Low-expansion microcellular coated sand and method for preparing the same
By introducing hollow amorphous silica micropowder and a composite system of nano-alumina and nano-silicon carbide into coated sand, and combining it with a silane coupling agent to form a chemical anchoring layer, a microporous system is constructed, which solves the problem of high high-temperature expansion rate of coated sand and improves the high-temperature stability and strength of castings.
Patent Information
- Application Number
- CN202611239423.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-08-17
AI Technical Summary
Existing coated sand has a high expansion rate at high temperatures, which leads to defects such as sand mold cracking and casting veins. Existing technologies cannot effectively reduce its restricted thermal expansion force.
By introducing amorphous silica micropowder with a controllable hollow structure and a composite system of nano-alumina and nano-silicon carbide into coated sand, and combining it with a silane coupling agent to form a chemical anchoring layer on the surface of sand particles, a microporous system is constructed to buffer expansion stress. Nano-silicon carbide and nano-alumina improve the high-temperature stability of the resin layer.
It effectively reduces the restricted thermal expansion force of the coated sand, improves the crack resistance and vein resistance of the casting, and maintains the structural stability and strength of the coated sand.
Smart Images

Figure CN122769372B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of casting molding technology, and in particular to a low-expansion-rate microporous coated sand and its preparation method. Background Technology
[0002] Coated sand is a molding material in which a resin film is coated on the surface of sand grains. It is currently widely prepared using a thermal process. Due to its advantages such as high strength and good dimensional accuracy of castings, it is increasingly used in the production of complex castings such as automobile cylinder blocks, cylinder heads, pipe fittings, and pump bodies. However, silica sand will undergo volume expansion during phase transformation, forming a large confined thermal expansion force. This is the main reason for defects such as sand mold cracking, veins in castings, and sand adhesion, which restricts the surface quality and dimensional accuracy of castings.
[0003] To reduce the high-temperature expansion rate of coated sand, Chinese patent CN121156170A discloses a low-gas-emission, high-heat-resistant coated sand and its preparation method. It uses organopolysilazane resin as the main binder and combines it with carbon nanotube powder to cause the sand mold to undergo a ceramic transformation during the casting stage. However, its fundamental solution is to avoid expansion by changing the material system, which is not a universal solution to the thermal expansion problem of quartz sand. On the other hand, Chinese patent CN110586847B discloses a high-temperature stable coated sand, which uses polylactic acid, lanthanum stearate and other raw materials, combined with the interconnection of nanoparticles, to form a spatial network structure with nanopores inside the coated sand.
[0004] However, the formation of micropores in this scheme depends on thermal decomposition reaction, and the flexibility of its pore size, distribution and porosity control needs to be improved. In the article "Study on the Restricted Thermal Expansion Force of Resin Sand" published in "Foundry", Wan Peng et al. pointed out that the restricted thermal expansion force can comprehensively reflect the expansion of the molding sand itself and its ability to accommodate thermal expansion. It is a key indicator for evaluating the expansion behavior of coated sand. This shows that the key to reducing the high temperature expansion rate of coated sand is not only to suppress the source of expansion, but also to improve the sand mold's ability to accommodate expansion stress under restricted conditions. Summary of the Invention
[0005] The technical problem to be solved by this invention is: how to construct a microporous system with controllable pore characteristics in the resin coating layer of coated sand, so that it can provide a controllable buffer space for expansion stress when the quartz sand undergoes α to β phase transformation expansion, thereby reducing the restricted thermal expansion force of the coated sand. To this end, we propose a low expansion rate microporous coated sand and its preparation method.
[0006] To achieve the above objectives, this application adopts the following technical solution: a low-expansion-rate microporous coated sand, wherein the coated sand is composed of 100 parts aggregate, 0.03-0.8 parts silane coupling agent, 0.37-13 parts expansion stress buffer, 1.2-4.5 parts resin, 8%-18% resin amount of curing agent, 0.1-0.5 parts lubricant, 0.3%-5% resin amount of organic pore-forming agent, and 0.05-0.5 parts short-cut heat-resistant fiber. The expansion stress buffer is a surface-modified composite powder, including 0.3-8 parts amorphous silica micro powder, 0.05-3 parts nano alumina, and 0.02-2 parts nano silicon carbide, wherein at least one of the amorphous silica micro powder and the nano alumina has a hollow structure.
[0007] Preferably, the aggregate is calcined silica sand, the calcination temperature of the calcined silica sand is 850-950℃, the calcination time is 30-90 minutes, and the particle size distribution is that more than 90% of the particles are distributed between 40 mesh and 140 mesh sieves.
[0008] Preferably, the silane coupling agent is selected from one of phenyltrimethoxysilane, diphenyldimethoxysilane, or a compound of phenyltrimethoxysilane and γ-aminopropyltriethoxysilane, wherein the mass ratio of the compound is 1:1 to 3:1.
[0009] Preferably, the curing agent is hexamethylenetetramine; and the lubricant is calcium stearate.
[0010] Preferably, the organic pore-forming agent is selected from one or more of polymethyl methacrylate microspheres, polystyrene microspheres, and azodicarbonamide, with an average particle size of 0.5-10 μm.
[0011] Preferably, the chopped heat-resistant fiber is selected from one or more of aluminum silicate fiber, aluminum borate fiber, and carbon fiber, and the fiber length is 50-200μm.
[0012] Preferably, the hollow amorphous silica micro powder has a particle size of 1-30 μm, a wall thickness of 0.1-2 μm, and a porosity of 30%-70%.
