following beneficial effects: (1) In this invention, nickel foam is used as a common current collector for copper negative electrode and cobalt positive electrode. The active material is directly loaded onto the surface of nickel foam by electrodeposition or hydrothermal method to form a stable electrode structure. This is beneficial to improve the bonding stability between the active material and the current collector, reduce the risk of the active layer falling off during long-term charge and discharge process, and thus improve the cycle stability of the battery.
[0017] (2) The present invention uses metallic copper as the negative electrode active material to replace the zinc negative electrode in the traditional zinc-cobalt battery, which effectively avoids the problem of dendrite growth that easily occurs in the zinc negative electrode during charging and discharging, reduces the risk of membrane puncture and internal short circuit caused by dendrites, improves the safety of battery use, and provides a foundation for achieving long cycle life.
[0018] (3) The present invention uses three-dimensional porous nickel foam as electrode current collector, which can provide sufficient loading space for copper active materials and cobalt-based oxide active materials, and is conducive to electrolyte wetting and the formation of electrode reaction interface, thereby improving the electron transport and ion diffusion conditions in the electrode reaction process and improving the stability of battery charging and discharging process.
[0019] (4) The preparation method of the present invention is simple. The electrode active material can be directly constructed on the surface of nickel foam by electrodeposition or hydrothermal method. The process flow is clear and has good repeatability. It is suitable for the preparation of copper-cobalt secondary batteries and provides a feasible technical solution for the preparation of aqueous secondary batteries with long cycle life and good stability.
[0020] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 This is a schematic diagram illustrating the operating principle of the copper-cobalt secondary battery of the present invention. Figure 2 This is a scanning electron microscope image of the copper negative electrode in the copper-cobalt secondary battery of the present invention. Figure 3 This is a scanning electron microscope image of the cobalt cathode in the copper-cobalt secondary battery of the present invention; Figure 4 This is the electrochemical impedance spectroscopy of the copper-cobalt secondary battery of the present invention; Figure 5 This is a charge-discharge voltage curve of the copper-cobalt secondary battery of the present invention under different cycle numbers. Detailed Implementation
[0023] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0024] Example 1: This embodiment provides a method for preparing a copper-cobalt secondary battery with a long cycle life, including the following steps: S1, Nickel foam pretreatment: Select nickel foam with a thickness of 0.5 mm, a surface density of 350 g / m², a porosity of 95%, and an average pore size of 200 μm, and cut it into square sheets of 2 cm × 2 cm. The sample was ultrasonically cleaned sequentially with acetone for 8 minutes, 1 M dilute hydrochloric acid for 5 minutes, deionized water for 5 minutes, and anhydrous ethanol for 8 minutes, and then dried in a vacuum drying oven at 70°C for 2 hours. S2, Preparation of copper negative electrode: Pretreated nickel foam was used as the cathode and a pure copper plate (99.99% purity) was used as the anode. Constant current electrodeposition was carried out in the electroplating solution, which consisted of 1.0 mol / L copper sulfate (CuSO4·5H2O) and 0.8 mol / L sulfuric acid (H2SO4). Electroplating conditions: current density 30 mA / cm², electroplating time 30 minutes; After electroplating, the nickel foam was removed, rinsed three times with deionized water, and vacuum dried at 60°C to obtain a copper anode with a copper loading of approximately 8 mg / cm². Figure 2 The scanning electron microscope images show that the copper layer consists of dense spherical particles that are uniformly distributed on the surface of the nickel foam, with an average particle size of 6 μm. S3. Cobalt cathode preparation: A cobalt cathode was prepared by loading cobalt-based oxide