Highly thermally conductive insulating silicone rubber composite material, preparation method and application thereof

CN122772376APending Publication Date: 2026-09-18GUANGZHOU POWER SUPPLY BUREAU GUANGDONG POWER GRID CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610997730.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-06
Publication Date
2026-09-18

AI Technical Summary

Technical Problem

[0006]有鉴于此,本申请的目的是提供一种高导热绝缘硅橡胶复合材料及其制备方法和应用,用于解决现有填充材料存在的填充量高、柔韧性劣化、导热网络连续性差、导热与绝缘性能难以兼顾等技术问题

Benefits of technology

[0017] In summary, this application provides a high thermal conductivity and insulating silicone rubber composite material, comprising a silicone rubber substrate, polydopamine-coated multi-walled carbon nanotubes, liquid-phase exfoliated boron nitride nanosheets, and graphene oxide. The liquid-phase exfoliated boron nitride nanosheets serve as the dominant thermal framework, with overlapping layers constructing in-plane high thermal conductivity pathways. Graphene oxide acts as an interface control phase; its abundant oxygen-containing functional groups provide numerous interfacial bonding sites, while simultaneously constructing a thermal resistance gradient transition region between the liquid-phase exfoliated boron nitride nanosheets, mitigating the problem of abrupt changes in thermal resistance at the filler interface. The polydopamine-coated multi-walled carbon nanotubes possess numerous amine and phenolic hydroxyl functional groups on their surface, which, through interfacial interactions, preferentially anchor at the oxygen-containing active sites of graphene oxide and the edge defects of the liquid-phase exfoliated boron nitride nanosheets, establishing directional thermally conductive bridges between the two-dimensional sheet-like fillers. Therefore, this application achieves a synergistic breakthrough in low filler content, high thermal conductivity, and electrical insulation performance through the synergistic effect of "polydopamine-coated multi-walled carbon nanotubes, liquid-phase exfoliated boron nitride nanosheets, and graphene oxide."

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122772376A_ABST
    Figure CN122772376A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of insulating material preparation, and particularly discloses a high-thermal-conductivity insulating silicone rubber composite material as well as a preparation method and application thereof. The high-thermal-conductivity insulating silicone rubber composite material is composed of a silicone rubber base material, polydopamine-coated multi-walled carbon nanotubes, liquid-phase-exfoliated boron nitride nanosheets and graphene oxide. The application can build a complete and continuous three-dimensional thermal conduction network only by using a very low filler filling amount, can greatly improve the thermal conductivity coefficient of the composite material, can still maintain the excellent electric insulation characteristics and inherent flexibility and processing performance of the silicone rubber base material, and solves the technical problems of high filling amount, flexibility deterioration, poor continuity of the thermal conduction network, and difficulty in balancing the thermal conduction and insulation performance of the existing filling materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of insulating material preparation technology, and in particular to a high thermal conductivity insulating silicone rubber composite material, its preparation method and application. Background Technology

[0002] Modern electronic devices are rapidly evolving towards higher integration, miniaturization, and higher power density, leading to a dramatic increase in chip-level heat flux density. Thermal management has become a core bottleneck restricting the reliability, lifespan, and energy efficiency of electronic devices. Thermal interface materials, as key functional layers that fill the microscopic gaps between heat sources and heat sinks, eliminate air thermal resistance, and reduce contact thermal resistance, directly determine the success or failure of the overall heat dissipation solution through their thermal conductivity and insulation properties. Silicone rubber, due to its excellent softness and compressibility, wide temperature range stability, chemical corrosion resistance, and intrinsic electrical insulation, is widely recognized as an ideal polymer matrix for thermal interface materials, effectively reducing contact thermal resistance caused by surface roughness between heat sources and heat sinks. However, pure silicone rubber has extremely low intrinsic thermal conductivity (0.16–0.23 W / m·K), resulting in a significant thermal resistance mismatch with metal or ceramic heat sinks, far from meeting the heat dissipation requirements of current high-power electronic devices.

