A stretching process for a bopp capacitive film base film
By using high isotactic homopolymer polypropylene resin and dynamic temperature control technology, the stretching process of BOPP capacitor film base film was optimized, solving the problems of insufficient dielectric breakdown strength and thermal shrinkage rate in existing technologies, and improving the dimensional stability and dielectric properties of the film at high temperatures.
Patent Information
- Application Number
- CN202611373470.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-09-07
AI Technical Summary
Existing thin-film dielectric processing technologies are insufficient in terms of enhancing dielectric breakdown strength, controlling high-temperature dielectric loss and thermal shrinkage when facing the increasing demands of capacitor operation. This makes it difficult to meet the high operating voltage, temperature and energy density requirements of new energy vehicle inverter systems, flexible DC power transmission, ultra-high voltage power transmission and high-frequency power electronic equipment.
Using high isotactic homopolymer polypropylene resin, the actual film temperature in the longitudinal and transverse stretching zones is controlled below the material crystal melting initiation temperature. Combined with a nano-ceramic composite anti-sticking layer containing fluorine and low surface energy, the biaxial orientation uniformity during the stretching process is optimized. Dynamic temperature control and multi-stage cooling are achieved through linear velocity and tension feedforward compensation combined with adaptive fuzzy proportional-integral-derivative control.
The dielectric breakdown strength of the BOPP capacitor film base film was improved, the high-temperature dielectric loss and thermal shrinkage rate were reduced, and the dimensional stability and thickness uniformity of the film were ensured, meeting the requirements for capacitor use at high temperatures.
Smart Images

Figure SMS_22
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer material processing and thin film dielectric technology, specifically a stretching process for BOPP capacitor film base film. Background Technology
[0002] Biaxially oriented polypropylene film has low dielectric loss, high volume resistivity, chemical resistance and self-healing properties, and is widely used in metallized film capacitors, pulse capacitors, AC filter capacitors and high voltage capacitors for new energy vehicles. With the development of new energy vehicle inverter systems, flexible DC power transmission, ultra-high voltage power transmission and high frequency power electronic equipment, the operating voltage, operating temperature and energy density of capacitors are constantly increasing, requiring capacitor films to have high dielectric breakdown strength, low dielectric loss at high temperature, low thermal shrinkage rate and high thickness uniformity. Summary of the Invention
[0003] To address the shortcomings of existing thin-film dielectric processing technologies in enhancing dielectric breakdown strength, controlling high-temperature dielectric loss and thermal shrinkage when facing increased capacitor operating requirements, this invention proposes a stretching process for BOPP capacitor film base films that improves biaxial orientation uniformity and optimizes film dimensional stability during the stretching process. The specific technical solution is as follows: A stretching process for a BOPP capacitor film base film includes the following steps: S1. The pure polypropylene resin is screened, dusted, and dehumidified and dried. S2. Pure polypropylene resin is melt-extruded, filtered, and formed by a flat die, and then cooled and cast on a casting roller at a temperature of 60-105℃. S3. The casting sheet is fed into the preheating and temperature homogenization zone, and preheating and temperature homogenization are performed sequentially on the heating rollers. S4. The homogenized film is fed into the synchronous stretching zone for simultaneous longitudinal and transverse stretching. The actual temperature of the film in the synchronous stretching zone is controlled at 140-165℃, the longitudinal stretching ratio is 5.3-8.0 times, and the transverse stretching ratio is 7.0-9.0 times. S5. While maintaining longitudinal tension and transverse clamping, heat-set the transversely stretched film at 160-175℃ for 1.5-5 seconds. S6. The heat-set film is successively cooled at 110-125℃, 80-105℃, 50-75℃ and 20-45℃. After cooling to a temperature of less than or equal to 40℃, online thickness detection, defect detection and winding are performed. In particular, the actual temperature of the film in the synchronous stretching zone is lower than the crystal melting initiation temperature of the polypropylene resin used, which is measured by differential scanning calorimetry. The test conditions of differential scanning calorimetry are as follows: under a high-purity nitrogen protective atmosphere, the film is continuously heated from 25°C to 200°C at a nominal heating rate of 10°C / min. During the stretching process, dynamic temperature control is achieved by combining linear velocity and tension feedforward compensation with the output heating compensation power controlled by the concealed multi-channel flow channel inside the heating roller.
[0004] Preferably, the pure polypropylene resin is a high isotactic homopolymer polypropylene resin with a mass fraction of 100%, and no other chemical nucleating agents, antioxidants, or acid absorbers are added to the raw material formulation. Here, a mass fraction of 100% indicates that only high isotactic homopolymer polypropylene resin is used in the resin raw material formulation, not that the chemical purity of the resin is 100%. The high isotactic homopolymer polypropylene resin has an isotacticity index of 96.5-99.5%, a melt flow rate of 1.5-5.0 g / 10 min at 230℃ and 2.16 kg, a weight-average molecular weight to number-average molecular weight ratio of 4.0-8.0, and a melting peak temperature of 164-170℃.
[0005] Preferably, in S1, the pure polypropylene resin is dried in dehumidified air at 60-90°C for 2-6 hours, and the moisture content after drying is controlled below 100ppm; the pure polypropylene resin does not require masterbatch premixing and can directly enter the extrusion process.
[0006] Preferably, in S2, the extruder adopts segmented heating along the material conveying direction, wherein the segmented temperatures are 40-60℃ for the feeding section, 190-215℃ for the compression section, 205-235℃ for the metering section, and 240-260℃ for the die head and melt pipeline; the melt is filtered through a 10-25μm continuous melt filter, the thickness of the cast sheet is 0.3-2.0mm, and the surface temperature uniformity of the cast sheet roller is controlled within ±0.5℃.