active materials onto the surface of nickel foam using a hydrothermal method, as detailed below: Preparation of hydrothermal reaction precursor solution: cobalt nitrate (Co(NO3)2·6H2O) 0.05 mol / L, urea 0.2 mol / L, ammonium chloride 0.1 mol / L, solvent is deionized water; The pretreated nickel foam was immersed in 50 mL of precursor solution and transferred to a 100 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene. After sealing, it was reacted in an oven at 120 °C for 8 hours. After naturally cooling to room temperature, the nickel foam was removed, rinsed three times alternately with deionized water and anhydrous ethanol, and then vacuum dried at 70 °C for 12 hours. The dried sample was then placed in a muffle furnace and heated to 350°C at a rate of 5°C / min, and heat-treated in air for 2 hours. After furnace cooling, a positive electrode with a nickel foam-supported Co3O4 nanowire array was obtained, with a cobalt-based oxide loading of approximately 6 mg / cm³. 2 , Figure 3 The scanning electron microscope images show that the cobalt-based oxide layer is arranged in a linear cluster and is uniformly distributed on the surface of the nickel foam. S4. Electrolyte preparation: Weigh 168.2 g of potassium hydroxide (KOH) and 4.4 g of zinc acetate (Zn(CH3COO)2·2H2O), dissolve them in deionized water, and make up to 500 mL to obtain an alkaline electrolyte with a KOH concentration of 6 mol / L and a zinc acetate concentration of 0.2 mol / L. S5. Diaphragm treatment: Glass fiber filter paper with a thickness of 200 μm and a pore size of 0.5 μm is used as the diaphragm, cut into 2.5cm × 2.5cm pieces, and soaked in the prepared electrolyte for 12 hours. S6. Performance Testing: A battery was assembled using a copper anode, a cobalt cathode, and a separator. A constant current charge-discharge test was conducted at 25°C with a current density of 500 mA / g (based on the mass of the cathode active material), and a voltage range of 0.3–1.2 V. The test results are as follows: Figure 4 and 5 As shown, compared to zinc-cobalt batteries, the ohmic impedance decreased from 3.2 Ω to 1.0 Ω, the initial discharge specific capacity was 309 mAh / g, and the coulombic efficiency was 99.3%. After 10,000 cycles, the discharge specific capacity remained at 264 mAh / g, with a capacity retention of 85.4%.
[0025] Example 2: This embodiment provides a method for preparing a copper-cobalt secondary battery with a long cycle life, including the following steps: S1, Nickel foam pretreatment: A thickness of 0.5 mm and a surface density of 350 g / m³ were selected. 2 Nickel foam with a porosity of 95% and an average pore size of 200 μm was cut into square sheets of 2 cm × 2 cm. The sample was ultrasonically cleaned sequentially with acetone for 8 minutes, 1 M dilute hydrochloric acid for 5 minutes, deionized water for 5 minutes, and anhydrous ethanol for 8 minutes, and then dried in a vacuum drying oven at 70°C for 2 hours.
[0026] S2, Preparation of copper negative electrode: Pretreated nickel foam was used as the cathode and a pure copper plate (99.99% purity) was used as the anode. Constant current electrodeposition was carried out in the electroplating solution, which consisted of 1.0 mol / L copper sulfate (CuSO4·5H2O) and 0.8 mol / L sulfuric acid (H2SO4). Electroplating conditions: Current density 30 mA / cm² 2 Electroplating time: 30 minutes; After electroplating, the nickel foam was removed, rinsed three times with deionized water, and vacuum dried at 60°C to obtain a copper loading of approximately 8 mg / cm³. 2 The copper negative electrode, Figure 2 The scanning electron microscope images show that the copper layer consists of dense spherical particles that are uniformly distributed on the surface of the nickel foam, with an average particle size of 6 μm. S3. Cobalt cathode preparation: A cobalt cathode was prepared by electrodepositing a cobalt-based oxide active material onto the surface of nickel foam, as detailed below: Prepare a cobalt electroplating solution with a cobalt nitrate concentration of 0.1 mol / L.
[0027] Pretreated nickel foam was used as the working electrode, a platinum sheet as the counter electrode, and a saturated calomel electrode (SCE) as the reference electrode. The electrodes were placed in a cobalt electroplating solution for constant voltage deposition at a voltage of -1.0 V (vs SCE) for 20 min.
