A positive electrode material, a preparation method thereof, a positive electrode sheet, and a battery
Patent Information
- Application Number
- CN202611219679.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-09-29
AI Technical Summary
[0007]综上,现有技术中公开的正极材料都有一定的缺陷,存在着残留锂浓度偏高,及在具有较高镍含量时,电子电导率不足的问题,从而导致无法满足电动汽车快充和高功率性能的要求
本发明提供的正极材料,通过含钴金属氧化物纳米颗粒与三元正极材料的表面残锂发生的界面反应,形成了由内至外依次为无序岩盐相组成的第一包覆层、富钴材料组成的第二包覆层的双层包覆结构,在第一包覆层与第二包覆层协同作用下,降低了三元正极材料表面残锂含量的同时,提升了正极材料的电子电导率、界面稳定性和结构稳定性;具体地,富钴材料组成的第二包覆层显著提升了正极材料的电子电导率,降低了界面电阻;无序岩盐相组成的第一包覆层在高脱锂状态下充当“结构支柱”,抑制了锂层坍塌和微裂纹生成,改善了正极材料的界面稳定性与内部结构稳定性,有效抑制了电池循环过程中正极材料发生的不可逆相变、过渡金属溶解以及颗粒内部微裂纹生成等一系列核心失效问题。因此,本发明提供的正极材料具有优异的综合性能,表面残锂含量不高于0.1wt%(远低于三元正极材料通常0.3wt%~0.5wt%的残留锂水平),且在具有较高镍含量时,表现出优异的电化学性能,即正极材料在0.1C倍率下的首次放电比容量不低于220mAh/g,首次库仑效率不低于90%,充分满足电动汽车动力电池对快充能力和高功率输出性能的严苛要求。
Smart Images

Figure CN122843349A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, relates to a cathode material, and particularly relates to a cathode material, a preparation method thereof, a cathode pole piece and a battery. Background Art
[0002] High-nickel low-cobalt single-crystal nickel-cobalt-manganese (NCM) ternary cathode material is a core cathode material for high-energy-density lithium-ion batteries, which is mainly used in electric vehicles, energy storage power stations and other fields, and can meet the performance requirements of power batteries for high energy density, long cycle life, fast charging capability and high power output.
[0003] With the rapid development of the electric vehicle industry, the market demand for high-energy-density lithium-ion batteries continues to grow. High-nickel single-crystal layered oxides with a nickel content of ≥90% have become the mainstream development direction of next-generation power battery cathode materials by virtue of their advantages of high specific capacity and low cost.
[0004] However, the high-nickel single-crystal ternary cathode material in the prior art has problems such as high concentration of residual lithium on the surface and low electronic conductivity caused by low-cobalt proportioning. Moreover, with the further increase of nickel content and further decrease of cobalt content (Co content ≤5%), the electronic conductivity of the high-nickel low-cobalt single-crystal NCM cathode material further decreases, which is difficult to meet the requirements of fast charging and high-power performance of electric vehicles. In order to solve the problems of high surface residual lithium concentration and low electronic conductivity caused by low-cobalt proportioning of ternary cathode materials, some improved cathode materials are disclosed in the prior art, but these improved cathode materials still have the problems of high surface residual lithium content and low electronic conductivity caused by low-cobalt proportioning.
[0005] For example, CN111755692A The present invention relates to a surface-reconstructed high-nickel cathode material and a preparation method thereof, belonging to the field of chemical energy storage batteries. The chemical formula of the material is Li(Ni x Co 1-x ) 1-y-z M y N z O2, wherein 0.7<x<1, 0<y≤0.1, 0<z<0.1, and y:z=m:1-m, 0.6<m<1; the material takes layered nickel-cobalt cathode material as a matrix, metal elements M and N are doped in the surface layer of primary particles of the matrix, and the outermost layer of the surface layer of the primary particles is a rock salt phase NiO thin layer.
[0006] For example, CN113851633A discloses a niobium-doped high-nickel ternary cathode material coated with niobium phosphate, comprising a niobium-doped high-nickel ternary cathode material and niobium phosphate coated on its surface; the niobium-doped high-nickel ternary cathode material refers to a high-nickel ternary cathode material doped with niobium element, wherein the molar ratio of the doping amount of niobium element to the total molar amount of nickel, cobalt and manganese transition metals in the high-nickel ternary cathode material is (0.005~0.1):1, and the mass ratio of the coating amount of niobium phosphate to the mass ratio of niobium-doped high-nickel ternary cathode material is (0.01~0.1):1.
[0007] In summary, existing cathode materials all have certain drawbacks, including high residual lithium concentrations and insufficient electronic conductivity at high nickel contents, which prevent them from meeting the requirements of fast charging and high-power performance in electric vehicles. Therefore, it is crucial to develop and design a novel cathode material and its preparation method, as well as cathode sheets and batteries. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide a cathode material, its preparation method, a cathode electrode sheet, and a battery. The cathode material provided by the present invention comprises a first coating layer composed of a disordered rock salt phase and a second coating layer composed of a cobalt-rich material. The outer cobalt-rich material can improve electronic conductivity and reduce interfacial resistance; the inner disordered rock salt phase acts as a structural support, suppressing lithium layer collapse, irreversible phase transition, and microcrack generation, thereby improving the stability of the interface and internal structure. The surface residual lithium content of the cathode material is not higher than 0.1 wt%, and with a high nickel content, the initial discharge specific capacity at 0.1C rate is not less than 220 mAh / g, and the initial coulombic efficiency is not less than 90%, which can meet the performance requirements of fast charging and high power output of power batteries.
