A polishing method for high-light arc-shaped edges of black slate plates

By using a composite polishing fluid of diamond micro powder, nano-silica, and modified travertine nanotubes, combined with ultrasonic vibration, the problems of unstable contact and uneven gloss of R10 rounded edges of black slabs were solved, achieving high gloss and surface uniformity in the processing of rounded edges of black slabs.

CN122851395BActive Publication Date: 2026-11-24GUANGDONG SANFI CERAMICS GRP CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611356269.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-24
Estimated Expiration
2046-09-03

AI Technical Summary

Technical Problem

During the R10 arc-shaped edge polishing process of black slab, the contact state between the polishing wheel and the arc surface is unstable, and the abrasive particles are prone to agglomeration and sedimentation, resulting in fluctuations in polishing load, local scratches, high surface roughness and uneven gloss, making it difficult to obtain a stable arc-shaped edge with high gloss and uniform surface quality.

Method used

A multi-scale abrasive system composed of diamond micro powder and nano-silica is used, which is combined with modified travertine nanotubes and two ionic liquids to form a composite ultra-fine polishing fluid. Through CNC rough grinding, graded fine grinding and ultrasonic-assisted ultra-fine polishing, grinding marks are removed step by step and the uniformity of gloss is improved.

Benefits of technology

It achieves high-precision machining of R10 arc surfaces, reduces the difference in surface roughness and gloss, reduces the number of compensation polishing times, and improves the machining quality and efficiency of R10 high-gloss arc-shaped edges of black slabs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses a grinding and polishing method for high-gloss rounded edges of black slabs, relating to the field of grinding and polishing technology. The method includes CNC rough grinding, graded fine grinding, ultrasonic-assisted ultra-fine polishing, and gloss calibration. By progressively reducing the abrasive grit size and applying ultrasonic vibration in the final polishing stage, the contact state between the polishing wheel and the rounded surface is stabilized. After polishing, the gloss at different locations is measured, and substandard areas are compensated for with additional polishing. Compared with existing technologies, this invention can reduce the surface roughness, number of scratches, and polishing load fluctuations of the rounded surface, reduce gloss differences, and improve the accuracy of the rounded contour, surface gloss uniformity, and processing stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of grinding and polishing technology, and in particular to a grinding and polishing method for high-gloss rounded edge of black slab. Background Technology

[0002] Black sintered stone slabs are characterized by their deep color, substantial texture, excellent wear resistance, and decorative properties, making them widely used in high-end countertops, furniture panels, and interior decorative components. To improve the feel and appearance of the slab's sides, they are typically machined into rounded shapes. Specifically, using R10 rounded edges allows for a smooth transition between the front and sides, reducing sharp edges and enhancing the overall product's integrity and decorative effect. For black sintered stone slabs, the surface roughness, gloss, and gloss consistency across different areas of the rounded surface directly impact the finished product's quality.

[0003] Existing slabs with rounded edges are typically processed through rough grinding, fine grinding, and polishing. Because the tangential direction and surface normal of the polishing wheel continuously change at different positions on the R10 rounded surface, it is difficult to maintain consistent contact area and pressure between the polishing wheel and the rounded surface at different locations. When the grinding wheel grit size, rotational speed, and feed rate are not properly matched, the grinding marks formed in the previous grinding stage are difficult to completely remove in subsequent stages, easily leading to high surface roughness, localized over-grinding, or a decrease in the accuracy of the rounded contour.

[0004] Black slabs, being darker in color, are more prone to showing defects such as fine scratches, matte finish, pitting, and localized darkening. Conventional polishing processes have limited abrasive particle size and precision, making it difficult to balance material removal efficiency and surface finishing. Furthermore, abrasive particles in the polishing slurry are prone to sedimentation, agglomeration, and localized enrichment, resulting in unstable abrasive concentration in the polishing contact area. This leads to fluctuations in polishing load, increased scratches, and inconsistent gloss levels at different locations on the curved surface.

[0005] Furthermore, existing processing techniques typically lack enhancements to the final polishing process and zonal inspection of post-processing gloss. When the polishing slurry is not adequately replenished and distributed on the curved surface, abrasive debris easily accumulates between the polishing wheel and the curved surface, causing repeated scratches or localized dry friction. If only an overall visual inspection is performed after polishing, it is difficult to promptly identify areas with insufficient gloss, requiring repeated rework, which affects processing efficiency and the consistency of batch products.

[0006] CN115805667A discloses a high-precision process for processing the beveled edges of slabs. This process involves cutting the slabs to size, chamfering them at 45°, removing dirt and dust, butt-jointing and bonding, and polishing, improving the ease and quality of splicing the beveled edges. CN109434664A discloses an automatic contour-tracking polishing device. This device acquires the workpiece contour using a laser sensor and compensates for the distance deviation between the polishing mechanism and the workpiece using an up-and-down moving mechanism, thereby improving polishing contact stability and precision. While these patents improve the processing or polishing performance of slabs from aspects such as beveled edge splicing and workpiece contour tracking, none of them integrate R10 arc contour forming, progressive fine grinding, ultrasonic-assisted ultra-fine polishing, and gloss calibration into a coordinated design. Furthermore, they lack a stable multi-scale abrasive supply mechanism suitable for the arc surfaces of black slab blanks. In actual processing, problems such as incomplete removal of previous grinding marks, abrasive settling or agglomeration, fluctuations in polishing load, localized scratches, and uneven gloss on the arc surfaces are still prone to occur. Therefore, developing a high-gloss arc-shaped edge grinding and polishing method for black slabs that can balance R10 arc contour accuracy, surface roughness, gloss, and processing stability is a technical problem that needs to be solved. Summary of the Invention

