A silicon isotope separation system and method capable of reducing side reactions

By employing negative pressure operation and adding low-boiling-point components in the silicon isotope separation system, the problem of side reactions at high temperatures was solved, enabling efficient separation and continuous production of high-purity silicon-28 isotopes, and reducing energy consumption and operating costs.

CN122828548BActive Publication Date: 2026-11-24TIANJIN TIANHESHENG NEW MATERIAL TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611340521.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-24
Estimated Expiration
2046-09-01

AI Technical Summary

Technical Problem

Existing chemical exchange methods for silicon isotope separation are prone to side reactions under high-temperature conditions, affecting product purity and equipment stability, making it difficult to achieve industrial production of high-purity silicon-28 isotopes.

Method used

By controlling the absolute pressure of the pyrolysis tower within a negative pressure range of 0.05 to 0.7 atm, and combining this with the addition of low-boiling-point components to lower the decomposition temperature, a synergistic approach of multi-stage chemical exchange and negative pressure decomposition is adopted to suppress the occurrence of side reactions.

Benefits of technology

It significantly reduced the probability of side reactions, improved the purity and abundance of silicon-28 isotopes, extended the service life of complexing agents, reduced energy consumption and operating costs, and achieved efficient silicon isotope separation and continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122828548B_ABST
    Figure CN122828548B_ABST
Patent Text Reader

Abstract

This application provides a silicon isotope separation system and method that can reduce side reactions, belonging to the field of isotope separation technology. It includes: a feed tower for inputting complexing agent raw materials and naturally abundant silicon tetrafluoride gas, mixing them, and causing a complexation reaction; a multi-stage exchange tower; a cracking tower for receiving the complexed reactants output from the final exchange tower and performing thermal decomposition; a purification tower for receiving the complexing agent mixture from the bottom outlet of the cracking tower, with the purified, lean solvent of the complexing agent being collected at the upper outlet of the purification tower; a complexing tower for receiving the lean solvent of the complexing agent from the purification tower and the silicon tetrafluoride gas input from the front-end exchange tower; and a negative pressure device connected to the top branch of the cracking tower via a gas-liquid separator. This application effectively suppresses side reactions under high-temperature conditions and improves the abundance of silicon-28 isotope products by controlling the absolute pressure of the cracking tower within a negative pressure range of 0.05 to 0.7 atm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of isotope separation technology, specifically to a silicon isotope separation system and method that can reduce side reactions. Background Technology

[0002] Silicon 28 ( 28 Si, as a stable isotope of silicon, possesses irreplaceable value in high-tech fields due to its zero nuclear spin, few lattice defects, and excellent thermal conductivity. In the semiconductor and microelectronics fields, high abundance... 28 Silicon (Si) is a core material for fabricating high-performance processors, power devices, and silicon-based integrated optical circuits. In the field of quantum computing, its spinless nature prevents interference with the coherence of qubits, making it a key material for building large-scale silicon-based quantum computers. Meanwhile, high-purity silicon... 28 Si is also used in metrology research, such as the precise determination of Avogadro's constant, as well as in cutting-edge applications such as ultrasensitive sensors and nuclear physics detection materials.

[0003] Currently, both domestically and internationally, [this has been achieved] 28 The main methods for separating Si include gas centrifugal cascade methods (using SiF4 or SiHCl3 as the medium), low-temperature distillation methods (SiH4, SiCl4, SiF4, or SiH3CH3 systems), laser methods (Si2F6, SiF4), and chemical exchange methods (separation systems of SiF4 with different complexing agents). Among these, the chemical exchange method is based on... 28 The more stable properties of the complexes formed by Si and the complexing agent are achieved through a complexation-distillation-pyrolysis cycle. 28 The enrichment of Si, with a large separation factor and regenerable complexing agent, has become the most promising method for the industrial separation of silicon isotopes.

[0004] CN105664718A discloses a multi-tower series separation process for enrichment production. 28 Si、 29 Si and 30 The Si method and its apparatus involve reacting SiF4 gas with a complexing agent to form a complex, then subjecting the complex to a chemical exchange reaction with SiF4 gas, followed by a pyrolysis reaction to obtain high-abundance SiF4. 28 Si、 29 Si and 30 Si.

[0005] US6146601A discloses an enrichment device for silicon or germanium isotopes, in which SiF4 gas and a complexing agent are introduced into a separation column, causing a complexation reaction between the two in the separation column, resulting in a high concentration of silicon or germanium isotopes. 28 The Si complex is introduced through the bottom of the column into a two-stage stripper and a reboiler for separation.

[0006] CN116832615A discloses a continuous production process for silicon isotopes, in which SiF4 gas and a complexing agent are sequentially passed through a feed tower, a complexing tower, an exchange tower, and a decomposition tower for a cyclic reaction to obtain high-abundance SiF4 isotopes. 28 The complexation products of Si are used for the continuous production of silicon isotope products.

[0007] In industrial practice, the "pyrolysis reaction" stage of the chemical exchange method is a key step in achieving the conversion of the target material and the separation of isotopes. This stage requires high-temperature operation to drive the reaction. However, high-temperature environments easily induce side reactions in raw material molecules and intermediate products. The impurities introduced by these side reactions directly affect… 28 The purity of Si is crucial. Therefore, there is an urgent need to develop an improved process for the "pyrolysis reaction" stage of the chemical exchange method to effectively suppress side reactions under high-temperature conditions and improve the reaction yield. Summary of the Invention

[0008] This application aims to at least partially solve one of the technical problems in the related art. To this end, this application provides a silicon isotope separation method and system that can reduce side reactions. By controlling the absolute pressure of the pyrolysis tower within a negative pressure range of 0.05 to 0.7 atm, the generation of side reactions under high temperature conditions is effectively suppressed, thereby increasing the abundance of silicon-28 isotope products.

[0009] To achieve the above objectives, in a first aspect, this application provides a silicon isotope separation system capable of reducing side reactions, comprising:

[0010] The feed tower is used to input complexing agent raw materials and naturally abundant silicon tetrafluoride gas, mix them, and cause a complexation reaction.

[0011] A multi-stage exchange tower includes at least three exchange towers connected in sequence, wherein the exchange tower located in the middle of the multi-stage exchange tower is used to receive complexed reactants from the feed tower;

[0012] The cracking tower is used to receive the complexed reactants output from the final exchange tower and to heat and decompose them. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the circulation port at the bottom of the final exchange tower through the main channel at the top of the cracking tower. This is used to provide gas phase reflux for multi-stage countercurrent exchange and to achieve repeated exchange and separation of silicon isotopes through countercurrent contact with liquid phase complexes.

[0013] The impurity removal tower is used to receive the complexing agent mixture from the bottom outlet of the cracking tower. The impurity-removed complexing agent and lean solvent are collected at the upper outlet of the impurity removal tower.

[0014] The complexation tower is used to receive the complexing agent and lean solvent from the impurity removal tower and the silicon tetrafluoride gas input from the front-end exchange tower, and to carry out the complexation reaction to obtain the complexed product;

[0015] The negative pressure device is connected to the top branch of the pyrolysis tower via a gas-liquid separator, and is used to control the absolute pressure inside the pyrolysis tower to be 0.05 to 0.7 atm.

[0016] Preferably, the silicon isotope separation system further includes:

[0017] A pressurization device is installed on the top main line of the cracking tower to pressurize the silicon tetrafluoride gas enriched with silicon-28 isotope and then transport it to the bottom circulation port of the final exchange tower.