[0007] Preferably, the preheating and temperature homogenization zone uses a heating roller with a composite anti-stick layer, which comprises, from the inside out: a metal or ceramic transition layer with a thickness of 10-50 μm, a nano-ceramic layer with a thickness of 5-30 μm, and a fluorine-containing low surface energy layer. The fluorinated low surface energy layer is composed of one or more of polytetrafluoroethylene, perfluoroalkoxy resin, or fluorinated inorganic-organic composite materials; the total thickness of the composite anti-stick layer is 20-150 μm, and the surface roughness Ra is 0.05-0.30 μm; the heating roller is provided with a multi-channel spiral flow channel inside, and an electromagnetic induction heating device is provided on the outer layer, and the roller surface temperature is calibrated by multi-point temperature detection and infrared thermometry.
[0008] Preferably, the preheating zone of S3 controls the actual film temperature to 120-165℃, and the temperature homogenization zone controls the actual film temperature to 140-150℃, using one or more of double-sided hot air, infrared radiation, or hot rollers for thickness-direction temperature homogenization; the synchronous stretching zone is equipped with synchronous clamps, and the synchronous stretching is completed by the expansion of the track and longitudinal acceleration of the synchronous clamps, and a segmented longitudinal strain rate with gradually increasing values is used along the stretching direction: the initial stretching segment is 20-60s. -1 The intermediate stretching period is 60-120 seconds. -1 The subsequent stretching period is 100-180 seconds. -1 .
[0009] Preferably, in S4, the synchronous stretching zone is provided with 2-5 synchronous stretching sub-zones with independent control of temperature, longitudinal speed and track spacing.
[0010] Preferably, in S5, the longitudinal tension during heat setting is adjusted by the longitudinal speed of the synchronous clamp, and the lateral spacing of the synchronous clamp remains unchanged or is retracted, with a retraction rate of 1%-10%; in S6, the temperature difference between adjacent cooling zones is controlled by a step-by-step cooling method, and the temperature difference between adjacent cooling zones is less than or equal to 40°C.
[0011] Preferably, the stretching process employs a combination of linear velocity and tension feedforward compensation with adaptive fuzzy proportional-integral-derivative (FID) control. The input parameters of this adaptive fuzzy proportional-integral-derivative (FID) control include production line speed, film width, film thickness, initial temperature of the film entering the heating zone, film tension, roller surface temperature, transverse temperature distribution of the film, ambient temperature, and cooling airflow. When the production line speed, film thickness, or film tension changes, the heating power is first adjusted through feedforward compensation, and then the heating compensation power is output through fuzzy proportional-integral-derivative (FID) control. A local hardware adjustment device consisting of a concealed multi-channel flow channel and an embedded temperature sensor located inside the heating roller is adopted. When the production line speed, film thickness or film tension changes, the heating power is first adjusted by feedforward compensation, and then the heating compensation power is output by adjusting the medium flow rate of the internal concealed flow channel. The film temperature is measured by an infrared temperature measurement system that has been calibrated by emissivity, thickness correction and standard blackbody calibration.
[0012] Preferably, the film after synchronous stretching maintains lateral clamping tension during heat setting and multi-stage cooling. After cooling to a temperature less than or equal to 40°C, it undergoes single-sided or double-sided corona treatment and is wound up using tapered tension control. The wound film is then cured at 40-60°C.
[0013] The beneficial effects of this invention are as follows: By using 100% high isotactic homopolymer polypropylene resin, the strain hardening ability during stretching is improved; by controlling the actual film temperature in the longitudinal and transverse stretching zones below the material crystal melting initiation temperature, the biaxial orientation uniformity is improved; and by using a nano-ceramic composite anti-stick layer with a fluorine-containing low surface energy layer, the adhesion, scratches, and surface defects between the sheet and the roller surface during high-temperature stretching are reduced. Detailed Implementation
[0014] The technical solutions in the embodiments of the present invention will be clearly and completely described below; the described embodiments are some embodiments of the present invention, but not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention. Example 1: This example provides a stretching process for the BOPP capacitor film base film, specifically including the following steps: S1. Raw material pretreatment and mixing High isotactic homopolymer polypropylene resin was selected, with an isotacticity index of 98.8%. At 230℃ and 2.16 kg, the melt flow rate was 2.3 g / 10 min, the weight-average molecular weight to number-average molecular weight ratio was 5.6, the melting peak temperature was 167.2℃, and the crystal melting initiation temperature was 159.8℃, determined by differential scanning calorimetry. The isotacticity index was determined by carbon nuclear magnetic resonance spectroscopy. The ratio of weight-average molecular weight to number-average molecular weight was determined by gel permeation chromatography in trichlorobenzene solvent at 150℃; the specific test conditions for differential scanning calorimetry were as follows: under a high-purity nitrogen protective atmosphere, the temperature was continuously increased from 25℃ to 200℃ at a nominal heating rate of 10℃ / min, the endothermic curve was recorded, and the temperature at the intersection of the baseline extension line of the endothermic peak deviating from the baseline and the tangent line at the maximum slope of the endothermic peak front was recorded as the crystal melting initiation temperature; The raw material composition by mass percentage is as follows: based on the total mass of resin raw materials, the raw material composition is 100% high-grade homopolymer polypropylene resin; after screening and dust removal, the pure polypropylene resin is directly processed by a metal detector and a magnetic iron removal device before entering the next stage. S2, melt extrusion and casting The mixture is fed into a single screw extruder; the temperatures of each section of the extruder are set sequentially as follows: feeding section 180℃, compression section 205℃, metering section 222℃, and die head and melt pipeline 228℃; the melt is filtered through a 15μm continuous melt filter and then extruded through a flat die onto a 35℃ casting roller for cooling and forming. The surface temperature uniformity of the casting roll is controlled within ±0.5℃ to obtain a casting sheet with a thickness of 0.92mm; after edge trimming and online thickness measurement, the casting sheet enters the longitudinal stretching section. S3, Preheating and