Preparation method of foamed layer, PVC artificial leather and PVC artificial leather
By combining microsphere foaming agent with chemical foaming agent and controlling temperature, the problem of uneven cell structure in PVC artificial leather foam layer was solved, thereby improving cell uniformity and interlayer bonding strength, and enhancing the product's lightweight, softness, and thermal insulation performance.
Patent Information
- Application Number
- CN202611359380.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-09-03
AI Technical Summary
The existing PVC artificial leather foam layer has uneven cell distribution, which easily leads to large bubbles and bubble aggregation, affecting the product's lightweight, softness, fullness of hand feel, and heat insulation performance.
A mixed foaming process combining microsphere foaming agent and chemical foaming agent is adopted. Through specific process sequence and temperature control, PVC resin and chemical foaming agent are mixed first, and then microsphere foaming agent is added. The material temperature is controlled to be lower than the initial foaming temperature of microsphere foaming agent to ensure that microsphere foaming agent maintains its complete structure before foaming. Uniform cells are formed through multi-stage heating foaming process.
This technology improves the uniformity of cell structure and the interlayer bonding strength. The product features uniform cell structure, clear surface texture, strong resistance to yellowing, and low content of volatile organic compounds, thus improving the overall performance of PVC artificial leather.
Smart Images

Figure CN122852004B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to a foaming layer, a method for preparing PVC artificial leather, and PVC artificial leather. Background Technology
[0002] PVC artificial leather consists of a base fabric layer, a backing fabric layer, a foam layer, and a top layer. The foam layer directly determines the product's lightweight, softness, fullness of feel, and heat insulation performance. The quality of these properties essentially depends on the quality of its internal cell structure, including the shape, size, uniformity, distribution density, and open / closed cell ratio of the cells.
[0003] In existing processes, the foaming layer generally uses purely chemical foaming agents, the most commonly used of which is AC foaming agent (azodicarbonamide). Its foaming principle is as follows: in the high-temperature stage after PVC plasticizes and melts (usually about 160-200℃), AC foaming agent decomposes under heat, producing gases such as nitrogen (N2), carbon monoxide (CO), and carbon dioxide (CO2). These gases nucleate, grow and fix in the PVC melt, forming cells.
[0004] However, in existing processes, when using pure AC foaming agent for chemical foaming, the decomposition and nucleation points of AC foaming agent are random, resulting in poor uniformity of cell distribution and a tendency for large bubbles and bubble co-occurrence. Summary of the Invention
[0005] This invention provides a foaming layer, a method for preparing PVC artificial leather, and PVC artificial leather, to solve the problem of uneven cell structure in the foaming layer in the prior art.
[0006] In a first aspect, the present invention provides a method for preparing a foamed layer, comprising the following steps: S1. The first PVC resin, the first chemical foaming agent and the first plasticizer are mixed for the first time to obtain the first mixture, and then the first mixture is mixed with the microsphere foaming agent for the second time to obtain the second mixture; S2. The second mixture is calendered to obtain the foaming layer; S3. The layer to be foamed is foamed to obtain the foamed layer; In steps S1 and S2, the temperature of the material is lower than the initial foaming temperature of the microsphere foaming agent. The temperature of the material refers to the temperature of the molten material monitored in real time throughout steps S1 and S2. The initial foaming temperature of the microsphere foaming agent refers to the critical temperature point at which the microsphere foaming agent begins to decompose and generate gas, resulting in volume expansion.
[0007] In one alternative embodiment, the first mixture further includes a first stabilizer, a first pigment, a first calcium powder, and a flame retardant.
[0008] In one optional embodiment, the first mixture, by weight, comprises the following components: 100 parts of first PVC resin, 72-105 parts of first plasticizer, 1-3 parts of first stabilizer, 0.5-1.0 parts of first pigment, 20-50 parts of first calcium powder, 18-25 parts of flame retardant, and 1-8 parts of first chemical foaming agent.
[0009] In one alternative embodiment, the first plasticizer comprises one or more of di(2-propylheptyl) phthalate, diisooctyl sebacate, and dioctyl azelate.
[0010] In an optional embodiment, the first plasticizer is composed of di(2-propylheptyl) phthalate, diisooctyl sebacate and dioctyl azelate in a mass ratio of (50-65):(20-45):(2-8).