[0018] Preferably, the pyrolysis tower is provided with a low-boiling-point component inlet for adding a low-boiling-point component to the complex reactants to be decomposed before heating and decomposition, so as to lower the boiling point of the system. The boiling point of the low-boiling-point component is lower than that of the complex reactants.

[0019] Preferably, the low-boiling-point component is at least one of alkanes, aromatics, halogenated hydrocarbons, carbonates, and ethers.

[0020] Preferably, the amount of the low-boiling-point component added is 20% to 40% of the complexing agent raw material, the pyrolysis temperature in the pyrolysis tower is 90°C to 150°C, and the residual rate of the complexing reactants to be decomposed is less than 0.3%.

[0021] Secondly, this application provides a silicon isotope separation method capable of reducing side reactions, based on any of the aforementioned silicon isotope separation systems, comprising:

[0022] S101. Naturally abundant silicon tetrafluoride and complexing agent raw materials are subjected to a complexation reaction, so that the resulting silicon tetrafluoride 28 isotope complex is enriched in the liquid phase, and silicon tetrafluoride 29 isotope complex and silicon tetrafluoride 30 isotope complex are enriched in the gas phase; wherein, the complexation reaction between the complexing agent raw material and silicon tetrafluoride gas is reversible.

[0023] S102. The complex generated in step S101 is subjected to multi-stage chemical exchange, followed by thermal decomposition. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the bottom circulation port of the final exchange tower to provide gas phase reflux for multi-stage countercurrent exchange. The repeated exchange and separation of silicon isotopes are achieved through countercurrent contact with the liquid phase complex.

[0024] S103. When the silicon isotope abundance in the complex product reaches the target abundance, silicon-28 isotope product is simultaneously extracted at the end of the system, and silicon-29 and silicon-30 isotope products are extracted at the front of the system.

[0025] The pyrolysis temperature in the pyrolysis tower is between 120°C and 200°C.

[0026] Preferably, the absolute pressure inside the pyrolysis tower is 0.05 to 0.45 atm, and the pyrolysis temperature inside the pyrolysis tower is 120°C to 190°C.

[0027] Preferably, in step S2, the silicon tetrafluoride gas enriched with silicon-28 isotope obtained after decomposition is input to the bottom circulation port of the final exchange tower through a pressurizing device, and the sealing gas of the pressurizing device is selected from the following: silicon tetrafluoride gas enriched with silicon-28 isotope extracted by a negative pressure device, wherein the negative pressure device is set at the top of the cracking tower and connected to the cracking tower to control the pressure inside the cracking tower; or supplied by supplemented inert gas.

[0028] Preferably, when the sealing gas of the booster device is provided by a supplemented inert gas, all the silicon tetrafluoride gas enriched with silicon-28 isotope extracted by the negative pressure device is delivered to the input end of the booster device.

[0029] The inert gas is nitrogen or argon, and the accumulated inert gas is discharged from the top of the complexing tower.

[0030] Preferably, when the sealing gas of the pressurizing device is provided by silicon tetrafluoride gas enriched with silicon-28 isotope extracted by the negative pressure device, a buffer tank is connected to the output end of the negative pressure device. The buffer tank is equipped with a pressure sensor. When the pressure is higher than a preset threshold, the excess silicon tetrafluoride gas is output to the inlet of the gas pressurizing device.

[0031] Based on the above technical solution, it can be seen that the silicon isotope separation system and method of this application, which can reduce side reactions, has at least one of the following beneficial effects compared with the prior art:

[0032] 1. This application significantly reduces the decomposition temperature of the complex by controlling the absolute pressure of the pyrolysis tower within a negative pressure range of 0.05 to 0.7 atm, thereby reducing the probability of side reactions occurring at high temperatures. Compared with atmospheric pressure operation, this method can achieve complex decomposition with lower energy consumption under negative pressure conditions, while avoiding side reactions such as carbonization and polymerization of the complexing agent caused by high temperatures. Furthermore, through the synergistic effect of multi-stage chemical exchange and negative pressure decomposition, efficient enrichment and continuous production of silicon-28 isotopes are achieved.

[0033] 2. This application employs a dual technical approach of "negative pressure operation + addition of low-boiling-point components" to synergistically reduce the decomposition temperature of the complex. Compared with existing technologies, the pyrolysis temperature can be reduced by 20-50℃, while also reducing energy consumption and increasing the decomposition rate of the complex. This "low-temperature, high-efficiency" decomposition mode greatly reduces the occurrence of high-temperature side reactions, extends the cycle life of the complexing agent, and lowers operating costs. Attached Figure Description

[0034] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0035] Figure 1 This is a schematic flowchart of Embodiment 1 of a silicon isotope separation system that can reduce side reactions provided in this application;

[0036] Figure 2 This is a schematic flowchart of Embodiment 2 of a silicon isotope separation system that can reduce side reactions provided in this application;

[0037] Figure 3 This is a schematic flowchart of Example 3 of a silicon isotope separation system provided in this application that can reduce side reactions.

[0038] In the diagram: 1. Feeding tower; 2. Complexation tower; 3. Front-end exchange tower; 4. Intermediate exchange tower; 5. Final exchange tower; 6. Cracking tower; 7. Impurity removal tower; 8. Negative pressure device; 9. Pressurization device; 10. Gas-liquid separator; 11. Buffer tank; 12. Low-boiling-point component inlet. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of this application clearer, the embodiments of this application will be described in further detail below with reference to the accompanying drawings.

[0040] Chinese patent application CN116832615A is the applicant's prior patent. This patent proposes a continuous production process for silicon isotopes, the specific steps of which include: S1, injecting a complexing agent and silicon tetrafluoride sequentially into a feed tower to react and obtain a reaction mixture. When the molar ratio of the complexing agent to silicon tetrafluoride in the reaction mixture reaches 1.5-3, the reaction mixture is injected into a complexing tower; S2, the reaction mixture is circulated along the complexing tower, the exchange tower, and the decomposition tower to obtain a complex product; S3, when the silicon-28 abundance in the complex product reaches the target abundance, the feed tower continuously injects the reaction mixture into the exchange tower located at the front, and collects the silicon-28 product from the bottom of the complexing tower and the by-product from the bottom of the exchange tower located at the rear.

[0041] For S2, the reaction mixture forms a complex in a complexing tower, then passes sequentially through multiple exchange towers before entering a decomposition tower. The complexing agent is obtained at the bottom outlet of the decomposition tower. The complexing agent then flows into a purification tower, and the purified complexing agent flows back to the top of the complexing tower for reuse. Silicon tetrafluoride gas is obtained at the top outlet of the decomposition tower, passes through a gas buffer tank, and then enters the final exchange tower. It then passes sequentially through multiple exchange towers from back to front before returning to the bottom of the complexing tower for recirculation.

[0042] Therefore, it can be seen that in the continuous silicon isotope production process proposed by the applicant, the complexing agent is circulated throughout the entire process. The section with the highest material consumption and losses in the entire process is the decomposition tower. The purpose of the decomposition tower is distillation to remove impurities; to decompose the complex, the temperature of the decomposition tower is approximately around the boiling point of the complex product. However, the higher temperature in the decomposition tower leads to increased side reactions and the generation of more impurities. The introduction of impurities not only lowers the upper limit of silicon 28 abundance but also impairs production capacity.