Temperature Homogenization The preheating zone uses heating rollers for preheating, and the actual measured temperature of the film is controlled at 142℃. The temperature homogenization zone uses a combination of double-sided hot air and hot rollers, and the actual measured temperature of the film is controlled at 148℃, while the temperature difference in the film thickness direction is controlled at 1.4℃. The preheating and homogenization zone uses a heating roller with a composite anti-stick layer. The composite anti-stick layer consists of a metal transition layer, a nano-ceramic layer, and a fluorine-containing low surface energy layer, with a total thickness of 68 μm. The metal transition layer has a thickness of 30 μm, the nano-ceramic layer has a thickness of 15 μm, the fluorine-containing low surface energy layer has a thickness of 23 μm, and the surface roughness Ra is 0.12 μm. The metal transition layer is a plasma-sprayed nickel-chromium alloy layer, the nano-ceramic layer is an alumina-titanium dioxide composite layer, and the fluorine-containing low surface energy layer is a polytetrafluoroethylene sintered layer. The forming process of the polytetrafluoroethylene sintered layer includes: uniformly coating the surface of the alumina-titanium dioxide nano-ceramic layer with a water-based polytetrafluoroethylene dispersion emulsion, pre-drying it at 90°C to 110°C, and then isothermally plasticizing and sintering it at 380°C to 400°C for 30 to 60 minutes to form a dense and non-stick surface layer. The heating roller has a multi-channel spiral flow channel inside, and adopts a combination of inner layer fluid temperature regulation and outer layer electromagnetic induction rapid heat replenishment. The power response delay time of the outer layer electromagnetic induction heat replenishment system is less than or equal to 0.1 seconds, and the local compensation heating rate of the roller surface is greater than or equal to 5℃ / s. The spiral flow channel is a three-head rectangular cross-section flow channel, and the electromagnetic induction heating frequency is 20kHz. The measured film temperature in the longitudinal main stretching zone was controlled at 154℃, lower than the crystal melting initiation temperature of the polypropylene resin used (159.8℃); the longitudinal stretching ratio was 5.4 times; longitudinal stretching was achieved through multi-roller speed difference, and the strain rate was segmented as follows: initial stretching segment 42s. -1 The middle stretching section lasted 92 seconds. -1 The subsequent stretching segment lasted 145 seconds. -1 ; A double-sided mid-wave infrared auxiliary heater is installed between the longitudinal main stretching rollers. The radiation center wavelength is 3.2μm and the single-zone power density is 18kW / m². It is used for heat replenishment and temperature homogenization before and after the stretching point. S4, Synchronous Stretching The measured film temperature in the synchronous stretching zone was controlled at 154-156℃, which is lower than the crystal melting initiation temperature of the polypropylene resin used, which is 159.8℃. The longitudinal stretching ratio was 5.4 times, and the transverse stretching ratio was 7.4 times. Synchronous stretching was completed by the track expansion and acceleration of the synchronous fixture. The longitudinal strain rate was segmented as follows: initial stretching segment 42s⁻¹, intermediate stretching segment 92s⁻¹, and subsequent stretching segment 145s⁻¹. A double-sided mid-wave infrared auxiliary heater is installed in the stretching zone, with a radiation center wavelength of 3.2μm and a single-zone power density of 18kW / m², for heat replenishment and temperature homogenization before and after the stretching point; The synchronous stretching zone is set up with 4 independent control sub-zones, and each sub-zone gradually and synchronously expands the clamp track spacing and increases the longitudinal speed; S5, Heat setting The film after synchronous stretching is heat-set while maintaining longitudinal tension and transverse clamping. The heat-setting temperature is 138℃ and the heat-setting time is 3.2 seconds. During the heat-setting process, the transverse clamp spacing is reduced by 4%, and the longitudinal tension is adjusted by the longitudinal speed of the synchronous clamp. S6, multi-stage cooling, inspection and winding After heat setting, the film undergoes four stages of cooling, with temperatures of 120℃, 96℃, 68℃ and 32℃ respectively. The measured temperature differences between adjacent cooling zones are 24℃, 28℃ and 36℃ respectively. After the film is cooled to below 40℃, online thickness measurement, defect detection and single-sided corona treatment are performed, and tapered tension control is used for winding. The initial winding tension of the tapered tension control is set to 120 to 150 N, and the final winding tension is set to 80 to 100 N. The tension taper value decreases linearly with the increase of the roll diameter, and the taper coefficient is set to 15% to 25%. The wound film is cured at 50°C for 8 hours, and the curing temperature is lower than the heat setting temperature. In this embodiment, a BOPP capacitor film base film with a thickness of 23.0 μm was obtained; The stretching process employs a combination of linear velocity and tension feedforward compensation and adaptive fuzzy proportional-integral-derivative (AI-DI) control. The input parameters for this adaptive fuzzy proportional-integral-derivative (AI-DI) control include production line speed, film width, film thickness, initial film temperature upon entering the heating zone, film tension, roller surface temperature, transverse film temperature distribution, ambient temperature, and cooling airflow. The feedforward compensation calculates the feedforward heating power based on the changes in linear velocity and tension. Adaptive fuzzy proportional-integral-derivative (PID) control takes temperature deviation and its rate of change as input, employs triangular membership functions, and adjusts the proportional, integral, and derivative parameters online using a fuzzy rule base. The sampling period is [missing information]. ;Specifically, the The temperature deviation of the second sampling is ,in For the first The temperature setpoint for the next sample. For the first The measured temperature of the thin film in the second sampling, the rate of change of discrete deviation is ,in The sampling period is set to 0.5 seconds. This is the sampling sequence number; when the measured temperature of the thin film is lower than the set temperature value... A positive value indicates a positive deviation, while a negative value indicates a negative deviation. The sign convention is the same as... domain of discourse The settings regarding zero symmetry are consistent; Domain of discourse , Domain of discourse The quantization was reduced to seven linguistic variables: {NB, NM, NS, ZO, PS, PM, PB}, with quantization factors Ke=1.5 and Kec=3.0, respectively. Indicates The discrete rate of change of temperature deviation over a time base; since the sampling period is fixed, the time information is determined by the sampling sequence number. Implicit representation, therefore Continuous-time variables will no longer be introduced separately.