[0011] In one optional embodiment, the first PVC resin includes at least one of SG-3 type PVC resin and SG-5 type PVC resin.
[0012] In one alternative embodiment, the first stabilizer includes at least one of calcium-zinc stabilizer and barium-zinc stabilizer.
[0013] In one alternative embodiment, the first chemical foaming agent includes at least one of azodicarbonamide and modified sodium bicarbonate.
[0014] In one alternative embodiment, the flame retardant comprises an antimony-based flame retardant.
[0015] In one alternative embodiment, the flame retardant includes one or more of antimony trioxide, antimony pentoxide, and sodium antimonate.
[0016] In one optional embodiment, the first calcium powder includes at least one of heavy calcium carbonate powder and light calcium carbonate powder.
[0017] In one alternative embodiment, the first pigment includes at least one of titanium dioxide (index number PW6), high yellow (index number PY110), carbon black (index number P.BK.7), and iron oxide red (index number PR101).
[0018] In one optional embodiment, the mass ratio of the microsphere foaming agent to the first PVC resin in S1 is (5-8):100.
[0019] In one alternative embodiment, the structure of the microsphere foaming agent includes an outer shell and an inner layer.
[0020] In one alternative embodiment, the outer shell of the microsphere foaming agent comprises an acrylonitrile-vinylidene chloride copolymer.
[0021] In one alternative embodiment, the inner layer of the microsphere foaming agent is gaseous, comprising hydrocarbon gas.
[0022] In one optional embodiment, the inner layer of the microsphere foaming agent is isobutane gas.
[0023] In one alternative embodiment, the average particle size of the microsphere foaming agent is 90-130 μm.
[0024] In one optional embodiment, the average particle size of the microsphere foaming agent is 100-120 μm.
[0025] In one optional embodiment, the method for preparing the foamed layer satisfies at least one of the following conditions: (1) The rotation speed of the first mixing is 1300-1700 r / min, and the time of the first mixing is 1-3 min; (2) The rotation speed of the second mixing is 1300-1700 r / min, and the time of the second mixing is 3-7 min; (3) The initial foaming temperature of the microsphere foaming agent is 182-188℃; (4) The second mixing process further includes heating the first mixture to T1; (5) The process before calendering also includes heating the second mixture to T2; (6) The temperature of the material in S1 and S2 is 165-175℃; (7) The S2 step, after calendering, also includes a first cooling step; (8) The foaming step in S3 includes sequentially performing a first heating stage, a second heating stage, a third heating stage and a fourth heating stage; the temperature of the first heating stage is 160-180℃, the temperature of the second heating stage is 200-210℃, the temperature of the third heating stage is 200-210℃, and the temperature of the fourth heating stage is 130-150℃. (9) The foaming time in S3 is 50s-240s; (10) S3 also includes a second cooling and winding step after foaming.
[0026] In one alternative implementation, T1 is 85-100°C.
[0027] In one alternative implementation, T2 is 105-115°C.
[0028] In one optional implementation, the foaming time in S3 is 144s-168s.
[0029] In one optional embodiment, step S2, after heating the second mixture to T2 and before calendering, further includes the steps of mixing and plasticizing.
[0030] In one optional embodiment, the mixing speed in S2 is 700-800 r / min, and the time is 340-360 s.
[0031] In one optional implementation, during the mixing and feeding process in S2, the hammer is raised every 90-110 seconds to observe whether there is any material sticking.
[0032] In an optional embodiment, the plasticizing step in S2 includes a first open mill and a second open mill; the equipment for the first open mill and the second open mill each independently includes a twin-roll mill; the twin-roll mill includes a front roll and a rear roll, the front roll and the rear roll operate simultaneously and are arranged in parallel, with their axes located in the same horizontal plane, an adjustable roll gap is formed between the front roll and the rear roll, and their rotation directions are opposite.
[0033] In one optional embodiment, the front and rear rolls of the two-roll mill in the first open milling process of S2 are at the same temperature, wherein the front roll temperature is 185-190°C.
[0034] In one optional embodiment, the front and rear rolls of the two-roll mill in the second open milling process of S2 are at the same temperature, wherein the front roll temperature is 180-185°C.