[0007] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is: when polishing the R10 arc-shaped edge of black slab, the tangential direction and surface normal of the arc surface change continuously along the circumferential direction, and the actual contact state between the polishing wheel and the arc surface is not easy to maintain. The abrasive particles in the conventional diamond polishing fluid are also prone to agglomeration and sedimentation, resulting in polishing load fluctuation, local scratches, high surface roughness and uneven gloss at different positions. Frequent compensation polishing is required, and it is difficult to stably obtain a high gloss and uniform surface quality arc-shaped edge.

[0008] To achieve the above objectives, the present invention provides a grinding and polishing method for the high-gloss rounded edge of black slab.

[0009] A method for grinding and polishing the high-gloss rounded edge of a black slab of rock includes the following steps:

[0010] Step 1, CNC rough grinding: The black slab is clamped on a CNC edge grinding machine and a diamond arc grinding wheel is used to rough grind the side to be processed to form an R10 arc surface, with a fine grinding allowance reserved.

[0011] Step 2, graded fine grinding: The arc surface formed by rough grinding is finely ground in stages by using a first diamond grinding wheel, a second diamond grinding wheel and a third diamond grinding wheel with different mesh sizes in sequence. During each stage of fine grinding, cooling water is used to cool and rinse the arc surface and the grinding wheels.

[0012] Step 3, Ultra-fine polishing: The finely ground arc surface is ultra-fine polished by sequentially using 1500-grit, 3000-grit, and 5000-grit resin-bonded polishing wheels. During the polishing process, a composite ultra-fine polishing solution is supplied between the polishing wheel and the arc surface. When the 5000-grit resin-bonded polishing wheel is used for the final polishing, ultrasonic vibration is applied to the polishing wheel or the arc surface.

[0013] Step 4, Gloss Calibration: Clean and dry the polished arc surface, and test the gloss at different locations on the arc surface; when the gloss at any test location is lower than the set value, use a 5000-mesh resin-bonded polishing wheel to perform compensatory polishing on the corresponding location.

[0014] In step 1, the thickness of the black slab is 10-12mm, and the Mohs hardness is 6-7; the diameter of the diamond arc grinding wheel is 25-35mm, the mesh size is 100-140, the grinding wheel speed is 3600-4400r / min, the feed speed is 6-10mm / s, and the fine grinding allowance is 0.2-0.4mm; the cooling water flow rate during the rough grinding process is 1.5-2.5L / min, and the water temperature is 20-25℃.

[0015] Preferably, the graded fine grinding is performed sequentially using diamond grinding wheels of 180-240 mesh, 350-450 mesh, and 700-900 mesh. The first diamond grinding wheel has a mesh size of 180-240, a rotation speed of 3200-3800 r / min, and a feed speed of 5-7 mm / s; the second diamond grinding wheel has a mesh size of 350-450, a rotation speed of 2700-3300 r / min, and a feed speed of 3-5 mm / s; the third diamond grinding wheel has a mesh size of 700-900, a rotation speed of 2200-2800 r / min, and a feed speed of 1-3 mm / s; after each stage of fine grinding, the arc surface and the corresponding diamond grinding wheel are rinsed with cooling water.

[0016] In step 3, the rotational speed of the resin-bonded polishing wheel is 1800-2200 r / min, the feed speed is 1.5-2.5 mm / s, and the polishing pressure is 0.08-0.12 MPa; the frequency of the ultrasonic vibration is 18-22 kHz, and the amplitude is 4-6 μm.

[0017] Preferably, during final polishing with a 5000-mesh resin-bonded polishing wheel, the ultrasonic vibration is applied to the polishing wheel or the arc surface to be processed.

[0018] Preferably, based on 100 kg of composite ultra-fine polishing fluid, the composite ultra-fine polishing fluid comprises: 14-18 kg of diamond micro powder with a particle size of 0.3-0.8 μm, 3-5 kg ​​of nano-silica with an average particle size of 20-40 nm, 0.2-0.4 kg of ammonium polyacrylate, 0.1-0.3 kg of polyvinylpyrrolidone, 1-2 kg of polyethylene glycol, 0.1-0.2 kg of alkyl glycoside, 0.05-0.15 kg of sodium gluconate, 0.02-0.05 kg of silicone defoamer, 0.6-1 kg of modified travertine nanotube aqueous dispersion with a solid content of 4-6%, and the balance being water.

[0019] Preferably, the preparation method of the modified travertine nanotube aqueous dispersion includes: dispersing travertine nanotubes in a mixture of water and anhydrous ethanol to obtain a travertine nanotube dispersion; adding an ionic liquid to the mixture of anhydrous ethanol and water to adjust the pH to obtain an ionic modified liquid; adding the ionic modified liquid to the travertine nanotube dispersion for reaction; and after the reaction is completed, cooling, centrifuging, washing, and redispersing in water to obtain the modified travertine nanotube aqueous dispersion.