[0015] The triangular membership functions are arranged sequentially on the normalized universe of discourse [-3,-2,-1,0,1,2,3]; ΔKp, ΔKi, and ΔKd are the outputs, with output universes of discourse of [-0.30,0.30], [-0.06,0.06], and [-0.12,0.12] respectively; the centroid method is used for defuzzification; the proportional-integral-differential online correction relationship is Kp=Kp0+ΔKp, Ki=Ki0+ΔKi, Kd=Kd0+ΔKd, where the initial parameters are Kp0=2.8, Ki0=0.35, and Kd0=0.12. The fuzzy rule base is established according to the principle of prioritizing increasing Kp and suppressing Ki when the absolute value of the deviation is large, appropriately increasing Ki when the deviation is close to zero and the rate of change is small, and increasing Kd to suppress overshoot when the rate of change of the deviation is large. For example, when e is PB and ec is PS, ΔKp is PB, ΔKi is NS, and ΔKd is PM. For other operating conditions, a complete matrix of 49 rules covering all combinations of the domains of e and ec is formulated according to the above principles to ensure the continuous and smooth transition of control parameters. When e is ZO and ec is ZO, ΔKp is ZO, ΔKi is PS, and ΔKd is NS; when e is NB and ec is NM, ΔKp is PM, ΔKi is NM, and ΔKd is PS; the feedforward heating power adopts the calibration formula Pff=P0+Kv(v-v0)+Kt(F-F0), where P0 is the steady-state reference power, v is the production line speed, and F is the film tension; In this embodiment, the calibration yielded Kv=0.42kW / (m / min), Kt=0.18kW / N, v0=72m / min, and F0=165N. During operation, the surface temperature fluctuation of the heating roller was controlled within ±0.4℃, the average transverse temperature fluctuation of the film was controlled within ±0.6℃, the instantaneous temperature fluctuation of the film at the stretching point was controlled within ±0.8℃, and the transverse temperature difference of the film was controlled within 1.7℃. The infrared thermometry system used for the actual film temperature measurement was set with an emissivity of 0.95, and thickness attenuation compensation and standard blackbody calibration were performed based on the data from the online thickness gauge. Example 2: This example provides a stretching process for the BOPP capacitor film base film, specifically including the following steps: S1. High isotactic homopolymer polypropylene resin was selected, with an isotacticity index of 97.4%, a melt flow rate of 3.6 g / 10 min, a weight-average molecular weight to number-average molecular weight ratio of 4.8, and a melting peak temperature of 165.6℃ and a crystal melting initiation temperature of 158.6℃ as measured by differential scanning calorimetry (DSC). The raw material composition by mass percentage is as follows: the raw material composition is 100% high isotactic homopolymer polypropylene resin by mass percentage of the total mass of resin raw materials; the resin is dried in dehumidified air at 65°C for 3 hours, and the moisture content after drying is controlled at 78ppm; the pure polypropylene resin directly enters the extrusion process. S2. Extrusion is carried out using a single screw extruder, with temperatures set sequentially to 175℃, 198℃, 215℃ and 222℃; the melt is filtered through a 20μm continuous melt filter and then extruded to a 30℃ casting roll, with a casting thickness of 1.10mm, and the surface temperature uniformity of the casting roll is controlled within ±0.5℃. S3. The measured temperature of the film in the preheating zone is controlled at 136℃, and the measured temperature of the film in the temperature homogenization zone is controlled at 144℃. Double-sided hot air is used for temperature homogenization in the thickness direction, and the temperature difference in the thickness direction is controlled at 2.6℃. The preheating and homogenization rollers are composite anti-stick layer heating rollers. The layer structure, materials of each layer, thickness, surface roughness and heating method of the composite anti-stick layer are the same as those in Example 1. That is, it is composed of a 30μm plasma-sprayed nickel-chromium alloy transition layer, a 15μm alumina-titanium dioxide nano-ceramic layer and a 23μm polytetrafluoroethylene fluorine-containing low surface energy layer, with a total thickness of 68μm and a surface roughness Ra of 0.12μm. The heating roller is equipped with a three-head rectangular cross-section multi-channel spiral flow channel. It adopts a combination of inner layer fluid temperature regulation and outer layer electromagnetic induction rapid heat replenishment. The electromagnetic induction heating frequency is 20kHz. S4. The measured temperature of the film in the synchronous stretching zone is controlled at 147-153℃, which is lower than the crystal melting initiation temperature of 158.6℃. The longitudinal stretching ratio is 4.7 times and the transverse stretching ratio is 6.4 times. The strain rate is segmented into 28s⁻¹, 68s⁻¹ and 112s⁻¹. The synchronous stretching zone is set with 3 independent control sub-zones for temperature, speed and track. A double-sided mid-wave infrared auxiliary heater is set in front of the stretching point with a radiation center wavelength of 3.1μm and a single-zone power density of 10kW / m². S5, heat setting temperature is 133℃, heat setting time is 2.2 seconds, and the lateral clamp spacing is reduced by 2%; S6. The cooling zone temperatures are 112℃, 90℃, 60℃ and 28℃ respectively. After cooling to below 40℃, online thickness measurement, defect detection, single-sided corona treatment and winding are performed. The wound film is cured at 45℃ for 6 hours. In this embodiment, a BOPP capacitor film base film with a thickness of 36.6 μm was obtained. During operation, the surface temperature of the heating roller fluctuated by ±0.5℃, the average transverse temperature fluctuation of the film was ±0.8℃, the instantaneous temperature fluctuation of the film at the stretching point was ±1.0℃, and the transverse temperature difference of the film was 2.0℃.