[0013] A method for preparing low-expansion-rate microporous coated sand includes the following steps: S1: heating calcined silica sand to 130-160℃; S2: mixing the preheated calcined silica sand with a diluted silane coupling agent, and stirring and activating the mixture at 130-160℃ for 2-8 minutes to allow the coupling agent to penetrate into the microcracks on the surface of the sand particles to form an anchoring layer; S3: mixing amorphous silica micropowder, nano-alumina, and nano-silicon carbide in a mass ratio of (0.5-5):(0.1-2):(0.5-5). Mix in a ratio of .05-1), add a coupling agent for surface modification, and obtain a surface-modified expansion stress buffer; S4: Add the surface-modified expansion stress buffer and thermoplastic phenolic resin to the sand mixer and mix. After adding the phenolic resin, add an organic pore-forming agent. After the phenolic resin melts and before adding the curing agent, add short-cut heat-resistant fibers. Finally, add the curing agent and lubricant and continue mixing; S5: Discharge, cool, and screen the mixed coated sand to obtain the finished coated sand.
[0014] Preferably, in step S3, the expansion stress buffer undergoes surface modification treatment, and the modifier used is γ-glycidyl etheroxypropyltrimethoxysilane or titanate coupling agent accounting for 0.5%-5% of the mass of the mixed powder.
[0015] Preferably, in step S2, the silane coupling agent is diluted with anhydrous ethanol or isopropanol to a mass fraction of 10%-30% before use.
[0016] The technical effects and advantages of this invention are as follows:
[0017] This invention utilizes a silane coupling agent containing an aromatic ring structure to form a chemical anchoring layer on the surface of sand particles and penetrate into microcracks, thereby suppressing the phase transformation expansion tendency of quartz sand from the interface source. Based on this, a composite system consisting of amorphous silica micropowder, nano-alumina, and nano-silicon carbide with a controllable hollow structure is introduced into the resin coating layer. This hollow structure actively absorbs thermal stress through compression deformation during the α-β phase transformation expansion of quartz sand, reducing the restricted thermal expansion force. Simultaneously, the high-temperature pinning effect of nano-silicon carbide and the reinforcing effect of nano-alumina jointly maintain the structural stability of the resin layer at high temperatures, preventing premature collapse of micropores. Unlike traditional methods that rely on the thermal decomposition of organic pore-forming agents to form micropores, this invention constructs stress buffer spaces using inorganic hollow microspheres, achieving controllable expansion stress without increasing gas generation, thus improving the crack resistance and vein resistance of the coated sand. Attached Figure Description
[0018] The disclosure of this invention is illustrated with reference to the accompanying drawings. It should be understood that the drawings are for illustrative purposes only and are not intended to limit the scope of protection of this invention. In the drawings, the same reference numerals are used to refer to the same parts:
[0019] Figure 1The bar chart shows the reduction rate of limited thermal expansion force in each embodiment and comparative example of Experimental Example 1 of the present invention;
[0020] Figure 2 This is a TEM image of the hollow amorphous silica micropowder in Experimental Example 3 of the present invention. Detailed Implementation
[0021] It is readily understood that, based on the technical solution of this invention, those skilled in the art can propose various interchangeable structural methods and implementations without altering the essential spirit of the invention. Therefore, the following detailed embodiments and accompanying drawings are merely illustrative examples of the technical solution of this invention and should not be considered as the entirety of the invention or as limitations or restrictions on the technical solution of this invention.
[0022] This invention provides a low-expansion-rate microporous coated sand, the components of which are as follows by weight: 100 parts aggregate, 0.03-0.8 parts silane coupling agent, 0.37-13 parts expansion stress buffer, 1.2-4.5 parts resin, 8%-18% resin amount of curing agent, 0.1-0.5 parts lubricant, 0.3%-5% resin amount of organic pore-forming agent, and 0.05-0.5 parts short-cut heat-resistant fiber. The expansion stress buffer is a surface-modified composite powder, comprising 0.3-8 parts amorphous silica micro powder, 0.05-3 parts nano alumina, and 0.02-2 parts nano silicon carbide.
[0023] The aggregate selected is calcined silica sand, which refers to the product of natural silica sand after high-temperature calcination treatment. The calcination temperature is 850℃-950℃ and the calcination time is 30-90 minutes. After calcination treatment, some clay minerals and organic impurities in the silica sand are removed, the microcracks on the surface of the sand particles increase, and the crystal transformation of the silica sand tends to be stable. Its linear expansion coefficient is reduced by 20%-35% compared with uncalcined silica sand. The particle size distribution of calcined silica sand, by mass, is that more than 90% of the particles are distributed between 40 mesh and 140 mesh sieves.
[0024] The silane coupling agent is selected from phenyltrimethoxysilane, diphenyldimethoxysilane, or a compound of phenyltrimethoxysilane and γ-aminopropyltriethoxysilane; the silane coupling agent containing an aromatic ring structure forms Si-O-Si covalent bonds with the sand grain surface after hydrolysis, achieving firm anchoring; its thermal decomposition temperature is ≥350℃; the rigid structure of the aromatic ring gives the self-assembled layer a low coefficient of thermal expansion, inhibiting expansion from the interface source.
[0025] Among them, phenyltrimethoxysilane has the molecular formula C9H. 14 O3Si, with a molecular weight of 198.29 and CAS number 2996-92-1; diphenyldimethoxysilane has the molecular formula C 14 H 16O2Si, with a molecular weight of 244.36 and CAS number 6843-66-9; the mass ratio of the compounded phenyltrimethoxysilane to γ-aminopropyltriethoxysilane is 1:1-3:1.