[0003] To improve the thermal conductivity of silicone rubber, existing technologies generally employ a strategy of modification with high thermal conductivity nanofillers. The main technical solutions include: First, using liquid-phase exfoliated boron nitride nanosheets, alumina, silicon carbide, and other ceramic fillers to construct heat transfer channels within the matrix, utilizing their high intrinsic thermal conductivity and good electrical insulation. Second, introducing carbon-based nanofillers such as graphene, graphene oxide, and carbon nanotubes to enhance thermal conductivity through their high thermal conductivity, large specific surface area, and long phonon mean free path. Third, combining different types or dimensions of fillers in binary or multi-component formulations to form hybrid filler systems, attempting to construct a three-dimensional thermally conductive network within the polymer matrix through the synergistic effect between fillers, aiming to achieve higher thermal conductivity with relatively low filler content. While these existing technical solutions have achieved varying degrees of thermal conductivity improvement on a laboratory scale, they essentially still rely primarily on the high volume or mass fraction of fillers to achieve connectivity of heat transfer pathways.

[0004] Currently, existing technical solutions suffer from the following drawbacks. First, single ceramic filler systems require extremely high filler amounts (typically >30wt%) to form a percolation thermally conductive network within the polymer matrix. This leads to a significant increase in the rigidity of the composite material, loss of flexibility, and a dramatic increase in processing viscosity. Furthermore, high-end ceramic fillers such as boron nitride are expensive, severely restricting large-scale application and lightweight design. Second, while single carbon-based fillers possess extremely high intrinsic thermal conductivity, fillers such as carbon nanotubes are prone to agglomeration in the matrix due to π-π interactions, resulting in poor dispersibility. Moreover, their high conductivity causes a sharp decline in the electrical insulation performance of the composite material, failing to meet the stringent requirements for electrical insulation in the cable insulation field. Third, although existing binary or multi-component hybrid filler systems can produce certain synergistic effects, the filler amounts are still generally too high (20–50wt%). Additionally, two-dimensional sheet fillers still exhibit numerous microscopic voids during random stacking, resulting in discontinuous phonon transport paths, high interfacial thermal resistance, and difficulty in achieving a breakthrough improvement in thermal conductivity at low filler amounts. Fourth, high filler loads inevitably damage the unique soft and compressible properties of silicone rubber substrates, leading to increased hardness of cable insulation and sheath, and an increased minimum allowable bending radius, which is not conducive to the laying and coiling of cables in confined spaces. At the same time, the increase in the material's elastic modulus weakens its ability to buffer the mechanical stress of conductor thermal expansion, and is prone to inducing microcracks and interface delamination in the insulation layer under long-term thermal cycling conditions, accelerating insulation aging. In addition, for silicone rubber prefabricated cable accessories (such as stress cones, cold shrink insulation sleeves, etc.), the decrease in flexibility and elastic recovery force will cause insufficient interface pressure, electric field distribution distortion and sealing failure, significantly increasing the risk of partial discharge and moisture intrusion, making them unsuitable for medium and high voltage cable systems, mining mobile cables, drag chain cables and wind power cables, and other scenarios with strict requirements for material flexibility and dynamic fatigue performance.

[0005] To address the technical challenges of existing technologies, such as the significant reduction in material flexibility due to high filler content, poor continuity of the filler thermal conductivity network, and the difficulty in simultaneously achieving thermal conductivity and insulation properties, there is an urgent need for a composite material that can comprehensively solve these problems. Summary of the Invention

[0006] In view of this, the purpose of this application is to provide a high thermal conductivity insulating silicone rubber composite material, its preparation method and application, to solve the technical problems of existing filler materials such as high filler content, deterioration of flexibility, poor continuity of thermal conductive network, and difficulty in balancing thermal conductivity and insulation performance.

[0007] To achieve the above technical objectives, this application provides a high thermal conductivity insulating silicone rubber composite material, comprising the following components in parts by weight: 80-100 parts of silicone rubber substrate; 1-2 parts of polydopamine-coated multi-walled carbon nanotubes; Liquid-phase exfoliation of boron nitride nanosheets, 6-7 parts; 2-3 parts of graphene oxide.