[0009] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a cathode material, the cathode material comprising a ternary cathode material core, and a first coating layer and a second coating layer sequentially covering the outside of the ternary cathode core; The first coating layer comprises disordered rock salt material; The second coating layer comprises cobalt-rich materials.
[0010] The cathode material provided by this invention forms a double-layer coating structure through an interfacial reaction between cobalt-containing metal oxide nanoparticles and residual lithium on the surface of a ternary cathode material. This structure consists of a first coating layer composed of a disordered rock salt phase and a second coating layer composed of cobalt-rich material, arranged sequentially from the inside out. The synergistic effect of the first and second coating layers reduces the residual lithium content on the surface of the ternary cathode material while simultaneously improving its electronic conductivity, interfacial stability, and structural stability. Specifically, the second coating layer, composed of cobalt-rich material, significantly improves the electronic conductivity of the cathode material and reduces the interfacial resistance. The first coating layer, composed of a disordered rock salt phase, acts as a "structural pillar" in a high-delithiation state, inhibiting lithium layer collapse and microcrack formation, and improving the interface of the cathode material. The stability and internal structural stability effectively suppress a series of core failure problems in the cathode material during battery cycling, such as irreversible phase transitions, transition metal dissolution, and microcrack formation within particles. Therefore, the cathode material provided by this invention has excellent comprehensive performance, with a surface residual lithium content of no more than 0.1 wt% (far lower than the typical residual lithium level of 0.3 wt% to 0.5 wt% for ternary cathode materials). Moreover, when it has a high nickel content (nickel content ≥ 90%), it exhibits excellent electrochemical performance, namely, the first discharge specific capacity of the cathode material at 0.1C rate is no less than 220 mAh / g, and the first coulombic efficiency is no less than 90%, which fully meets the stringent requirements of electric vehicle power batteries for fast charging capability and high power output performance.
[0011] Preferably, the core of the ternary cathode material comprises a high-nickel, low-cobalt single-crystal ternary cathode material.
[0012] Preferably, the disordered rock salt material is generated by the interdiffusion of nickel-cobalt cations during the sintering process.
[0013] Preferably, the oxidation state of nickel in the first coating layer is lower than that of nickel in the core.
[0014] Preferably, the cobalt content in the second coating layer gradually decreases along the direction from the second coating layer to the core of the ternary cathode material.
[0015] Preferably, the average particle size of the ternary cathode material core is 1μm to 5μm, for example, it can be 1.0μm, 1.5μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm or 5.0μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0016] Preferably, the thickness of the first coating layer is 10nm to 25nm, for example, it can be 10nm, 12nm, 14nm, 16nm, 18nm, 20nm, 22nm or 25nm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0017] Preferably, the thickness of the second coating layer is 20nm to 50nm, for example, it can be 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0018] In a second aspect, the present invention provides a method for preparing the cathode material described in the first aspect, the method comprising: The ternary cathode material is dry-mixed with cobalt-containing metal oxide nanoparticles and then sintered to obtain the cathode material.
[0019] Currently, the mainstream modification methods for high-nickel single-crystal ternary cathode materials, which suffer from problems such as residual lithium on the surface and low electronic conductivity due to low cobalt ratio, are mainly as follows: The first method is water washing, which involves mixing high-nickel single-crystal ternary cathode material with deionized water in a certain proportion. The water dissolves residual lithium compounds such as Li2CO3 and LiOH on the surface of the material. After filtration and drying, the treated material is obtained. This is currently the most widely used method for removing residual lithium on the surface in the industrial field. The second method is wet coating, which involves dispersing high-nickel single-crystal ternary cathode material in an aqueous solution or organic solvent containing metal salts (such as cobalt salts, aluminum salts, zirconium salts, etc.). A uniform coating layer is formed on the surface of the material through precipitation, hydrolysis, or sol-gel processes. After filtration, drying, and high-temperature calcination, the coated modified material is obtained. This method can not only remove some residual lithium on the surface, but also improve the interfacial stability and electrochemical performance of the material.
[0020] Although both water washing and wet coating methods can modify high-nickel single-crystal ternary cathode materials to some extent, both have certain drawbacks.
[0021] The water washing method consumes a large amount of deionized water and requires multiple processes such as filtration and drying, resulting in high energy consumption and long production cycles, which significantly increases the material preparation cost. At the same time, water molecules can penetrate into the layered structure of the material during the washing process, causing local layered structure collapse and inducing the dissolution of a small amount of transition metal ions, leading to a decrease in the material's specific capacity and cycle stability. More importantly, water washing can only remove soluble residual lithium compounds on the surface of the material and cannot effectively remove residual lithium that is tightly bound to the material body. Furthermore, when the washed material is stored in the air, it is very easy to reabsorb carbon dioxide and moisture, regenerating residual lithium compounds and causing surface problems to recur.
[0022] Wet coating methods also have significant drawbacks. Some wet coating processes require the use of organic solvents, which not only further increases production costs but also leads to environmental pollution and safety hazards. During the coating process, the precipitation or hydrolysis reaction of metal salts on the material surface is difficult to proceed uniformly, easily causing uneven coating thickness and directly affecting the consistency of material performance. To achieve sufficient improvement in electronic conductivity, wet coating requires the use of large amounts of cobalt salts, which not only significantly increases material costs and exacerbates the global cobalt resource shortage but also results in extremely low cobalt resource utilization. Furthermore, the effect of wet coating is only concentrated on the material surface, improving only interfacial stability and failing to effectively address the collapse of the layered structure and the formation of microcracks within the material under high delithiation conditions.