[0035] In one alternative embodiment, the apparatus for calendering the second mixture in S2 includes a four-roll calender.
[0036] In one optional embodiment, the four-roll calender is an inverted L-shaped four-roll calender, including a first roll, a second roll, a third roll, and a fourth roll. The second roll and the first roll are at the same horizontal height and parallel to each other. The first roll, the third roll, and the fourth roll are vertically arranged in a straight line, aligned vertically, and their axes are located in the same vertical plane. The rotation directions of adjacent rolls are opposite. The third roll is fixed in position as a reference roll, and the positions of the first roll, the second roll, and the fourth roll can be adjusted independently to adjust the size of the roll gap between each roll. Under the frictional traction of the rolls, the material passes through the roll gaps between the first roll and the second roll, between the first roll and the third roll, and between the third roll and the fourth roll in sequence to complete multiple calendering passes.
[0037] In one optional embodiment, the temperature of the first roll of the four-roll calender in S2 is 185-190°C, the temperature of the second roll is 185-190°C, the temperature of the third roll is 180-185°C, and the temperature of the fourth roll is 175-180°C.
[0038] In one optional embodiment, the devices for the first cooling in S2 and the second cooling in S3 each independently include cooling rollers; the cooling rollers are arranged in pairs, one above the other, for a total of three pairs, wherein the first two pairs of cooling rollers are circulated with low-temperature cold water, and the last pair of cooling rollers are circulated with room-temperature water, and the second mixture passes between each pair of rollers to achieve simultaneous cooling on both sides; the axis of the cooling rollers is parallel to the rollers of the four-roll calender, and the second mixture, after being calendered, winds around each cooling roller in an “S” shaped path. This feeding method can effectively increase the contact area between the sheet and the roller surface and extend the cooling stroke time, thereby improving the cooling efficiency.
[0039] In one optional embodiment, the temperature of the low-temperature cold water in the cooling roller during the first cooling in S2 and the second cooling in S3 is 0-8°C.
[0040] In one optional embodiment, the temperature of the room temperature water in the cooling roller during the first cooling in S2 and the second cooling in S3 is 23-25°C.
[0041] Secondly, the present invention provides a method for preparing PVC artificial leather, comprising the following steps: S1'. Obtain the base fabric layer and the backing fabric layer and perform the first bonding to obtain the first connecting layer; S2'. The first PVC resin and the first chemical foaming agent are mixed for the first time to obtain the first mixture. Then the first mixture is mixed with the microsphere foaming agent for the second time to obtain the second mixture. The second mixture is calendered to obtain the foaming layer. The temperature of the material in S1' and S2' is lower than the initial foaming temperature of the microsphere foaming agent; S3'. The foaming layer is bonded to the fabric side of the first connecting layer for the second time to obtain the second connecting layer; S4'. Obtain the surface layer, and bond the surface layer to the surface of the foaming layer of the second connecting layer for the third time to obtain a semi-finished product; S5'. The semi-finished product is foamed to obtain the PVC artificial leather; The preparation methods for S2'-S5' are the same as those for S1-S3.
[0042] In an alternative implementation, step S4' further includes heating the surface layer before the third bonding.
[0043] In one alternative embodiment, the temperature of the rear layer after heating in S4' is 175-185°C.
[0044] In one alternative implementation, the third bonding step in S4' includes roll bonding.
[0045] In one optional embodiment, the inter-roller pressure of the roll bonding in S4' is 20-25 MPa.
[0046] In an alternative implementation, the third bonding step in S4' further includes a cooling step.
[0047] In an optional embodiment, S5' further includes performing a water-based treatment on the surface layer of the semi-finished product before foaming.
[0048] In one alternative embodiment, the reagent for the aqueous treatment includes one or more of aqueous polyurethane, crosslinking agent, and hand feel agent.
[0049] In one optional embodiment, the water-based crosslinking agent includes one or more of aziridine crosslinking agents, polycarbodiimide crosslinking agents, and polyisocyanate crosslinking agents.
[0050] In one alternative embodiment, the water-based hand-feeling agent includes an organosilicon-based hand-feeling agent.
[0051] In one alternative embodiment, the waterborne polyurethane for waterborne treatment includes one or more of Stahl 3649, PERMUTEX® WF-78-486, and WF-43-417.