[0008] Furthermore, it includes the following components in parts by mass: 90 parts of silicone rubber substrate; 1-2 parts of polydopamine-coated multi-walled carbon nanotubes; Liquid-phase exfoliation of boron nitride nanosheets, 6-7 parts; Two parts of graphene oxide.

[0009] Furthermore, the silicone rubber substrate comprises silicone rubber and a platinum catalyst, wherein the amount of platinum catalyst added is 0.5% to 1.5% of the mass of the silicone rubber.

[0010] Furthermore, the preparation method of polydopamine-coated multi-walled carbon nanotubes is as follows: multi-walled carbon nanotubes are dispersed in an ethanol aqueous solution, dopamine hydrochloride is added, the pH value is adjusted to 8-9, and the reaction is stirred for 10-14 hours to obtain polydopamine-coated multi-walled carbon nanotubes.

[0011] Furthermore, the mass concentration of multi-walled carbon nanotubes in the ethanol aqueous solution is 1–2 g / L, and the mass concentration of dopamine hydrochloride in the ethanol aqueous solution is 5–6 g / L.

[0012] Furthermore, the preparation method of liquid-phase exfoliated boron nitride nanosheets is as follows: the hexagonal boron nitride dispersion is centrifuged at 2000-2500 rpm for 20-25 min, and the supernatant is collected; the supernatant is centrifuged at 3000-4000 rpm for 15-25 min, the solid product is collected and dried to obtain liquid-phase exfoliated boron nitride nanosheets.

[0013] This application provides a method for preparing a high thermal conductivity insulating silicone rubber composite material, comprising the following steps: Step S1: Dissolve the silicone rubber substrate in an organic solvent to obtain a silicone rubber solution; Step S2: Disperse the liquid-phase exfoliated boron nitride nanosheets, graphene oxide powder, and polydopamine-coated multi-walled carbon nanotube powder in an organic solvent until they are evenly dispersed to obtain a filler dispersion. Step S3: Mix the filler dispersion and silicone rubber liquid evenly, and then cure to obtain a high thermal conductivity insulating silicone rubber composite material.

[0014] Furthermore, the organic solvent includes at least one of tetrahydrofuran, toluene, xylene, and n-hexane.

[0015] Further, in step S1, the mass-to-volume ratio of the silicone rubber substrate to the organic solvent is 1:5 to 6; in step S2, the mass-to-volume ratio of the total mass of the liquid-phase exfoliated boron nitride nanosheets, graphene oxide powder, and polydopamine-coated multi-walled carbon nanotube powder to the organic solvent is 1:80 to 100.

[0016] This application provides an electronic insulating material, including a high thermal conductivity insulating silicone rubber composite material.

[0017] In summary, this application provides a high thermal conductivity and insulating silicone rubber composite material, comprising a silicone rubber substrate, polydopamine-coated multi-walled carbon nanotubes, liquid-phase exfoliated boron nitride nanosheets, and graphene oxide. The liquid-phase exfoliated boron nitride nanosheets serve as the dominant thermal framework, with overlapping layers constructing in-plane high thermal conductivity pathways. Graphene oxide acts as an interface control phase; its abundant oxygen-containing functional groups provide numerous interfacial bonding sites, while simultaneously constructing a thermal resistance gradient transition region between the liquid-phase exfoliated boron nitride nanosheets, mitigating the problem of abrupt changes in thermal resistance at the filler interface. The polydopamine-coated multi-walled carbon nanotubes possess numerous amine and phenolic hydroxyl functional groups on their surface, which, through interfacial interactions, preferentially anchor at the oxygen-containing active sites of graphene oxide and the edge defects of the liquid-phase exfoliated boron nitride nanosheets, establishing directional thermally conductive bridges between the two-dimensional sheet-like fillers. Therefore, this application achieves a synergistic breakthrough in low filler content, high thermal conductivity, and electrical insulation performance through the synergistic effect of "polydopamine-coated multi-walled carbon nanotubes, liquid-phase exfoliated boron nitride nanosheets, and graphene oxide."