[0023] In this invention, the technical principle of the reaction between the ternary cathode material and cobalt-containing metal oxide nanoparticles during sintering to form a first coating layer composed of a disordered rock salt phase and a second coating layer composed of cobalt-rich material is as follows: During the sintering process, the cobalt-containing metal oxide nanoparticles attached to the surface of the ternary cathode material first undergo a solid-phase interface reaction with the residual lithium compound on the surface of the ternary cathode material, consuming the residual lithium on the surface; at the same time, cobalt diffuses to the surface of the ternary cathode material, and nickel and manganese cations on the surface of the ternary cathode material migrate outward, enriching the outermost layer of the obtained cathode material to form a cobalt-rich oxide phase (cobalt-rich material), constituting the second coating layer. In the subsurface layer close to the substrate, the mutual diffusion of nickel and cobalt cations triggers cation mixing and lattice reconstruction, generating disordered rock salt material, constituting the first coating layer, and finally forming a double-layer gradient coating structure from the inside to the outside.
[0024] The preparation method provided by this invention adopts a solvent-free surface modification strategy. First, cobalt-containing metal oxide nanoparticles are uniformly coated on the surface of the ternary cathode material through dry mixing, and then sintering is performed. By utilizing the interfacial reaction between the cobalt-containing metal oxide nanoparticles and the residual lithium on the surface of the ternary cathode material, the removal of residual lithium and the construction of a double-layer coating are achieved simultaneously. No water or organic solvents are used throughout the process. The process is simple (eliminating multiple steps such as filtration, washing, and solvent recovery), low in cost (reducing equipment investment), and environmentally friendly (no wastewater or exhaust gas emissions, meeting the requirements of green chemical production). While efficiently removing residual lithium on the surface of the ternary cathode material, it avoids the irreversible damage to the bulk structure of the ternary cathode material caused by solvents in traditional processes.
[0025] In summary, the preparation method provided by this invention is simple, low-cost, and environmentally friendly, and is fully applicable to large-scale industrial production, providing solid technical support for the industrial application of next-generation high-energy-density lithium-ion batteries.
[0026] Preferably, the ternary cathode material includes a high-nickel, low-cobalt single-crystal ternary cathode material, wherein the general chemical formula of the high-nickel, low-cobalt single-crystal ternary cathode material is LiNi. x Co y Mn z O2, wherein 0.90≤x≤0.98, 0.005≤y≤0.05, 0.01≤z≤0.08, and satisfying x+y+z=1; the average particle size of the primary particles of the high-nickel low-cobalt single-crystal ternary cathode material is 1μm~5μm.
[0027] In this invention, 0.90≤x≤0.98, and the value of x can be, for example, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97 or 0.98, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0028] In this invention, 0.005≤y≤0.05, and the value of y can be, for example, 0.005, 0.010, 0.015, 0.020, 0.025, 0.030, 0.035, 0.040, 0.045 or 0.050, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0029] In this invention, 0.01≤z≤0.08, and the value of z can be, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07 or 0.08, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0030] In this invention, the average particle size of the primary particles of the high-nickel, low-cobalt single-crystal ternary cathode material is 1 μm to 5 μm, for example, it can be 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm or 5.0 μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0031] Preferably, the cobalt-containing metal oxide nanoparticles include any one or a combination of at least two of Co3O4 nanoparticles, CoO nanoparticles, or NiCo2O4 nanoparticles. Typical but non-limiting combinations include combinations of Co3O4 nanoparticles and CoO nanoparticles, combinations of NiCo2O4 nanoparticles and Co3O4 nanoparticles, combinations of CoO nanoparticles and NiCo2O4 nanoparticles, or combinations of Co3O4 nanoparticles, CoO nanoparticles, and NiCo2O4 nanoparticles, with Co3O4 nanoparticles being the most preferred.
[0032] Preferably, the average particle size of the cobalt-containing metal oxide nanoparticles is 5nm to 20nm, for example, it can be 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm or 20nm, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0033] Preferably, the preparation method further includes a pretreatment before the dry mixing, the pretreatment including: placing the ternary cathode material in a vacuum drying oven and drying it at a temperature of 80℃~120℃ for 6h~12h to remove surface-adsorbed moisture and gas.
[0034] In this invention, drying is carried out at a temperature of 80°C to 120°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0035] In this invention, the drying time is 6h to 12h, for example, it can be 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h or 12h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0036] Preferably, in the dry mixing process, the mass ratio of the ternary cathode material to the cobalt-containing metal oxide nanoparticles is 100:(0.5~5), for example, it can be 100:0.5, 100:1.0, 100:1.5, 100:2.0, 100:2.5, 100:3.0, 100:3.5, 100:4.0, 100:4.5 or 100:5.0, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0037] The preparation method provided by this invention uses only 0.5wt% to 5wt% of cobalt-containing metal oxide nanoparticles as a percentage of the mass of the ternary cathode material, which improves the electronic conductivity of the cathode material. The utilization rate of cobalt is much higher than that of the traditional wet coating process, effectively reducing the amount of cobalt used and the cost of the cathode material.
[0038] Preferably, the dry mixing method includes: adding ternary cathode material and cobalt-containing metal oxide nanoparticles into a high-energy mixer at a mass ratio of 100:(0.5~5), and mixing at a rotation speed of 1000rpm~5000rpm for 5min~30min, so that the cobalt-containing metal oxide nanoparticles are uniformly and densely coated on the surface of the ternary cathode material.