[0052] In one optional embodiment, the first bonding step in S1' further includes steps of stirring and mixing the fabric layer material, mixing and kneading, plasticizing, calendering and cooling.
[0053] In one optional embodiment, the stirring speed in S1' is 1300-1700 r / min, and the stirring time is 500-600 s.
[0054] In one optional embodiment, the speed of the mixing and pounding in S1' is 700-800 r / min, and the mixing and pounding time is 340-360 s.
[0055] In an alternative implementation, the plasticizing step in S1' includes a first open mill and a second open mill.
[0056] In one alternative implementation, the equipment for the first and second open milling processes in S1' each independently includes a two-roll open mill.
[0057] In one optional embodiment, the front and rear rolls of the two-roll mill in the first open milling process of S1' have the same temperature, wherein the front roll temperature is 185-190°C.
[0058] In one optional embodiment, the front and rear rolls of the two-roll mill in the second open milling process of S1' have the same temperature, wherein the front roll temperature is 180-185°C.
[0059] In one alternative embodiment, the calendering equipment in S1' includes a four-roll calender.
[0060] In one optional embodiment, the temperature of the first roll of the four-roll calender in S1' is 185-190°C, the temperature of the second roll is 185-190°C, the temperature of the third roll is 180-185°C, and the temperature of the fourth roll is 175-180°C.
[0061] In one optional embodiment, the equipment for the cooling step in S1' and the cooling step in S4' each independently includes cooling rollers; the cooling rollers are arranged in pairs, one above the other, for a total of three pairs, wherein the first two pairs of cooling rollers are circulated with low-temperature cold water, and the last pair of cooling rollers are circulated with room temperature water.
[0062] In one optional embodiment, the temperature of the low-temperature cold water in the cooling roller during the cooling steps S1' and S4' is 0-8°C.
[0063] In one optional embodiment, the temperature of the room temperature water in the cooling roller during the cooling steps S1' and S4' is 23-25°C.
[0064] In one optional embodiment, the method for preparing the PVC artificial leather satisfies at least one of the following conditions: (1) The base fabric layer in S1' includes at least one of knitted fabric and non-woven fabric; (2) The fabric layer in S1' comprises the following components by mass: 100 parts of second PVC resin, 72-105 parts of second plasticizer, 1-3 parts of second stabilizer, 0.5-1.0 parts of second pigment, 1-2 parts of second chemical foaming agent, and 20-50 parts of second calcium powder. (3) The S4' middle layer, by mass, includes the following components: 100 parts of third PVC resin, 80-100 parts of third plasticizer, 3-5 parts of third stabilizer, 1-3 parts of third pigment, and 2-5 parts of third calcium powder.
[0065] In one optional embodiment, the method for preparing the PVC artificial leather satisfies at least one of the following conditions: (1) The second plasticizer and the third plasticizer each independently include one or more of di(2-propylheptyl) phthalate, diisooctyl sebacate, and dioctyl azelate; (2) The second PVC resin and the third PVC resin each independently include at least one of SG-3 type PVC resin and SG-5 type PVC resin; (3) The second stabilizer and the third stabilizer each independently include at least one of calcium-zinc stabilizer and barium-zinc stabilizer; (4) The second chemical foaming agent includes at least one of azodicarbonamide and modified sodium bicarbonate; (5) The second calcium powder and the third calcium powder each independently include at least one of heavy calcium carbonate powder and light calcium carbonate powder; (6) The second pigment and the third pigment each independently include at least one of titanium dioxide (index number PW6), high yellow (index number PY110), carbon black (index number P.BK.7), and iron oxide red (index number PR101).
[0066] In one alternative embodiment, the second plasticizer and the third plasticizer are each independently composed of di(2-propylheptyl) phthalate, diisooctyl sebacate and dioctyl azelate in a mass ratio of (50-65):(20-45):(2-8).
[0067] Thirdly, the present invention provides a PVC artificial leather, which is prepared according to the preparation method described above.
