Method for high-purity antimony based on metal medium alloying synergistic zone melting
Patent Information
- Application Number
- CN202611252364.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-09-25
AI Technical Summary
然而,砷的分配系数接近于1,很难通过区域熔炼直接脱除
[0025]本发明提供了一种基于金属介质合金化协同区域熔炼高纯锑的方法。具备以下有益效果:
Smart Images

Figure CN122811543A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-purity metal preparation technology, specifically a method for high-purity antimony based on metal-medium alloying and synergistic zone melting. Background Technology
[0002] High-purity antimony (purity ≥ 99.999%, i.e., 5N grade and above) is an indispensable key raw material in semiconductor doping, infrared detectors, thermoelectric power generation materials, and the military industry. Currently, the preparation methods for high-purity antimony of 5N grade and above mainly fall into two categories: physical methods and chemical methods.
[0003] Among physical methods, vacuum distillation and zone melting are the most common. Vacuum distillation has advantages such as a short process, no chemical reagents, and no emissions of waste. However, it is limited by the fact that arsenic and antimony are adjacent elements in Group VA of the periodic table, and their highly similar physicochemical properties result in vapor pressure curves that are very close at conventional distillation temperatures, meaning vacuum distillation can only achieve a purity of 3-4N. Zone melting is one of the most effective methods for purifying and preparing ultra-high purity impurities, and it has a good removal effect on most impurities with a partition coefficient not equal to 1. However, arsenic has a partition coefficient close to 1, making it difficult to remove directly by zone melting. Therefore, although traditional zone melting can achieve a purity of 3-4N for antimony, it is limited by the removal of arsenic and cannot reach the 5N standard.
[0004] While chemical methods can achieve high purity, they typically involve long processes, low product recovery rates, require the use of hazardous chemicals such as chlorine or ammonia, and generate large amounts of hydrochloric acid and waste liquid, resulting in significant environmental pressure.
[0005] Therefore, there is an urgent need to develop a clean preparation method that can break through the efficiency limit of As removal in traditional zone smelting, has a short process, low pollution, and is suitable for directly preparing high-purity antimony of grade 5N or above from 3N antimony. Summary of the Invention
[0006] Technical problems to be solved
[0007] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for preparing high-purity antimony of 5N and above by adding a metallic medium to crude antimony to create a compound, followed by synergistic zone melting. This invention addresses the fundamental problem of the difficulty in removing As (As) in traditional zone melting due to its partition coefficient being close to 1. By adding a specific metallic medium Me to 3N antimony, the key impurity As is transformed into an easily segregated alloy compound Me. x As y Then, by utilizing the directional solidification characteristics of zone melting, As-containing compounds are enriched, migrated, and removed along the liquidus line, thereby achieving a short-process clean preparation of high-purity antimony from 3N to 5N grade and above.
[0008] Technical solution
[0009] To achieve the above objectives, the present invention provides the following technical solution: a method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting, comprising the following steps: Step 1: Raw Material Preparation Using industrial-grade antimony with a purity of 99.9% (3N) as raw material, antimony ingots are crushed into particles or small pieces with a particle size of 1~10mm and placed in an inert atmosphere for later use.
[0010] Step 2: Add a metallic medium to crude antimony to create a compound: A metallic medium Me is added to the 3N antimony obtained in step one. The metallic medium Me is one or more combinations of Al and Cu. The amount of metallic medium Me added is 0.05% to 2.0% of the mass of the 3N antimony. 3N antimony and metallic medium Me are placed in a melting furnace under inert gas protection and heated to 650~850℃, held for 30~120min, so that metallic medium Me reacts fully with As impurities in antimony to form a high-melting-point alloy compound Me. x As y The high-melting-point alloy compound includes one or more of AlAs, Cu3As, and Cu5As2. The alloying reaction is carried out under the protection of inert gases such as Ar and N2.
[0011] Step 3: Directional solidification of ingots: The alloyed melt obtained in step two is cast into antimony ingots. The cooling rate is controlled to allow As compounds to be initially enriched at the tail of the ingot, thus obtaining alloyed pretreated antimony ingots.
[0012] Step 4: Zone smelting and purification The alloyed pretreated antimony ingots obtained in step three are placed in a quartz boat or graphite boat in a zone melting device and zone melted under a vacuum or inert gas protective atmosphere. The process parameters for zone melting are controlled as follows: Melting zone temperature: 630~750℃, the melting zone temperature is higher than the melting point of antimony, which is 630.5℃; Zone melting rate: 0.1~5 mm / min; Melting zone length: 10~30 mm; Number of zone melting cycles: 5~30; Protective atmosphere: High-purity Ar / H2 atmosphere; In particular, during the zone melting process, the high-melting-point alloy compound Me x As y Segregation occurs at the solid-liquid interface, and the antimony ingot is enriched and migrates along the liquidus line to the tail end of the antimony ingot.