[0039] In this invention, the mixing is carried out at a speed of 1000rpm to 5000rpm, for example, 1000rpm, 1500rpm, 2000rpm, 2500rpm, 3000rpm, 3500rpm, 4000rpm, 4500rpm or 5000rpm, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0040] In this invention, the mixing time is 5 min to 30 min, for example, it can be 5 min, 7 min, 9 min, 11 min, 13 min, 15 min, 17 min, 19 min, 21 min, 23 min, 25 min, 27 min or 30 min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0041] Preferably, the sintering is carried out in an oxygen-containing atmosphere, preferably an oxygen-containing atmosphere with an oxygen volume concentration of not less than 95%, such as 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98%, 98.5%, 99%, 99.5% or 100%, but not limited to the listed values, other unlisted values within this range are also applicable.
[0042] Preferably, the oxygen-containing atmosphere includes an oxygen atmosphere, an air atmosphere, or a mixed atmosphere containing oxygen and a protective gas.
[0043] Preferably, the preparation method further includes heating before sintering, wherein the heating includes heating to the sintering temperature at a heating rate of 2℃ / min to 10℃ / min. The heating rate may be, for example, 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min or 10℃ / min, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0044] Preferably, the sintering temperature is 650℃~780℃ and the time is 2h~8h.
[0045] In this invention, the sintering temperature is 650℃~780℃, for example, it can be 650℃, 660℃, 670℃, 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃ or 780℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0046] In this invention, the sintering time is 2h to 8h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0047] Preferably, the preparation method further includes cooling after sintering, wherein the cooling includes: naturally cooling from the sintering temperature to room temperature at a cooling rate of 1℃ / min to 5℃ / min. The cooling rate may be, for example, 1℃ / min, 1.5℃ / min, 2℃ / min, 2.5℃ / min, 3℃ / min, 3.5℃ / min, 4℃ / min, 4.5℃ / min or 5℃ / min, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0048] Thirdly, the present invention provides a positive electrode sheet, the positive electrode sheet comprising the positive electrode material described in the first aspect.
[0049] Fourthly, the present invention provides a battery comprising the positive electrode sheet described in the third aspect.
[0050] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0051] Compared with the prior art, the present invention has the following beneficial effects: The cathode material provided by this invention forms a double-layer coating structure through the interfacial reaction between cobalt-containing metal oxide nanoparticles and residual lithium on the surface of a ternary cathode material. This structure consists of a first coating layer composed of a disordered rock salt phase and a second coating layer composed of cobalt-rich material, arranged sequentially from the inside out. The synergistic effect of the first and second coating layers reduces the residual lithium content on the surface of the ternary cathode material while improving its electronic conductivity, interfacial stability, and structural stability. Specifically, the second coating layer composed of cobalt-rich material significantly improves the electronic conductivity of the cathode material and reduces the interfacial resistance. The first coating layer, composed of a disordered rock salt phase, acts as a "structural pillar" in a high-delithiation state, suppressing lithium layer collapse and microcrack formation, improving the interfacial stability and internal structural stability of the cathode material, and effectively suppressing a series of core failure problems during battery cycling, such as irreversible phase transitions, transition metal dissolution, and microcrack formation within the particles. Therefore, the cathode material provided by this invention has excellent comprehensive performance, with a surface residual lithium content of no more than 0.1 wt% (far lower than the typical residual lithium level of 0.3 wt% to 0.5 wt% for ternary cathode materials), and exhibits excellent electrochemical performance when it has a high nickel content. That is, the cathode material has an initial discharge specific capacity of no less than 220 mAh / g and an initial coulombic efficiency of no less than 90% at a 0.1C rate, which fully meets the stringent requirements of electric vehicle power batteries for fast charging capability and high power output performance. Attached Figure Description
[0052] Figure 1 The image shows the SEM image of the cathode material provided in Example 1 after 200 cycles.
[0053] Figure 2 SEM image of the cathode material provided in Comparative Example 1 after 200 cycles.
[0054] Figure 3 SEM image of the cathode material provided for Comparative Example 2 after 200 cycles. Detailed Implementation
[0055] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0056] The "range" disclosed in this invention can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. This type of range definition can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be arbitrarily combined, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for specific parameters, it is understood that ranges of 60~110 and 80~120 are also expected. Furthermore, if minimum range values 1 and 2 are listed, and maximum range values 3, 4, and 5 are also listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this invention, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0" and "5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2~10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0057] In this invention, "a combination of at least two" refers to a quantity greater than or equal to two, unless otherwise specified. For example, "any combination of one or at least two" means one or more or more items. It can be understood that when referring to "a combination of at least two," it refers to any suitable combination of multiple items, that is, a combination of "at least two" items carried out in a manner that does not conflict with and enables the implementation of this invention.
[0058] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0059] The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.
[0060] Those skilled in the art will understand that the order in which the steps are written in the methods of the various embodiments does not imply a strict execution order. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, but are preferably performed sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), meaning that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0061] In this invention, open-ended technical features or solutions described using terms such as "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or exclude additional members. This can be considered as providing both technical features or solutions where "A is composed of a1, a2, and a3" or "A is selected from a1, a2, and a3," and technical features or solutions where "A includes not only a1, a2, and a3, but also other members."
[0062] In this invention, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a group consisting of A, B, and "a combination of A and B". "Containing A and / or B" can mean "containing A, containing B, and containing A and B", or "containing A, containing B, or containing A and B", and can be appropriately understood according to the context.
[0063] In this invention, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on the quantity.