[0018] Compared to existing technologies, this invention requires only a very low filler content to construct a complete and continuous three-dimensional thermally conductive network. While significantly improving the thermal conductivity of the composite material, it can still maintain the excellent electrical insulation properties and inherent flexible processing performance of the silicone rubber substrate. It can be adapted to electrical scenarios such as medium and high voltage power cables, flexible cable accessories, mining cables, and new energy cables, and solve the industry's application needs for easy-to-process, long-life, high-performance thermal management insulation materials. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 A schematic diagram of the process flow for the high thermal conductivity insulating silicone rubber composite material provided in the embodiments of this application; Figure 2 This is a schematic diagram of the filler distribution and heat conduction path in silicone rubber. Detailed Implementation

[0021] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. Based on the embodiments in this application specification, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection claimed in this application.

[0022] In the description of this application, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," indicating orientation or positional relationships, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0023] Unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0024] The raw materials used in this invention are not particularly restricted in terms of their source; they can be purchased on the market or prepared using conventional methods known to those skilled in the art.

[0025] This application provides a high thermal conductivity insulating silicone rubber composite material, comprising the following components in parts by weight: 80-100 parts of silicone rubber substrate; 1-2 parts of polydopamine-coated multi-walled carbon nanotubes; Liquid-phase exfoliation of boron nitride nanosheets, 6-7 parts; 2-3 parts of graphene oxide.

[0026] It should be noted that there is a triple mechanism of action inside the composite material: (1) Interface selective anchoring mechanism. Polydopamine is used to coat the surface of multi-walled carbon nanotubes. After modification, the surface of carbon nanotubes is enriched with a large number of amine and phenolic hydroxyl active functional groups, thereby endowing them with specific adsorption and binding ability for oxygen-containing functional groups on the surface of graphene oxide and edge defect sites of boron nitride nanosheets exfoliated in liquid phase; one-dimensional carbon nanotubes are no longer randomly dispersed in the matrix, but are oriented and overlapped at the interface gap between the two types of two-dimensional fillers, realizing controllable interface assembly between fillers, laying the structural foundation for the construction of a continuous thermally conductive network. (2) Thermal resistance gradient construction mechanism. Liquid-phase exfoliated boron nitride nanosheets possess ultra-high intrinsic in-plane thermal conductivity, serving as the main thermally conductive framework to construct an efficient in-plane phonon transport channel; graphene oxide acts as a flexible interface transition phase, optimizing the interfacial compatibility between different types of fillers, and constructing a gradually transitioning thermal resistance hierarchy structure in the interlayer gaps of liquid-phase exfoliated boron nitride nanosheets, significantly reducing phonon scattering loss at the interface, and ensuring stable and continuous heat transfer within the filler system. (3) Low-filling thermal conductivity over-percolation mechanism. Relying on the aforementioned selective anchoring effect of the filler interface, one-dimensional polydopamine-coated multi-walled carbon nanotubes form a large number of thermally conductive bridge points between the mutually separated two-dimensional liquid-phase exfoliated boron nitride nanosheets and graphene oxide sheets, and can build a continuous three-dimensional thermally conductive pathway through the whole under low load conditions of only about 10wt% total filler content. Compared with the traditional single sheet / granular filler system relying on ultra-high filling content to achieve thermal conductivity, this scheme can significantly reduce the filler addition ratio, while improving thermal conductivity and fully preserving the excellent flexibility and electrical insulation properties of the silicone rubber substrate.

[0027] In some embodiments, the components include the following parts by weight: 90 parts of silicone rubber substrate; 1-2 parts of polydopamine-coated multi-walled carbon nanotubes; 6-7 parts of liquid-phase exfoliated boron nitride nanosheets; 2 parts of graphene oxide.