[0020] More preferably, the preparation method of the modified travertine nanotube aqueous dispersion is as follows: Travertine nanotubes are added to a mixture of water and anhydrous ethanol, wherein the mass ratio of the travertine nanotubes to the mixture is 1:(80-120), and the mass ratio of water to anhydrous ethanol is (1-3):1. The mixture is stirred at 500-700 r / min for 20-40 min, and then ultrasonically dispersed for 15-30 min to obtain the travertine nanotube dispersion. An ionic liquid is added to a modified solvent composed of anhydrous ethanol and water, wherein the ionic liquid is used... The amount of ethanol is 10-20% of the mass of the travertine nanotubes, and the mass ratio of anhydrous ethanol to water is (3-5):1. The pH of the system is adjusted to 4-5, and the mixture is stirred for 20-40 min to obtain an ion-modified solution. The ion-modified solution is added dropwise to the travertine nanotube dispersion and reacted at 55-65℃ for 4-8 h. After the reaction is completed, the mixture is cooled to room temperature, centrifuged at 6000-9000 r / min for 8-15 min, washed with water 2-3 times, and then redispersed in water to obtain a modified travertine nanotube aqueous dispersion with a solid content of 4-6%.

[0021] Preferably, the ionic liquid is at least one of 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride and 1-hydroxyethyl-3-methylimidazolium phosphate dihydrogen salt; more preferably, the ionic liquid is formed by mixing 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride and 1-hydroxyethyl-3-methylimidazolium phosphate dihydrogen salt in a mass ratio of (1-3):(1-3).

[0022] Preferably, the preparation method of the composite ultra-fine polishing fluid is as follows: sodium gluconate, polyethylene glycol, polyvinylpyrrolidone and alkyl glycosides are added to a portion of water and stirred to dissolve, ammonium polyacrylate and nano silica are added and further dispersed; then diamond micro powder is added and stirred and ultrasonically dispersed to obtain a mixed dispersion; modified travertine nanotube aqueous dispersion is added to the mixed dispersion, stirred evenly, and then an organosilicon defoamer is added to adjust the pH of the system to 8, and water is added to the set mass to obtain the composite ultra-fine polishing fluid.

[0023] This invention employs a multi-scale abrasive system composed of diamond micropowder and nano-silica. Diamond micropowder is used to remove major protrusions and grinding marks on the arc surface, while nano-silica is used for fine finishing of minor depressions and residual scratches. Ammonium polyacrylate and polyvinylpyrrolidone can improve the dispersion stability of abrasive particles, while polyethylene glycol and alkyl glycosides can improve the wetting and lubrication of the polishing fluid on the arc surface.

[0024] Imazoite nanotubes are hydrated aluminosilicate nanomaterials with a hollow single-walled tubular structure. Their outer surface is mainly distributed with aluminum hydroxyl groups, while the inner surface is mainly distributed with silanol groups. They possess good hydrophilicity, a large aspect ratio, abundant surface hydroxyl groups, and ease of surface functionalization. Imazoite nanotubes can form a tubular dispersion network in aqueous phases, restricting the sedimentation of diamond powder and nano-silica. Their surface hydroxyl groups can also undergo silane condensation, hydrogen bonding, and ion association with functionalized imidazolium-type ionic liquids. Modified Imazoite nanotubes can improve the dispersion stability and interfacial hydration capacity of composite ultra-fine polishing slurries, and help maintain the continuity of the R10 arc-shaped polishing slurry film, reducing the probability of abrasive agglomeration, debris redeposition, and localized dry friction. Imazoite nanotubes synergistically modified with two ionic liquids can form abrasive-bearing and spatial barrier structures in the polishing slurry, inhibiting the sedimentation, agglomeration, and localized enrichment of diamond powder and nano-silica. Among them, triethoxysilyl imidazolium chloride is beneficial to improving the binding stability between the ion-modified components and the iridoid nanotubes, while hydroxyethyl imidazolium dihydrogen phosphate is beneficial to improving the hydrophilicity and interfacial lubrication properties of the modified nanotubes. The synergistic effect of the two can take into account interfacial anchoring, hydrophilic dispersion and lubrication regulation, so that the abrasive particles can enter the contact area between the polishing wheel and the R10 arc surface uniformly and continuously. Applying ultrasonic vibration during the final polishing process can promote the renewal and flow of polishing fluid at different positions on the arc surface, reduce the retention of abrasive debris and the local accumulation of abrasive particles, and make the contact load between the polishing wheel and the arc surface more stable, thereby reducing surface roughness and the number of scratches, and improving the gloss and uniformity of the arc surface.

[0025] The beneficial effects of this invention are:

[0026] 1. This invention uses a step-by-step processing method of CNC rough grinding, graded fine grinding and ultrasonic-assisted ultra-fine polishing to stably form an R10 arc surface, and gradually remove rough grinding marks and fine scratches, thereby improving the processing accuracy and surface finish of the arc surface.

[0027] 2. The present invention uses diamond micro powder, nano-silica and modified chalcedony nanotubes to form a composite polishing system, which can improve the suspension stability and distribution uniformity of abrasive particles, and reduce abrasive sedimentation, agglomeration and local enrichment.