[0028] After electrodeposition, the electrode was removed and rinsed with deionized water, then heat-treated at 400 °C for 2 h in air to convert the deposited cobalt-based precursor into a cobalt-based oxide active layer, thus preparing a cobalt cathode with a cobalt-based oxide loading of approximately 5 mg / cm³. 2 ; S4. Electrolyte preparation: Weigh 168.2 g of potassium hydroxide (KOH) and 4.4 g of zinc acetate (Zn(CH3COO)2·2H2O), dissolve them in deionized water, and make up to 500 mL to obtain an alkaline electrolyte with a KOH concentration of 6 mol / L and a zinc acetate concentration of 0.2 mol / L. S5. Diaphragm treatment: Glass fiber filter paper with a thickness of 200 μm and a pore size of 0.5 μm is used as the diaphragm, cut into 2.5cm × 2.5cm pieces, and soaked in the prepared electrolyte for 12 hours. S6. Performance Testing: A battery was assembled from a copper anode, a cobalt cathode, and a separator. Constant current charge-discharge tests were conducted at 25°C with a current density of 500 mA / g (based on the mass of the cathode active material). The voltage range was 0.3–1.2 V. Compared to a zinc-cobalt battery, the ohmic impedance decreased from 3.2Ω to 2.0Ω. The initial discharge specific capacity was 287.0 mAh / g, with a coulombic efficiency of 99.1%. After 10,000 cycles, the discharge specific capacity remained at 230.5 mAh / g, with a capacity retention of 80.3%.
[0029] Example 3: This embodiment provides a method for preparing a copper-cobalt secondary battery with a long cycle life, including the following steps: S1, Nickel foam pretreatment: A thickness of 0.5 mm and a surface density of 350 g / m³ were selected. 2 Nickel foam with a porosity of 95% and an average pore size of 200 μm was cut into square sheets of 2 cm × 2 cm. The sample was ultrasonically cleaned sequentially with acetone for 8 minutes, 1 M dilute hydrochloric acid for 5 minutes, deionized water for 5 minutes, and anhydrous ethanol for 8 minutes, and then dried in a vacuum drying oven at 70°C for 2 hours. S2, Preparation of copper negative electrode: Pretreated nickel foam was used as the cathode and a pure copper plate (99.99% purity) was used as the anode. Constant current electrodeposition was carried out in the electroplating solution, which consisted of 1.0 mol / L copper sulfate (CuSO4·5H2O) and 0.8 mol / L sulfuric acid (H2SO4). Electroplating conditions: Current density 10 mA / cm² 2 Electroplating time: 30 minutes; After electroplating, the nickel foam was removed, rinsed three times with deionized water, and vacuum dried at 60°C to obtain a copper loading of approximately 4 mg / cm³. 2 The copper anode has a copper layer consisting of dense spherical particles that are uniformly distributed on the surface of the nickel foam, with an average particle size of 10 μm. S3. Cobalt cathode preparation: A cobalt cathode was prepared by loading cobalt-based oxide active materials onto the surface of nickel foam using a hydrothermal method, as detailed below: Preparation of hydrothermal reaction precursor solution: cobalt nitrate (Co(NO3)2·6H2O) 0.05 mol / L, urea 0.2 mol / L, ammonium chloride 0.1 mol / L, solvent is deionized water; The pretreated nickel foam was immersed in 50 mL of precursor solution, transferred to a 100 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene, sealed, and reacted in an oven at 120 °C for 8 hours. After naturally cooling to room temperature, remove the nickel foam, rinse it three times alternately with deionized water and anhydrous ethanol, and vacuum dry it at 70°C for 12 hours. The dried sample was then placed in a muffle furnace and heated to 350°C at a rate of 5°C / min, and heat-treated in air for 2 hours. After furnace cooling, a positive electrode with a nickel foam-supported Co3O4 nanowire array was obtained, with a cobalt-based oxide loading of approximately 6 mg / cm³. 2 .
[0030] S4. Electrolyte preparation: Weigh 168.2 g of potassium hydroxide (KOH) and 4.4 g of zinc acetate (Zn(CH3COO)2·2H2O), dissolve them in deionized water, and make up to 500 mL to obtain an alkaline electrolyte with a KOH concentration of 6 mol / L and a zinc acetate concentration of 0.2 mol / L. S5. Diaphragm treatment: Glass fiber filter paper with a thickness of 200 μm and a pore size of 0.5 μm is used as the diaphragm, cut into 2.5cm × 2.5cm pieces, and soaked in the prepared electrolyte for 12 hours. S6. Performance Testing: A battery was assembled using a copper anode, a cobalt cathode, and a separator. Constant current charge-discharge testing was conducted at 25°C with a current density of 500 mA / g (based on the mass of the cathode active material), and a voltage range of 0.3–1.2 V. In terms of performance, the initial discharge specific capacity was 287 mAh / g, with a coulombic efficiency of 98.7%. After 10,000 cycles, the discharge specific capacity remained at 236 mAh / g, representing a capacity retention of 82.2%.