[0026] The expansion stress buffer is composed of amorphous silica micro powder, nano-alumina and nano-silicon carbide, wherein at least one of the amorphous silica micro powder and the nano-alumina has a hollow structure.
[0027] Among them, the nano-alumina is selected from either α-Al₂O₃ or γ-Al₂O₃ crystal form, with an average particle size of 10-100 nm and a specific surface area ≥50 m². 2 / g; Nano-silicon carbide is selected from either β-SiC (cubic crystal system) or α-SiC (hexagonal crystal system), with an average particle size of 20-150nm and a purity ≥99.0%;
[0028] The preparation method of hollow amorphous silica micropowder is as follows: using polystyrene microspheres with a particle size of 1-30 μm as templates, they are dispersed in an ethanol-water-ammonia aqueous solution of tetraethyl orthosilicate, stirred for 6-12 hours, centrifuged and dried, and finally calcined at 500-600℃ for 2-4 hours to remove the template, thus obtaining hollow silica microspheres; the obtained hollow microspheres have a particle size of 1-30 μm, a wall thickness of 0.1-2 μm, and a porosity of 30%-70%; hollow alumina microspheres are prepared by spray drying: aluminum sol is spray dried in a spray dryer at an inlet temperature of 200-300℃ and an outlet temperature of 100-120℃, and the solid product is collected and then calcined at 500-600℃ for 2 hours to obtain hollow alumina microspheres.
[0029] The resin is a thermoplastic phenolic resin with a softening point of 70-110℃, a flowability of 50-120mm, and a free phenol content of ≤3.0%.
[0030] The curing agent is hexamethylenetetramine, which is used to crosslink and cure the thermoplastic phenolic resin. It can be pre-dissolved in water to prepare a solution with a mass fraction of 30%-50% and then added, or a powdered curing agent can be used directly.
[0031] The lubricant is calcium stearate, used to improve the flowability and release properties of the coated sand.
[0032] The organic pore-forming agent is selected from one or more of polymethyl methacrylate (PMMA) microspheres, polystyrene (PS) microspheres, and azodicarbonamide, and the average particle size of the organic pore-forming agent is 0.5-10 μm.
[0033] The heat-resistant fiber is selected from one or more of aluminum silicate fiber, aluminum borate fiber, and carbon fiber, with a fiber length of 50-200μm. The fiber forms a three-dimensional network structure in the resin layer. When the hollow structure of the expansion stress buffer is compressed to the limit, the fiber can still maintain the structural integrity of the sand core through bridging, preventing the generation and expansion of veins.
[0034] This invention also provides a method for preparing low-expansion-rate microporous coated sand, specifically including the following steps:
[0035] S1: The calcined silica sand is metered by the raw sand feeding system and fed into the heating furnace, where it is heated to 130-160℃ under stirring conditions.
[0036] S2: The preheated calcined silica sand is transported to the sand mixer. The diluted silane coupling agent is evenly sprayed onto the surface of the sand particles through an atomizing spray gun with the assistance of compressed air at 0.2-0.5MPa. The spraying time is controlled at 10-30 seconds. The sand mixer is started and stirred at a speed of 600-1200rpm for 0.5-2 minutes. Under the condition of 130-160℃, the mixture is stirred at a speed of 400-800rpm for 2-8 minutes for activation treatment.
[0037] S3: Mix amorphous silica micro powder, nano alumina and nano silicon carbide in a mass ratio of (0.5-5):(0.1-2):(0.05-1), add coupling agent, and mix in a high-speed mixer at 800-1500 rpm for 5-15 minutes to obtain a surface-modified expansion stress buffer.
[0038] S4: Add the surface-pretreated expansion stress buffer and thermoplastic phenolic resin to the sand mixer, and continue to mix at 600-1200 rpm for 1-4 minutes. Add the organic pore-forming agent 30-60 seconds after adding the phenolic resin. Add the short-cut fibers after the phenolic resin melts and before adding the curing agent. Finally, add the curing agent and lubricant to the sand mixer, and continue to mix at 600-1000 rpm for 0.5-2 minutes.
[0039] S5: The coated sand after mixing and grinding is discharged and sent to a cooler to cool to room temperature. The cooled coated sand is then passed through a 5-10mm screen for impurity removal and a 2-5mm screen for crushing. Finally, it is classified by a vibrating screen to obtain finished coated sand with a particle size distribution of more than 90% of the particles distributed between 40-140 mesh screens. The finished coated sand is then metered and packaged by a packaging machine and put into storage.
[0040] In step S1, if the preheating temperature is below 130°C, the hydrolysis rate of the silane coupling agent is too slow and the penetration is insufficient; if the temperature is above 160°C, the coupling agent may volatilize or condense prematurely, affecting the modification effect.
[0041] Step S2 involves reducing viscosity to facilitate atomization and spraying. Before use, the silane coupling agent is diluted with anhydrous ethanol or isopropanol to a mass fraction of 10%-30%. The viscosity of the diluted coupling agent solution at 25°C is 1-5 mPa·s, which facilitates penetration into the microcracks on the surface of the sand particles. No resin or other components should be added during the activation process to avoid interfering with the direct reaction between the coupling agent and the sand particles. If the activation process is carried out by keeping the temperature constant, it needs to be stirred every 1-2 minutes to prevent local overheating. The activation process allows the coupling agent to penetrate into the microcracks on the surface of the sand particles to a depth of 5-15 μm.