[0068] The technical solution of this invention has the following advantages: 1. The method for preparing a foamed layer provided by the present invention includes the following steps: S1. Mixing a first PVC resin, a first chemical foaming agent, and a first plasticizer for the first time to obtain a first mixture, and then mixing the first mixture with a microsphere foaming agent for the second time to obtain a second mixture; S2. Calendering the second mixture to obtain a foamed layer; S3. Foaming the foamed layer to obtain the foamed layer; wherein the temperature of the material in S1 and S2 is lower than the initial foaming temperature of the microsphere foaming agent.
[0069] This invention employs a hybrid foaming process combining microsphere foaming and chemical foaming, along with a specific process sequence and synergistic effects of temperature control on the material. This not only increases the foaming ratio but also solves the problem of uneven cell size caused by traditional chemical foaming agents during the foaming process.
[0070] This invention employs a "post-addition method," where the first PVC resin is mixed with the first chemical foaming agent and the first plasticizer before the microsphere foaming agent is added. The core purpose of this addition sequence is to prevent the microsphere foaming agent from contacting the plasticizer in the system too early, thereby preventing premature breakage during mixing. The main reason is that both the plasticizer and the microsphere shell are organic polymer materials with good compatibility. If the microsphere foaming agent is added too early, at room temperature, the plasticizer molecules will gradually migrate and embed themselves between the molecular chains of the microsphere shell. Long-term contact will cause the shell to soften, swell, or even completely dissolve, severely damaging the integrity of the microsphere foaming agent's structure and ultimately leading to foaming failure. The "post-addition method" significantly shortens the contact time between the microsphere foaming agent and the plasticizer, effectively protecting the microsphere shell and ensuring that the foaming agent performs its intended foaming properties in subsequent processing.
[0071] This invention controls the temperature of the materials in S1 and S2 to be lower than the initial foaming temperature of the microsphere foaming agent, ensuring that the microsphere foaming agent remains in an unfoamed state before the foaming step in S3. By limiting the temperature of the materials in S1 and S2 to below the initial foaming temperature of the microsphere foaming agent, this invention achieves plasticization of the PVC resin and uniform dispersion of the microspheres, avoiding premature foaming of the microsphere foaming agent. This results in a more uniform pore size in the microsphere foaming agent, leading to PVC artificial leather with advantages such as uniform pore size, high interlayer bonding strength, clear surface texture (due to gentle foaming after calendering, without gas impact), strong resistance to yellowing, and extremely low volatile organic compound content. The calendering process temperature being lower than the initial foaming temperature of the microsphere foaming agent maintains its original state and prevents the microspheres from rupturing.
[0072] This invention combines microsphere foaming agents with chemical foaming agents, significantly improving cell uniformity in PVC artificial leather processing. The microsphere foaming agent itself consists of uniformly sized solid particles. When the temperature reaches its initial foaming temperature, the outer shell softens, and the internal gas expands, forming independent, closed, and highly uniform cells. Simultaneously, the microspheres exhibit good compatibility with PVC resin. Before plasticization, the PVC macromolecular chains adsorb onto the microsphere surface, creating an anchoring effect that ensures the microspheres are stably dispersed in the matrix and do not float or sink. This avoids the problem of inconsistent cell size caused by uneven thermal decomposition and random nucleation of gas molecules in traditional chemical foaming agents. The addition of chemical foaming agents further increases the foaming ratio, while the addition of plasticizers adjusts the melt viscosity by reducing the intermolecular forces of PVC molecules, placing it in a highly elastic state suitable for cell growth. This ensures smooth cell growth while maintaining cell independence and size uniformity. Furthermore, the insertion of plasticizer molecules into PVC chains increases the intermolecular free volume, facilitating the more uniform and dense formation of initial gas nuclei from the decomposition of the foaming agent. The more numerous and evenly distributed these gas nuclei, the finer and more uniform the final cells. These three factors work synergistically: the pre-nucleation effect of microspheres dominates cell size consistency, the chemical foaming agent compensates for insufficient foaming ratio, and the plasticizer optimizes the melt environment. Ultimately, this reduces chemical residues and irritating odors while achieving a high degree of uniformity in the cell structure.
[0073] 2. The foaming step in S3 includes sequentially performing a first heating stage, a second heating stage, a third heating stage, and a fourth heating stage; the temperature of the first heating stage is 160-180℃, the temperature of the second heating stage is 200-210℃, the temperature of the third heating stage is 200-210℃, and the temperature of the fourth heating stage is 130-150℃.