[0064] Example 1 This embodiment provides a cathode material, which includes a ternary cathode material core with an average particle size of 3 μm (composed of high nickel and low cobalt single crystal ternary cathode material), and a first coating layer with a thickness of 13 nm and a second coating layer with a thickness of 26 nm sequentially coated on the outside of the ternary cathode core. The first coating layer comprises disordered rock salt material (generated by the interdiffusion of nickel and cobalt cations during sintering), and the oxidation state of nickel in the first coating layer is lower than that of nickel in the core. The second coating layer comprises cobalt-rich materials, and the cobalt content in the second coating layer gradually decreases along the direction from the second coating layer to the core of the ternary cathode material.
[0065] The method for preparing the cathode material is as follows: (1) The ternary cathode material (chemical formula LiNi) 0.96 Co 0.01 Mn 0.03 O2 (with an average particle size of 3 μm) was placed in a vacuum drying oven and dried at 100°C for 8 hours to remove surface-adsorbed moisture and gas, thus obtaining the activated ternary cathode material. (2) The activated ternary cathode material obtained in step (1) and cobalt metal oxide nanoparticles (Co3O4 nanoparticles with an average particle size of 10 nm) are added to a high-energy mixer at a mass ratio of 100:1.0 and mixed at a speed of 3000 rpm for 15 min to coat the surface of the ternary cathode material with cobalt metal oxide nanoparticles to obtain a mixture. (3) In an oxygen-containing atmosphere with an oxygen volume concentration of not less than 99%, the temperature is raised to 720°C at a heating rate of 5°C / min, and then sintered at 720°C for 4 hours. The temperature is then lowered to 25°C at a cooling rate of 2°C / min to obtain the cathode material.
[0066] Example 2 This embodiment provides a cathode material, which includes a ternary cathode material core with an average particle size of 2.5 μm (composed of high-nickel and low-cobalt single-crystal ternary cathode material), and a first coating layer with a thickness of 15 nm and a second coating layer with a thickness of 29 nm sequentially coated on the outside of the ternary cathode core. The first coating layer comprises disordered rock salt material (generated by the interdiffusion of nickel and cobalt cations during sintering), and the oxidation state of nickel in the first coating layer is lower than that of nickel in the core. The second coating layer comprises cobalt-rich materials, and the cobalt content in the second coating layer gradually decreases along the direction from the second coating layer to the core of the ternary cathode material.
[0067] The method for preparing the cathode material is as follows: (1) The ternary cathode material (chemical formula LiNi) 0.94 Co 0.02 Mn 0.04 O2 (with an average particle size of 2.5 μm) was placed in a vacuum drying oven and dried at 90°C for 10 h to remove surface-adsorbed moisture and gas, thus obtaining the activated ternary cathode material. (2) The activated ternary cathode material obtained in step (1) and cobalt metal oxide nanoparticles (Co3O4 nanoparticles with an average particle size of 8 nm) are added to a high-energy mixer at a mass ratio of 100:1.5 and mixed at a speed of 2500 rpm for 20 min to coat the surface of the ternary cathode material with cobalt metal oxide nanoparticles to obtain a mixture. (3) In an oxygen-containing atmosphere with an oxygen volume concentration of not less than 99%, the temperature is raised to 700°C at a heating rate of 4°C / min, and then sintered at 700°C for 5 hours. The temperature is then lowered to 25°C at a cooling rate of 3°C / min to obtain the cathode material.
[0068] Example 3 This embodiment provides a cathode material, which includes a ternary cathode material core with an average particle size of 3.5 μm (composed of high nickel and low cobalt single crystal ternary cathode material), and a first coating layer with a thickness of 18 nm and a second coating layer with a thickness of 35 nm sequentially coated on the outside of the ternary cathode core. The first coating layer comprises disordered rock salt material (generated by the interdiffusion of nickel and cobalt cations during sintering), and the oxidation state of nickel in the first coating layer is lower than that of nickel in the core. The second coating layer comprises cobalt-rich materials, and the cobalt content in the second coating layer gradually decreases along the direction from the second coating layer to the core of the ternary cathode material.
[0069] The method for preparing the cathode material is as follows: (1) The ternary cathode material (chemical formula LiNi) 0.92 Co 0.03 Mn 0.05 O2 (with an average particle size of 3.5 μm) was placed in a vacuum drying oven and dried at 110 °C for 7 h to remove surface-adsorbed moisture and gas, thus obtaining the activated ternary cathode material. (2) The activated ternary cathode material obtained in step (1) and cobalt metal oxide nanoparticles (CoO nanoparticles with an average particle size of 12 nm) are added to a high-energy mixer at a mass ratio of 100:2.0 and mixed at a speed of 3500 rpm for 10 min to coat the surface of the ternary cathode material with cobalt metal oxide nanoparticles to obtain a mixture. (3) In an oxygen-containing atmosphere (composed of oxygen and argon) with an oxygen volume concentration of 80%, the temperature is raised to 750°C at a heating rate of 6°C / min, and then sintered at 750°C for 3 hours. The temperature is then lowered to 25°C at a cooling rate of 1.5°C / min to obtain the cathode material.
[0070] Example 4 This embodiment provides a cathode material, which includes a ternary cathode material core with an average particle size of 1 μm (composed of high nickel and low cobalt single crystal ternary cathode material), and a first coating layer with a thickness of 10 nm and a second coating layer with a thickness of 20 nm sequentially coated on the outside of the ternary cathode core. The first coating layer comprises disordered rock salt material (generated by the interdiffusion of nickel and cobalt cations during sintering), and the oxidation state of nickel in the first coating layer is lower than that of nickel in the core. The second coating layer comprises cobalt-rich materials, and the cobalt content in the second coating layer gradually decreases along the direction from the second coating layer to the core of the ternary cathode material.