[0028] In some embodiments, the silicone rubber substrate comprises silicone rubber and a platinum catalyst, wherein the amount of platinum catalyst added is 0.5% to 1.5% of the mass of the silicone rubber.

[0029] In some specific embodiments, the raw materials used in this application are: silicone rubber specifically methyl vinyl silicone rubber with a vinyl molar content of 0.25% and a molecular weight of 650,000; and platinum catalyst specifically Karstedt catalyst.

[0030] In some embodiments, the preparation method of polydopamine-coated multi-walled carbon nanotubes is as follows: multi-walled carbon nanotubes are dispersed in an aqueous ethanol solution, dopamine hydrochloride is added, the pH value is adjusted to 8-9, and the reaction is stirred for 10-14 hours to obtain polydopamine-coated multi-walled carbon nanotubes.

[0031] In some preferred embodiments, the mass concentration of multi-walled carbon nanotubes in the aqueous ethanol solution is 1–2 g / L, and the mass concentration of dopamine hydrochloride in the aqueous ethanol solution is 5–6 g / L.

[0032] In some embodiments, the preparation method of liquid-phase exfoliated boron nitride nanosheets is as follows: centrifuge the hexagonal boron nitride dispersion at 2000-2500 rpm for 20-25 min, and collect the supernatant; centrifuge the supernatant at 3000-4000 rpm for 15-25 min, collect the solid product and dry it to obtain liquid-phase exfoliated boron nitride nanosheets.

[0033] This application provides a method for preparing a high thermal conductivity insulating silicone rubber composite material, comprising the following steps: Step S1: Dissolve the silicone rubber substrate in an organic solvent to obtain a silicone rubber solution; Step S2: Disperse the liquid-phase exfoliated boron nitride nanosheets, graphene oxide powder, and polydopamine-coated multi-walled carbon nanotube powder in an organic solvent until they are evenly dispersed to obtain a filler dispersion. Step S3: Mix the filler dispersion and silicone rubber liquid evenly, and then cure to obtain a high thermal conductivity insulating silicone rubber composite material.

[0034] In some embodiments, the organic solvent includes at least one of tetrahydrofuran, toluene, xylene, and n-hexane.

[0035] In some embodiments, in step S1, the mass-to-volume ratio of the silicone rubber substrate to the organic solvent is 1:5 to 6; in step S2, the mass-to-volume ratio of the total mass of the liquid-phase exfoliated boron nitride nanosheets, graphene oxide powder, and polydopamine-coated multi-walled carbon nanotube powder to the organic solvent is 1:80 to 100.

[0036] This application provides an electronic insulating material, including a high thermal conductivity insulating silicone rubber composite material.

[0037] The applicant further provides the following specific embodiments to describe the present invention. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.

[0038] Preparation Example 1

[0039] This preparation example provides a polydopamine-coated multi-walled carbon nanotube (PDA@MWCNT) powder, the preparation method of which includes the following steps: Step S1: Disperse 0.1g of multi-walled carbon nanotubes (MWCNTs) in an ethanol aqueous solution and sonicate for 1 hour to ensure uniform dispersion of MWCNTs, thereby obtaining a MWCNT dispersion; the ethanol aqueous solution is prepared by mixing 50mL of anhydrous ethanol and 40mL of deionized water. Step S2: Add 0.5 g of dopamine hydrochloride (Dopamine·HCl, CAS 62-31-7) to the MWCNT dispersion and stir magnetically for 10 minutes at room temperature; then add Tris buffer solution dropwise to the MWCNT dispersion to adjust the pH to 8.5, thus obtaining the reaction precursor solution; Step S3: The reaction precursor solution is stirred at room temperature for 12 hours. The solid phase is washed several times by centrifugation with deionized water. The solid phase is then dried in a vacuum drying oven at 80°C for 6 hours to obtain PDA@MWCNT powder.