[0013] Step 5: Cut off the head and tail: After zone melting is completed, the ingot is cooled to room temperature, and the section at the tail end of the ingot that is rich in impurities is removed (the length of the tail end removed is 10% to 30% of the total length of the ingot). A small section at the head is also removed as needed to obtain a high-purity antimony product of grade 5N or above.
[0014] Step 6: Repeat zone melting: The high-purity antimony obtained in step five is subjected to zone melting 1 to 3 times again as in step four to improve its purity.
[0015] Preferably, the metallic medium Me is Al, and the amount of Al added is 0.05% to 0.5% of the mass of 3N antimony.
[0016] Preferably, the metal medium Me is a composite addition of Al and Cu, with a mass ratio of Al to Cu of 1:0.5~2.
[0017] Preferably, the alloying treatment temperature is 680~780℃, and the holding time is 45~90min.
[0018] Preferably, the zone melting rate is 1~3 mm / min, and the number of zone melting cycles is 8~20.
[0019] Preferably, the zone melting is carried out in a horizontal zone melting device, and either induction heating or resistance heating can be used.
[0020] Preferably, after the alloying reaction in step two, a slag removal step is also included to remove the As-containing slag phase floating on the surface of the melt.
[0021] Working Principle: The fundamental reason why traditional zone melting struggles to remove As (As) is that the partition coefficient of As in antimony is approximately 1, meaning that the solubility of As in the solid and liquid phases is similar, making effective segregation of As difficult during directional solidification. This invention addresses this by adding a specific metallic medium, Me (such as Al or Cu), to the antimony melt. Utilizing the strong chemical affinity between Me and As, As is transformed from its free state dissolved in antimony into a high-melting-point alloy compound, Me. x As y Taking the addition of Al as an example, Al reacts with As to form AlAs; when Cu is added, Cu3As or Cu5As2 is formed.
[0022] These alloy compounds have the following key characteristics: (1) their melting point is much higher than that of antimony (AlAs melting point exceeds 1700℃, Cu3As melting point is about 850℃), and they exist in solid particle form at zone melting temperature; (2) their solubility in antimony melt is extremely low, and they have a strong tendency to segregate; (3) their density differs from that of antimony melt, and they are easily repelled by the solid-liquid interface and enriched in the liquid phase during solidification.
[0023] Therefore, during subsequent zone melting, these As-containing compounds are effectively repelled at the solid-liquid interface and migrate continuously along the liquidus direction as the melting zone moves, eventually accumulating at the tail of the antimony ingot. Deep removal of As can be achieved by cutting off the tail. Studies have shown that adding Al can increase the removal rate of As impurities in antimony from 67.27% to 83.24%. By optimizing the type and amount of metal medium, the alloying process, and the synergistic control of zone melting parameters, deep removal of As impurities from the 3N level to levels above 5N can be achieved.
[0024] Beneficial effects
[0025] This invention provides a method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting. It has the following beneficial effects: 1. This invention provides a method for high-purity antimony based on metal-medium alloying and synergistic zone melting, overcoming the limitations of traditional zone melting for As removal: Traditional zone melting cannot effectively remove As- due to the As distribution coefficient K≈1. This invention transforms As into easily segregated compounds through alloying, substantially changing the effective As distribution coefficient and breaking through the limits of traditional zone melting technology for As removal efficiency. It can directly produce high-purity antimony of 5N grade and above from 3N antimony. This invention requires only two core processes: "alloying treatment + zone melting," significantly shortening the process compared to the multi-step purification process of traditional chemical methods, resulting in a shorter production cycle and suitability for large-scale production.
[0026] 2. This invention provides a method for high-purity antimony smelting based on metal medium alloying and synergistic zone melting. The entire process is carried out under vacuum or inert atmosphere, without using hazardous chemicals such as chlorine and ammonia, and without generating acidic or heavy metal-containing waste liquid, making it environmentally friendly. During the zone melting process, there is almost no loss of the antimony matrix, the amount of metal medium Me added is extremely small (0.05%~2.0%), and it can be centrally recovered by tail cutting, resulting in a high overall recovery rate.