[0074] The expansion process of the microsphere foaming agent can be divided into the following stages: In the first heating stage at a relatively low temperature (160-180℃), the microsphere foaming agent maintains its basic morphology, the shell has not yet softened significantly, and the internal foaming agent is in an unactivated or partially activated state; when the temperature rises to the second heating stage (200-210℃) in step S3, that is, reaching and exceeding the initial foaming temperature of the microsphere foaming agent, the polymer shell of the microsphere foaming agent begins to soften, the internal foaming agent vaporizes to generate internal pressure, and the microspheres begin to expand; entering the third heating stage ( At 200-210℃, the microsphere foaming agent is in the fully foaming range under the continuous action of high temperature. The volume of the microspheres increases slowly and continuously until they expand to their maximum volume. At this time, some of the microsphere foaming agent shells rupture due to excessive internal pressure, and the foaming process is basically over. When entering the fourth heating stage (130-150℃), the temperature decreases, the foamed matrix material gradually cools and solidifies, the microsphere foaming agent shell hardens, the expanded microsphere structure is fixed, and the shrinkage of the unruptured microspheres is limited, finally obtaining a stable foamed structure. Attached Figure Description
[0075] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0076] Figure 1 This is a cell diagram of the PVC artificial leather sample obtained in Example 4 of the present invention when the foaming time is 50s; Figure 2 This is a cell diagram of the foam layer of the PVC artificial leather sample obtained in Example 1 of the present invention; Figure 3 This is a cell diagram of the foamed layer of the PVC artificial leather sample obtained in Example 5 of the present invention; Figure 4 This is a cell diagram of the foam layer of the PVC artificial leather sample prepared in Comparative Example 2 of this invention. Figure 5 This is a cell diagram of the foam layer of the PVC artificial leather sample prepared in Comparative Example 1 of this invention. Figure 6 This is a cell diagram of the foam layer of the PVC artificial leather sample prepared in Comparative Example 3 of this invention. Figure 7 This is a cell diagram of the foam layer of the PVC artificial leather sample prepared in Comparative Example 4 of this invention. Figure 8 This is a cell diagram of the foam layer of the PVC artificial leather sample prepared in Comparative Example 5 of this invention. Figure 9 This is a schematic diagram of the structure of the inverted L-shaped four-roll calender in Embodiments 1-5 of the present invention.
[0077] Explanation of reference numerals in the attached figures: 1. One roller; 2. Two rollers; 3. Three rollers; 4. Four rollers. Detailed Implementation
[0078] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.
[0079] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0080] The raw materials and their sources used in the embodiments and comparative examples of this invention are as follows: Knitted fabric, model 150D / 96F circular knitting machine, manufacturer: Jiangsu Songbai Textile Co., Ltd. Microsphere foaming agent, model 980DU100, manufacturer: AkzoNobel, the average particle size of the microsphere foaming agent is 100-120μm, the outer shell is acrylonitrile-vinylidene chloride copolymer, the inner layer is isobutane gas, and the initial foaming temperature is 185℃; AC foaming agent (azodicarbonamide), model 110S, manufacturer: Jiangmen Guangyue Electrochemical Co., Ltd. Two-component polyurethane adhesive, model: BR-8877B, manufacturer: Qingyuan Meijiale Environmental Protection New Materials Co., Ltd. Di(2-propylheptyl) phthalate, model: DPHP, manufacturer: Zhuhai Liancheng Chemical Industry Co., Ltd.; Diisooctyl sebacate, model: DOS, manufacturer: Jiangsu Senhe Chemical Technology Co., Ltd. Dioctyl azelate, model: DOA, manufacturer: Zhongshan Liancheng Chemical Industry Co., Ltd.; Barium-zinc stabilizer, model: FS-469, manufacturer: Xiamen United Chemical Co., Ltd. Tinted black (index number PK7), model: 502, manufacturer: Juli Pigment & Plastics Industry Co., Ltd. Heavy calcium carbonate powder, model: B-928, manufacturer: Yifeng Powder Co., Ltd. Calcium and zinc stabilizer, model: SP-200A, manufacturer: ADEKA; Titanium dioxide (index number PW6), model: 404, manufacturer: Huihecai Pigment Co., Ltd. Water-based treatment agent A is prepared by polyurethane main paste A and polyisocyanate crosslinking agent at a mass ratio of 100:4; Water-based treatment agent B is formulated from polyurethane main paste B, polycarbodiimide crosslinking agent and hand feel agent in a mass ratio of 100:4:8; Polyurethane main paste A, model: WF-43-417, manufacturer: Stahl. Polyisocyanate crosslinking agent, model: XR-28-404, manufacturer: Stahl. Polyurethane main paste B, model: Stahl 3649, manufacturer: Stahl. Polycarbodiimide crosslinking agent, model: XR-5580, manufacturer: Stahl. Hand feel agent, model: HM-13-678, manufacturer: Stahl.