[0016] Example 3: This example provides a stretching process for the BOPP capacitor film base film, specifically including the following steps: S1. High isotactic homopolymer polypropylene resin was selected, with an isotacticity index of 99.1%, a melt flow rate of 1.9 g / 10 min, a weight-average molecular weight to number-average molecular weight ratio of 6.2, a melting peak temperature of 168.4℃ measured by DSC, and a crystal melting initiation temperature of 160.8℃. The raw material composition by mass percentage is as follows: the raw material composition is 100% high isotactic homopolymer polypropylene resin by mass percentage of total resin raw material; the resin is dried in dehumidified air at 80℃ for 5 hours, and the moisture content after drying is controlled to be 48ppm; pure polypropylene resin directly enters the extrusion process. S2. Extrusion is carried out using a single screw extruder, with temperatures set sequentially to 182℃, 208℃, 226℃ and 232℃; the melt is filtered through a 12μm continuous melt filter and then extruded onto a 38℃ casting roll, with a casting thickness of 0.84mm, and the surface temperature uniformity of the casting roll is controlled within ±0.4℃. S3. The measured temperature of the film in the preheating zone is controlled at 144℃, and the measured temperature of the film in the temperature homogenization zone is controlled at 149℃. The thickness direction temperature is homogenized by a combination of double-sided hot air, infrared radiation and hot rollers, and the thickness direction temperature difference is controlled at 1.1℃. The preheating and homogenization zone uses a composite anti-stick layer heating roller. The layer structure, material of each layer, thickness, surface roughness and heating method of the composite anti-stick layer are the same as those in Example 1. That is, it is composed of a 30μm plasma-sprayed nickel-chromium alloy transition layer, a 15μm alumina-titanium dioxide nano-ceramic layer and a 23μm polytetrafluoroethylene fluorine-containing low surface energy layer, with a total thickness of 68μm and a surface roughness Ra of 0.12μm. The heating roller is equipped with a three-head rectangular cross-section multi-channel spiral flow channel. It adopts a combination of inner layer fluid temperature regulation and outer layer electromagnetic induction rapid heat replenishment. The electromagnetic induction heating frequency is 20kHz. S4. The measured temperature of the film in the synchronous stretching zone is controlled at 155-157℃, which is lower than the crystal melting initiation temperature of 160.8℃. The longitudinal stretching ratio is 5.6 times, and the transverse stretching ratio is 7.9 times. The strain rate is segmented into 50s⁻¹, 108s⁻¹, and 168s⁻¹. The synchronous stretching zone is set with 5 independent control sub-zones for temperature, speed, and track. A set of double-sided mid-wave infrared auxiliary heaters is set before and after the stretching point. The radiation center wavelength is 3.3μm, and the power density of a single zone is 22kW / m². S5. The heat setting temperature is 140℃, the heat setting time is 3.8 seconds, and the lateral clamp spacing is reduced by 5%. S6. The cooling zone temperatures are 122℃, 100℃, 72℃ and 35℃ respectively. After cooling to below 40℃, online thickness measurement, defect detection, double-sided corona treatment and winding are performed. The wound film is cured at 55℃ for 8 hours. In this embodiment, a BOPP capacitor film base film with a thickness of 19.0 μm was obtained. During operation, the surface temperature of the heating roller fluctuated by ±0.3℃, the average transverse temperature fluctuation of the film was ±0.5℃, the instantaneous temperature fluctuation of the film at the stretching point was ±0.7℃, and the transverse temperature difference of the film was 1.5℃.