[0042] The chemical mechanism of the activation treatment is as follows:
[0043] Taking phenyltrimethoxysilane as an example, under conditions of 130-160℃, adsorbed water on the surface of sand particles and trace amounts of water vapor in the air first initiate the hydrolysis reaction of the coupling agent, and the methoxy group (-OCH3) hydrolyzes to generate silanol groups (-Si-OH):
[0044]
[0045] Subsequently, the generated silanol groups undergo a condensation reaction with the silanol groups (≡Si-OH) on the surface of the sand particles to form Si-O-Si covalent bonds:
[0046]
[0047] Wherein, ≡Si represents silicon atoms on the surface of the sand grain.
[0048] At the same time, condensation also occurs between adjacent silane molecules, forming a self-assembled monolayer or thin layer of polysiloxane film on the surface of the sand grains, which forms a strong chemical bond with the surface of the sand grains.
[0049] For sealed sand mixers, after the coupling agent is injected and during the activation treatment, a negative pressure of -0.02 to -0.05 MPa can be applied to the inside of the sand mixer and maintained for 1-3 minutes to help the coupling agent penetrate into the deep layers of microcracks.
[0050] In step S3, to improve the dispersibility of the expansion stress buffer in phenolic resin and its interfacial bonding strength with the resin, the expansion stress buffer is pretreated before addition. Amorphous silica micro powder, nano alumina and nano silicon carbide are mixed in proportion, and 0.5%-5% of γ-glycidyl etheroxypropyltrimethoxysilane or titanate coupling agent is added. The mixture is then mixed in a high-speed mixer at 800-1500 rpm for 5-15 minutes to obtain a surface-modified expansion stress buffer.
[0051] In step S4, when adding the expansion stress buffer and phenolic resin, any of the following methods can be used: simultaneous addition, pre-mixing addition, or stepwise addition. When the current of the sand mixer tends to stabilize, it indicates that the resin has completely melted and the powder has been uniformly dispersed. The organic pore-forming agent should be added after the phenolic resin to avoid premature decomposition. The short-cut fibers should be added after the phenolic resin has melted and before the curing agent is added to ensure that the fibers are fully coated by the resin. After adding the curing agent, the current of the sand mixer will show a change peak of first rising and then falling. When the current tends to stabilize, it indicates that the curing reaction is basically completed.
[0052] In step S5, the cooling air volume and cooling time should be automatically adjusted according to the discharge temperature to ensure that the material is fully cooled to room temperature. At the outlet of the impurity removal screen, samples should be taken and tested according to GB / T 2684 standard for indicators such as bending strength and gas generation. Only after passing the test can the material be packaged and stored.
[0053] The core technical principle of this invention can be summarized as a synergistic mechanism integrating interface anchoring, stress buffering, and structural stability:
[0054] First, a silane coupling agent containing an aromatic ring structure forms a stable chemical anchoring layer on the surface of the sand particles. This layer not only improves the interfacial bonding strength between the resin and the sand particles, but also reduces the expansion tendency of the sand particles by penetrating and filling the microcracks in the sand particles.
[0055] Secondly, the expansion stress buffer dispersed in the resin coating layer provides a hollow microporous structure. When the quartz sand undergoes α to β phase transformation expansion at 573℃, the expansion stress is transferred to the resin layer. The hollow structure absorbs the volume increment through compression deformation, reducing the restricted thermal expansion force transferred to the outer surface of the sand core.
[0056] Finally, the high-temperature pinning effect of nano-silicon carbide and the reinforcing effect of nano-alumina work together to maintain the structural stability of the resin layer at high temperatures, prevent the microporous structure from collapsing prematurely, and ensure that the stress buffering function continues to play its role until the later stage of casting.
[0057] The technical solution of the present invention will be described in detail below with reference to specific embodiments. The following embodiments are only used to illustrate the technical solution of the present invention more clearly, and should not be construed as limiting the scope of protection of the present invention. Those skilled in the art should understand that various modifications and changes can be made to the present invention without departing from the technical principles of the present invention, and these modifications and changes should also fall within the scope of protection of the present invention.
[0058] Example 1
[0059] This embodiment provides a low-expansion-rate microporous coated sand, the components of which, by weight, include: 100 parts calcined silica sand, 0.2 parts phenyltrimethoxysilane, 2.0 parts amorphous silica micro powder, 0.5 parts nano alumina, 0.2 parts nano silicon carbide, 2.5 parts thermoplastic phenolic resin, 0.3 parts hexamethylenetetramine, 0.2 parts calcium stearate, 0.075 parts polymethyl methacrylate (PMMA) microspheres, and 0.2 parts aluminum silicate fiber.
[0060] This embodiment also provides a method for preparing low-expansion-rate microporous coated sand, including the following steps:
[0061] S1: The calcined silica sand is fed into a heating furnace and heated to 150°C with stirring.
[0062] S2: The preheated calcined silica sand is fed into a sand mixer. Phenylacetyltrimethoxysilane is diluted with anhydrous ethanol to a mass fraction of 20%, and then sprayed evenly onto the surface of the sand particles through an atomizing spray gun with the assistance of 0.3MPa compressed air for 20 seconds. The sand mixer is started and stirred at 800rpm for 1 minute. At 150℃, the mixture is stirred at 600rpm for 5 minutes for activation treatment.
[0063] S3: Mix amorphous silica micro powder, nano alumina and nano silicon carbide in a certain proportion, add γ-glycidyl etheroxypropyltrimethoxysilane accounting for 2% of the mass of the mixed powder, and mix in a high-speed mixer at 1200 rpm for 10 minutes to obtain a surface-modified expansion stress buffer.
