Method for alkaline hydrothermal regeneration of adsorbent, regenerated adsorbent and use thereof
By using a mixed alkaline solution of sodium hydroxide and calcium hydroxide for thermal regeneration, combined with weakly acidic washing, the problems of adsorption performance recovery and PFAS removal during the regeneration of porous carbon adsorbents were solved, achieving efficient and safe regeneration results.
Patent Information
- Application Number
- CN202611355166.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-09-02
AI Technical Summary
Existing porous carbon adsorbents are difficult to regenerate efficiently after adsorption saturation, and traditional regeneration methods are energy-intensive, costly, and prone to material damage and secondary pollution risks. They cannot simultaneously restore adsorption performance and safely remove perfluorinated compounds.
Sodium hydroxide and calcium hydroxide are used as a mixed alkali for alkaline thermal regeneration. The adsorption performance of porous carbon is restored by the nucleophilic attack of OH⁻ on PFASs molecules and the strong coordination of Ca²⁺ with oxygen-containing functional groups. Combined with weakly acidic washing, the adsorption performance of porous carbon is restored.
It achieves the restoration of the adsorption capacity of porous carbon adsorbent to 90-96% of that of fresh adsorbent, while safely removing PFASs, avoiding high-temperature burn-off and secondary pollution, and reducing regeneration costs.
Smart Images

Figure CN122850135B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of adsorbent regeneration technology, specifically to a method for alkaline thermal regeneration of an adsorbent, the regenerated adsorbent, and its applications. Background Technology
[0002] Perfluoroalkyl and polyfluoroalkyl substances (PFASs) are a class of organic pollutants with extremely high chemical stability and persistence. Porous carbon materials, due to their wide availability of raw materials, rich pore structure, and simple preparation process, have shown excellent application prospects in the adsorption treatment of PFAS-containing wastewater. However, as the adsorption process proceeds, porous carbon adsorbents gradually approach adsorption saturation. If the saturated carbon is not regenerated or disposed of in a timely and effective manner, it will not only significantly increase the cost of using the adsorbent material, but also easily lead to desorption and secondary release of adsorbed PFASs, thereby posing a risk of secondary environmental pollution.
[0003] Currently, the regeneration and treatment technologies for adsorbed saturated porous carbon are mainly divided into two categories: thermal regeneration and chemical elution regeneration. However, both of these methods have significant bottlenecks in practical applications.
[0004] Thermal regeneration typically involves sequential steps of drying, pyrolysis, and high-temperature oxidation, resulting in a complex process with extremely high overall energy consumption and poor applicability to waste carbon with high moisture content. Furthermore, within the low-to-medium temperature pyrolysis range, adsorbed PFASs are prone to incomplete decomposition, generating volatile organic fluorine byproducts, posing a serious risk of toxic gas emissions. In addition, the high-temperature heat transfer process easily leads to mass loss, pore structure collapse, and irreversible damage to surface functional groups in porous carbon materials, significantly reducing the cycle life of the regenerated products. Chemical elution regeneration mainly relies on organic solvents such as methanol and ethanol, or strong acids / bases, for elution. Its elution efficiency is generally limited, and it consumes large amounts of organic solvents, leading to difficulties in solvent recovery and potential secondary pollution. More importantly, chemical elution only transfers PFASs from the solid phase to the liquid eluent, failing to achieve the intrinsic harmless degradation of adsorbed PFASs, making it difficult to simultaneously meet the dual requirements of restoring the performance of the adsorbent material and safely eliminating PFASs.
[0005] Therefore, how to develop a regeneration method that can efficiently restore the adsorption performance of porous carbon, simultaneously achieve in-situ / harmless elimination of adsorbed PFASs, and maintain the integrity and long-term cycle stability of the porous carbon framework is a key technical problem that urgently needs to be solved in the industrial recycling of porous carbon adsorbents. Summary of the Invention
[0006] This invention provides a method for alkaline thermal regeneration of an adsorbent, the regenerated adsorbent, and its application to overcome the aforementioned defects. This invention utilizes sodium hydroxide and calcium hydroxide as a mixed alkali for alkaline thermal regeneration to regenerate the adsorbent. The regenerated adsorbent has a complete framework, PFASs within the adsorbent are safely removed, and the adsorption activity for PFASs is almost restored to that of a fresh adsorbent.