[0017] Example 4: This example provides a stretching process for the BOPP capacitor film base film, specifically including the following steps: S1. High isotactic homopolymer polypropylene resin was selected, with an isotacticity index of 98.1%, a melt flow rate of 2.8 g / 10 min, a weight-average molecular weight to number-average molecular weight ratio of 5.2, a melting peak temperature of 166.3℃ measured by DSC, and a crystal melting initiation temperature of 159.1℃. The raw material composition by mass percentage is as follows: the raw material composition is 100% high isotactic homopolymer polypropylene resin by mass percentage of the total mass of resin raw material; the resin is dried in dehumidified air at 75°C for 4 hours, and the moisture content after drying is controlled at 55ppm; the pure polypropylene resin directly enters the extrusion process. S2. Extrusion is carried out using a single screw extruder, with temperatures set sequentially to 178℃, 202℃, 220℃ and 226℃; the melt is filtered through an 18μm continuous melt filter and then extruded onto a 33℃ casting roll, with a casting thickness of 0.98mm, and the surface temperature uniformity of the casting roll is controlled within ±0.5℃. S3. The measured film temperature in the preheating zone is controlled at 140℃, and the measured film temperature in the temperature homogenization zone is controlled at 146℃. Double-sided hot air and infrared radiation are used to homogenize the film temperature in the thickness direction, and the temperature difference in the thickness direction is controlled at 1.8℃. The preheating homogenization uses a composite anti-stick layer heating roller. S4. The measured temperature of the film in the synchronous stretching zone is controlled at 152-155℃, which is lower than the crystal melting initiation temperature of 159.1℃. The longitudinal stretching ratio is 5.1 times, and the transverse stretching ratio is 7.0 times. The strain rate is segmented into 36s⁻¹, 82s⁻¹, and 132s⁻¹. The synchronous stretching zone is set with 4 independent control sub-zones for temperature, speed, and track. A double-sided mid-wave infrared auxiliary heater is set before the stretching point, with a radiation band of 2.8-3.2μm and a single-zone power density of 16kW / m². S5. The heat setting temperature is 136℃, the heat setting time is 3.0 seconds, and the lateral clamp spacing is reduced by 3%. S6. The cooling zone temperatures are 118℃, 94℃, 66℃ and 30℃ respectively. After cooling to below 40℃, online thickness measurement, defect detection, single-sided corona treatment and winding are performed. The wound film is cured at 48℃ for 6 hours. In this embodiment, a BOPP capacitor film base film with a thickness of 27.5 μm was obtained. During operation, the surface temperature of the heating roller fluctuated by ±0.4℃, the average transverse temperature fluctuation of the film was ±0.7℃, the instantaneous temperature fluctuation of the film at the stretching point was ±0.9℃, and the transverse temperature difference of the film was 1.9℃.
[0018] Comparative Example 1: The difference between this comparative example and Example 1 is that the measured temperature of the film in the synchronous stretching zone was changed from 154-156℃ to 132-145℃, while the other operating steps and process parameters were exactly the same as in Example 1.
[0019] Comparative Example 2: The difference between this comparative example and Example 1 is that the linear speed and tension feedforward compensation combined with the internal buried multi-channel flow channel adjustment are cancelled. The synchronous stretching zone is controlled by the conventional temperature setting method, without feedforward compensation and fuzzy proportional integral derivative adjustment. Other operating steps and process parameters are exactly the same as in Example 1. During operation, the surface temperature fluctuation of the heating roller is ±1.7℃, the average transverse temperature fluctuation of the film is ±2.1℃, the instantaneous temperature fluctuation of the film at the stretching point is ±2.5℃, and the transverse temperature difference of the film is 4.6℃.
[0020] Comparative Example 3: The difference between this comparative example and Example 1 is that the heat setting step in S5 is omitted, and the film in the synchronous stretching zone directly enters the multi-stage cooling zone. Other operation steps and process parameters are exactly the same as in Example 1.
[0021] Comparative Example 4: The difference between this comparative example and Example 1 is that the double-sided mid-wave infrared auxiliary heater in the synchronous stretching zone is removed, while the other operating steps and process parameters are exactly the same as in Example 1.
[0022] Comparative Example 5: The difference between this comparative example and Example 1 is that the segmented longitudinal strain rate in Example 1 is changed to a single constant strain rate of 95s⁻¹, while the other operating steps and process parameters are exactly the same as in Example 1.
[0023] Comparative Example 6: The difference between this comparative example and Example 1 is that the four-stage cooling in Example 1 is changed to synchronous stretching followed by direct cooling to below 40°C via a 40°C cooling roller. The graded cooling processes of 110-125°C, 80-105°C, and 50-75°C are eliminated. Other operating steps and process parameters are exactly the same as in Example 1.
[0024] Performance Testing and Datasheets Dielectric breakdown strength was determined using a DC breakdown test method with the same electrode conditions, the same voltage ramp rate, and the same sample pretreatment conditions. Ten samples were used in each group, and the result was taken as the characteristic breakdown field strength of the Weibull distribution. The tests were conducted at 25℃ and 105℃ respectively. Thickness deviation was determined using a combination of online thickness measurement and offline verification. Thermal shrinkage rate was measured under specified temperature conditions, and the longitudinal and transverse shrinkage rates were measured and the average value was taken. Dielectric loss was measured using an inductance-capacitance-resistance analyzer; visible defects were statistically analyzed using a high-resolution charge-coupled device surface defect online detection system; the lifetime of adjacent electron phanoids was measured using positron annihilation lifetime spectroscopy with a radioactive source. 22 Na and fast-fast coincidence spectrometer, test temperature 25℃, free volume related parameters are based on relative comparison under the same test conditions.