[0071] The method for preparing the cathode material is as follows: (1) The ternary cathode material (chemical formula LiNi) 0.92 Co 0.03 Mn 0.05 O2 (with an average particle size of 1 μm) was placed in a vacuum drying oven and dried at 100°C for 9 hours to remove surface-adsorbed moisture and gas, thus obtaining the activated ternary cathode material. (2) The activated ternary cathode material obtained in step (1) and cobalt metal oxide nanoparticles (NiCo2O4 nanoparticles with an average particle size of 5 nm) are added to a high-energy mixer at a mass ratio of 100:0.5 and mixed at a speed of 3000 rpm for 15 min to coat the surface of the ternary cathode material with cobalt metal oxide nanoparticles to obtain a mixture. (3) In an oxygen-containing atmosphere with an oxygen volume concentration of not less than 99%, the temperature is raised to 780°C at a heating rate of 5°C / min, and then sintered at 780°C for 2 hours. The temperature is then lowered to 25°C at a cooling rate of 1°C / min to obtain the cathode material.
[0072] Example 5 This embodiment provides a cathode material, which includes a ternary cathode material core with an average particle size of 5 μm (composed of high nickel and low cobalt single crystal ternary cathode material), and a first coating layer with a thickness of 25 nm and a second coating layer with a thickness of 50 nm sequentially coated on the outside of the ternary cathode core. The first coating layer comprises disordered rock salt material (generated by the interdiffusion of nickel and cobalt cations during sintering), and the oxidation state of nickel in the first coating layer is lower than that of nickel in the core. The second coating layer comprises cobalt-rich materials, and the cobalt content in the second coating layer gradually decreases along the direction from the second coating layer to the core of the ternary cathode material.
[0073] The method for preparing the cathode material is as follows: (1) The ternary cathode material (chemical formula LiNi) 0.92 Co 0.03 Mn 0.05 O2 (with an average particle size of 5 μm) was placed in a vacuum drying oven and dried at 100°C for 9 hours to remove surface-adsorbed moisture and gas, thus obtaining the activated ternary cathode material. (2) The activated ternary cathode material obtained in step (1) and cobalt metal oxide nanoparticles (Co3O4 nanoparticles with an average particle size of 20 nm) are added to a high-energy mixer at a mass ratio of 100:5 and mixed at a speed of 3000 rpm for 20 min, so that the cobalt metal oxide nanoparticles are coated on the surface of the ternary cathode material to obtain a mixture. (3) In an oxygen-containing atmosphere with an oxygen volume concentration of not less than 99%, the temperature is raised to 650°C at a heating rate of 5°C / min, and then sintered at 650°C for 8 hours. The temperature is then lowered to 25°C at a cooling rate of 5°C / min to obtain the cathode material.
[0074] Example 6 This embodiment provides a cathode material. Except that the thickness of the first coating layer is 5 nm and the thickness of the second coating layer is 14 nm, that is, in step (2) of the preparation method of the cathode material, the activated ternary cathode material and cobalt-containing metal oxide nanoparticles are added to the high-energy mixer at a mass ratio of 100:0.2, the rest is the same as in embodiment 1.
[0075] Example 7 This embodiment provides a cathode material. Except that the thickness of the first coating layer is 29 nm and the thickness of the second coating layer is 64 nm, that is, in step (2) of the preparation method of the cathode material, the activated ternary cathode material and cobalt-containing metal oxide nanoparticles are added to the high-energy mixer at a mass ratio of 100:8, the rest is the same as in embodiment 1.
[0076] Example 8 This embodiment provides a cathode material. Except for step (2) of the cathode material preparation method, in which the average particle size of the cobalt-containing metal oxide nanoparticles is 2 nm, the rest is the same as in Example 1.
[0077] Example 9 This embodiment provides a cathode material. Except for step (2) of the cathode material preparation method, in which the average particle size of the cobalt-containing metal oxide nanoparticles is 30 nm, the rest is the same as in Example 1.
[0078] Example 10 This embodiment provides a positive electrode material. Except for step (3) of the preparation method of the positive electrode material, which involves heating to 600°C and then sintering at 600°C, the rest is the same as in Example 1.
[0079] Example 11 This embodiment provides a positive electrode material. Except for step (3) of the preparation method of the positive electrode material, which involves heating to 850°C and then sintering at 850°C, the rest is the same as in Example 1.
[0080] Comparative Example 1 This comparative example provides a cathode material, which includes only commercially available high-nickel, low-cobalt single-crystal ternary cathode materials (chemical formula LiNi). 0.96 Co 0.01 Mn 0.03 O2, with an average particle size of 3 μm for primary particles.
[0081] Comparative Example 2 This comparative example provides a cathode material comprising a high-nickel, low-cobalt single-crystal ternary cathode material core and a cobalt-containing Co material shell covering the high-nickel, low-cobalt single-crystal ternary cathode material core. The preparation method of the cathode material is as follows: First, 100g of high-nickel, low-cobalt single-crystal ternary cathode material was dispersed in 500mL of deionized water and stirred to form a suspension. Then, 3g of Co(NO3)2·6H2O was dissolved in 100mL of deionized water and slowly added dropwise to the resulting suspension. At the same time, the pH value of the system was adjusted to 9.0 with ammonia water. After stirring for 2 hours, the mixture was filtered, washed, and then dried at 120℃ for 12 hours. Finally, the dried material was calcined at 700℃ for 5 hours in an oxygen-containing atmosphere with an oxygen volume concentration of not less than 99% to obtain the wet-coated modified material.