[0043] Analysis of the reasons: The bottom of the decomposition tower is where the abundance of silicon-28 in the system is highest. If impurities react with silicon tetrafluoride, and are subsequently removed by a purification tower, material loss will occur. If it is recycled directly without purification, the impurities will continue to carry the naturally abundant silicon, failing to achieve the effect of isotope separation, thus leading to a decrease in product purity. For example, even if the impurities reacting with silicon tetrafluoride account for only 0.1%, the naturally abundant silicon tetrafluoride contains 92% silicon-28, 4% silicon-29, and 4% silicon-30, respectively. If it is recycled directly without purification, at least 0.008% of silicon-29 and silicon-30 will be carried in the recycling. Therefore, the upper limit of silicon-28 purity that can be purified is 99.992%, which will inevitably prevent the acquisition of silicon-28 with a purity of 99.999% or higher, directly affecting the economic benefits of industrial production.

[0044] To address the aforementioned issues, this application proposes an improved process for the decomposition reaction stage. In industrial applications, to ensure effective decomposition of the complexed products under boiling conditions, the operating temperature of the decomposition reaction stage typically needs to be controlled within the range of 190°C to 300°C. However, under these high-temperature conditions, various side reactions are easily initiated within the system, and the higher the temperature, the more complex the types and extent of the side reactions, resulting in more impurities and severely impacting product purity and system stability.

[0045] Taking the silicon tetrafluoride + trimethyl phosphate system as an example, the main side reactions that may occur within this temperature range include:

[0046] (1) Thermal decomposition of complexing agents: Trimethyl phosphate [P(OCH3)3] may undergo ester bond cleavage at high temperatures (especially near or above its boiling point), resulting in disproportionation or elimination reactions. For example, it may generate dimethyl phosphate, methyl phosphate, and methanol or dimethyl ether; under extreme conditions, it may even generate pyrophosphate esters. These decomposition products not only pollute silicon tetrafluoride gas but may also alter the complexation chemical equilibrium of the system.

[0047] (2) Complexing agent decomposition under the catalysis of silicon tetrafluoride or hydrogen fluoride: The trace amount of hydrogen fluoride present in the system (produced by the hydrolysis of silicon tetrafluoride) or the Lewis acidity of silicon tetrafluoride itself will catalytically break the POC bond of trimethyl phosphate, significantly reducing its thermal decomposition temperature, resulting in decomposition under originally relatively mild conditions, generating phosphorus oxides or fluoride impurities.

[0048] (3) Formation of fluorination byproducts: Under high temperature or local overheating conditions, silicon tetrafluoride may undergo a fluorination / exchange reaction with the methoxy group (-OCH3) in the complexing agent. This may generate fluorocarbon compounds such as fluoromethane (CH3F) and difluoromethane (CH2F2). In addition, small amounts of fluorophosphorus compounds, such as phosphoric acid fluoride (POF3) or fluorophosphates, may be generated in the reaction system. These impurities are extremely difficult to remove from the product.

[0049] (4) Polymerization / condensation reaction: Some silicon-fluorine intermediates (such as SiF2) may undergo dimerization at high temperatures, or form Si-O-Si bonds with trace amounts of moisture / silica in the system to produce oligomeric siloxanes. At the same time, phosphorus-containing species may also undergo condensation to generate high-boiling-point substances such as polyphosphate esters. These byproducts may remain in gel or solid form, adhering to the tower wall or heat exchange surface, reducing heat transfer efficiency.

[0050] (5) Carbonization and coking: If the temperature is not properly controlled, especially if there is local overheating, trimethyl phosphate or its carbon-containing decomposition products may undergo deep cracking and carbonization on the heated surface, forming carbonaceous deposits (coke). This can lead to blockage of pipes and equipment and further catalyze the occurrence of more side reactions.

[0051] Therefore, side reactions under high-temperature conditions not only affect the enrichment of silicon-28 products but also increase the maintenance burden on equipment. Thus, how to reduce operating temperature and suppress side reactions while ensuring effective decomposition of the complex is a pressing technical problem that needs to be solved.

[0052] Example 1

[0053] To suppress side reactions, this application modifies the original atmospheric pressure decomposition tower to negative pressure operation, thereby reducing the pyrolysis temperature by lowering the system pressure and thus reducing the occurrence of side reactions.

[0054] like Figure 1 As shown, a silicon isotope separation system capable of reducing side reactions is specifically provided, comprising:

[0055] Feeding tower 1 is used to input complexing agent raw materials and naturally abundant silicon tetrafluoride gas, mix them and cause a complexing reaction;

[0056] A multi-stage exchange tower includes at least three exchange towers connected in sequence, wherein the exchange tower located in the middle of the multi-stage exchange tower is used to receive complexed reactants from feed tower 1;

[0057] The cracking tower 6 is used to receive the complexed reactants output from the final exchange tower and to heat and decompose them. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the circulation port at the bottom of the final exchange tower 5 through the main channel at the top of the cracking tower 6. This is used to provide gas phase reflux for multi-stage countercurrent exchange and to achieve repeated exchange and separation of silicon isotopes through countercurrent contact with liquid phase complexes.

[0058] The impurity removal tower 7 is used to receive the complexing agent mixture from the bottom outlet of the cracking tower 6. The impurity-removed complexing agent and lean solvent are collected at the upper outlet of the impurity removal tower 7.

[0059] Complexing tower 2 is used to receive the complexing agent and lean solvent from impurity removal tower 7 and silicon tetrafluoride gas input from front-end exchange tower 3, and carry out a complexing reaction to obtain complexed products;

[0060] The negative pressure device 8 is connected to the top branch of the cracking tower 6 through the gas-liquid separator 10, and is used to control the absolute pressure inside the cracking tower 6 to be 0.05 to 0.7 atm.

[0061] Feeding tower 1 is the starting unit of the system. Its function is to mix and contact fresh complexing agent raw materials with naturally abundant silicon tetrafluoride gas (i.e., natural SiF4 gas without isotopic separation, in which the abundances of silicon-28, silicon-29, and silicon-30 are approximately 92.2%, 4%, and 4%, respectively), and to allow a preliminary complexing reaction to occur under suitable temperature and pressure conditions. The complexing agent raw materials can be oxygen-containing organic compounds such as trimethyl phosphate and pentanol, whose molecules contain oxygen atoms that can form coordinate bonds with silicon.

[0062] A multi-stage exchange tower consists of at least three exchange towers connected in sequence, forming the core unit for isotope separation. Each exchange tower contains a gas-liquid contact component (such as packing or trays). The liquid phase complex flows downwards, while the gaseous silicon tetrafluoride flows upwards, resulting in an isotope exchange reaction during countercurrent contact. Because the complex formed by silicon-28 and the complexing agent is more stable, silicon-28 tends to be enriched in the liquid phase, while silicon-29 and silicon-30 are relatively enriched in the gas phase. After multiple stages of exchange, the abundance of silicon-28 increases progressively. The exchange tower located in the middle stage (e.g., ...) Figure 1The intermediate exchange tower 4 receives the complexed reactants from feed tower 1. This design aims to fully utilize the separation capacity of each exchange tower, ensuring that the material reaches a certain enrichment level before entering the core area of ​​the separation system. The intermediate location of the exchange tower to receive the complexed reactants from feed tower 1 also facilitates the simultaneous extraction of silicon-28 isotope products at the end of the system and silicon-29 and silicon-30 isotope products at the beginning of the system when the silicon isotope abundance in the complexed products reaches the target abundance.