[0031] Example 4: This embodiment provides a method for preparing a copper-cobalt secondary battery with a long cycle life, including the following steps: S1, Nickel foam pretreatment: A thickness of 0.5 mm and a surface density of 350 g / m³ were selected. 2 Nickel foam with a porosity of 95% and an average pore size of 200 μm was cut into square sheets of 2 cm × 2 cm. The sample was ultrasonically cleaned sequentially with acetone for 8 minutes, 1 M dilute hydrochloric acid for 5 minutes, deionized water for 5 minutes, and anhydrous ethanol for 8 minutes, and then dried in a vacuum drying oven at 70°C for 2 hours. S2, Preparation of copper negative electrode: Pretreated nickel foam was used as the cathode and a pure copper plate (99.99% purity) was used as the anode. Constant current electrodeposition was carried out in the electroplating solution, which consisted of 1.0 mol / L copper sulfate (CuSO4·5H2O) and 0.8 mol / L sulfuric acid (H2SO4). Electroplating conditions: Current density 30 mA / cm² 2 Electroplating time: 40 minutes; After electroplating, the nickel foam was removed, rinsed three times with deionized water, and vacuum dried at 60°C to obtain a copper loading of approximately 10 mg / cm³. 2 The copper anode has a copper layer consisting of dense spherical particles that are uniformly distributed on the surface of the nickel foam, with an average particle size of 12 μm. S3. Cobalt cathode preparation: A cobalt cathode was prepared by loading cobalt-based oxide active materials onto the surface of nickel foam using a hydrothermal method, as detailed below: Preparation of hydrothermal reaction precursor solution: cobalt nitrate (Co(NO3)2·6H2O) 0.05 mol / L, urea 0.2 mol / L, ammonium chloride 0.1 mol / L, solvent is deionized water; Another piece of pretreated nickel foam (same size as above) was immersed in 50 mL of precursor solution, transferred to a 100 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene, sealed and reacted in an oven at 120°C for 8 hours. After naturally cooling to room temperature, remove the nickel foam, rinse it three times alternately with deionized water and anhydrous ethanol, and vacuum dry it at 70°C for 12 hours. The dried sample was then placed in a muffle furnace and heated to 350°C at a rate of 5°C / min, and heat-treated in air for 2 hours. After furnace cooling, a positive electrode with a nickel foam-supported Co3O4 nanowire array was obtained, with a cobalt-based oxide loading of approximately 6 mg / cm³. 2 ; S4. Electrolyte preparation: Weigh 168.2 g of potassium hydroxide (KOH) and 4.4 g of zinc acetate (Zn(CH3COO)2·2H2O), dissolve them in deionized water, and make up to 500 mL to obtain an alkaline electrolyte with a KOH concentration of 6 mol / L and a zinc acetate concentration of 0.2 mol / L. S5. Diaphragm treatment: Glass fiber filter paper with a thickness of 200 μm and a pore size of 0.5 μm is used as the diaphragm, cut into 2.5cm × 2.5cm pieces, and soaked in the prepared electrolyte for 12 hours. S6. Performance Testing: The above-mentioned positive and negative electrode materials and separator were assembled into a battery. A constant current charge-discharge test was conducted at 25°C with a current density of 500 mA / g (based on the mass of the positive electrode active material), and a voltage range of 0.3–1.2 V. In terms of performance, the initial discharge specific capacity was 310 mAh / g, with a coulombic efficiency of 99.5%. After 10,000 cycles, the discharge specific capacity remained at 233.7 mAh / g, with a capacity retention of 75.4%.