[0082] The surface residual lithium content of the cathode materials provided in the above embodiments and comparative examples was tested. The test method was as follows: 2.00 g of cathode material powder was weighed and placed in 50 mL of deionized water. The mixture was magnetically stirred at 25 °C for 30 min to fully extract the surface Li2CO3 and LiOH. After centrifugation at 8000 r / min for 10 min, the supernatant was collected. Using phenolphthalein as an indicator, the solution was titrated to the endpoint with 0.01 mol / L standard hydrochloric acid solution. The total surface residual lithium content was calculated based on the amount of hydrochloric acid consumed. The surface residual lithium content of the cathode materials was obtained as shown in Table 1.
[0083] The electronic conductivity of the cathode materials provided in Examples 1-11 and Comparative Examples 1-2 was tested using a four-probe resistivity meter. The electronic conductivity of the cathode materials obtained in Examples 1-11 and Comparative Examples 1-2 is shown in Table 1.
[0084] Table 1 The positive electrode materials provided in Examples 1-11 and Comparative Examples 1-2 were used to prepare lithium batteries. The preparation method was as follows: the positive electrode material, acetylene black, and polyvinylidene fluoride were added to N-methylpyrrolidone in a mass ratio of 8:1:1 and stirred into a uniform slurry. After being coated on the surface of an aluminum current collector, the slurry was vacuum dried at 120°C for 12 hours and then rolled and punched into a positive electrode sheet with a diameter of 14 mm. A lithium metal sheet was used as the counter electrode and Celgard 2400 was used as the separator. The CR2032 button lithium battery was assembled in an argon glove box.
[0085] The electrochemical performance of the obtained lithium battery was tested using the following methods: constant current charge-discharge test was performed in a constant temperature environment of 25℃ within a voltage range of 2.8V to 4.3V; the initial discharge specific capacity and initial coulombic efficiency were tested at a rate of 0.1C, the discharge specific capacity was tested at a rate of 5.0C, and the capacity retention rate was calculated after 200 cycles at a rate of 1C; the proportion of fast-charging capacity to rated capacity was calculated by charging at a constant current of 1C for 30 minutes. The initial discharge specific capacity at a rate of 0.1C, the initial coulombic efficiency at a rate of 0.1C, the discharge specific capacity at a rate of 5.0C, the capacity retention rate after 200 cycles at a rate of 1C, and the proportion of fast-charging capacity after 30 minutes are shown in Tables 2 and 3.
[0086] The CR2032 button lithium battery, after 200 cycles, was disassembled in an argon glove box. The positive electrode sheet was removed, cleaned with dimethyl carbonate, and vacuum dried. The positive electrode active material on the electrode sheet was then scraped off. XRD and SEM were used to test the scraped positive electrode active material. The SEM image of the positive electrode material provided in Example 1 after 200 cycles is shown below. Figure 1 As shown; the SEM image of the cathode material provided in Comparative Example 1 after 200 cycles is shown below. Figure 2As shown; the SEM image of the cathode material provided in Comparative Example 2 after 200 cycles is shown below. Figure 3 As shown, the scraped positive electrode active material was tested using inductively coupled plasma atomic emission spectrometry. The amount of transition metal dissolved after 200 cycles of the positive electrode material provided in Example 1 was 1.2 ppm, the amount of transition metal dissolved after 200 cycles of the positive electrode material provided in Comparative Example 1 was 12.8 ppm, and the amount of transition metal dissolved after 200 cycles of the positive electrode material provided in Comparative Example 2 was 5.6 ppm.
[0087] Depend on Figures 1-3 Based on the measured transition metal dissolution, it can be seen that the unmodified material (the cathode material provided in Comparative Example 1) has a transition metal dissolution of 12.8 ppm; the traditional wet coating material (the cathode material provided in Comparative Example 2) has improved somewhat, but the transition metal dissolution is 5.6 ppm; while the cathode material provided by the present invention (the cathode material provided in Example 1) has a complete surface structure and a transition metal dissolution of only 1.2 ppm.
[0088] Table 2 Table 3 From Table 1, we can obtain: (1) The cathode materials provided in Examples 1 to 5 of the present invention have low surface residual lithium content and exhibit high electronic conductivity. The batteries prepared with the cathode materials provided in Examples 1 to 5 have a first discharge specific capacity of not less than 220 mAh / g at 0.1C rate and a first coulombic efficiency of not less than 90%.
[0089] (2) By comparing Example 1 with Examples 6 and 7, it can be seen that when the thickness of the first coating layer of the cathode material provided by the present invention is 10nm~25nm and the thickness of the second coating layer is 20nm~50nm, the cathode material and battery exhibit better overall performance. This is because when the coating layer is too thin, it cannot form a continuous structural barrier, the structural support is insufficient, and it is difficult to effectively suppress irreversible phase transition and transition metal dissolution during cycling. When the coating layer is too thick, it will increase the lithium ion diffusion resistance, increase the interface impedance, and reduce the rate and fast charging performance. This thickness range can achieve the optimal balance between the structural stability and ion transport efficiency of the cathode material.
[0090] (3) By comparing Example 1 with Examples 8 and 9, it can be seen that when the average particle size of the cobalt-containing metal oxide nanoparticles used in the preparation method of the cathode material provided by the present invention is 5nm~20nm, the cathode material and battery exhibit better comprehensive performance. This is because when the average particle size of the cobalt-containing metal oxide nanoparticles is too small, they are prone to agglomeration, resulting in uneven coating thickness and insufficient local modification effect; when the particle size is too large, the contact area with the ternary cathode material is limited, the interfacial solid phase reaction is insufficient, the residual lithium removal effect and coating uniformity decrease. The cobalt-containing metal oxide nanoparticles in this particle size range have both good dispersibility and reactivity, which is conducive to forming a uniform and continuous double-layer coating structure.