[0064] S4: Add the surface-modified expansion stress buffer and thermoplastic phenolic resin to the sand mixer and mix at 800 rpm. Add PMMA microspheres 45 seconds after adding the phenolic resin. Add aluminum silicate fiber after the phenolic resin melts and before adding the curing agent. The total mixing time is 2.5 minutes. Finally, add hexamethylenetetramine and calcium stearate and continue mixing for 1 minute.
[0065] S5: Discharge the material and send it to the cooler to cool it to below 40℃. Then, it passes through an 8mm impurity removal screen and a 3mm crushing screen in sequence, and is then graded by a vibrating screen to obtain finished coated sand with more than 90% of the particles distributed on a 40-140 mesh screen. The finished product is then packaged and stored.
[0066] Example 2
[0067] This embodiment provides a low-expansion-rate microporous coated sand and its preparation method. The difference from Example 1 is that the silane coupling agent is a compound of phenyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 2:1. The composition includes 3.0 parts of amorphous silica powder, 0.8 parts of nano-alumina, 0.3 parts of nano-silicon carbide, 3.0 parts of thermoplastic phenolic resin, 0.36 parts of hexamethylenetetramine, and 0.25 parts of calcium stearate. In the preparation method, the activation treatment time of S2 is 4 minutes, the mixing time of S4 is 2.5 minutes, and the rest is the same as in Example 1.
[0068] Example 3
[0069] This embodiment provides a low-expansion-rate microporous coated sand and its preparation method. The difference from Embodiment 1 is that 100 parts of calcined silica sand, 0.03 parts of phenyltrimethoxysilane, 0.3 parts of amorphous silica micro powder, 0.05 parts of nano-alumina, 0.02 parts of nano-silicon carbide, 1.2 parts of thermoplastic phenolic resin, 0.096 parts of hexamethylenetetramine, 0.1 parts of calcium stearate, 0.0036 parts of organic pore-forming agent, and 0.05 parts of chopped heat-resistant fiber are used. The rest are the same as in Embodiment 1.
[0070] Example 4
[0071] This embodiment provides a low-expansion-rate microporous coated sand and its preparation method. The difference from Example 1 is that phenyltrimethoxysilane is 0.8 parts; amorphous silica micro powder is 8.0 parts; nano-alumina is 3.0 parts; nano-silicon carbide is 2.0 parts; thermoplastic phenolic resin is 4.5 parts; hexamethylenetetramine is 0.81 parts; calcium stearate is 0.5 parts; organic pore-forming agent is 0.225 parts; chopped heat-resistant fiber is 0.5 parts, and the rest is the same as in Example 1.
[0072] Example 5
[0073] This embodiment provides a low-expansion-rate microporous coated sand and its preparation method. The difference from Embodiment 1 is that in S1, the stirring and heating are carried out to 130°C; in S2, the coupling agent is diluted with anhydrous ethanol to a mass fraction of 10% and sprayed in for 30 seconds; the stirring and mixing time is 0.5 minutes and the rotation speed is 600 rpm; the activation treatment time is 2 minutes and the stirring speed is 400 rpm; in S3, the high-speed mixing time is 5 minutes and the rotation speed is 800 rpm; in S4, the mixing and grinding speed is 600 rpm and the total mixing and grinding time is 1 minute; in S5, the cooling is carried out to room temperature, and the rest is the same as in Embodiment 1.
[0074] Comparative Example 1
[0075] This comparative example provides a low-expansion-rate microporous coated sand and its preparation method. The difference from Example 1 is that the expansion stress buffer, organic pore-forming agent and short-cut heat-resistant fiber are not added to the components. Specifically, it consists of 100 parts calcined silica sand, 0.2 parts phenyltrimethoxysilane, 2.5 parts thermoplastic phenolic resin, 0.3 parts hexamethylenetetramine, and 0.2 parts calcium stearate. In the preparation method, the expansion stress buffer is not prepared. In step S4, thermoplastic phenolic resin is added to the sand mixer and mixed at 800 rpm for 1 minute. Then, hexamethylenetetramine and calcium stearate are added and mixed for another minute. The expansion stress buffer, organic pore-forming agent and short-cut fiber are not added. The remaining steps are the same as in Example 1.
[0076] Comparative Example 2
[0077] This comparative example provides a low-expansion-rate microporous coated sand and its preparation method. The difference from Example 1 is that in step S2, the preheated calcined silica sand is transported to a sand mixer without first spraying a coupling agent. In step S4, undiluted phenyltrimethoxysilane, expansion stress buffer and thermoplastic phenolic resin are added simultaneously and mixed at 800 rpm for 2 minutes. Then, hexamethylenetetramine and calcium stearate are added and mixed for 1 minute. The rest is the same as in Example 1.
[0078] Comparative Example 3
[0079] This comparative example provides a low expansion rate microporous coated sand and its preparation method. The difference from Example 1 is that the amorphous silica micro powder is selected with a solid structure instead of hollow microspheres, while the rest is the same as in Example 1.
[0080] Comparative Example 4
[0081] This comparative example provides a low expansion rate microporous coated sand and its preparation method. The difference from Example 1 is that only hollow amorphous silica micro powder is used, and nano alumina and nano silicon carbide are not added. The rest is the same as Example 1.
[0082] Comparative Example 5
[0083] This comparative example provides a low-expansion-rate microporous coated sand and its preparation method. The difference between this example and Example 1 is that the coupling agent activation treatment and hollow structure are both omitted, while the rest are the same as in Example 1.