[0081] Example 1 This embodiment provides a method for preparing PVC artificial leather, including the following steps: S1'. Obtaining the base fabric layer: Apply a layer of thermosetting adhesive (two-component polyurethane adhesive) to the base fabric (knitted fabric), and dry it (drying is done by setting the temperature and time to 170℃, 0.3min and 180℃, 0.3min respectively) to make the adhesive semi-cured to form the base fabric layer. Obtaining the backing layer: The backing layer components (by weight, including 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptaethyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (barium zinc stabilizer), 0.8 parts of pigment (carbon black, index number P.BK.7), 2 parts of AC foaming agent (azodicarbonamide), and 50 parts of calcium powder (heavy calcium carbonate powder)) are stirred and mixed (stirring speed 1700 r / min, stirring time 500 s), internally mixed (internal mixing speed 750 r / min, internal mixing time 340 s), and plasticized (the front and rear roll temperatures of the two-roll mill are both 185℃ in the first open mill and the front and rear roll temperatures of the two-roll mill are both 185℃ in the second open mill) to obtain the backing layer material. Then, the backing layer material is processed using a four-roll calender (e.g., Figure 9 As shown, the material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 190℃, roll 2 at 190℃, roll 3 at 185℃ and roll 4 at 180℃), and then cooled (the cooling rolls are arranged in pairs, with a total of three pairs; the first two pairs of cooling rolls are circulated with 0℃ low-temperature cold water, and the last pair of cooling rolls is circulated with 25℃ room temperature water) and then bonded to the base fabric layer for the first time to obtain the first bonding layer.
[0082] S2'. By weight, 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (calcium-zinc stabilizer), 0.8 parts of pigment (titanium dioxide, index number PW6), 2 parts of AC foaming agent (azodicarbonamide), 50 parts of calcium powder (heavy calcium carbonate powder), and 18 parts of flame retardant (antimony trioxide) are mixed for the first time (mixing speed 1500 r / min, mixing time 3 min) to obtain the first mixture. The first mixture is then heated to T1=1. After reaching 00℃, a second mixing was performed with 5 parts of microsphere foaming agent (average particle size 115μm) (mixing speed 1500r / min, mixing time 5.5min) to obtain a second mixture. The mixture was then heated to T2=115℃ and subjected to intensive mixing (intensive mixing speed 700r / min, intensive mixing time 340s, with hammering every 90-110s to check for material sticking) and plasticizing (temperatures of the front and rear rolls of the two-roll mill were 185℃ in the first intensive mixing and 180℃ in the second intensive mixing) to obtain the foamed layer material. This foamed layer material was then processed using a four-roll calender (e.g., Figure 9 The material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 185℃, roll 2 at 185℃, roll 3 at 180℃ and roll 4 at 175℃), and then cooled (the first two pairs of cooling rolls are circulated with 0℃ cold water, and the last pair of cooling rolls are circulated with 25℃ room temperature water) to obtain the foaming layer. The material temperature is monitored in real time throughout steps S1' and S2' at 170-175℃.
[0083] S3'. The foaming layer is bonded to the fabric side of the first bonding layer for the second time to obtain the second bonding layer.