[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for thermal regeneration of an adsorbent using alkaline water, comprising: S1. Remove the porous carbon adsorbent containing perfluorinated compounds and dry it; S2. The dried porous carbon adsorbent is placed in a mixed alkaline solution of sodium hydroxide and calcium hydroxide and subjected to a hydrothermal reaction at 200~300℃ for 1~5 h; the molar ratio of sodium hydroxide to calcium hydroxide in the mixed alkaline solution is 1:(0.5~2). S3. After the hydrothermal reaction is completed, the regenerated porous carbon adsorbent is obtained by cleaning and drying.
[0008] In regenerating porous adsorbents using alkaline thermal regeneration, the inventors introduced a strong alkali, sodium hydroxide, and utilized OH... - Nucleophilic attack on the CF bonds of PFASs molecules achieves deep defluorination and mineralization of adsorbed PFASs, restoring their adsorption performance. However, it was found that the adsorption capacity of the adsorbent obtained after multiple regeneration cycles could only recover to about 60% of the adsorption capacity of the fresh adsorbent. This may be because, under the high temperature and high pressure environment of strong alkaline hydrothermal conditions, the porous carbon surface inevitably becomes exposed and generates a large number of oxygen-containing functional groups (such as carboxyl-COO groups). - (Hydroxyl-OH). These negatively charged oxygen groups generate strong electrostatic repulsion with the anions of similarly negatively charged perfluorinated compounds, leading to a drastic decrease in adsorption capacity after simple alkaline thermal regeneration.
[0009] To address this problem encountered during the alkaline thermal regeneration of sodium hydroxide alone, the inventors, after extensive experimentation, determined that sodium hydroxide and calcium hydroxide should be used as a mixed alkali for alkaline thermal regeneration. Ultimately, they discovered that the adsorption capacity of the adsorbent obtained after multiple regeneration cycles can be restored to approximately 90% of the adsorption capacity of the fresh adsorbent.
[0010] Preferably, in S1, the porous carbon adsorbent is derived from porous carbon or biomass-derived porous carbon.
[0011] Most porous carbon, such as biomass-derived porous carbon, is inherently rich in -OH and COC bonds. During pyrolysis and carbonization, although most oxygen elements are removed as H2O, CO, and CO2, some oxygen atoms remain at the edges of the carbon framework, forming porous carbon with oxygen-containing functional groups. Under alkaline hydrothermal conditions, the number of oxygen-containing functional groups in this porous carbon increases.
[0012] A small portion of commercially available porous carbon may lack oxygen-containing functional groups, but during the alkaline thermal regeneration process, due to the high temperature of OH groups... - It will forcefully attack the defect sites on the porous carbon framework and also produce oxygen-containing groups.
[0013] Therefore, the inventors have proposed a method for alkaline hydrothermal regeneration using sodium hydroxide and calcium hydroxide as a mixed alkali, which can solve the problem that the adsorption capacity of the regenerated adsorbent is low due to the blockage of adsorption sites by oxygen-containing functional groups after conventional alkaline hydrothermal regeneration.
[0014] Preferably, in S1, the biomass-derived porous carbon is selected from at least one of waste cotton fabrics, waste paper, straw, peanut shells, canna lilies, walnut shells or coffee grounds, which are obtained by calcination as powder or block porous carbon.
[0015] In addition to the biomass-derived porous carbon listed herein, other biomass-derived porous carbons with porous adsorption structures can be used as objects for alkaline thermal regeneration. Alkaline thermal regeneration is used to restore their adsorption capacity and remove residual PFASs from the adsorbent after adsorption.
[0016] Preferably, the preparation method of the biomass-derived porous carbon is as follows: under an inert atmosphere, the carbon is heated at 800-1200°C for 1-3 h at a heating rate of 3-5°C / min; after the heating is completed, the carbon is taken out, ground, and cleaned.
[0017] More preferably, the molar ratio of sodium hydroxide to calcium hydroxide in the mixed alkaline solution is 1:(0.6~2). More preferably, the molar ratio of sodium hydroxide to calcium hydroxide in the mixed alkaline solution is 1:(1~2). More preferably, the molar ratio of sodium hydroxide to calcium hydroxide in the mixed alkaline solution is 1:1.