[0040] Preparation Example 2

[0041] This preparation example provides a liquid-phase exfoliated boron nitride nanosheet (BNNS) powder, the processing method of which is as follows: Step S1: 25 mg of hexagonal boron nitride (h-BN) is dispersed in 10 mL of organic solution and sonicated for 2 hours to fully exfoliate and disperse h-BN, thus obtaining an h-BN dispersion; the organic solution is prepared by mixing isopropanol and deionized water in a volume ratio of 3:7. Step S2: Centrifuge the h-BN dispersion at 2100 rpm for 25 minutes, take the supernatant and centrifuge at 3500 rpm for 20 minutes, transfer the solid to a petri dish, and then dry it in an oven at 80°C for 3 hours to obtain BNNS powder.

[0042] Example 1

[0043] See Figure 1 This embodiment provides a method for preparing a high thermal conductivity insulating silicone rubber composite material, including the following steps: Step S1: Dissolve 5g of silicone rubber (specifically methyl vinyl silicone rubber with a vinyl molar content of 0.25% and a molecular weight of 650,000) and 50mg of Karstedt catalyst in 25mL of tetrahydrofuran (THF), and stir to allow the raw silicone rubber to fully swell and dissolve, thereby obtaining a silicone rubber solution. Step S2: The BNNS powder, graphene oxide (GO) powder obtained in Preparation Example 2, and PDA@MWCNT powder obtained in Preparation Example 1 are dispersed in 10 mL of THF and ultrasonically treated for 30 minutes to ensure uniform dispersion of the three fillers, thereby obtaining a filler dispersion; wherein the mass ratio of BNNS powder, GO powder, and PDA@MWCNT powder is 1.6:6.4:2. Step S3: The filler dispersion is added to the silicone rubber solution and magnetically stirred at room temperature for 1 hour, followed by ultrasonic treatment for 2 hours to ensure that the filler is uniformly dispersed in the silicone rubber solution, thus obtaining a composite solution; the total mass ratio of BNNS powder, GO powder and PDA@MWCNT powder to the raw silicone rubber is 1:9. Step S4: The composite adhesive liquid is poured into a polytetrafluoroethylene (PTFE) petri dish and left to stand overnight at room temperature to allow the solvent to fully evaporate, thus obtaining a pre-cured adhesive film. The pre-cured adhesive film is placed in a vacuum oven and cured at 175°C for 2 hours, followed by a post-curing at 200°C for 2 hours. After natural cooling and demolding, a high thermal conductivity insulating silicone rubber composite material is obtained.

[0044] Comparative Example 1

[0045] This comparative example provides a method for preparing a high thermal conductivity insulating silicone rubber composite material. The difference from Example 1 is that graphene oxide is replaced by reduced graphene oxide (rGO) in equal amounts.

[0046] The preparation method of reduced graphene oxide (rGO) is as follows: 5g of GO is dispersed in 500mL of deionized water, 5mL of hydrazine hydrate is added, and the reaction is carried out at 95°C for 24h. The solid phase is then dried to obtain rGO.

[0047] Comparative Example 2

[0048] This comparative example provides a method for preparing a high thermal conductivity insulating silicone rubber composite material. The difference from Example 1 is that graphene oxide is replaced in equal amounts with silane-modified graphene oxide (mGO).

[0049] The preparation method of silane-modified graphene oxide (mGO) is as follows: 1 g of GO is dispersed in 200 mL of ethanol aqueous solution, 2 mL of 3-aminopropyltriethoxysilane (APTES) is added, and the mixture is refluxed at 70°C for 12 h. The solid phase is then dried to obtain mGO. The ethanol aqueous solution is obtained by mixing ethanol and deionized water in a 1:1 volume ratio.

[0050] Comparative Example 3

[0051] This comparative example provides a method for preparing a high thermal conductivity insulating silicone rubber composite material. The difference from Example 1 is that graphene oxide is replaced by an equal amount of fluorinated graphene oxide (FGO).

[0052] The preparation method of fluorinated graphene oxide (FGO) is as follows: 1g of GO is placed in a mixed gas composed of fluorine and nitrogen, and reacted at 150°C for 6h to obtain FGO. The volume ratio of fluorine to nitrogen in the mixed gas is 1:9.