[0084] Comparative Example 6
[0085] This comparative example refers to the scheme described in Example 1 of Chinese Patent Application Publication No. CN110586847B. The difference between this example and Example 1 is that the expansion stress buffer is not added, but instead PMMA microspheres with the same particle size and amount as the hollow microspheres in Example 1 are added. The specific composition is 100 parts of calcined silica sand, 0.2 parts of phenyltrimethoxysilane, 2.7 parts of PMMA microspheres, 2.5 parts of thermoplastic phenolic resin, 0.3 parts of hexamethylenetetramine, and 0.2 parts of calcium stearate. Step S3 is omitted. In step S4, the PMMA microspheres and phenolic resin are added to the sand mixer at the same time. The rest is the same as in Example 1.
[0086] The following experimental examples demonstrate the performance testing and comparative analysis of the coated sand samples prepared in the above embodiments and comparative examples.
[0087] Experimental Example 1
[0088] Coated sand samples were prepared according to the formulations and preparation methods of Examples 1-5 and Comparative Examples 1-6, respectively. All samples were prepared using the same batch of calcined silica sand under the same environmental conditions. Three batches of each sample were prepared, and three parallel samples were taken from each batch. The average value of the test results was taken.
[0089] Take 200g of each sample coated sand and prepare Φ50mm×50mm cylindrical specimens using a core shooter under the conditions of sand shooting pressure of 0.4MPa, mold temperature of 220℃, and curing time of 90 seconds. Place the specimens in a rigid constraint mold and heat them from room temperature to 900℃ at a rate of 10℃ / min. Record the pressure and temperature curves, and take the peak pressure as the maximum confined thermal expansion force. Based on the measured value of Comparative Example 1, calculate the reduction rate of each sample relative to Comparative Example 1. Determine the flexural strength using a universal strength testing machine with a loading speed of 0.5mm / min. According to GB / T According to GB / T 2684-2025 "Test Methods for Foundry Sand and Mixtures", the gas evolution was tested by weighing 1.000g ± 0.005g of each sample, heating it at 1000℃ for 3 minutes, and recording the total gas evolution. For the loss on ignition test, 2.000g ± 0.005g of each sample was weighed, ignited in a muffle furnace at 900℃ for 2 hours, cooled, weighed, and the loss on ignition was calculated. The results are shown in Table 1 and... Figure 1 As shown.
[0090]
[0091] As can be seen from Table 1, Comparative Example 1, which did not add an expansion stress buffer, had the highest limited thermal expansion force; Comparative Example 2, which did not undergo coupling agent activation treatment, had a lower expansion force reduction rate than the other examples; Comparative Example 3, which used solid silica, had a limited expansion force reduction rate; Comparative Example 4, which used only single hollow silica, had a reduction rate lower than Example 1; Comparative Example 5, which lacked both activation treatment and a hollow structure, had an expansion force reduction rate close to that of Comparative Example 1; and Comparative Example 6, which used an organic pore-forming agent to replace inorganic hollow microspheres, had a lower expansion force reduction rate than the other examples, and its gas generation was significantly higher.
[0092] All embodiments achieved a reduction in the limited thermal expansion force. The reduction rate of Embodiment 2 was relatively high among the embodiments. Embodiment 3, due to the use of the lower limit of the component, had a relatively low reduction rate, but it was still significantly better than Comparative Example 1. Embodiment 4, using the upper limit of the component, had a higher reduction rate than Embodiment 1. Embodiment 5, using the lower limit of the process parameters, had a slightly lower reduction rate than Embodiment 1, but it was still within an acceptable range. The gas generation of each embodiment was lower than that of Comparative Example 6 and close to that of Comparative Example 1. In terms of bending strength, all embodiments could meet the requirements of conventional casting.
[0093] Experiment Example 2
[0094] Take the coated sand samples from Example 1, Comparative Example 2, and Comparative Example 5. During the preparation process, samples were taken after the S2 activation treatment and before the addition of S4 resin. The sand particles were fixed with epoxy resin by cold mounting, and after grinding and polishing, the distribution of silicon elements on the cross section of the sand particles was detected by SEM combined with EDS. Measurements were taken at 1 μm intervals from the surface to the center, and the depth at which the silicon content dropped to 50% of the surface was recorded as the penetration depth.
[0095] The finished coated sand from Example 1 and Comparative Example 2 were used to determine the bonding strength between the resin layer and the sand particles using the scratch method: the coated sand particles were fixed, and an increasing load was applied to the surface of the resin layer with a diamond indenter. The critical load at peeling was recorded. Ten particles were tested for each sample, and the average value was taken. The results are shown in Table 2.
[0096]
[0097] As can be seen from Table 2, the penetration depth of the coupling agent in Example 1 is significantly greater than that in Comparative Example 2, indicating that the activation treatment helps the coupling agent penetrate into the deep layers of microcracks on the surface of sand particles; the critical peeling load of the resin-sand particle interface in Example 1 is higher than that in Comparative Example 2, indicating that the chemical anchoring layer formed by the activation treatment can improve the interfacial bonding strength.
[0098] Experimental Example 3
[0099] The finished coated sand particles from Example 1 were resin-inserted, ground, and polished. The original morphology of the hollow silica microspheres in the resin coating layer was observed using SEM. Another coated sand from Example 1 was used to prepare cylindrical samples according to the method in Experimental Example 1. The samples were heated to 700°C at 10°C / min in a rigid constraint mold, held for 5 minutes, and then cooled. The sand particles were taken out and the same samples were prepared for observation. The aspect ratios of 100 hollow microspheres before and after heating were statistically analyzed using ImageJ software. The results are shown in Table 3.