[0018] Preferably, in step S2, the mass-to-volume ratio of the dried porous carbon adsorbent to the mixed alkaline solution is 0.5~1.5 g / mL. More preferably, the mass-to-volume ratio of the dried porous carbon adsorbent to the mixed alkaline solution is 0.8~1.2 g / mL.
[0019] Preferably, in step S2, the hydrothermal reaction is carried out at 220~280°C for 1~3 h. More preferably, the hydrothermal reaction is carried out at 240~260°C for 1~3 h.
[0020] Preferably, in step S3, the washing is performed until the pH of the final filtrate is 6 to 6.5.
[0021] During the cleaning stage following the hydrothermal reaction, using slightly acidic washing conditions can quickly neutralize and remove excess free OH groups remaining in the system. - This reduces the negative potential of the porous carbon surface, thereby effectively weakening the electrostatic repulsion of negatively charged PFASs anions by oxygen-containing functional groups. On the other hand, the mild, weakly acidic environment avoids damaging the Ca atoms already bound to the carbon surface. 2+ Excessive stripping and leaching consumption ensures Ca 2+ It is stably retained on the porous carbon surface. Under these conditions, Ca... 2+ It undergoes strong coordination with newly formed oxygen-containing functional groups on the porous carbon surface, stabilizing to form a -COO-like structure. - ···Ca 2+ The complex structure of the compound was obtained. The cationic bridging effect was cleverly utilized to transform the negatively charged oxygen-containing functional groups that originally hindered adsorption into novel high-affinity adsorption sites, eliminating side effects while further consolidating the Ca complex structure. 2+ The bridging adsorption effect ultimately allows the adsorbent obtained from multiple regeneration cycles to recover its adsorption capacity to about 96% of that of the fresh adsorbent.
[0022] Preferably, in step S3, the cleaning is performed using a 0.05~0.2 M hydrochloric acid solution and deionized water.
[0023] The present invention also provides a regenerated adsorbent prepared by a method for thermal regeneration of an adsorbent using alkaline water.
[0024] The present invention also provides the application of the above-mentioned regenerated adsorbent in the treatment of water containing perfluorinated compounds.
[0025] Therefore, the present invention has the following beneficial effects: (1) The present invention uses sodium hydroxide and calcium hydroxide as a mixed alkali for alkaline thermal regeneration to regenerate the adsorbent. The regenerated adsorbent has a complete skeleton, and the PFASs in the adsorbent are safely removed. The adsorption capacity of the regenerated adsorbent can be restored to about 90% of the adsorption capacity of the fresh adsorbent.
[0026] (2) This invention introduces calcium hydroxide, utilizing Ca 2+ (Hard acid) undergoes strong coordination with newly formed oxygen-containing functional groups (hard base) on the carbon surface, forming a structure similar to -COO. - ···Ca 2+ The stable complex structure. This cation bridging effect transforms the oxygen-containing functional groups that originally hindered adsorption into new high-affinity adsorption sites, thereby restoring the adsorption capacity of the regenerated adsorbent to about 90% of that of the fresh adsorbent.
[0027] (3) This invention achieves efficient removal of excess free OH groups by controlling slightly acidic washing conditions. - Neutralizing the surface negative charge to eliminate the electrostatic repulsion of PFASs anions while avoiding the impact on the fixed Ca 2+ The stripping consumption. This makes Ca 2+ It can stably coordinate with oxygen-containing functional groups on the carbon surface to form -COO - ···Ca 2+ The complex successfully transformed the oxygen-containing groups that hindered adsorption into high-affinity adsorption sites, ultimately restoring the adsorption capacity of the regenerated adsorbent to approximately 96% of that of the fresh adsorbent.
[0028] (4) The dual-alkali hydrothermal system used in this invention can not only efficiently restore the adsorption activity of porous carbon at 200~300℃, but also the strong alkali effect in the hydrothermal system can defluorinate and degrade the PFASs molecules enriched on the secondary adsorbent (the waste carbon adsorbed with PFASs) in situ and deeply mineralize them, thus completely blocking the hidden danger of secondary pollution caused by the transfer of PFASs to the liquid phase in the traditional chemical elution method. Moreover, the process does not require the consumption of high-cost organic solvents and there is no risk of high-temperature burning of the carbon skeleton.