[0053] Comparative Example 4

[0054] This comparative example provides a method for preparing a high thermal conductivity insulating silicone rubber composite material, which differs from Example 1 in that graphene oxide is replaced by molybdenum disulfide in equal amounts.

[0055] Table 1. Comparison of process parameters and performance of high thermal conductivity insulating silicone rubber composite materials

[0056] As shown in Table 1, reduction-modified graphene oxide, silane-grafted graphene oxide, and fluorinated graphene oxide all physically degrade the overall performance of the filler. When graphene oxide is treated with reduction modification, the carbon conjugated skeleton of the material is repaired, and the conductivity is greatly improved, resulting in a significant decrease in the insulation performance of the composite insulating material. If silane is used to graft and modify the filler surface, a low thermal conductivity organic layer will be coated on the filler surface, forming a phonon scattering barrier, which greatly increases the interfacial thermal resistance and weakens the heat transfer efficiency. This invention relies on the synergistic mechanism of the filler interface to retain a large number of oxygen-containing functional groups on the surface of graphene oxide sheets, using them as active anchoring points for constructing a highly efficient thermally conductive network. The native oxygen-containing functional groups on the surface can form a high-strength synergistic interface with polydopamine-modified carbon nanotubes through hydrogen bonding, allowing the polydopamine-coated multi-walled carbon nanotubes to act as nanobridge structures, efficiently connecting liquid-phase exfoliated boron nitride nanosheets and graphene oxide. Through the tight interfacial contact between one-dimensional carbon nanotubes and two-dimensional graphene oxide sheets, a low-loss phonon conduction pathway is established, achieving highly efficient thermal conductivity. This invention abandons redundant filler surface modification processes and adopts an interface synergistic self-assembly strategy, maximizing the thermal conductivity of the composite material under extremely low filler loading conditions.

[0057] Compared with existing technologies, this invention achieves a synergistic breakthrough in the field of silicone rubber thermal conductivity modification, characterized by low filler content, high thermal conductivity, and electrical insulation properties. See also... Figure 2 The diagram shows the filler distribution and heat conduction path in silicone rubber. In existing technologies, a single ceramic filler system requires a filling amount exceeding 30 wt% to form a percolation thermal conductivity network, resulting in increased material rigidity, processing difficulties, and high costs. While single carbon-based fillers offer excellent thermal conductivity, their high electrical conductivity prevents them from meeting electrical insulation requirements. Although binary mixed filler systems can produce a certain synergistic effect, the filling amount is generally still too high, and the microscopic voids generated by the stacking of two-dimensional sheet fillers cause discontinuous phonon transport paths, making it difficult to achieve a substantial improvement in thermal conductivity at low filling amounts. This invention constructs a three-dimensional continuous thermal conductivity network with a total filler load of only 10 wt%, achieving a composite material thermal conductivity of 0.743 W / m·K, an improvement of 223% compared to pure silicone rubber.

[0058] Furthermore, this invention effectively avoids the damage to the soft and compressible properties of the silicone rubber substrate caused by high filler load through a low filler content design. In existing technologies, high filler content leads to material hardening, increasing the minimum permissible bending radius of the cable insulation and sheath, which is detrimental to laying and coiling in confined spaces. It also weakens the material's ability to buffer the mechanical stress of conductor thermal expansion, easily inducing microcracks and interface delamination in the insulation layer under long-term thermal cycling conditions. This invention improves thermal conductivity while maintaining the excellent flexibility and elastic recovery of the silicone rubber substrate with a total filler load of only 10 wt%, making it suitable for medium and high voltage cable systems, flexible cable accessories, mining mobile cables, and wind power cables—applications with strict requirements for material flexibility and dynamic fatigue performance. Simultaneously, the low filler content reduces the proportion of high-end ceramic fillers such as boron nitride. By introducing a small amount of relatively economical polydopamine-coated multi-walled carbon nanotubes to replace some of the expensive graphene oxide, performance is improved while maintaining cost-effectiveness.