[0100] The hollow amorphous silica micropowder used in Example 1 was examined for its microstructure using a transmission electron microscope (TEM). The results are as follows: Figure 2 As shown.
[0101]
[0102] As can be seen from Table 3, in the unheated state, most of the hollow microspheres maintain an approximately spherical shape. After being heated and subjected to constrained compression, the average aspect ratio decreases and the proportion of circular cross-sections decreases, indicating that the hollow microspheres have undergone compressive deformation. At the same time, some microsphere shells rupture. This observation is consistent with the mechanism by which hollow structures absorb thermal stress through compressive deformation.
[0103] Experiment Example 4
[0104] The coated sand samples from Examples 1, 3, and 4 were used to prepare flexural strength test specimens according to GB / T 2684-2025 "Test Methods for Foundry Sand and Mixtures". The test specimens were tested using a high-temperature flexural strength testing machine. The temperature was increased from room temperature to each set temperature point at a rate of 10℃ / min: room temperature, 200℃, 400℃, 600℃, and 800℃. After holding at the temperature for 10 minutes, a load was applied. Five specimens were tested at each temperature point, and the average value was taken. The results are shown in Table 4.
[0105]
[0106] As can be seen from Table 4, the flexural strength of each sample decreased with increasing temperature. At around 600℃, the strength of Example 1 was higher than that of Comparative Example 3 and Comparative Example 4. At 800℃, Example 1 still maintained a certain strength, while the other two samples had lower strength. This indicates that the ternary composite system of Example 1 has better structural stability at high temperatures.
[0107] Experimental Example 5
[0108] The coated sand samples prepared in Example 1 and Comparative Example 6 were heated at 700°C and then cooled. The pore size distribution of the internal pores was determined by mercury porosimetry. The testing instrument was a mercury porosimeter with a pressure range of 0.5-60000 psi and a measurable pore size range of 0.003-360 μm. Each sample was tested three times and the average value was taken. The results are shown in Table 5.
[0109]
[0110] As can be seen from Table 5, the pore size distribution of Example 1 is relatively concentrated, with the most probable pore size being about 5 μm. The pore size distribution of Comparative Example 6 is also relatively concentrated, but its porosity is slightly higher than that of Example 1, and its gas generation is significantly higher. This indicates that the inorganic hollow microsphere route can achieve acceptable porosity under the premise of controlling the gas generation.
[0111] Experimental Example 6
[0112] A fixed amount of calcined silica sand (100 parts), phenyltrimethoxysilane (0.2 parts), thermoplastic phenolic resin (2.5 parts), hexamethylenetetramine (0.3 parts), and calcium stearate (0.2 parts) was used. The total amount of expansion stress buffer was adjusted, and the mass ratio of amorphous SiO2:nano Al2O3:nano SiC was kept constant at 2.0:0.5:0.2. Five gradients were set: 0 parts, 1.0 parts, 2.7 parts, 5.0 parts, and 8.0 parts. Coated sand samples were prepared according to the method of Example 1. The reduction rate of limited thermal expansion force, flexural strength, and gas generation of each sample were tested. The results are shown in Table 6.
[0113]
[0114] As shown in Table 6, with the increase of the amount of expansion stress buffer, the reduction rate of restricted thermal expansion force gradually increases, but the increase slows down after the amount exceeds 2.7 parts; the flexural strength gradually decreases with the increase of the amount added; the gas generation increases slightly with the increase of the amount added; in the range of 1.0-5.0 parts, a balance can be achieved between reducing expansion force and maintaining strength; after the amount added exceeds 5.0 parts, the reduction of expansion force is limited while the strength decreases more significantly.
[0115] Experimental Example 7
[0116] To verify the superiority of the aromatic ring-containing silane coupling agent defined in this invention over conventional coupling agents in reducing constrained thermal expansion forces, the following comparative group was set up:
[0117] The following components were used: 100 parts calcined silica sand, 2.0 parts amorphous silica micro powder, 0.5 parts nano alumina, 0.2 parts nano silicon carbide, 2.5 parts thermoplastic phenolic resin, 0.3 parts hexamethylenetetramine, 0.2 parts calcium stearate, 0.075 parts PMMA microspheres, and 0.2 parts aluminum silicate fiber. Only the type and amount of coupling agent were changed, with the amount of coupling agent always being 0.2 parts: Group A: phenyltrimethoxysilane; Group B: diphenyldimethoxysilane; Group C: γ-aminopropyltriethoxysilane; Group D: γ-glycidoxypropyltrimethoxysilane; Group E: no coupling agent.
[0118] Each group was prepared according to the preparation method of Example 1, and the reduction rate of limited thermal expansion force and flexural strength were tested according to the method of Experimental Example 1. The results are shown in Table 7.
[0119]
[0120] As shown in Table 7, the coupling agent containing aromatic ring structure has a higher rate of reduction in restricted thermal expansion force and higher flexural strength than conventional coupling agents. This indicates that the rigid structure of aromatic ring imparts a low coefficient of thermal expansion to the self-assembled layer, which can more effectively suppress the phase transformation expansion of quartz sand from the interface source.