[0025] Table 1 Summary of performance test data for each embodiment and comparative example
[0026] As can be seen from the comparison of the test results of Example 1 and Comparative Example 1 in Table 1, after the synchronous stretching temperature was reduced to a conventionally low level, the DC breakdown field strength at 25℃ decreased from 838V / μm to 724V / μm, the DC breakdown field strength at 105℃ decreased from 672V / μm to 548V / μm, the lifetime of the ortho-electron diazo increased from 1.83ns to 2.08ns, and the thermal shrinkage rate increased from 0.68% to 1.36%. The lack of high-temperature solid-state stretching conditions close to the crystal melting initiation temperature results in insufficient polypropylene wafer slip, lamellar rotation, and amorphous chain segment orientation. This leads to an increase in local non-uniform orientation regions, an increase in the free volume of the amorphous region, and a greater likelihood of forming electrical breakdown weak points in the local loose structure. Consequently, both breakdown strength and dimensional stability decrease. As can be seen from the comparison of the test results of Example 1 and Comparative Example 2 in Table 1, after canceling the linear velocity and tension feedforward compensation and adjusting the internal buried multi-channel flow channel, the DC breakdown field strength at 25℃ decreased from 838V / μm to 756V / μm, the DC breakdown field strength at 105℃ decreased from 672V / μm to 584V / μm, the thickness deviation increased from ±1.0% to ±2.3%, and the number of visible defects increased from 0.4 per m² to 2.1 per m². Changes in linear velocity, tension, and heat carried away during film operation cannot be reflected in the heating power adjustment in a timely manner. The measured temperature fluctuation near the stretching point increases, the transverse temperature difference increases, resulting in inconsistent local tensile stress, uneven orientation and thickness distribution, an increase in local overstretched and understretched areas, and an increase in the number of thin weak points and surface defects, thus deteriorating the breakdown data and consistency. As can be seen from the comparison of the test results of Example 1 and Comparative Example 3 in Table 1, after removing the heat setting under tension, the DC breakdown field strength at 25°C decreased from 838V / μm to 781V / μm, the DC breakdown field strength at 105°C decreased from 672V / μm to 601V / μm, and the heat shrinkage rate increased from 0.68% to 1.48%. After high-temperature biaxial synchronous stretching, the molecular chain is in a state of high orientation stress. If it is not heat-set at 130-145℃, the crystal and the confined amorphous chain segments cannot be controlled and stabilized in time under tension constraints. A lot of residual internal stress is retained, and shrinkage and local relaxation are more likely to occur during subsequent cooling and testing, resulting in decreased dimensional stability and reduced high-temperature breakdown strength. As can be seen from the comparison of the test results of Example 1 and Comparative Example 4 in Table 1, after the double-sided mid-wave infrared auxiliary heating was removed, the DC breakdown field strength at 25℃ decreased from 838V / μm to 774V / μm, the DC breakdown field strength at 105℃ decreased from 672V / μm to 596V / μm, the thickness deviation increased from ±1.0% to ±1.6%, and the lifetime of the ortho-electron diazo increased from 1.83ns to 1.97ns. The lack of rapid heat replenishment before and after the stretching point reduces the temperature homogenization between the film surface and core layer and different parts in the transverse direction. In areas with low local temperature, the chain segment mobility is insufficient, while in areas with high local temperature, stress relaxation differences are more likely to occur, resulting in inconsistent orientation in the thickness direction and transverse direction, increased free volume-related structural parameters, and decreased breakdown strength. As can be seen from the comparison of the test results of Example 1 and Comparative Example 5 in Table 1, after changing the segmented strain rate to a single constant strain rate, the DC breakdown field strength at 25℃ decreased from 838V / μm to 768V / μm, the DC breakdown field strength at 105℃ decreased from 672V / μm to 589V / μm, the thickness deviation increased from ±1.0% to ±1.8%, and the number of visible defects increased from 0.4 per m² to 1.5 per m². Without a progressively increasing piecewise strain rate, the sheet cannot achieve uniform yielding smoothly in the initial stretching stage, and subsequently cannot fully utilize the orientation-induced strain hardening effect to suppress local necking. Local stress concentration is more likely to induce microcracks and thickness fluctuations, thus reducing the breakdown performance and film thickness uniformity. As can be seen from the comparison of the test results of Example 1 and Comparative Example 6 in Table 1, after changing the multi-stage gradient cooling to direct cooling, the DC breakdown field strength at 25℃ decreased from 838V / μm to 762V / μm, the DC breakdown field strength at 105℃ decreased from 672V / μm to 578V / μm, the thermal shrinkage rate increased from 0.68% to 1.72%, and the dielectric loss increased from 0.00019 to 0.00028. If the film after high-temperature orientation is directly and suddenly cooled, the temperature drop of the surface layer and the core layer will be asynchronous. Larger thermal stress and orientation freezing differences will easily form in the thickness direction, increasing the number of local microcracks and discontinuous areas at the interface. The residual internal stress will also be difficult to release effectively, thus reducing the thermal shrinkage rate, dielectric loss and breakdown strength. Based on the test results of Examples 1 to 4, it can be seen that within the defined raw material system, stretching temperature, stretching ratio, temperature control, heat setting and multi-stage cooling range, the obtained films all have high breakdown strength, low thermal shrinkage rate and low dielectric loss. In Example 2, a stretching temperature and ratio close to the lower limit of the range were used, and the performance met the requirements but was slightly lower than that of Example 1. In Example 3, a higher degree of orientation and stronger temperature homogenization conditions were used, and the thickness uniformity and breakdown strength were maintained within the target parameter range. Example 4 uses an intermediate parameter combination, and the performance is at a stable level. The above results show that the combination of controlled high-temperature solid stretching, dynamic temperature control, tension-maintaining heat setting and gradient cooling helps to reduce the local defect density and free volume related structural parameters, and improve the dielectric properties and dimensional stability of the BOPP capacitor film base film.