[0063] The cracking tower 6 is a key piece of equipment in the decomposition reaction. Its function is to receive the highly silicon-28-enriched liquid complex from the final-stage exchange tower 5 and decompose it into silicon tetrafluoride gas and a complexing agent through a reverse reaction by heating. The top of the cracking tower 6 has a gas phase outlet, divided into a main path and a branch path: the main path is used to return the silicon tetrafluoride gas enriched with silicon 28 produced by decomposition to the bottom of the final-stage exchange tower 5 as a gas phase reflux; the branch path is connected to a negative pressure device 8 to control the pressure inside the tower. The bottom of the cracking tower 6 has a bottom outlet for discharging the remaining complexing agent mixture after decomposition.

[0064] The function of the impurity removal tower 7 is to purify the complexing agent mixture discharged from the cracking tower 6. After long-term recycling, various impurities generated by side reactions may accumulate in the complexing agent, such as dimethyl phosphate, methanol, and fluorocarbons. If these impurities are not removed in time, they will affect the performance of the complexing agent and ultimately contaminate the product. The impurity removal tower 7 separates the impurities from the complexing agent through distillation. The lean solvent of the high-purity complexing agent is collected from the upper section of the tower and returned to the complexing tower 2 for recycling, while the heavy component impurities are discharged from the bottom of the tower.

[0065] The function of complexing tower 2 is to re-complex the purification complexing agent from impurity removal tower 7 with the gaseous silicon tetrafluoride from front-end exchange tower 3. The resulting complex is returned to feed tower 1 or directly enters the multi-stage exchange tower to form a complete material cycle.

[0066] The negative pressure device 8 is a key piece of equipment for realizing the core innovation of this application. The negative pressure device 8 can be a water ring vacuum pump, a rotary vane vacuum pump, or a Roots vacuum pump, or any other device capable of generating negative pressure. The negative pressure device 8 is connected to the top branch of the pyrolysis tower 6 via a gas-liquid separator 10. The function of the gas-liquid separator 10 is to prevent liquid droplets entrained in the gas from entering the negative pressure device 8 and causing damage. By adjusting the pumping rate of the negative pressure device 8, the absolute pressure inside the pyrolysis tower 6 can be precisely controlled within the range of 0.05 to 0.7 atm.

[0067] Because the boiling point of a liquid decreases with decreasing pressure, controlling the pressure of the cracking tower 6 within a negative pressure range (0.1-0.7 atm) can significantly lower the boiling point of the complex, thereby achieving effective decomposition at a lower temperature. For example, a complex that requires 190-300℃ to decompose under normal pressure may be completely decomposed at only 120-180℃ under a negative pressure of 0.3 atm.

[0068] Negative pressure can also increase the theoretical upper limit of silicon-28 isotope abundance. The reaction occurring inside the cracking tower is the reverse process of the complexation reaction. When the complexing agent is an alcohol, the chemical reaction formula for the reverse process inside the cracking tower is: This is an endothermic reaction that increases in volume.

[0069] Endothermic properties: This means that increasing the temperature is beneficial for forward pyrolysis. However, simply increasing the temperature can trigger side reactions.

[0070] Increased volume means that reducing pressure (decompression) also favors forward cracking. According to Le Chatelier's principle, reducing system pressure shifts the equilibrium towards the direction of increasing gas molecule number (i.e., forward cracking).

[0071] The core technical concept of this application lies in the fact that pressure and temperature are the "two variables" controlling the equilibrium. By applying negative pressure to the pyrolysis tower, that is, by using the means of "reducing pressure", the equilibrium is forcibly shifted to the right, making the pyrolysis reaction more thorough, the decomposition of the complex more complete, reducing the residual rate of the complex, and ultimately increasing the theoretical upper limit of the abundance of silicon-28 isotopes.

[0072] Lowering the decomposition temperature brings multiple benefits: First, it directly suppresses the occurrence of high-temperature side reactions. Furthermore, according to the Arrhenius equation, the reaction rate constant decreases exponentially with decreasing temperature; therefore, a temperature reduction of 10-40℃ can reduce the side reaction rate by more than 50%. Second, it avoids the thermal decomposition and carbonization of the complexing agent, extending its service life. Third, it reduces the formation of fluorination byproducts, improving the purity of the silicon tetrafluoride product.

[0073] In this chemical exchange system with a very small separation factor (the separation factor of the complexation reaction is about 1.02), the upper limit of the abundance of the product silicon-28 depends not only on the main reaction, but also on the irreversible contamination introduced by the side reactions.

[0074] In the pyrolysis section, there are two types of competing reactions:

[0075] Main reaction (target pyrolysis): endothermic, with a high activation energy.

[0076] Side reactions (such as carbonization and fluorination) often have lower activation energies, but their reaction rates increase dramatically at high temperatures.

[0077] According to the Arrhenius equation, temperature has an exponential effect on reaction rates. A 10°C decrease inhibits all reactions, but to varying degrees. For the main reaction, the negative pressure provides a thermodynamic driving force, so while the rate decreases, it still meets production throughput requirements. For side reactions, lacking this "negative pressure-driven" compensation mechanism, their rates decrease exponentially with decreasing temperature. Therefore, when the temperature is lowered by 10°C, the main reaction is maintained due to the negative pressure, while the side reactions are significantly inhibited. This "kinetic screening" effect drastically reduces the total amount of impurities entering the circulation system. As mentioned earlier, even 0.1% impurities, amplified by a large reflux ratio, would lock the upper limit of silicon-28 abundance at 99.992%. This application achieves this crucial temperature drop through negative pressure, successfully suppressing impurity levels to extremely low levels, thereby removing the limitation on the upper limit of product abundance and making it possible to obtain silicon-28 with 99.999% or even higher purity.

[0078] This application determined the pressure range of 0.05 to 0.7 atm through extensive experiments. While the decomposition temperature can be further reduced below 0.05 atm, excessively low pressure leads to an excessively rapid evaporation rate of silicon tetrafluoride gas and an increased gas linear velocity, potentially causing mist entrainment and reducing separation efficiency. Simultaneously, excessively low pressure places higher demands on vacuum equipment, significantly increasing energy consumption and reducing economic efficiency. Above 0.7 atm, the cooling effect is not significant, the decomposition temperature remains high, and it is difficult to effectively suppress side reactions. Therefore, controlling the pressure within the range of 0.05 to 0.7 atm achieves the optimal balance between suppressing side reactions, reducing energy consumption, and ensuring separation efficiency.

[0079] When the absolute pressure inside the cracking tower is 0.05 to 0.7 atm, the cracking temperature is 120°C to 200°C. Compared to atmospheric pressure cracking, the amount of by-products generated is reduced by more than 30%, and the complex residue rate is ≤1.5%. Under these conditions, the amount of by-reaction products generated can be reduced by more than 50%, and the single-pass loss rate of the complexing agent is reduced from 1.2-2% to below 0.5%. Simultaneously, the impurity content in the silicon tetrafluoride product is significantly reduced, and the abundance of silicon-28 can reach over 99.99%. This cracking tower with its 6-level absolute pressure range is suitable for low-purity coarse separation and small-scale batch test devices.

[0080] Preferably, when the absolute pressure inside the pyrolysis tower is 0.05 to 0.45 atm, the pyrolysis temperature inside the tower is 120°C to 190°C, and the residual rate of the complex can be reduced to less than 0.3%. This is a further preferred range of process parameters. Experimental verification shows that when the pressure is controlled at 0.1-0.45 atm, the pyrolysis temperature can be reduced to 120-190°C. Under these conditions, the amount of by-reaction products generated can be reduced by more than 60%, and the single-pass loss rate of the complexing agent is reduced from 1.2-2% to below 0.4%. Simultaneously, the impurity content in the silicon tetrafluoride product is significantly reduced, and the abundance of silicon-28 can reach over 99.999%. This is suitable for mainstream industrial continuous production lines.