[0032] Example 5: This embodiment provides a copper-cobalt secondary battery, which is prepared by the preparation method of a copper-cobalt secondary battery with long cycle life described in any one of Embodiments 1 to 3. Its overall structure includes a copper negative electrode, a separator, a cobalt positive electrode, and an alkaline electrolyte. Among them, the negative electrode uses nickel foam as the current collector, and a copper active layer is formed on the surface of the three-dimensional skeleton of nickel foam by electrodeposition. The resulting copper is uniformly loaded on the surface of nickel foam as the negative electrode active material. Nickel foam serves as both the current collector for electron transport and the supporting skeleton for the negative electrode active material. The positive electrode also uses nickel foam as the current collector. Cobalt-based oxide active materials are loaded onto the surface of the nickel foam via electrodeposition or hydrothermal methods. When using electrodeposition, the cobalt-based active material is first deposited on the nickel foam surface, and after heat treatment, a cobalt-based oxide active layer is formed. When using hydrothermal methods, a cobalt-based precursor is first grown in situ on the nickel foam surface, and after heat treatment, a cobalt-based oxide active layer is formed. The resulting cobalt-based oxide is uniformly distributed on the surface of the three-dimensional framework of the nickel foam, forming the positive electrode active layer. A membrane impregnated with alkaline electrolyte is disposed between the negative electrode and the positive electrode. The membrane can effectively isolate the positive and negative electrodes, preventing direct contact between the two electrodes, while allowing ions in the electrolyte to migrate through the membrane during charging and discharging, thereby completing ion conduction inside the battery. Preferably, the membrane can be a glass fiber membrane, a cellulose membrane, or a hydrophilic polyolefin membrane, and is fully impregnated in alkaline electrolyte before assembly. The alkaline electrolyte includes potassium hydroxide and may further include zinc oxide and / or zinc acetate to provide the ion-conducting medium required during charging and discharging. During assembly, the copper negative electrode, the separator soaked in electrolyte, and the cobalt positive electrode are stacked in sequence, and an appropriate amount of alkaline electrolyte is added to the inside of the battery to fully wet the separator and the two electrodes before encapsulation, thus obtaining a copper-cobalt secondary battery.
[0033] In this embodiment, both the copper negative electrode and the cobalt positive electrode use nickel foam as the current collector, and metallic copper and cobalt-based oxides are directly loaded onto the surface of the nickel foam to form the electrode structure. Compared with batteries that use traditional metal foil as the current collector, nickel foam has a three-dimensional porous framework structure, which can provide a larger loading space for the active material, which is conducive to the uniform distribution of the active material and enhances the bonding stability between the active layer and the current collector, thereby helping to improve the cycle stability and charge-discharge performance of the copper-cobalt secondary battery.
[0034] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0035] The foregoing has shown and described the basic principles, main features, and advantages of this application. Those skilled in the art should understand that this application is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of this application. Various changes and modifications can be made to this application without departing from the spirit and scope thereof, and all such changes and modifications fall within the scope of the claims of this application.
Claims
1. A method for preparing a copper-cobalt secondary battery with a long cycle life, characterized in that, Includes the following steps: S1. Pre-treat the nickel foam to obtain a nickel foam matrix that meets the requirements for electrode preparation; S2. Using the nickel foam substrate obtained in step S1 as the negative electrode current collector, copper active material is deposited in situ onto the surface of the nickel foam by electrodeposition to prepare a copper negative electrode. S3. Using the nickel foam substrate obtained in step S1 as the positive electrode current collector, a cobalt-based oxide active material is loaded onto the surface of the nickel foam by electrodeposition or hydrothermal method to prepare a cobalt positive electrode. S4. Prepare an alkaline electrolyte and wet the diaphragm with the alkaline electrolyte, and place the treated diaphragm between the copper negative electrode and the cobalt positive electrode. S5. The copper negative electrode prepared in step S2, the separator treated in step S4, and the cobalt positive electrode prepared in step S3 are stacked and assembled in sequence, and the alkaline electrolyte is added to obtain a copper-cobalt secondary battery. In this embodiment, both the copper negative electrode and the cobalt positive electrode use nickel foam as the current collector, and the copper active material and the cobalt-based oxide active material are respectively loaded on the surface of the corresponding nickel foam substrate to form the electrode.
2. The method for preparing a copper-cobalt secondary battery with long cycle life according to claim 1, characterized in that: In step S1, the nickel foam is pretreated as follows: S11, selecting the thickness of 0.2-1.0 mm, the area density of 200-500 g / m 2 , the porosity of 90%-98%, the pore size of 100-500 μm of the nickel foam; S12. Place the nickel foam in an organic solvent in sequence for ultrasonic degreasing; S13. Use pickling solution to remove the oxide layer on the surface of the foamed nickel; S14. Rinse repeatedly with deionized water until neutral; S15. After rinsing with anhydrous ethanol, the material is dried to obtain a clean and activated nickel foam matrix.