[0028] 3. This invention can reduce the surface roughness of the arc surface and the gloss difference between different positions, improve the average gloss, reduce the number of compensation polishing times, and help improve the processing quality and production efficiency of R10 high-gloss arc-shaped edges of black slab. Detailed Implementation

[0029] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0030] The polyvinylpyrrolidone used is PVP K30 type polyvinylpyrrolidone produced by Henan Pengfei New Materials Co., Ltd.

[0031] The alkyl glycosides used are APG0810 type alkyl glycosides produced by Yangzhou Chenhua New Materials Co., Ltd.

[0032] Ammonium polyacrylate, product number: P856899, Shanghai Maclean Biochemical Technology Co., Ltd.;

[0033] The silicone defoamer is the AT-882 type silicone defoamer produced by Foshan Nanhai Datian Chemical Co., Ltd.

[0034] Other raw materials not mentioned are all common raw materials. The above content is only for the purpose of illustrating the present invention and should not be construed as a strict limitation of the present invention. Those skilled in the art can directly purchase the same / similar raw materials from the market or prepare them themselves.

[0035] The technical solutions of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] Comparative Example 1

[0037] A method for grinding and polishing the high-gloss rounded edge of a black slab of rock includes the following steps: Step 1, CNC rough grinding:

[0038] A black slab with a thickness of 11 mm and a Mohs hardness of 6.5 was used as the processing object. The black slab was clamped on a CNC-3020 CNC edge grinding machine, and a 30 mm diameter, 120-grit diamond arc grinding wheel was used to rough grind the side to be processed. The grinding wheel speed was 4000 r / min, the feed speed was 8 mm / s, and the water cooling system was turned on during the rough grinding process. The cooling water flow rate was 2 L / min and the temperature was 25℃. An R10 arc surface was formed, and a 0.3 mm fine grinding allowance was reserved. The surface roughness Ra of the arc surface after rough grinding was 2 μm.

[0039] Step 2, Graded Fine Grinding:

[0040] The arc surface formed by rough grinding was successively polished using 200-mesh, 400-mesh, and 800-mesh diamond grinding wheels. During the fine grinding process, the water cooling system was continuously turned on, with a cooling water flow rate of 2L / min and a water temperature controlled at 25℃.

[0041] The first stage of fine grinding was performed using a 200-mesh diamond grinding wheel at a speed of 3500 r / min and a feed rate of 6 mm / s. The surface roughness Ra of the arc surface after fine grinding was 1.2 μm.

[0042] The second stage of fine grinding was performed using a 400-mesh diamond grinding wheel at a speed of 3000 r / min and a feed rate of 4 mm / s. The surface roughness Ra of the arc surface after fine grinding was 0.8 μm.

[0043] The third stage of fine grinding was performed using an 800-mesh diamond grinding wheel at a speed of 2500 r / min and a feed rate of 2 mm / s. The surface roughness Ra of the arc surface after fine grinding was 0.5 μm.

[0044] After each stage of fine grinding is completed, the arc surface is rinsed with cooling water to remove the grinding debris adhering to the arc surface and the grinding wheel surface, so as to prevent the coarse grinding debris generated by the previous stage of grinding from entering the fine grinding area of ​​the next stage.

[0045] Step 3, Ultra-fine polishing:

[0046] The polishing was performed sequentially using 1500-mesh, 3000-mesh, and 5000-mesh resin-bonded polishing wheels on their arc surfaces, along with a diamond polishing slurry with a particle size of 0.5 μm and a solid content of 20%. The polishing wheel speed was 2000 r / min, the feed rate was 2 mm / s, and the polishing pressure was 0.1 MPa.

[0047] After polishing with a 1500-mesh resin-bonded polishing wheel, the surface roughness Ra of the arc surface was reduced to 0.3 μm; after polishing with a 3000-mesh resin-bonded polishing wheel, the surface roughness Ra of the arc surface was reduced to 0.2 μm; when using a 5000-mesh resin-bonded polishing wheel for final polishing, ultrasonic vibration with a frequency of 20 kHz and an amplitude of 5 μm was activated, and polishing was performed continuously for 6 times.

[0048] Step 4, Gloss Standard:

[0049] After polishing, the curved surface is rinsed with water and dried. Then, a 60° angle gloss meter is used to test the gloss of the curved surface. When the gloss is lower than 85 GU, a 5000-grit polishing wheel is used for local compensation polishing until the requirements are met.

[0050] Comparative Example 2

[0051] A method for grinding and polishing the high-gloss rounded edge of a black slab of rock includes the following steps: Step 1, CNC rough grinding:

[0052] A black slab with a thickness of 11 mm and a Mohs hardness of 6.5 was used as the processing object. The black slab was clamped on a CNC-3020 CNC edge grinding machine, and a 30 mm diameter, 120-grit diamond arc grinding wheel was used to rough grind the side to be processed. The grinding wheel speed was 4000 r / min, the feed speed was 8 mm / s, and the water cooling system was turned on during the rough grinding process. The cooling water flow rate was 2 L / min and the temperature was 25℃. An R10 arc surface was formed, and a 0.3 mm fine grinding allowance was reserved. The surface roughness Ra of the arc surface after rough grinding was 2 μm.