[0081] Preferably, when the absolute pressure inside the pyrolysis tower is 0.2 to 0.3 atm, the pyrolysis temperature inside the tower is 123°C to 185°C. Under these conditions, the amount of by-products generated can be reduced by more than 70%, and the single-pass loss rate of the complexing agent is reduced from 1.2-2% to below 0.25%. Simultaneously, the impurity content in the silicon tetrafluoride product is significantly reduced, and the final silicon-28 isotope abundance can reach over 99.999%. This is suitable for dedicated production lines for quantum computing and metrology-grade ultra-high purity raw materials.

[0082] In one possible implementation, the silicon isotope separation system also includes a pressurization device 9, which is installed on the top main line of the cracking tower 6, for pressurizing the silicon tetrafluoride gas enriched with silicon-28 isotope and then conveying it to the bottom circulation port of the final exchange tower 5.

[0083] This application resolves the conflict between negative pressure operation and gas reflux through a combined design of negative pressure device 8 and pressurization device 9. Negative pressure device 8 draws gas from the top branch of the cracking tower 6 to maintain negative pressure within the tower; while the high-value enriched silicon-28 isotope silicon tetrafluoride gas produced by decomposition enters the pressurization device 9 through the top main branch, and after pressurization, returns to the bottom of the final-stage exchange tower 5. This ensures both low-pressure operation of the cracking tower 6 and provides sufficient pressure for gas phase reflux in the exchange tower, ensuring the normal operation of multi-stage exchange.

[0084] The booster unit 9 can be a compressor or a blower. Its function is to pressurize the silicon tetrafluoride gas collected under negative pressure, making its pressure higher than the operating pressure inside the exchange tower, so that it can smoothly enter the bottom of the exchange tower. The selection of the booster unit 9 needs to consider the corrosiveness and purity requirements of the gas. Oil-free diaphragm compressors or Roots blowers are usually used.

[0085] The pressurization device 9 enables a closed-loop system: all the gas produced by the decomposition of the cracking tower 6 is returned to the exchange system, avoiding product loss. At the same time, the gas can be appropriately heated before entering the exchange tower through the compression action of the pressurization device 9, which helps to maintain the temperature distribution inside the exchange tower and promotes gas-liquid mass transfer.

[0086] In one possible implementation, the suction port of the negative pressure device 8 is connected to the top of the cracking tower 6.

[0087] The gas extracted by the negative pressure device 8 mainly contains silicon tetrafluoride and possibly small amounts of low-boiling-point impurities. To reduce product loss, a condenser is installed at the outlet of the negative pressure device 8 to cool the gas to a low temperature (e.g., -20°C to -30°C), causing most of the silicon tetrafluoride to condense and be recovered, returning to the system. Non-condensable gases (such as nitrogen, oxygen, etc.) are discharged or sent to the tail gas treatment system. Silicon tetrafluoride can also be recovered by adsorption or absorption, and is not limited to this method.

[0088] In one possible implementation, the bottom of the cracking tower 6 is equipped with a liquid level control system to maintain a stable liquid level in the bottom and prevent liquid from being entrained by gas or the bottom from drying out.

[0089] The liquid level control system may include a liquid level gauge, a controller, and a regulating valve. When the liquid level is higher than the set value, the discharge flow rate from the bottom of the tower is increased; when the liquid level is lower than the set value, the discharge flow rate is reduced or discharge is suspended. Stable liquid level control is crucial for ensuring the long-term stable operation of the cracking tower 6.

[0090] This embodiment provides a complete silicon isotope separation system. Through the coordinated operation of each unit, continuous production from raw material input to product output is achieved. The combined design of the negative pressure device and the pressurization device ensures both low-pressure operation of the pyrolysis tower and provides stable gas-phase reflux power for the exchange tower, resolving the contradiction between negative pressure operation and gas delivery in traditional processes. This system is compact, stable in operation, and highly efficient, making it suitable for industrial applications.

[0091] Example 2

[0092] This embodiment will improve the sealing gas design scheme of the pressurization device based on Embodiment 1.

[0093] In one possible implementation, such as Figure 2 As shown, in step S102, the silicon tetrafluoride gas enriched with silicon-28 isotope obtained after decomposition is input to the bottom circulation port of the final exchange tower 5 through the pressurization device 9, and the sealing gas of the pressurization device 9 is selected from one of the following:

[0094] Option A: The silicon tetrafluoride gas enriched with silicon-28 isotope is provided by the negative pressure device 8, wherein the negative pressure device 8 is located at the top of the cracking tower 6 and is connected to the cracking tower 6 to control the pressure inside the cracking tower 6.

[0095] Option B: Provided by supplemental inert gas.

[0096] The above technical features are explained below:

[0097] Pressure boosting devices (such as compressors) typically require a sealing gas to prevent working gas from leaking through the shaft seal. The choice of sealing gas directly affects the system's material balance and product purity.

[0098] Option A uses silicon tetrafluoride gas extracted by the negative pressure device 8 as the sealing gas. The gas extracted by the negative pressure device 8 from the top of the cracking tower 6 is itself high-purity enriched silicon-28 tetrafluoride. Introducing it into the sealing system of the pressurization device 9 allows for complete recycling of the gas within the system, without introducing any external impurities or diluting the product gas. This option is suitable for applications requiring extremely high product purity.

[0099] Option B uses a supplementary inert gas as a sealing gas. The inert gas can be nitrogen, argon, or other gases that do not react with silicon tetrafluoride. This option simplifies piping connections, avoids the risk of cross-contamination between the sealing gas and process gases, and is suitable for applications with slightly lower purity requirements or during system startup. The amount of inert gas used is typically 1%-2% of the compressor inlet flow rate, having a minimal impact on product purity.

[0100] In one possible implementation, when the sealing gas of the booster 9 is supplied by a supplemented inert gas, all the silicon tetrafluoride gas enriched with silicon-28 isotopes extracted by the negative pressure device 8 is delivered to the input end of the booster 9; the inert gas is nitrogen or argon, and the accumulated inert gas is discharged from the top of the complexing tower 2.

[0101] In this configuration, the gas extracted by the negative pressure device 8 is not used directly as sealing gas, but is instead entirely channeled into the inlet of the booster device 9, where it is compressed together with the product gas and returned to the exchange tower. The advantage of this approach is that it maximizes the recovery of product gas and avoids losses. However, the introduction of inert gas will gradually accumulate within the system, affecting mass transfer efficiency. Therefore, an exhaust port needs to be installed at the top of the complexing tower 2 to periodically discharge the accumulated inert gas. The discharged gas contains a small amount of silicon tetrafluoride, which can be recovered through condensation or adsorption before discharge.

[0102] In one possible implementation, when the sealing gas of the pressurizing device 9 is provided by silicon tetrafluoride gas enriched with silicon-28 isotope extracted by the negative pressure device 8, the output end of the negative pressure device 8 is connected to a buffer tank 11, which is equipped with a pressure sensor. When the pressure is higher than a preset threshold, the excess silicon tetrafluoride gas is output to the inlet of the gas pressurizing device 9.