[0029] (5) The alkaline water thermal regeneration method for adsorbents provided by the present invention can regenerate adsorbents that are saturated or partially adsorbed with PFASs. It can safely remove residual PFASs and restore the ability to adsorb PFASs for porous carbon adsorbents in different adsorption states. Attached Figure Description
[0030] Figure 1 SEM images and EDS elemental mappings of waste cotton-based porous carbon adsorbent CF-1000-1 are shown, where (a) is the SEM image, (b) is the magnified view within the dashed box in a, (c) is the C element, and (d) is the O element.
[0031] Figure 2 XPS C1s spectra of CF-1000-1-Rx (x = 0, 1 or 5) with different regeneration numbers; where (a) CF-1000-1-R0, (b) CF-1000-1-R1, (c) CF-1000-1-R5. Detailed Implementation
[0032] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0033] In this section, the abbreviations of perfluorinated compounds correspond to the following full names: PFOA, Perfluorooctanoic acid; PFHpA, Perfluoroheptanoic acid; PFHxA, Perfluorohexanoic acid; PFPeA, Perfluoropentanoic acid; PFBA, Perfluorobutanoic acid.
[0034]
Example
[0035] 2. Preparation of secondary adsorbent PFASs adsorption treatment: Waste cotton-based porous carbon adsorbent was added to 50 mL of a 150 mg / L PFOA solution at a dosage of 1 g / L. The solution was incubated at 25°C and subjected to rotational mixing at 50 r / min for 24 h. After 24 h of adsorption, the saturated adsorbent was collected, filtered, washed, and dried in a vacuum oven at 80°C for 12 h before being collected and stored to obtain the secondary adsorbent.
[0036] 3. Alkaline thermal regeneration of secondary adsorbent The secondary adsorbent was added to a hydrothermal reactor at a dosage of 1 g / L, along with 50 mL of a mixed alkaline solution (1 M NaOH solution and 1 M Ca(OH)2 solution mixed in a 1:1 volume ratio). After vortexing to ensure thorough solid-liquid mixing, the reactor was sealed and placed in a forced-air drying oven at 250°C for 2 h. After the reaction was complete, the reactor was allowed to cool naturally to room temperature. The reactor was then opened, and the entire mixture was transferred to centrifuge tubes. The mixture was centrifuged at 10000 r / min for 10 min to achieve solid-liquid separation. The resulting solid was washed with 0.1 M HCl and deionized water until the pH of the final filtrate was close to 6-6.5. The washed solid was then transferred to a vacuum drying oven and dried under vacuum at 80°C to constant weight to obtain the regenerated adsorbent.
[0037] Comparative Example 1 This comparative example is basically the same as Example 1, except that: 25 mL of 1 M Ca(OH)₂ solution is replaced with an equal amount of CaO according to the molar amount of Ca, and 25 mL of deionized water is added instead of the original Ca(OH)₂ solution. The secondary adsorbent is first added and mixed with 25 mL of 1 M NaOH solution, and then CaO and 25 mL of deionized water are added sequentially.
[0038] Comparative Example 2 This comparative example is basically the same as Example 1, except that the 50 mL mixed alkaline solution obtained by mixing 1 M NaOH solution and 1 M Ca(OH)2 solution in a volume ratio of 1:1 is replaced with 50 mL of 1 M NaOH solution.
[0039] Comparative Example 3 This comparative example is basically the same as Example 1, except that the 50 mL mixed alkaline solution obtained by mixing 1 M NaOH solution and 1 M Ca(OH)2 solution in a volume ratio of 1:1 is replaced with 50 mL of 1 M Ca(OH)2 solution.
[0040] Comparative Example 4 Add 50 mL of a mixed alkaline solution (1 M NaOH solution and 1 M Ca(OH)2 solution mixed in a 1:1 volume ratio) to 50 mL of a 150 mg / L PFOA solution. Incubate the mixture at 25°C in a rotary mixer at 50 r / min for 24 h. After 24 h, collect the reacted solution and determine the PFOA residue.
[0041] Comparative Example 5 This comparative example is basically the same as Example 1, except that: "3. Alkaline thermal regeneration of secondary adsorbent" does not add mixed alkaline solution, and 50 mL of mixed alkaline solution is replaced with 50 mL of deionized water.