[0053] Step 2, Graded Fine Grinding:

[0054] The arc surface formed by rough grinding was successively polished using 200-mesh, 400-mesh, and 800-mesh diamond grinding wheels. During the fine grinding process, the water cooling system was continuously turned on, with a cooling water flow rate of 2L / min and a water temperature controlled at 25℃.

[0055] The first stage of fine grinding was performed using a 200-mesh diamond grinding wheel at a speed of 3500 r / min and a feed rate of 6 mm / s. The surface roughness Ra of the arc surface after fine grinding was 1.2 μm.

[0056] The second stage of fine grinding was performed using a 400-mesh diamond grinding wheel at a speed of 3000 r / min and a feed rate of 4 mm / s. The surface roughness Ra of the arc surface after fine grinding was 0.8 μm.

[0057] The third stage of fine grinding was performed using an 800-mesh diamond grinding wheel at a speed of 2500 r / min and a feed rate of 2 mm / s. The surface roughness Ra of the arc surface after fine grinding was 0.5 μm.

[0058] After each stage of fine grinding is completed, the arc surface is rinsed with cooling water to remove the grinding debris adhering to the arc surface and the grinding wheel surface, so as to prevent the coarse grinding debris generated by the previous stage of grinding from entering the fine grinding area of ​​the next stage.

[0059] Step 3, Ultra-fine polishing:

[0060] The arc surface was ultra-fine polished sequentially using 1500-mesh, 3000-mesh, and 5000-mesh resin-bonded polishing wheels, with a composite ultra-fine polishing fluid used throughout the polishing process; the polishing wheel speed was 2000 r / min, the feed speed was 2 mm / s, and the polishing pressure was 0.1 MPa.

[0061] After polishing with a 1500-mesh resin-bonded polishing wheel, the surface roughness Ra of the arc surface was reduced to 0.3 μm; after polishing with a 3000-mesh resin-bonded polishing wheel, the surface roughness Ra of the arc surface was reduced to 0.2 μm; when using a 5000-mesh resin-bonded polishing wheel for final polishing, ultrasonic vibration with a frequency of 20 kHz and an amplitude of 5 μm was activated, and polishing was performed continuously for 6 times.

[0062] Step 4, Gloss Standard:

[0063] After polishing, the curved surface is rinsed with water and dried. Then, a 60° angle gloss meter is used to test the gloss of the curved surface. When the gloss is lower than 85 GU, a 5000-grit polishing wheel is used for local compensation polishing until the requirements are met.

[0064] The preparation method of the composite ultra-fine polishing fluid is as follows: Taking the preparation of 100kg of composite ultra-fine polishing fluid as an example, weigh 16kg of diamond micro powder with a particle size of 0.5μm, 4kg of nano-silica with an average particle size of 20-40nm, 0.3kg of ammonium polyacrylate, 0.2kg of polyvinylpyrrolidone, 1.5kg of polyethylene glycol 400, 0.15kg of alkyl glycoside, 0.1kg of sodium gluconate, 0.03kg of organosilicon defoamer, and 77.72kg of water; first, add sodium gluconate, polyethylene glycol 400, polyvinylpyrrolidone, and alkyl glycoside to 1 / 3 of the water and stir at 500r / min for 10min; add ammonium polyacrylate and nano-silica and continue stirring for 15min; add diamond micro powder and stir at 800r / min for 20min and ultrasonically disperse for 10min; finally, add organosilicon defoamer, adjust the pH to 8, add the remaining water to a total mass of 100kg, stir evenly, and obtain the composite ultra-fine polishing fluid.

[0065] Comparative Example 3

[0066] It is basically the same as Comparative Example 2, except that the composite ultra-fine polishing fluid is different.

[0067] Taking the preparation of 100kg of composite ultra-fine polishing fluid as an example, the following are weighed: 16kg of diamond micro powder with a particle size of 0.5μm, 4kg of nano-silica with an average particle size of 20-40nm, 0.3kg of ammonium polyacrylate, 0.2kg of polyvinylpyrrolidone, 1.5kg of polyethylene glycol 400, 0.15kg of alkyl glycoside, 0.1kg of sodium gluconate, 0.03kg of organosilicon defoamer, 0.8kg of 5% solid content imacite nanotube aqueous dispersion, and 76.92kg of water; first, sodium gluconate, polyethylene glycol 400, and polyvinylpyrrolidone... Ketones and alkyl glycosides were added to 1 / 3 of the water and stirred at 500 rpm for 10 min. Ammonium polyacrylate and nano-silica were added and stirred for another 15 min. Diamond micro powder was added and stirred at 800 rpm for 20 min and ultrasonically dispersed for 10 min to obtain a mixed dispersion. Iridium chalcedony nanotube aqueous dispersion was added to the above mixed dispersion and stirred at 500 rpm for another 15 min. Finally, organosilicon defoamer was added, the pH was adjusted to 8, and the remaining water was added to a total mass of 100 kg. The mixture was stirred evenly to obtain a composite ultra-fine polishing solution.

[0068] Example 1

[0069] It is basically the same as Comparative Example 2, except that the composite ultra-fine polishing fluid is different.