[0103] When using this configuration, precise control of the balance between the gas extraction volume of the negative pressure device 8 and the sealing gas demand of the booster device 9 is required. The buffer tank 11 acts as a buffer and regulator: when the gas extraction volume of the negative pressure device 8 exceeds the sealing gas demand, the pressure in the buffer tank 11 increases. When the pressure sensor detects that the pressure exceeds the set value (e.g., 0.5 atm gauge pressure), it automatically opens the valve to send the excess gas to the inlet of the booster device 9; when the gas extraction volume is less than the sealing gas demand, the pressure in the buffer tank 11 decreases, the valve closes, and the gas stored in the buffer tank 11 maintains the sealing requirements of the booster device 9. This closed-loop control system achieves dynamic material balance, requires no external gas replenishment, and prevents product loss.

[0104] Example 3

[0105] This embodiment will supplement the design scheme of adding a low-boiling-point component at the inlet of the cracking tower based on the design scheme of embodiment 2.

[0106] In one possible implementation, such as Figure 3 As shown, the cracking tower 6 is provided with a low-boiling-point component inlet 12, which is used to add a low-boiling-point component to the complex reactant to be decomposed before heating and decomposition, so as to lower the boiling point of the system. The boiling point of the low-boiling-point component is lower than that of the complex reactant.

[0107] Low-boiling-point components refer to organic solvents with boiling points significantly lower than those of the complexing products. The low-boiling-point component inlet 12 is usually located on the feed line of the cracking tower 6, preferably before the feed preheater, to ensure that the low-boiling-point component is fully mixed with the complexing reactants before entering the cracking tower 6.

[0108] The mechanism of action of low-boiling-point components is as follows: According to Raoult's law, adding low-boiling-point components to a solution lowers the boiling point of the entire system. When the mixture is heated, the low-boiling-point components preferentially vaporize, generating a large number of bubbles. These bubbles not only carry away heat but, more importantly, disrupt the liquid-phase aggregate state of the complex, resulting in more uniform heat transfer. Simultaneously, the vaporization of the low-boiling-point components acts as a "gas lift," shifting the equilibrium of the complex decomposition reaction to the right and improving decomposition efficiency.

[0109] Low-boiling-point components should meet the following conditions: good chemical inertness, not reacting with silicon tetrafluoride and complexing agents; boiling point significantly lower than that of the complex; good miscibility with the system; good thermal stability, not easily decomposed at operating temperature; non-toxic or low-toxic, and easy to recycle.

[0110] In one possible implementation, the low-boiling-point component is at least one of alkanes, aromatics, halogenated hydrocarbons, carbonates, and ethers. Specifically, it can be n-pentane (boiling point 36℃), cyclopentane (boiling point 49℃), n-hexane (boiling point 69℃), dichloromethane (boiling point 40℃), diethyl ether (boiling point 34.6℃), dimethyl carbonate (boiling point 90℃), etc. These substances all have low boiling points and good chemical inertness.

[0111] Low-boiling-point components can be used alone or in combination of two or more. Combining them may produce an azeotropic effect, further lowering the system's boiling point. For example, mixing n-hexane and dimethyl carbonate in a certain proportion can lower the system's boiling point to below 80°C.

[0112] In one possible implementation, the addition of low-boiling-point components can be combined with negative pressure operation, with an absolute pressure of 0.05 to 0.7 atm in the cracking tower, the amount of low-boiling-point components added being 20% ​​to 40% of the complexing agent raw material, the cracking temperature in cracking tower 6 being 75°C to 140°C, and the residual rate of complexing reactants to be decomposed being less than 0.3%.

[0113] In one possible implementation, the absolute pressure inside the cracking tower 6 is 0.4 atm, trimethyl phosphate is used as a complexing agent, the low-boiling component is n-hexane with an addition amount of 35%, and the cracking temperature can be reduced to 75°C.

[0114] Negative pressure operation and the addition of low-boiling-point components have a synergistic effect: negative pressure operation lowers the equilibrium boiling point of the system, and low-boiling-point components further lower the boiling point by changing the solution composition. The combination of the two can reduce the decomposition temperature to an even lower level. Under mild conditions of 75℃, almost all high-temperature side reactions are effectively suppressed. When combined with negative pressure operation conditions of 0.05 to 0.45 atm in the cracking tower, the complexing agent hardly decomposes, the single-pass loss can be reduced to below 0.1%, and the decomposition rate of the complex can reach over 99.9%.

[0115] The selection of the addition amount is based on the following considerations: when the addition amount is below 20%, the effect of lowering the boiling point is limited, the decomposition temperature remains high, and the residual rate is difficult to reduce to below 0.3%; when the addition amount is above 40%, although the decomposition temperature can be further reduced, the reactant concentration is excessively diluted, leading to a decrease in the processing capacity of cracking tower 6, a reduction in unit equipment capacity, and a deterioration in economic efficiency. Therefore, controlling the addition amount within the range of 20%-40% can achieve the best balance between reducing the decomposition temperature, increasing the decomposition rate, and maintaining equipment capacity.

[0116] Experimental data show that the optimal effect is achieved when the addition amount is 30%-35%. For example, using trimethyl phosphate as a complexing agent and n-hexane as a low-boiling-point component, with an addition amount of 30% of the complexing agent volume, and an absolute pressure of 0.7 atm in cracking tower 6, the cracking temperature can be reduced to 80℃, and the residual rate of the complex can be controlled below 0.23%. Compared with the process without the addition of the low-boiling-point component (cracking temperature 140℃, residual rate 1.5%), the decomposition temperature is reduced by 60℃, and the residual rate is reduced by 85%, demonstrating significant effects.

[0117] In one possible implementation, the gas produced after pyrolysis is condensed to separate silicon tetrafluoride, and the low-boiling-point components are recovered and recycled.

[0118] Because the boiling points of low-boiling-point components (such as n-hexane 69℃ and n-pentane 36℃) are significantly higher than that of silicon tetrafluoride (-86℃), this large difference in boiling points can be utilized to achieve efficient separation of the two through staged condensation. Specifically, the pyrolysis gas is first cooled to 0-10℃ in a cooler, causing most of the low-boiling-point components to condense into liquid for recovery. Silicon tetrafluoride (boiling point -86℃), at this temperature, remains a gas and is drawn from the top of the condenser, compressed, and returned to the exchange system. The condensed and recovered low-boiling-point liquid can be returned to the front section of cracking tower 6 and mixed with fresh feed for recycling. This method is suitable for situations where the low-boiling-point components are of high value and require recycling. Experiments show that the recovery rate of low-boiling-point components such as n-hexane can reach over 95%, with only a small amount of loss needing to be replenished in each cycle.

[0119] The separation methods are not limited to those described above. Those skilled in the art can select appropriate separation and recovery processes based on the specific type of the low-boiling-point component, economic requirements, and product purity requirements.

[0120] Example 4

[0121] In one possible implementation, this application provides a silicon isotope separation method capable of reducing side reactions, implemented based on the aforementioned silicon isotope separation system, comprising:

[0122] S101. Naturally abundant silicon tetrafluoride and complexing agent raw materials are subjected to a complexation reaction so that the resulting silicon tetrafluoride 28 isotope complex is enriched in the liquid phase, and silicon tetrafluoride 29 isotope complex and silicon tetrafluoride 30 isotope complex are enriched in the gas phase; wherein, the complexation reaction between the complexing agent raw material and silicon tetrafluoride gas is reversible.