[0042] Example 2 This embodiment is basically the same as embodiment 1, except that in "3. Alkaline thermal regeneration of secondary adsorbent", the volume ratio of 1 M NaOH solution and 1 M Ca(OH)2 solution is changed.
[0043] A: A mixed alkaline solution is obtained by mixing 1 M NaOH solution and 1 M Ca(OH)2 solution in a volume ratio of 1:2.
[0044] B: A mixed alkaline solution is obtained by mixing 1 M NaOH solution and 1 M Ca(OH)2 solution in a volume ratio of 2:1.
[0045] C: A mixed alkaline solution is obtained by mixing 1 M NaOH solution and 1 M Ca(OH)2 solution in a volume ratio of 2:3.
[0046] D: A mixed alkaline solution is obtained by mixing 1 M NaOH solution and 1 M Ca(OH)2 solution in a volume ratio of 3:2.
[0047] Example 3 This embodiment is basically the same as embodiment 1, except that the cleaning conditions are changed in "3. Alkaline thermal regeneration of secondary adsorbent".
[0048] A: The obtained solid phase was washed with 0.1 M HCl and deionized water until the pH of the final filtrate was neutral.
[0049] B: The obtained solid phase was washed with 0.1 M HCl and deionized water until the pH of the final filtrate was 8-9.
[0050] [Performance Testing] The detection methods involved in this section are as follows: (1) Preparation of PFASs stock solution and standard curve Taking PFOA as an example, PFOA stock solution: Weigh 0.04 g of PFOA into a 1 L polypropylene volumetric flask, add deionized water to dilute to the final volume, place in a constant temperature water bath shaker and shake at 150 rpm for 24 h, sonicate for 1 h, which is 40 mg / L PFOA stock solution, and then pour into a high-density polyethylene bottle for storage in the dark.
[0051] Standard Curve: By analyzing standard samples with known PFOA concentrations, a linear relationship between PFOA concentration and instrument response value is established to obtain a standard curve for PFOA concentration detection. Then, the response value of unknown samples is substituted into the standard curve to calculate the PFOA concentration in the unknown samples. In this experiment, 40 mg / L PFOA stock solution was taken and diluted to concentrations of 0.5 µg / L, 1 µg / L, 2 µg / L, 5 µg / L, 10 µg / L, 2 mg / L, 6 mg / L, 10 mg / L, 15 mg / L, and 20 mg / L. The y-axis represents the instrument response value (peak area), and the x-axis represents the PFOA concentration. A standard curve was then plotted.
[0052] (2) Analysis of PFAS concentration after adsorption After high-speed centrifugation, water samples at various time points in the adsorption experiment were collected, and the supernatant was filtered through a 0.22 μm filter membrane. The PFOA concentration in the solution was determined by liquid chromatography-tandem mass spectrometry (LC–MS / MS), and the PFOA concentration in the sample was quantitatively calculated based on a standard curve. The instrument used was an ultra-high performance liquid chromatography-triple quadrupole tandem mass spectrometer (Waters ACQUITY UPLC XevoTQS micro, Waters Corporation, USA). The instrument operating parameters are as follows: Chromatographic conditions: ACQUITY BEH C18 column (2.1 mm × 100 mm, 1.7 μm, Waters Corporation, USA); mobile phase A was 5 mmol / L ammonium acetate aqueous solution, and mobile phase B was acetonitrile; flow rate: 0.4 mL / min; column temperature: 40°C; injection volume: 2 μL. The gradient elution degree is shown in the table below.
[0053] Table 1 Gradient elution program
[0054] Mass spectrometry conditions: Ultra-high performance liquid chromatography-triple quadrupole tandem mass spectrometer (equipped with an electrospray ionization source), Waters ACQUITY UPLC Xevo TQS micro, Waters Corporation, USA. Ion source: ESI source; Ionization mode: negative ion mode; Capillary voltage: 1.5 kV; Ion source temperature: 150℃; Cone backflush gas flow rate: 50 L / Hr; Desolvation gas temperature: 500℃; Desolvation gas flow rate: 900 L / Hr; Monitoring mode: MRM mode. The mass spectrometry conditions are shown in the table below.