3. The method for preparing a copper-cobalt secondary battery with long cycle life according to claim 2, characterized in that: The organic solvent is acetone; The pickling solution is a hydrochloric acid solution; The drying process is either natural drying or oven drying.
4. The method for preparing a copper-cobalt secondary battery with long cycle life according to claim 1, characterized in that: In step S2, copper active material is deposited in situ onto the surface of nickel foam by electrodeposition to prepare a copper anode, as detailed below: S21. Using the nickel foam obtained in step S1 as the cathode and the copper plate as the anode, the copper plate is placed in a copper electrodeposition electrolyte for constant current electrodeposition, so that copper grains are uniformly deposited along the surface of the nickel foam to form a copper active layer covering the surface of the nickel foam. S22. After electroplating, the foamed nickel is removed by rinsing with deionized water and drying, and a copper negative electrode is obtained. The copper electrodeposition electrolyte includes copper sulfate with a concentration of 0.5–2 mol / L and sulfuric acid with a concentration of 0.3–1 mol / L; the current density is 10–50 mA / cm²; and the deposition time is 10–60 min.
5. The method for preparing a copper-cobalt secondary battery with long cycle life according to claim 1, characterized in that: In step S3, a cobalt-based oxide active material is loaded onto the surface of nickel foam by electrodeposition to prepare a cobalt cathode, as detailed below: The cobalt-based oxide active layer is formed by constant current electrodeposition in a cobalt plating solution and heat treatment, wherein the cobalt plating solution comprises 0.1-0.5 mol / L cobalt sulfate and 0.5-1.0 mol / L sulfuric acid, the current density is 10-50 mA / cm 2 , and the electrodeposition time is 10-60 minutes.
6. The method for preparing a copper-cobalt secondary battery with long cycle life according to claim 1, characterized in that: In step S3, a cobalt cathode is prepared by loading a cobalt-based oxide active material onto the surface of nickel foam using a hydrothermal method, as detailed below: Prepare a hydrothermal reaction precursor solution, which includes cobalt nitrate, urea, and ammonium chloride, wherein the concentration of cobalt nitrate is 0.01–0.1 mol / L, the concentration of urea is 0.05–0.5 mol / L, and the concentration of ammonium chloride is 0.05–0.5 mol / L. The nickel foam is immersed in a hydrothermal reactor containing the hydrothermal reaction precursor solution at a hydrothermal temperature of 120–180°C for 4–12 hours. The hydrothermally treated nickel foam is removed, washed with deionized water, vacuum dried at 60–100°C, and then heat-treated in air at 300–500°C for 1–4 hours to obtain a cobalt cathode with nickel foam loaded with cobalt-based oxide.
7. The method for preparing a copper-cobalt secondary battery with long cycle life according to claim 1, characterized in that: The alkaline electrolyte comprises potassium hydroxide and zinc salt, wherein the zinc salt is zinc oxide and / or zinc acetate, and the concentration of potassium hydroxide is 1-6 mol / L and the concentration of zinc salt is 0.1-0.5 mol / L. The separator is made of glass fiber, cellulose, or hydrophilic polyolefin and is used for battery assembly after being completely immersed in the alkaline electrolyte.
8. A copper-cobalt secondary battery, prepared using the method for preparing a copper-cobalt secondary battery with long cycle life as described in any one of claims 1 to 7, characterized in that, The common current collector of the negative and positive electrodes is nickel foam, the negative electrode active material is metallic copper electroplated on nickel foam, and the positive electrode active material is cobalt-based oxide electroplated or hydrothermally deposited on nickel foam. A diaphragm impregnated with electrolyte is provided between the positive and negative electrodes.
9. The copper-cobalt secondary battery according to claim 8, characterized in that: The diaphragm is made of glass fiber, cellulose, or hydrophilic polyolefin, with a thickness of 100–300 μm and a pore size of 0.1–5 μm.
10. The copper-cobalt secondary battery according to claim 8, characterized in that: The cobalt-based oxide is Co3O4, which is directly loaded on the surface of the nickel foam skeleton and forms a tightly bonded positive electrode structure with the nickel foam current collector.