[0121] Experimental Example 8
[0122] To verify the effectiveness of the coated sand of this invention in actual casting production, a typical flat casting prone to vein defects was selected. Sand cores were made using the coated sand prepared in Example 1, Comparative Example 1, and Comparative Example 6, respectively. Three castings were cast in each group. The casting was a rectangular flat plate, 300 mm long, 150 mm wide, and 15 mm thick. A raised rib 5 mm wide, 3 mm deep, and 300 mm long was provided along the center line of the plate. This structure is prone to vein defects due to thermal expansion of the sand core during the casting process. The casting material was HT250 gray cast iron. The casting surface was required to be free of veins and sand adhesion defects, and the surface roughness Ra≤12.5μm. The casting process was medium-frequency induction furnace melting, casting temperature 1420±10℃, casting speed 3 kg / s. After casting, the casting was naturally cooled to room temperature. After cleaning the sand, the surface defects of the casting were observed. The results are shown in Table 8.
[0123]
[0124] As shown in Table 8, Comparative Example 1 exhibited severe vein and sand adhesion defects, and the sand core cracked during the casting process. Although Comparative Example 6 showed some improvement in vein and sand adhesion, some castings exhibited porosity defects due to excessive gas generation. Example 1 effectively suppressed vein and sand adhesion while not observing porosity defects, had the lowest surface roughness, and its overall casting effect was superior to the two comparative examples.
[0125] The technical scope of this invention is not limited to the content described above. Those skilled in the art can make various modifications and variations to the above embodiments without departing from the technical concept of this invention, and all such modifications and variations should fall within the protection scope of this invention.
Claims
1. A low-expansion-rate microporous coated sand, characterized in that, The coated sand is composed of 100 parts calcined silica sand, 0.03-0.8 parts silane coupling agent, 0.37-13 parts expansion stress buffer, 1.2-4.5 parts resin, 8%-18% resin amount of curing agent, 0.1-0.5 parts lubricant, 0.3%-5% resin amount of organic pore-forming agent, and 0.05-0.5 parts short-cut heat-resistant fiber. The expansion stress buffer is a surface-modified composite powder, including 0.3-8 parts amorphous silica micro powder, 0.05-3 parts nano alumina, and 0.02-2 parts nano silicon carbide, wherein the amorphous silica micro powder has a hollow structure. The silane coupling agent is selected from phenyltrimethoxysilane, diphenyldimethoxysilane, or a compound of phenyltrimethoxysilane and γ-aminopropyltriethoxysilane.
2. The low-expansion-rate microporous coated sand according to claim 1, characterized in that: The roasting temperature of the roasted silica sand is 850-950℃, the roasting time is 30-90 minutes, and the particle size distribution is that more than 90% of the particles are distributed between 40 mesh and 140 mesh sieves.
3. The low-expansion-rate microporous coated sand according to claim 1, characterized in that: In the compound, the mass ratio of phenyltrimethoxysilane to γ-aminopropyltriethoxysilane is 1:1 to 3:
1.
4. The low-expansion-rate microporous coated sand according to claim 1, characterized in that: The curing agent is hexamethylenetetramine; the lubricant is calcium stearate.
5. The low-expansion-rate microporous coated sand according to claim 1, characterized in that: The organic pore-forming agent is selected from one or more of polymethyl methacrylate microspheres, polystyrene microspheres, and azodicarbonamide, with an average particle size of 0.5-10 μm.
6. The low-expansion-rate microporous coated sand according to claim 1, characterized in that: The chopped heat-resistant fiber is selected from one or more of aluminum silicate fiber, aluminum borate fiber, and carbon fiber, and the fiber length is 50-200μm.
7. The low expansion rate microporous coated sand according to claim 1, characterized in that: The hollow amorphous silica micro powder has a particle size of 1-30 μm, a wall thickness of 0.1-2 μm, and a porosity of 30%-70%.
8. A method for preparing low-expansion-rate microporous coated sand as described in any one of claims 1-7, characterized in that, Includes the following steps: S1: Heat the calcined silica sand to 130-160℃; S2: Mix the preheated calcined silica sand with the diluted silane coupling agent, and stir and activate it at 130-160℃ for 2-8 minutes to allow the coupling agent to penetrate into the microcracks on the surface of the sand particles to form an anchoring layer. S3: Mix amorphous silica micro powder, nano alumina and nano silicon carbide in a mass ratio of (0.5-5):(0.1-2):(0.05-1), add a modifier to perform surface modification, and obtain a surface-modified expansion stress buffer. S4: Add the surface-modified expansion stress buffer and thermoplastic phenolic resin to the sand mixer and mix. After adding the phenolic resin, add the organic pore-forming agent. After the phenolic resin melts and before adding the curing agent, add the short-cut heat-resistant fiber. Finally, add the curing agent and lubricant and continue mixing. S5: Discharge, cool, and screen the mixed and milled coated sand to obtain the finished coated sand.
9. The method for preparing low-expansion-rate microporous coated sand according to claim 8, characterized in that: In step S3, the expansion stress buffer undergoes surface modification treatment. The modifier used is γ-glycidyl etheroxypropyltrimethoxysilane or titanate coupling agent, accounting for 0.5%-5% of the mass of the mixed powder.
10. The method for preparing a low-expansion-rate microporous coated sand according to claim 8, characterized in that: In step S2, the silane coupling agent is diluted with anhydrous ethanol or isopropanol to a mass fraction of 10%-30% before use.
Citation Information
Patent Citations
A high-temperature stable coated sand
CN110586847B
Low-gas-forming and high-heat-resistance precoated sand and preparation method thereof
CN121156170A
Low temperature coated particles for use as proppants or in gravel packs, methods for making and using the same.
CN102167969A
Room temperature vulcanized fireproof elastomer plate and preparation method thereof