[0123] In practice, naturally abundant silicon tetrafluoride gas (approximately 92.2% silicon-28, 4.7% silicon-29, and 3.1% silicon-30) is introduced from the bottom of feed tower 1. The temperature inside feed tower 1 is controlled at 25-35°C and the pressure at 1.2-1.5 atm, allowing silicon tetrafluoride to undergo a reversible complexation reaction with trimethyl phosphate to form a SiF4·P(OCH3)3 complex. Because the coordination bond strength between silicon-28 and oxygen atoms is slightly higher than that between silicon-29 and silicon-30, silicon-28 is preferentially enriched in the liquid phase complex, while silicon-29 and silicon-30 are relatively enriched in the unreacted gas phase.

[0124] S102. The complex generated in step S101 is subjected to multi-stage chemical exchange, followed by thermal decomposition. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the bottom circulation port of the final exchange tower 5 to provide gas phase reflux for multi-stage countercurrent exchange. Repeated exchange and separation of silicon isotopes are achieved through countercurrent contact with the liquid phase complex.

[0125] In practice, the complex generated by S101 is fed into a three-stage exchange tower (such as...). Figure 2 The system comprises a multi-stage countercurrent exchange system consisting of a front-end exchange tower 3, an intermediate exchange tower 4, and a final-stage exchange tower 5. The liquid-phase complex flows in from the top of the front-end exchange tower 3 and flows downwards stage by stage; the gaseous silicon tetrafluoride flows upwards countercurrently from the bottom of the final-stage exchange tower 5. After multi-stage exchange, the silicon-enriched complex is collected from the bottom of the final-stage exchange tower 5 and enters the cracking tower 6. The cracking tower 6 operates under negative pressure, with the absolute pressure inside the tower controlled at 0.3 atm by a negative pressure device 8. At a cracking temperature of 150°C, the complex decomposes into silicon tetrafluoride gas and trimethyl phosphate liquid. The silicon tetrafluoride gas enriched with silicon 28 produced by decomposition is collected from the top of the cracking tower 6, compressed by a pressurizing device 9, and returned to the bottom of the final-stage exchange tower 5 as a gaseous reflux; the trimethyl phosphate liquid is discharged from the bottom of the cracking tower 6 and enters the impurity removal tower 7.

[0126] S103. When the silicon isotope abundance in the complex product reaches the target abundance, silicon-28 isotope product is simultaneously extracted at the end of the system, and silicon-29 and silicon-30 isotope products are extracted at the front end of the system.

[0127] In practice, when the system is running stably and the abundance of silicon 28 in the liquid phase complex at the bottom of the final exchange tower 5 or the abundance of silicon 28 in the gas phase at the top of the cracking tower 6 reaches the target value (e.g., 99.999%), the silicon 28-enriched product is collected from the gas phase at the bottom of the final exchange tower 5 or the top of the cracking tower 6, and after processing, the silicon 28 product is obtained; at the same time, the gas phase silicon tetrafluoride enriched with silicon 29 and silicon 30 is collected from the top of the front exchange tower 3 as a by-product.

[0128] Specifically, when the absolute pressure inside cracking tower 6 is 0.05 to 0.7 atm, the cracking temperature inside cracking tower 6 is 120℃ to 200℃. This temperature range was chosen based on the following considerations: below 120℃, even under negative pressure, the decomposition rate of the complex is too slow to meet the processing capacity requirements of industrial production; above 200℃, side reactions begin to increase significantly, especially near 300℃, where the side reactions become extremely vigorous. Therefore, controlling the cracking temperature within the range of 120-200℃ can effectively suppress side reactions while ensuring the decomposition rate.

[0129] In one possible implementation, the absolute pressure inside the cracking tower 6 is 0.05 to 0.45 atm, and the cracking temperature inside the cracking tower 6 is 120°C to 180°C. This is a further preferred parameter range, within which side reactions can be reduced by more than 60%, and product purity can reach more than 99.9%.

[0130] This application significantly reduces the decomposition temperature of the complex by controlling the absolute pressure of the pyrolysis tower within a negative pressure range of 0.05 to 0.7 atm, thereby reducing the probability of side reactions at high temperatures and increasing the abundance of silicon-28 isotope products. Compared with atmospheric pressure operation, this method can achieve complex decomposition with lower energy consumption under negative pressure conditions, while avoiding side reactions such as carbonization and polymerization of the complexing agent caused by high temperatures. Furthermore, through the synergistic combination of multi-stage chemical exchange and negative pressure decomposition, efficient enrichment and continuous production of silicon-28 isotopes are achieved.

[0131] To verify the effectiveness of the technical solution presented in this application, a series of comparative experiments were conducted. The experiments used trimethyl phosphate as a complexing agent and silicon tetrafluoride as the raw material gas. The system structure is as follows: Figure 2 and Figure 3 As shown.

[0132] Experiment 1: Effect of Pressure on Decomposition Temperature and Residue Rate

[0133] Table 1. Experimental results on the effect of pressure on decomposition temperature and residue rate.

[0134] The experimental results in Table 1 show that as the pressure decreases, the pyrolysis temperature drops significantly, and the residual rate of the complex and the amount of by-products also decrease accordingly. When the pressure is below 0.1 atm, although the residual rate decreases further, the equipment investment and operating energy consumption increase significantly, and the excessively fast evaporation rate of silicon tetrafluoride leads to increased entrainment losses. Taking all factors into consideration, 0.1-0.7 atm is the preferred range, and 0.1-0.45 atm is a more preferred range.

[0135] Experiment 2: Synergistic Effect of Negative Pressure and Low-Boiling-Point Components

[0136] To verify the synergistic effect of negative pressure operation and the addition of low-boiling-point components, a gradient experiment of low-boiling-point component addition was conducted under negative pressure conditions. Experimental conditions: the complexing agent was trimethyl phosphate, the low-boiling-point component was n-hexane (boiling point 69℃), and the absolute pressure of the cracking tower was controlled at 1.0 atm (atmospheric pressure), 0.5 atm, and 0.3 atm, respectively.

[0137] Table 2. Experimental results of the synergistic effect between negative pressure and low-boiling-point components.

[0138] The following patterns can be drawn from the experimental data in Table 2:

[0139] Negative pressure and low-boiling-point components have an approximately additive effect on reducing the cracking temperature. For example, 0.5 atm alone reduces the temperature by 30°C (from 198°C to 168°C), adding 20% ​​n-hexane alone reduces the temperature by 56°C (from 198°C to 142°C), and the combination of the two reduces the temperature by 86°C (from 198°C to 112°C), which is close to the sum of the two.

[0140] The synergistic effect of negative pressure and low-boiling-point components in reducing residue levels. For example, under a negative pressure of 0.3 atm, adding only 10% of the low-boiling-point component can reduce the residue rate to 0.22% (below the target line of 0.3%); adding 20% ​​further reduces the residue rate to 0.08%. This indicates that the synergistic effect of negative pressure and low-boiling-point components can achieve the same decomposition effect with a smaller amount added.

[0141] Based on synergistic effect experiments, the following preferred operating window was determined:

[0142] Economic window: pressure 0.5 atm, low boiling point addition 15-20%, pyrolysis temperature 110-130℃, residual rate <0.3%, by-products <20%.

[0143] High-purity window: pressure 0.3 atm, low boiling point addition 20-25%, pyrolysis temperature 90-100℃, residual rate <0.1%, by-products <10%.

[0144] Balanced window: pressure 0.4 atm, low boiling point addition 20%, pyrolysis temperature about 105℃, residual rate about 0.15%, balancing effectiveness and economy.