[0055] Table 2 Mass Spectrometry Conditions
[0056] Note: Indicates quantitative ion pairs.
[0057] (3) Experiment on the extraction of perfluorinated compounds from porous carbon based on waste cotton fabric after adsorption PFOA adsorbed on porous carbon adsorbent based on waste cotton fabric was extracted using ammonium acetate in methanol solution. A 100 mM ammonium acetate in methanol solution was prepared, and three 5 mg aliquots of the corresponding adsorbent were added to 50 mL polypropylene centrifuge tubes. 10 mL of the 100 mM ammonium acetate in methanol solution was added to each tube, and the mixture was shaken well and then sonicated for 30 min. After sonication, the tubes were centrifuged at 10000 r / min for 10 min to achieve solid-liquid separation. The liquid was filtered through a 0.22 μm nylon filter and stored. This dispersion and separation process was repeated three times, and the total extracted amount was the PFOA adsorbed by the corresponding adsorbent.
[0058] (4) Cyclic regeneration stability test To evaluate the recyclability of porous carbon adsorbent, five consecutive "adsorption-alkaline hydrothermal regeneration" cycles were conducted. The experimental procedure involved batch adsorption of a 150 mg / L PFOA solution using either fresh or regenerated adsorbent. The porous carbon adsorbent dosage was 1 g / L. Adsorption was performed at 25℃ and 50 r / min for 24 h with shaking. The PFOA concentration in the solution after adsorption equilibrium was then measured, and the equilibrium adsorption capacity of the porous carbon adsorbent was calculated. The saturated porous carbon adsorbent was then collected by centrifugation, dried, and subjected to alkaline hydrothermal regeneration. This process was repeated in the next cycle. The regeneration efficiency was calculated by measuring the PFOA adsorption capacity of the porous carbon adsorbent after each cycle.
[0059] The calculation formula used is as follows: ①PFOA adsorption capacity The amount of PFOA adsorbed by the adsorbent when adsorption reaches equilibrium, Q e The calculation formula is as follows: ; In the formula: Q e The adsorption capacity of the adsorbent for PFOA at equilibrium is mg / g; V is the volume of the solution, L; m is the mass of the adsorbent material, g; C0 is the initial concentration of PFOA, mg / L; C e t represents the concentration of PFOA at time t, in mg / L.
[0060] ②PFOA degradation rate The formula for calculating the degradation rate D (%) of PFOA is as follows: ; In the formula: C liq The mass (mg) of PFOA remaining in the liquid phase after the hydrothermal reaction; C solm0 represents the mass (mg) of PFOA remaining on the porous carbon solid phase of waste cotton fabric after the hydrothermal reaction; m0 represents the total mass (mg) of PFOA initially adsorbed on the saturated porous carbon of waste cotton fabric.
[0061] ③Defluorination rate The formula for calculating the PFOA defluorination rate DF (%) is as follows: ; In the formula: C F ω represents the concentration of fluoride ions in the liquid phase after the hydrothermal reaction (mg / L); V represents the volume of the reaction solution (L); F The mass fraction of fluorine in a PFOA molecule (ω in PFOA) F ≈ 67.04%); m0 is the total mass (mg) of PFOA initially adsorbed on the porous carbon substrate of saturated waste cotton fabric.
[0062] ④ Regeneration efficiency The formula for calculating the regeneration efficiency (RE) of porous carbon based on waste cotton fabric is as follows: ; In the formula: q re The equilibrium adsorption capacity (mg / g) of PFOA on porous carbon based on recycled waste cotton fabric; q fresh The equilibrium adsorption capacity (mg / g) of PFOA on porous carbon based on fresh waste cotton fabric is given.
[0063] 1. Structural characterization The structure of fresh waste cotton-based porous carbon adsorbent was characterized, and the results are as follows: Figure 1 As shown, after calcining the waste cotton-based porous carbon adsorbent at 1000℃ for 1 h, the surface fiber outline became coarser and the surface became rougher. Under high magnification, a large number of uniformly distributed micropores and mesopores could be seen. This is because the volatile components fully escaped at high temperature, forming a large number of pores, confirming that a porous carbon material with rich pore structure was synthesized.