[0027] The above are merely specific embodiments of the present invention and are not intended to limit the present invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments for application in other fields. However, any conventional modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the technical solution of the present invention shall still fall within the protection scope of the technical solution of the present invention.
Claims
1. A stretching process for a BOPP capacitor film base film, characterized in that, Includes the following steps: S1. The pure polypropylene resin is screened, dusted, and dehumidified and dried. S2. Pure polypropylene resin is melt-extruded, filtered, and formed by a flat die, and then cooled and cast on a casting roller at a temperature of 35°C. S3. The casting sheet is fed into the preheating and temperature homogenization zone, and preheating and temperature homogenization are performed sequentially on the heating rollers. S4. The homogenized film is fed into the synchronous stretching zone for simultaneous longitudinal and transverse stretching. The actual temperature of the film in the synchronous stretching zone is controlled at 154-156℃, the longitudinal stretching ratio is 5.4 times, and the transverse stretching ratio is 7.4 times. S5. While maintaining longitudinal tension and transverse clamping, heat-set the transversely stretched film at 138°C for 3.2 seconds. S6. The heat-set film is successively cooled at 120℃, 96℃, 68℃ and 32℃. After cooling to below 40℃, online thickness detection, defect detection and winding are performed. Among them, the actual temperature of the film in the synchronous stretching zone is lower than the crystal melting initiation temperature of the polypropylene resin used by differential scanning calorimetry. The test conditions of differential scanning calorimetry are: under the protection of high-purity nitrogen, the film is continuously heated from 25°C to 200°C at a nominal heating rate of 10°C / min. During the stretching process, the heating compensation power is dynamically controlled by combining linear velocity and tension feedforward compensation with the hidden multi-channel flow channel inside the heating roller. The pure polypropylene resin is a high isotactic homopolymer polypropylene resin with a mass fraction of 100%. The isotacticity index of the high isotactic homopolymer polypropylene resin is 98.8%, the melt flow rate at 230℃ and 2.16kg is 2.3g / 10min, the ratio of weight-average molecular weight to number-average molecular weight is 5.6, and the melting peak temperature is 167.2℃.
2. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, In S2, the extruder adopts segmented heating along the material conveying direction. The segmented temperatures are 180°C for the feeding section, 205°C for the compression section, 222°C for the metering section, and 228°C for the die head and melt pipeline. The melt is filtered through a 15μm continuous melt filter, the casting thickness is 0.92mm, and the surface temperature uniformity of the casting roller is controlled within ±0.5°C.
3. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, The preheating and temperature homogenization zone uses a heating roller with a composite anti-stick layer, which consists of, from the inside out: a 30 μm thick metal transition layer, a 15 μm thick nano-ceramic layer, and a fluorine-containing low surface energy layer. The fluorine-containing low surface energy layer is a polytetrafluoroethylene sintered layer; the total thickness of the composite anti-stick layer is 68μm, and the surface roughness Ra is 0.12μm; the heating roller is equipped with a multi-channel spiral flow channel inside, and an electromagnetic induction heating device is provided on the outer layer, and the roller surface temperature is calibrated by multi-point temperature detection and infrared thermometry.
4. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, The preheating zone of S3 controls the actual film temperature to 142℃, and the temperature homogenization zone controls the actual film temperature to 148℃. It also uses a combination of double-sided hot air and hot rollers to homogenize the temperature in the thickness direction. A synchronous clamp is provided within the synchronous stretching zone. The synchronous stretching is achieved through the expansion of the track and longitudinal acceleration of the synchronous clamp, and a segmented longitudinal strain rate with gradually increasing values is adopted along the stretching direction: the initial stretching segment is 42s. -1 The intermediate stretching period is 92 seconds. -1 The subsequent stretching period is 145 seconds. -1 .
5. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, In S4, the synchronous stretching zone is divided into four synchronous stretching sub-zones with independent control over temperature, longitudinal speed, and track spacing.
6. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, In S5, during heat setting, the longitudinal tension is adjusted by the longitudinal speed of the synchronous clamp, and the lateral spacing of the synchronous clamp remains unchanged or is retracted, with a retraction rate of 4%; in S6, the heat-set film undergoes four-stage cooling in sequence, with temperatures of 120℃, 96℃, 68℃ and 32℃ respectively, and the measured temperature differences between adjacent cooling zones are 24℃, 28℃ and 36℃ respectively.
7. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, A local hardware adjustment device consisting of a concealed multi-channel flow channel and an embedded temperature sensor located inside the heating roller is adopted. When the production line speed, film thickness or film tension changes, the heating power is first adjusted by feedforward compensation, and then the heating compensation power is output by adjusting the medium flow rate of the internal concealed flow channel. The film temperature is measured by an infrared temperature measurement system that has been calibrated by emissivity, thickness correction and standard blackbody calibration.
8. The stretching process of the BOPP capacitor film base film according to claim 1, characterized in that, The film, after being stretched synchronously, maintains lateral clamping tension during heat setting and multi-stage cooling. After cooling to below 40°C, it undergoes single-sided corona treatment and is wound up using tapered tension control. The wound film is then cured at 50°C.
Citation Information
Patent Citations
Preparation process of high-performance polypropylene capacitor film
CN120865590A
Two-step synchronous drawing process and equipment for producing BOPP (Biaxially-oriented Polypropylene)
CN121871093A