[0070] Taking the preparation of 100kg of composite ultra-fine polishing fluid as an example, 16kg of diamond micro powder with a particle size of 0.5μm, 4kg of nano-silica with an average particle size of 20-40nm, 0.3kg of ammonium polyacrylate, 0.2kg of polyvinylpyrrolidone, 1.5kg of polyethylene glycol 400, 0.15kg of alkyl glycoside, 0.1kg of sodium gluconate, 0.03kg of organosilicon defoamer, 0.8kg of modified travertine nanotube aqueous dispersion with a solid content of 5%, and 76.92kg of water are weighed.

[0071] The modified piranite nanotube aqueous dispersion is prepared as follows: 5g of piranite nanotubes are added to a mixture of 350g water and 150g anhydrous ethanol, stirred at 600r / min for 30min, and then ultrasonically dispersed for 20min to obtain a piranite nanotube dispersion; 0.75g of ionic liquid is added to 20g anhydrous ethanol and 5g water, the pH is adjusted to 4.5, and stirred for 30min to obtain an ion-modified liquid; the ion-modified liquid is added dropwise to the piranite nanotube dispersion, reacted at 60℃ for 6h, cooled, centrifuged, washed, and redispersed in water, and the solid content is adjusted to 5% to obtain the modified piranite nanotube aqueous dispersion; the ionic liquid is 1-methyl-3-[3-(triethoxysilyl)propyl] Imidazolium chloride (CAS: 338741-79-0) and 1-hydroxyethyl-3-methylimidazolium dihydrogen phosphate (CAS: 1803314-42-2) are mixed in a mass ratio of 2:1.

[0072] Example 2

[0073] It is basically the same as Example 1, except that the ionic liquid is 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride.

[0074] Example 3

[0075] It is basically the same as Example 1, except that the ionic liquid is 1-hydroxyethyl-3-methylimidazolium phosphate.

[0076] Comparative Example 4

[0077] The method is basically the same as Example 1, except that: instead of preparing modified travertine nanotubes in advance, travertine nanotubes and two ionic liquids are added to the composite ultra-fine polishing solution.

[0078] Taking the preparation of 100kg of composite ultra-fine polishing fluid as an example, the following are weighed: 16kg of diamond micro powder with a particle size of 0.5μm, 4kg of nano-silica with an average particle size of 20-40nm, 0.3kg of ammonium polyacrylate, 0.2kg of polyvinylpyrrolidone, 1.5kg of polyethylene glycol 400, 0.15kg of alkyl glycoside, 0.1kg of sodium gluconate, 0.03kg of organosilicon defoamer, 0.0348kg of iridoid nanotubes, 0.0035kg of 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride, 0.0017kg of 1-hydroxyethyl-3-methylimidazolium dihydrogen phosphate, and 77.68kg of water.

[0079] First, disperse diamond micro powder and nano silica according to the method of Comparative Example 2. Then, add chalcedony nanotubes and two ionic liquids directly to the resulting mixed dispersion in sequence. Stir at 500 r / min for 15 min. Finally, add organosilicon defoamer and adjust the pH to 8 to obtain a composite ultra-fine polishing liquid.

[0080] Comparative Example 5

[0081] It is basically the same as Example 1, except that: no iridescent travertine nanotubes are added to the composite ultrafine polishing liquid, only two kinds of free ionic liquids are added.

[0082] Taking the preparation of 100kg of composite ultra-fine polishing fluid as an example, the following are weighed: 16kg of diamond micro powder, 4kg of nano silica, 0.3kg of ammonium polyacrylate, 0.2kg of polyvinylpyrrolidone, 1.5kg of polyethylene glycol 400, 0.15kg of alkyl glycoside, 0.1kg of sodium gluconate, 0.03kg of organosilicon defoamer, 0.0035kg of 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride, 0.0017kg of 1-hydroxyethyl-3-methylimidazolium dihydrogen phosphate, and 77.7148kg of water.

[0083] The two ionic liquids were added after the diamond powder and nano silica were dispersed, and the remaining preparation steps were the same as those in Comparative Example 2.

[0084] Example 4

[0085] It is basically the same as Example 1, except that the ionic liquid is composed of 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride and 1-hydroxyethyl-3-methylimidazolium phosphate dihydrogen salt in a mass ratio of 1:2.

[0086] Test Example 1

[0087] Twenty samples of black slabs from the same batch, 11 mm thick and with a Mohs hardness of 6.5, were selected for each group. R10 rounded edges were formed according to the processing methods of each embodiment and comparative example. The same grinding wheel, polishing wheel, equipment, and processing procedure were used for each group, and testing was conducted after a final polishing with 5000 grit.

[0088] (1) Surface roughness:

[0089] The surface roughness Ra of the arc surface was detected using a three-dimensional white light interferometric profilometer. Three positions—front, middle, and rear—were selected along the length of the arc shape edge of each sample, and a detection point was selected at the top, middle, and bottom of the arc at each position. The measurement profile was extracted along the length of the arc shape edge at each detection point. After fitting and subtracting the R10 macroscopic arc profile, Ra was calculated. The average value of the nine detection points was taken as the surface roughness of the sample.

[0090] (2) Gloss and gloss difference:

[0091] The gloss of the above 9 test points was measured using a small-aperture 60° angle gloss meter equipped with a curved surface positioning fixture. During the measurement, the tangent plane of the arc at the test point was kept consistent with the measurement reference plane of the instrument by using the positioning fixture. The average gloss of each test point was calculated, and the difference between the maximum gloss and the minimum gloss was taken as the gloss difference value.