[0064] X-ray photoelectron spectroscopy was used to analyze the elemental composition and chemical state of carbon on the surface of fresh waste cotton-based porous carbon adsorbent. The results are as follows: Figure 2 As shown in Figure a and Table 3, by performing peak fitting on the high-resolution C 1s spectrum, the spectrum can be decomposed into six characteristic bond types, corresponding to the following: sp at 284.6 eV. 2 Hybridized graphitized C-C bonds are a core feature of the conjugated aromatic ring framework of carbon materials, and their peak area ratio can directly reflect the degree of graphitization and sp. 2 Carbon content percentage; sp at 285.0 eV. 3 Hybridized aliphatic C-C bonds correspond to amorphous carbon and saturated carbon structures with carbon framework defect sites; the peak area ratio of the two is a quantitative characterization factor for the sp(s) of materials.2 / sp 3 The core indicator of carbon composition. Peaks at 286.1 eV, 287.6 eV, and 290.1 eV belong to C-OH / COC (ether bond), C=O (carbonyl group), and -COOH (carboxyl group), respectively, representing the main oxygen-containing functional groups on the surface of carbon materials. These peaks reflect the oxygen bonding form of the carbon skeleton and the degree of oxidation on the material surface. The peak at 291.2 eV represents π-π... Excitation peak is sp 2 The characteristic accompanying peaks of the hybrid carbon conjugated aromatic ring structure, and their signal intensity can corroborate the degree of conjugation development of the aromatic carbon skeleton in the material.
[0065] Cyclic regeneration stability experiments were conducted on the regenerated adsorbent obtained by treatment with sodium hydroxide alone (Comparative Example 2), revealing a significant decline in adsorption capacity after the first cycle. Furthermore, to investigate the cause of this performance change, XPS characterization was performed on the adsorbent after one and five cycles, with the results as follows: Figure 2 The results are shown in Figures b-c and Table 3. After one alkaline thermal regeneration, the CC sp in CF-1000-1-R1... 2 The relative content increased slightly from 39.41% to 39.77%, CC sp 3 The percentage decreased from 35.17% to 34.35%. Based on the data in Table 3, the percentage of positive samples (SP) was calculated. 2 / sp 3 The increase from 1.12 to 1.16 indicates a slight increase in the proportion of aromatic carbon skeletons on the material surface after a single regeneration, while the proportion of amorphous or saturated carbon structures decreases. When the number of regeneration cycles increases to 5, the CC sp in CF-1000-1-R5... 2 The relative content was 38.87%, slightly lower than CF-1000-1-R1, but the CC sp³ further decreased to 32.55%. According to Table 3, the sp³ content was calculated... 2 / sp 3 The ratio further increased to 1.19; at the same time, the relative contents of CO, C=O, and COOH increased to 17.81%, 6.47%, and 3.09%, respectively, with the total proportion of oxygen-containing functional groups significantly higher than that of R0 and R1, π-π The excitation peak remained at 1.21%.
[0066] This indicates that after multiple individual sodium hydroxide alkaline water thermal regeneration cycles, the carbon skeleton on the material surface did not undergo severe disintegration. Instead, while maintaining the overall stability of the aromatic conjugated skeleton, more oxygen-containing functional groups and edge active sites were gradually generated on the surface.
[0067] Table 3. Elemental composition of CF-1000-1-Rx (x = 0, 1, or 5) for different regeneration cycles.
[0068] 2. Adsorption capacity of the regenerated adsorbent To determine the adsorption capacity of the regenerated adsorbents obtained under different treatment schemes, the PFOA adsorption capacity, PFOA degradation rate, PFOA defluorination rate, and PFOA regeneration efficiency of each adsorbent were measured, and the results are shown in Tables 4 and 5.
[0069] Table 4. PFOA degradation and defluorination effect and regenerated porous carbon adsorption performance of the first alkaline thermal regeneration process.
[0070] Table 5. Regeneration efficiency of the regenerated adsorbent obtained by the continuous alkaline thermal regeneration process.
[0071] Note that R represents the number of regenerations, where R = 1, 2, 3, 4, 5.