[0091] (4) By comparing Example 1 with Examples 10 and 11, it can be seen that the cathode material preparation method provided by the present invention exhibits better comprehensive performance when the sintering temperature is 650℃~780℃. This is because when the sintering temperature is too low, the interfacial solid phase reaction and cation diffusion are insufficient, making it difficult to form a complete disordered rock salt phase and cobalt-rich coating layer, resulting in poor residual lithium removal. When the sintering temperature is too high, excessive cation diffusion will occur, leading to an excessively thick coating layer, damage to the bulk layer structure, and a decrease in the specific capacity of the material.
[0092] (5) By comparing Example 1 with Comparative Example 1, it can be seen that the cathode material provided by the present invention forms a double-layer coating structure consisting of a first coating layer composed of disordered rock salt phase and a second coating layer composed of cobalt-rich material through the interfacial reaction between cobalt-containing metal oxide nanoparticles and residual lithium on the surface of the ternary cathode material. Under the synergistic effect of the first coating layer and the second coating layer, the residual lithium content on the surface of the ternary cathode material is reduced, while the electronic conductivity, interfacial stability and structural stability of the cathode material are improved. Specifically, the second coating layer composed of cobalt-rich material significantly improves the electronic conductivity of the cathode material and reduces the interfacial resistance. The first coating layer composed of disordered rock salt phase acts as a "structural pillar" in the high delithiation state, inhibiting lithium layer collapse and microcrack generation, improving the interfacial stability and internal structural stability of the cathode material, and effectively suppressing a series of core failure problems such as irreversible phase transition, transition metal dissolution and microcrack generation inside particles that occur in the cathode material during battery cycling. Therefore, the cathode material provided by this invention has excellent comprehensive performance, with a surface residual lithium content of no more than 0.1 wt% (far lower than the typical residual lithium level of 0.3 wt% to 0.5 wt% for ternary cathode materials), and exhibits excellent electrochemical performance when it has a high nickel content. That is, the cathode material has an initial discharge specific capacity of no less than 220 mAh / g and an initial coulombic efficiency of no less than 90% at a 0.1C rate, which fully meets the stringent requirements of electric vehicle power batteries for fast charging capability and high power output performance.
[0093] (6) By comparing Example 1 and Comparative Example 2, it can be seen that the solventless dry coating and sintering process adopted in this invention achieves a better modification effect with a cobalt content much lower than that of the traditional wet coating process. It not only significantly reduces the residual lithium content on the surface of the cathode material and improves the electronic conductivity, but also significantly improves the rate performance, fast charging capability and cycle stability of the ternary cathode material.
[0094] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A positive electrode material, characterized in that, The cathode material includes a ternary cathode material core, and a first coating layer and a second coating layer sequentially covering the outside of the ternary cathode core; The first coating layer comprises disordered rock salt material; The second coating layer comprises cobalt-rich materials.
2. The cathode material according to claim 1, characterized in that, The core of the ternary cathode material comprises high-nickel, low-cobalt single-crystal ternary cathode material.
3. The cathode material according to claim 1, characterized in that, The disordered rock salt material is generated by the interdiffusion of nickel-cobalt cations during the sintering process; And / or, the oxidation state of nickel in the first coating layer is lower than the oxidation state of nickel in the core.
4. The cathode material according to claim 1, characterized in that, Along the direction from the second coating layer to the core of the ternary cathode material, the cobalt content in the second coating layer gradually decreases.
5. The cathode material according to any one of claims 1 to 4, characterized in that, The average particle size of the ternary cathode material core is 1μm~5μm; And / or, the thickness of the first coating layer is 10nm~25nm; And / or, the thickness of the second coating layer is 20nm~50nm.
6. A method for preparing the cathode material according to any one of claims 1 to 5, characterized in that, The preparation method includes: The ternary cathode material is dry-mixed with cobalt-containing metal oxide nanoparticles and then sintered to obtain the cathode material.
7. The preparation method according to claim 6, characterized in that, The ternary cathode material includes a high-nickel, low-cobalt single-crystal ternary cathode material, the general chemical formula of which is LiNi. x Co y Mn z O2, wherein 0.90≤x≤0.98, 0.005≤y≤0.05, 0.01≤z≤0.08, and satisfying x+y+z=1; the average particle size of the primary particles of the high-nickel low-cobalt single-crystal ternary cathode material is 1μm~5μm; And / or, the cobalt-containing metal oxide nanoparticles include any one or a combination of at least two of Co3O4 nanoparticles, CoO nanoparticles or NiCo2O4 nanoparticles, preferably Co3O4 nanoparticles; And / or, the average particle size of the cobalt-containing metal oxide nanoparticles is 5 nm to 20 nm.
8. The preparation method according to claim 6 or 7, characterized in that, In the dry mixing process, the mass ratio of the ternary cathode material to the cobalt-containing metal oxide nanoparticles is 100:(0.5~5). And / or, the sintering is carried out in an oxygen-containing atmosphere; And / or, the sintering temperature is 650℃~780℃, and the time is 2h~8h.
9. A positive electrode sheet, characterized in that, The positive electrode sheet comprises the positive electrode material according to any one of claims 1 to 5.
10. A battery, characterized in that, The battery includes the positive electrode sheet as described in claim 9.
Citation Information
Patent Citations
High-nickel positive electrode material with reconstructed primary particle surface layer and preparation method thereof
CN111755692A
Niobium phosphate coated niobium-doped high-nickel ternary positive electrode material and preparation method thereof