[0092] (3) Number of scratches:

[0093] The arc surface was observed using a 200x digital microscope. Five fields of view were randomly selected for each sample. Linear scratches with a length of not less than 50 μm were counted and converted into the number of scratches per square centimeter on the arc surface.

[0094] (4) Compensation polishing rate

[0095] After six rounds of 5000-grit polishing, nine gloss measurement points were tested on each sample. If the gloss level at any measurement point was below 85 GU, the sample was deemed to require compensation polishing. The percentage of samples requiring compensation polishing out of the total number of samples in the group is the compensation polishing rate.

[0096] (5) Polishing load fluctuation test:

[0097] During the final polishing process using a 5000-mesh resin-bonded polishing wheel, the spindle current of the edge grinding machine was collected at a frequency of 10 times / s. Data from the beginning and end of each polishing stage were removed, and the coefficient of variation of the spindle current during the stable polishing stage was calculated as the polishing load fluctuation coefficient. A lower polishing load fluctuation coefficient indicates a more stable friction and contact state between the polishing wheel and the R10 arc surface.

[0098] Table 1 Test results of polishing quality of R10 rounded edge of black slab.

[0099] As shown in Table 1, Example 1 has the lowest surface roughness, gloss difference, number of scratches, compensated polishing rate, and polishing load fluctuation coefficient, and the highest average gloss. This indicates that the synergistic modification of the travertine nanotubes with two ionic liquids can improve the dispersion uniformity of diamond powder and nano silica, and improve the wettability and interfacial stability of the polishing liquid, so that the abrasive can act continuously and uniformly on the R10 arc surface.

[0100] Comparative Example 1, lacking a composite polishing system, resulted in abrasive agglomeration and poor polishing quality. Comparative Example 2, with the addition of nano-silica and dispersing agents, improved abrasive dispersibility. Comparative Example 3 further incorporated illite nanotubes, whose tubular structure helped stabilize abrasive particles; however, the unmodified nanotubes still tended to aggregate. Examples 2 and 3, using only one type of ionic liquid for modification, lacked either hydrophilic lubrication or stabilizing anchoring effects, resulting in performance lower than Example 1. Comparative Example 4, without pre-modified nanotubes, showed insufficient bonding between the ionic liquid and nanotubes. Comparative Example 5, lacking nanotubes, failed to form an effective abrasive bearing structure. In Example 4, changing the ratio of the two ionic liquids decreased the balance between interfacial anchoring and hydrophilic lubrication, thus its overall performance was slightly lower than Example 1.

[0101] Test Example 2

[0102] Polishing slurry stratification stability test:

[0103] 100 mL of the polishing solution used in each example and its comparative example was placed in a stoppered graduated cylinder, with three parallel samples for each polishing solution. The samples were allowed to stand at 25°C for 7 days, and the percentage of the height of the supernatant liquid relative to the total height of the polishing solution was measured. The average value of the three parallel samples was taken as the stratification rate after 7 days of standing. A lower stratification rate indicates better suspension stability of the polishing solution for diamond micropowder and nano-silica.

[0104] Table 2. Test results of the stratification stability of the polishing slurry after 7 days of standing.

[0105] As shown in Table 2, Example 1 exhibited the lowest stratification rate after 7 days of standing, indicating that its polishing slurry had the best suspension stability. The synergistic modification with the two ionic liquids improved the dispersibility of travertine nanotubes in the aqueous phase and enhanced the interfacial interaction between them and diamond powder and nano-silica, thereby inhibiting abrasive sedimentation and agglomeration.

[0106] Comparative Example 1 lacked an effective dispersing and stabilizing component, resulting in the highest stratification rate. Comparative Example 2 showed improved stability after the addition of a polymeric dispersant. Comparative Example 3, with the addition of unmodified travertine nanotubes, could slow sedimentation through spatial barrier effects, but the nanotubes themselves were still prone to aggregation. Examples 2 and 3 used single ionic liquid modification, resulting in less stabilizing effects than the compound system. Comparative Example 4, lacking pre-modification, struggled to form a stable surface-modified layer. Comparative Example 5 lacked the spatial support effect of travertine nanotubes. In Example 4, due to the altered ratio of the two ionic liquids, the interfacial anchoring and hydrophilic dispersion effects did not reach an optimal balance, thus resulting in a higher stratification rate than Example 1.