[0059] The above are merely preferred embodiments of this application and are not intended to limit the present invention. Although this application has been described in detail with reference to examples, those skilled in the art can still modify the technical solutions described in the foregoing examples or make equivalent substitutions for some of the technical features. However, any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A high thermal conductivity insulating silicone rubber composite material, characterized in that, The components include the following parts by mass: 80-100 parts of silicone rubber substrate; 1-2 parts of polydopamine-coated multi-walled carbon nanotubes; Liquid-phase exfoliation of boron nitride nanosheets, 6-7 parts; 2-3 parts of graphene oxide.

2. The high thermal conductivity insulating silicone rubber composite material according to claim 1, characterized in that, The components include the following parts by mass: 90 parts of silicone rubber substrate; 1-2 parts of polydopamine-coated multi-walled carbon nanotubes; Liquid-phase exfoliation of boron nitride nanosheets, 6-7 parts; Two parts of graphene oxide.

3. The high thermal conductivity insulating silicone rubber composite material according to claim 1 or 2, characterized in that, The silicone rubber substrate comprises silicone rubber and a platinum catalyst, wherein the amount of platinum catalyst added is 0.5% to 1.5% of the mass of the silicone rubber.

4. The high thermal conductivity insulating silicone rubber composite material according to claim 1 or 2, characterized in that, The preparation method of the polydopamine-coated multi-walled carbon nanotubes is as follows: multi-walled carbon nanotubes are dispersed in an ethanol aqueous solution, dopamine hydrochloride is added, the pH value is adjusted to 8-9, and the reaction is stirred for 10-14 hours to obtain polydopamine-coated multi-walled carbon nanotubes.

5. The high thermal conductivity insulating silicone rubber composite material according to claim 4, characterized in that, The mass concentration of the multi-walled carbon nanotubes in the ethanol aqueous solution is 1-2 g / L, and the mass concentration of the dopamine hydrochloride in the ethanol aqueous solution is 5-6 g / L.

6. The high thermal conductivity insulating silicone rubber composite material according to claim 1 or 2, characterized in that, The method for preparing the liquid-phase exfoliated boron nitride nanosheets is as follows: The hexagonal boron nitride dispersion was centrifuged at 2000–2500 rpm for 20–25 min, and the supernatant was collected. The supernatant was then centrifuged at 3000–4000 rpm for 15–25 min, and the solid product was collected and dried to obtain liquid-phase exfoliated boron nitride nanosheets.

7. A method for preparing a high thermal conductivity insulating silicone rubber composite material according to any one of claims 1 to 6, characterized in that, Includes the following steps: Step S1: Dissolve the silicone rubber substrate in an organic solvent to obtain a silicone rubber solution; Step S2: Disperse the liquid-phase exfoliated boron nitride nanosheets, graphene oxide powder, and polydopamine-coated multi-walled carbon nanotube powder in an organic solvent until they are evenly dispersed to obtain a filler dispersion. Step S3: Mix the filler dispersion and silicone rubber liquid evenly, and then cure to obtain a high thermal conductivity insulating silicone rubber composite material.

8. The method for preparing the high thermal conductivity insulating silicone rubber composite material according to claim 7, characterized in that, The organic solvent includes at least one of tetrahydrofuran, toluene, xylene, and n-hexane.

9. The method for preparing the high thermal conductivity insulating silicone rubber composite material according to claim 7, characterized in that: In step S1, the mass-to-volume ratio of the silicone rubber substrate to the organic solvent is 1:5-6. In step S2, the total mass ratio of the liquid-phase exfoliated boron nitride nanosheets, graphene oxide powder, and polydopamine-coated multi-walled carbon nanotube powder to the organic solvent is 1:80-100.

10. An electronic insulating material, characterized in that, It includes the high thermal conductivity insulating silicone rubber composite material according to any one of claims 1 to 6, or the high thermal conductivity insulating silicone rubber composite material obtained by the preparation method of any one of claims 7 to 9.