[0145] The above experiments demonstrate that the negative pressure technology proposed in this application can significantly reduce the pyrolysis temperature, effectively suppress side reactions, and improve product purity and yield. Furthermore, by combining this with the addition of low-boiling-point components, a synergistic effect can be achieved, reducing the pyrolysis temperature to below 100℃, the residual rate to below 0.1%, and the abundance of silicon-28 isotope products to over 99.999%, meeting the stringent requirements for semiconductor-grade silicon isotopes.

[0146] In this specification, the same or similar parts between the various embodiments can be referred to mutually. Each embodiment focuses on describing the differences from other embodiments. In particular, the descriptions of the embodiments described later are relatively simple, and relevant parts can be referred to the descriptions of the foregoing embodiments.

[0147] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A silicon isotope separation system capable of reducing side reactions, characterized by, include: The feed tower is used to input complexing agent raw materials and naturally abundant silicon tetrafluoride gas, mix them, and cause a complexation reaction. A multi-stage exchange tower includes at least three exchange towers connected in sequence, wherein the exchange tower located in the middle of the multi-stage exchange tower is used to receive complexed reactants from the feed tower; The cracking tower is used to receive the complexed reactants output from the final exchange tower and to heat and decompose them. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the circulation port at the bottom of the final exchange tower through the main channel at the top of the cracking tower. This is used to provide gas phase reflux for multi-stage countercurrent exchange and to achieve repeated exchange and separation of silicon isotopes through countercurrent contact with liquid phase complexes. The impurity removal tower is used to receive the complexing agent mixture from the bottom outlet of the cracking tower. The impurity-removed complexing agent and lean solvent are collected at the upper outlet of the impurity removal tower. The complexation tower is used to receive the complexing agent and lean solvent from the impurity removal tower and the silicon tetrafluoride gas input from the front-end exchange tower, and to carry out the complexation reaction to obtain the complexed product; The negative pressure device is connected to the top branch of the pyrolysis tower via a gas-liquid separator, and is used to control the absolute pressure inside the pyrolysis tower to be 0.05 to 0.7 atm.

2. The silicon isotope separation system of claim 1, wherein, The silicon isotope separation system also includes: A pressurization device is installed on the top main line of the cracking tower to pressurize the silicon tetrafluoride gas enriched with silicon-28 isotope and then transport it to the bottom circulation port of the final exchange tower.

3. The silicon isotope separation system of claim 1, wherein, The pyrolysis tower is equipped with a low-boiling-point component inlet, which is used to add a low-boiling-point component to the complex reactants to be decomposed before heating and decomposition, so as to lower the boiling point of the system. The boiling point of the low-boiling-point component is lower than that of the complex reactants.

4. The silicon isotope separation system of claim 3, wherein, The low-boiling-point component is at least one of alkanes, aromatics, halogenated hydrocarbons, carbonates, and ethers.

5. The silicon isotope separation system of claim 4, wherein, The amount of the low-boiling-point component added is 20 vol% to 40 vol% of the complexing agent raw material, the pyrolysis temperature in the pyrolysis tower is 90°C to 150°C, and the residual rate of the complexing reactants to be decomposed is less than 0.3%.

6. A method for separating silicon isotopes capable of reducing side reactions, characterized by, The silicon isotope separation system according to claim 5 includes: S101. Naturally abundant silicon tetrafluoride and complexing agent raw materials are subjected to a complexation reaction, so that the resulting silicon tetrafluoride 28 isotope complex is enriched in the liquid phase, and silicon tetrafluoride 29 isotope complex and silicon tetrafluoride 30 isotope complex are enriched in the gas phase; wherein, the complexation reaction between the complexing agent raw material and silicon tetrafluoride gas is reversible. S102. The complex generated in step S101 is subjected to multi-stage chemical exchange, followed by thermal decomposition. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the bottom circulation port of the final exchange tower to provide gas phase reflux for multi-stage countercurrent exchange. The repeated exchange and separation of silicon isotopes are achieved through countercurrent contact with the liquid phase complex. S103. When the silicon isotope abundance in the complex product reaches the target abundance, silicon-28 isotope product is simultaneously extracted at the end of the system, and silicon-29 and silicon-30 isotope products are extracted at the front of the system. The pyrolysis temperature in the pyrolysis tower is 90°C to 150°C.

7. A method for separating silicon isotopes capable of reducing side reactions, characterized by, The silicon isotope separation system based on any one of claims 1-4 comprises: S101. Naturally abundant silicon tetrafluoride and complexing agent raw materials are subjected to a complexation reaction, so that the resulting silicon tetrafluoride 28 isotope complex is enriched in the liquid phase, and silicon tetrafluoride 29 isotope complex and silicon tetrafluoride 30 isotope complex are enriched in the gas phase; wherein, the complexation reaction between the complexing agent raw material and silicon tetrafluoride gas is reversible. S102. The complex generated in step S101 is subjected to multi-stage chemical exchange, followed by thermal decomposition. The silicon tetrafluoride gas enriched with silicon-28 isotopes obtained after decomposition is fed into the bottom circulation port of the final exchange tower to provide gas phase reflux for multi-stage countercurrent exchange. The repeated exchange and separation of silicon isotopes are achieved through countercurrent contact with the liquid phase complex. S103. When the silicon isotope abundance in the complex product reaches the target abundance, silicon-28 isotope product is simultaneously extracted at the end of the system, and silicon-29 and silicon-30 isotope products are extracted at the front of the system. The pyrolysis temperature in the pyrolysis tower is 120°C to 200°C.

8. The silicon isotope separation method according to claim 7, characterized in that, The absolute pressure inside the pyrolysis tower is 0.05 to 0.45 atm, and the pyrolysis temperature inside the pyrolysis tower is 120°C to 190°C.

9. The silicon isotope separation method according to claim 7, characterized in that, In step S102, the silicon tetrafluoride gas enriched with silicon-28 isotope obtained after decomposition is input to the bottom circulation port of the final exchange tower through a pressurization device, and the sealing gas of the pressurization device is selected from the following: silicon tetrafluoride gas enriched with silicon-28 isotope extracted by a negative pressure device, wherein the negative pressure device is set at the top of the cracking tower and connected to the cracking tower to control the pressure inside the cracking tower; or supplied by supplemented inert gas.

10. The silicon isotope separation method according to claim 9, characterized in that, When the sealing gas of the booster is supplied by the replenished inert gas, all the silicon tetrafluoride gas enriched with silicon-28 isotope extracted by the negative pressure device is delivered to the input end of the booster. The inert gas is nitrogen or argon, and the accumulated inert gas is discharged from the top of the complexing tower.

11. The silicon isotope separation method according to claim 9, characterized in that, When the sealing gas of the pressurizing device is provided by silicon tetrafluoride gas enriched with silicon-28 isotope extracted by the negative pressure device, the output end of the negative pressure device is connected to a buffer tank. The buffer tank is equipped with a pressure sensor. When the pressure is higher than a preset threshold, the excess silicon tetrafluoride gas is output to the inlet of the gas pressurizing device.

Citation Information

Patent Citations

  • Method for isolating and producing enriched 28Si, 29Si and 30Si by serially connected multiple towers and apparatus used by method

    CN105664718A

  • Silicon isotope continuous production process method

    CN116832615A

  • Enrichment of silicon or germanium isotopes

    US6146601A

  • Method for preparing silicon-28 isotope with abundance of more than 99% by using silane as medium and gas diffusion cascade

    CN117282267A

  • Method and device for separating silicon isotopes through low-temperature rectification

    CN120586648A