[0107] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A grinding and polishing method for high-gloss rounded arc-shaped edges of black slabs, characterized in that, Includes the following steps: Step 1, CNC rough grinding: The black slab is clamped on a CNC edge grinding machine, and a diamond arc grinding wheel is used to rough grind the side of the black slab to be processed to form an R10 arc surface, with a fine grinding allowance reserved. Step 2, graded fine grinding: The arc surface formed by rough grinding is finely ground in stages by using a first diamond grinding wheel, a second diamond grinding wheel and a third diamond grinding wheel with different mesh sizes in sequence. During each stage of fine grinding, cooling water is used to cool and rinse the arc surface and the corresponding diamond grinding wheel. Step 3, Ultra-fine polishing: The finely ground arc surface is ultra-fine polished by sequentially using 1500-mesh, 3000-mesh and 5000-mesh resin-bonded polishing wheels. During the polishing process, a composite ultra-fine polishing fluid is supplied between the polishing wheel and the arc surface. When the 5000-mesh resin-bonded polishing wheel is used for final polishing, ultrasonic vibration is applied to the polishing wheel or the arc surface. Step 4, Gloss calibration: Clean and dry the ultra-polished arc surface, and test the gloss at different positions on the arc surface. When the gloss at any test position is lower than the set gloss, use a 5000-mesh resin-bonded polishing wheel to perform compensatory polishing on the corresponding position. Based on 100 kg of composite ultra-fine polishing fluid, the composite ultra-fine polishing fluid comprises 14-18 kg of diamond micro powder with a particle size of 0.3-0.8 μm, 3-5 kg ​​of nano-silica with an average particle size of 20-40 nm, 0.2-0.4 kg of ammonium polyacrylate, 0.1-0.3 kg of polyvinylpyrrolidone, 1-2 kg of polyethylene glycol, 0.1-0.2 kg of alkyl glycoside, 0.05-0.15 kg of sodium gluconate, 0.02-0.05 kg of organosilicon defoamer, 0.6-1 kg of modified travertine nanotube aqueous dispersion with a solid content of 4-6%, and the balance being water; The preparation method of the modified travertine nanotube aqueous dispersion includes: dispersing travertine nanotubes in a mixture of water and anhydrous ethanol to obtain a travertine nanotube dispersion; adding an ionic liquid to a modified solvent composed of anhydrous ethanol and water to adjust the pH of the system to obtain an ionic modified liquid; adding the ionic modified liquid dropwise to the travertine nanotube dispersion for reaction; and after the reaction is completed, cooling, centrifuging, washing, and redispersing in water to obtain the modified travertine nanotube aqueous dispersion. The mass ratio of the epidermal nanotubes to the mixture is 1:(80-120), the mass ratio of water to anhydrous ethanol in the mixture is (1-3):1, the epidermal nanotubes are stirred at 500-700 r / min for 20-40 min, and then ultrasonically dispersed for 15-30 min; the amount of the ionic liquid is 10-20% of the mass of the epidermal nanotubes, the mass ratio of anhydrous ethanol to water in the modified solvent is (3-5):1, the pH of the ionic modified liquid is 4-5; the reaction temperature is 55-65℃, the reaction time is 4-8 h; the reaction product is centrifuged at 6000-9000 r / min for 8-15 min, washed with water 2-3 times, and then redispersed in water; The ionic liquid is composed of 1-methyl-3-[3-(triethoxysilyl)propyl]imidazolium chloride and 1-hydroxyethyl-3-methylimidazolium dihydrogen phosphate in a mass ratio of (1-3):(1-3).

2. The grinding and polishing method for the high-gloss rounded arc-shaped edge of black slab as described in claim 1, characterized in that: In step 1, the thickness of the black slab is 10-12mm, and the Mohs hardness is 6-7; the diameter of the diamond arc grinding wheel is 25-35mm, the mesh size is 100-140, the grinding wheel speed is 3600-4400r / min, the feed speed is 6-10mm / s, and the fine grinding allowance is 0.2-0.4mm; the cooling water flow rate during the rough grinding process is 1.5-2.5L / min, and the water temperature is 20-25℃.

3. The grinding and polishing method for the high-gloss rounded arc-shaped edge of black slab as described in claim 1, characterized in that: In step 2, the mesh sizes of the first diamond grinding wheel, the second diamond grinding wheel, and the third diamond grinding wheel are 180-240 mesh, 350-450 mesh, and 700-900 mesh, respectively.

4. The grinding and polishing method for the high-gloss rounded arc-shaped edge of black slab as described in claim 1, characterized in that: The first diamond grinding wheel has a mesh size of 180-240, a rotation speed of 3200-3800 r / min, and a feed speed of 5-7 mm / s; the second diamond grinding wheel has a mesh size of 350-450, a rotation speed of 2700-3300 r / min, and a feed speed of 3-5 mm / s; the third diamond grinding wheel has a mesh size of 700-900, a rotation speed of 2200-2800 r / min, and a feed speed of 1-3 mm / s; after each stage of fine grinding, the arc surface and the corresponding diamond grinding wheel are rinsed with cooling water.

5. The grinding and polishing method for the high-gloss rounded arc-shaped edge of black slab as described in claim 1, characterized in that: In step 3, the rotational speed of the resin-bonded polishing wheel is 1800-2200 r / min, the feed speed is 1.5-2.5 mm / s, and the polishing pressure is 0.08-0.12 MPa; the frequency of the ultrasonic vibration is 18-22 kHz, and the amplitude is 4-6 μm.

6. The grinding and polishing method for the high-gloss rounded arc-shaped edge of black slab as described in claim 1, characterized in that: In step 4, the gloss of the arc surface is detected using a 60° angle gloss meter, and the set gloss is 85 GU. After gloss calibration, the surface roughness Ra of the arc surface is not greater than 0.2 μm, the average gloss is not less than 85 GU, and the gloss difference between different detection positions of the arc surface is not greater than 3 GU.

Citation Information

Patent Citations

  • Automatic-contour-tracking polishing device

    CN109434664A

  • High-precision rock plate bevel edge treatment process

    CN115805667A

  • Rare earth polishing powder and preparation method thereof

    CN103555206A

  • Special polishing agent for marble

    CN108342158A