[0027] 3. This invention provides a method for high-purity antimony based on metal medium alloying and zone melting. By controlling multiple parameters such as the type and amount of metal medium, alloying temperature and time, and zone melting rate and number of times, the efficiency of As removal can be precisely controlled to adapt to the requirements of raw materials and products with different purity. The equipment used is a conventional melting furnace and zone melting device, which does not require special high-end equipment, requires less investment, and is easy to promote industrially. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the process for preparing high-purity antimony of grade 5N or higher according to the present invention; Figure 2 This is a schematic diagram of the physical structure of the present invention. Detailed Implementation
[0029] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0030] (1) Take 2 kg of 3N industrial grade antimony ingots and crush them into particles with a diameter of about 5 mm; (2) Add 5g of metallic Al powder with a purity ≥99.9999% (addition amount 0.05wt%) to the antimony particles, mix evenly and place in a vacuum melting furnace; (3) Evacuate to a vacuum degree of 10 Pa, raise the temperature to 700 °C at 10 °C / min, and keep it at that temperature for 60 min to allow Al and As to react fully to form AlAs-; (4) Cast the alloyed melt into antimony ingots and allow them to cool naturally; (5) Place the antimony ingot in the quartz boat of the horizontal melting device, evacuate to ≤10-2 Pa and then introduce argon protective gas, use resistance heating to form a melting zone, control the temperature of the melting zone at 720~730℃, and the length of the melting zone is 20mm. (6) Perform zone melting at a rate of 1 mm / min, and repeat the zone melting 15 times; (7) After zone melting is completed, cool to room temperature and cut off about 25% of the tail section to obtain a high-purity antimony product of grade 5N or above, with a purity of ≥99.9999% and an As content of <0.1ppm. Example 2
[0031] (1) Take 5 kg of 3N industrial grade antimony ingots and crush them into particles with a diameter of about 3 mm; (2) Add 30g of metallic Cu powder (0.3wt%) to the antimony particles, mix evenly, and place in a smelting furnace under Ar atmosphere protection; (3) Heat to 750℃ and keep warm for 90 min to allow Cu to react with As to generate Cu3As and Cu5As2; (4) Cast the alloyed melt into antimony ingots; (5) Place the antimony ingot in a zone melting device and carry out zone melting under an argon protective atmosphere. The temperature of the melting zone is controlled at 700~710℃, the length of the melting zone is 15mm, and the melting is carried out 20 times at a rate of 1.5mm / min. (6) After cooling, about 20% of the tail section is removed to obtain a high-purity antimony product of grade 5N or above. Example 3
[0032] (1) Take 10 kg of 3N industrial grade antimony ingots and crush them into particles with a diameter of about 8 mm; (2) Add 10g of metallic Al powder and 10g of metallic Cu powder to the antimony particles (compound addition, total addition amount 0.2wt%, Al:Cu=1:1). (3) Evacuate to a vacuum degree of 5 Pa and introduce argon gas for protection, heat to 720℃, and keep warm for 75 min to allow Al, Cu and As to react to generate AlAs, Cu3As and other composite compounds. (4) Cast the alloyed melt into antimony ingots; (5) Place the antimony ingot in the zone smelting apparatus and evacuate it to ≤10 -2 Pa was introduced and high-purity nitrogen was introduced for protection, and the zone was melted 20 times at a rate of 3 mm / min; (6) After cooling, about 30% of the tail section is cut off to obtain a high-purity antimony product of grade 5N or above.
[0033] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing high-purity antimony of grade 5N or higher based on alloying synergistic zone melting, characterized in that, Includes the following steps: Step (1) Use 3N industrial grade antimony as raw material and crush it into particles; Step (2) Add a metallic medium Me to 3N antimony, wherein the metallic medium Me is one or more of Al, Cu, and Mn, and the amount added is 0.05% to 2.0% of the mass of 3N antimony; Step (3) Under vacuum or inert gas protection, heat 3N antimony and metallic medium Me to 650~850℃ and hold for 30~120min to allow the metallic medium Me to react with the As impurities in antimony to form a high-melting-point alloy compound Me. x As y ; Step (4) Cast the alloyed melt into antimony ingots; Step (5) Place the antimony ingot in a zone melting device and carry out zone melting under inert gas protection. The zone melting temperature is 630~750℃, the zone melting rate is 0.5~5mm / min, the melting zone length is 10~30mm, and the number of zone meltings is 5~30. After the zone melting in step (6) is completed and cooled, the section of the antimony ingot with impurities accumulated at the tail is cut off to obtain high-purity antimony of grade 5N or above.
2. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The metallic medium Me is Al, and the amount of Al added is 0.05% to 0.5% of the mass of 3N antimony.
3. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The metallic medium Me is a composite addition of Al and Cu, with a mass ratio of Al to Cu of 1:0.5~2.
4. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The high-melting-point alloy compound MexAsy includes one or more of AlAs, Cu3As, and Cu5As2.
5. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The alloying treatment in step (3) is carried out at a temperature of 680~780℃ and a holding time of 45~90min.
6. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The melting rate in step (5) is 13 mm / min, and the number of melting cycles is 8-20.
7. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The zone melting described in step (5) is carried out in a high-purity Ar atmosphere.
8. The method for high-purity antimony smelting based on metal-medium alloying and synergistic zone melting according to claim 1, characterized in that: The length of the tail section cut off in step (6) is 10% to 30% of the total length of the antimony ingot.