[0072] Analysis of the data in Tables 4 and 5 shows that sodium hydroxide alone, as a regeneration adsorbent for the alkaline solution, has poor regeneration adsorption capacity. Combined with the XPS results, it is hypothesized that the increased number of oxygen-containing functional groups leads to enhanced electrostatic repulsion with PFOA, resulting in poorer adsorption. However, when calcium hydroxide and sodium hydroxide are used as a mixed alkaline solution, the overall OH... - The quantity remained unchanged, but some Ca was introduced through calcium hydroxide. 2+ And Ca 2+ It can undergo strong coordination with oxygen-containing functional groups on the porous carbon surface, forming a hard acid-hard base relationship, similar to -COO. - ···Ca 2+ The stable complex structure. This cation bridging effect transforms the oxygen-containing functional groups that originally hindered adsorption into new high-affinity adsorption sites, thereby restoring the adsorption capacity of the regenerated adsorbent to 90% of that of the fresh adsorbent.
[0073] Cleaning is usually done to remove excess OH- - To remove other impurity ions, washing until the final filtrate is neutral is generally sufficient. However, the inventors adjusted the washing conditions and found that under slightly acidic conditions, the adsorption capacity of the regenerated adsorbent could be restored to 96% of that of the fresh adsorbent. This is likely because the mildly acidic environment avoids damaging the Ca atoms already bound to the carbon surface. 2+ Excessive stripping and leaching consumption ensures Ca 2+ It is stably retained on the porous carbon surface. Then, Ca is utilized. 2+ The cation bridging effect increases the adsorption capacity of the regenerated adsorbent.
[0074] In addition, Ca 2+Both the concentration and source of Ca2+ affect its cation bridging effect. 2+ The adsorption capacity of the CaO sourced in Example 1 (CaO + H₂O → Ca(OH)₂) is weaker than that in Example 1. This may be because the process of CaO hydration to form Ca(OH)₂ may easily lead to agglomeration, resulting in extremely uneven dispersion of the calcium source on the porous carbon surface, making it impossible to form a uniform CaO. 2+ The anchoring point affects the final bridging and adsorption effect.
[0075] 3. PFAS removal status Table 6 shows the adsorption capacity of regenerated porous carbon for different PFASs obtained from the first alkaline thermal regeneration process.
[0076] To investigate the broad treatment capacity of the regenerated adsorbent obtained in Example 1, the regenerated adsorbent was subjected to adsorption treatment with various PFASs. The treatment targets were 150 mg / L PFOA, 150 mg / L PFHpA, 150 mg / L PFHxA, 150 mg / L PFPeA, and 150 mg / L PFBA. The treatment results are shown in Table 6.
Claims
1. A method of hydrothermally regenerating a sorbent with a base, characterized by, The method comprises the following steps: S1. Taking out and drying the porous carbon adsorbent adsorbing perfluorinated compounds; S2. Placing the dried porous carbon adsorbent in a mixed alkali liquor of sodium hydroxide and calcium hydroxide, and performing a hydrothermal reaction at 200-300 ℃ for 1-5 h; the molar ratio of sodium hydroxide to calcium hydroxide in the mixed alkali liquor is 1:(0.5-2); S3. After the hydrothermal reaction, washing with 0.05-0.2 M hydrochloric acid solution and deionized water until the pH value of the final filtrate is 6-6.5, and drying to obtain the regenerated porous carbon adsorbent.
2. The method of claim 1, wherein, In S1, the source of the porous carbon adsorbent is biomass-derived porous carbon.
3. The method of claim 2, wherein, In S1, the biomass-derived porous carbon is selected from at least one of the following: powdered or block-shaped porous carbon obtained by calcining waste cotton fabric, waste paper, straw, peanut shell, canna, walnut shell or coffee grounds.
4. The method of claim 1, wherein, In S2, the mass-volume ratio of the dried porous carbon adsorbent to the mixed alkali liquor is 0.5-1.5 g / mL.
5. The method of claim 1, wherein, In S2, the hydrothermal reaction is performed at 220-280 ℃ for 1-3 h.
6. The regenerated adsorbent prepared by the method according to any one of claims 1-5.
7. The use of the regenerated adsorbent according to claim 6 in treating water bodies containing perfluorinated compounds.
Citation Information
Patent Citations
Preparation method of modified activated carbon and application of modified activated carbon in PFASs adsorption
CN121988285A
Adsorptive-desorptive activated carbon for per- and polyfluoroalkyl substances
JP2024155878A