[0084] S4'. Obtaining the surface layer: By weight, 100 parts of PVC resin (SG-3 type PVC resin), 99 parts of plasticizer (di(2-propylheptaethyl phthalate), 5 parts of stabilizer (calcium zinc stabilizer), 3 parts of pigment (carbon black (index number P.BK.7)) and 5 parts of calcium powder (heavy calcium carbonate powder) are mixed (stirring speed is 1700 r / min, stirring time is 10 min), and after intensive mixing (stirring speed is 750 r / min, intensive mixing time is 360 s) to obtain the surface layer material, the surface layer material is heated to 177-183℃ and then bonded to the surface of the second bonding layer to be foamed for the third time (roller bonding, roller pressure is 20 MPa), and cooled by cooling rollers (the first two pairs of cooling rollers are circulated with 0℃ low temperature cold water, and the last pair of cooling rollers are circulated with 25℃ room temperature water) to obtain the semi-finished product.
[0085] S5'. A water-based treatment agent is applied to the surface of the semi-finished product using a gravure roller coating method for surface treatment. The first layer uses water-based treatment agent A, which is applied using a 100-mesh anilox roller at a speed of 20 m / min through a 6-m long oven at 135°C. The second layer uses water-based treatment agent B, which is applied using a 130-mesh anilox roller at a speed of 20 m / min through a 15-m long oven at 115°C. Then, cooling is performed (0°C low-temperature cold water is introduced into the first two pairs of cooling rollers, and 25°C room temperature water is introduced into the last pair of cooling rollers) to improve the product's feel. Then, foaming is performed. During foaming, four drying ovens are set up in sequence inside the foaming furnace. Each drying oven is 6m long. The semi-finished product after water-based treatment passes through linearly and continuously. Each section is independently temperature controlled. The temperatures of the four drying ovens are set to 170-208-208-140℃, and the foaming time is 2.8min. During the foaming process, the material conveying speed in the foaming furnace is 8.6m / min. After cooling (the first two pairs of cooling rollers are circulated with 0℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 25℃ room temperature water), the product is rolled up to obtain PVC artificial leather.
[0086] Example 2 This embodiment provides a method for preparing PVC artificial leather, including the following steps: S1'. Obtaining the base fabric layer: Apply a layer of thermosetting adhesive (two-component polyurethane adhesive) to the base fabric (knitted fabric), and dry it (drying is done by setting the temperature and time to 170℃, 0.3min and 180℃, 0.3min respectively) to make the adhesive semi-cured to form the base fabric layer. Obtaining the backing layer: The backing layer components (by weight, including 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (65 parts of di(2-propylheptaethyl) phthalate, 35 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (barium zinc stabilizer), 0.8 parts of pigment (carbon black, index number P.BK.7), 2 parts of AC foaming agent (azodicarbonamide), and 50 parts of calcium powder (heavy calcium carbonate powder)) are stirred and mixed (stirring speed 1500 r / min, stirring time 600 s), internally mixed (internal mixing speed 800 r / min, internal mixing time 340 s), and plasticized (the front and rear roll temperatures of the two-roll mill are both 190℃ in the first open mill and 185℃ in the second open mill) to obtain the backing layer material. Then, the backing layer material is processed using a four-roll calender (e.g., Figure 9The material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 185°C, roll 2 at 185°C, roll 3 at 180°C and roll 4 at 175°C), and then cooled (the cooling rolls are arranged in pairs, with three pairs in total; the first two pairs of cooling rolls are circulated with 5°C low-temperature cold water, and the last pair of cooling rolls is circulated with 23°C room-temperature water) and then bonded to the base fabric layer for the first time to obtain the first bonding layer.
[0087] S2'. By weight, 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (65 parts of di(2-propylheptyl) phthalate, 35 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (barium zinc stabilizer), 0.8 parts of pigment (titanium dioxide, index number PW6), 2 parts of AC foaming agent (azodicarbonamide), 50 parts of calcium powder (heavy calcium carbonate powder), and 18 parts of flame retardant (antimony trioxide) are mixed for the first time (mixing speed 1500 r / min, mixing time 2 min) to obtain the first mixture. The first mixture is then heated to T1= After reaching 93℃, a second mixing process was performed with 5 parts of microsphere foaming agent (average particle size 100μm) (mixing speed 1500r / min, mixing time 380s) to obtain a second mixture. The mixture was then heated to T2=105℃ and subjected to intensive mixing (intensive mixing speed 700r / min, intensive mixing time 340s, with hammering every 90-110s to check for material sticking) and plasticizing (temperatures of the front and rear rolls of the two-roll mill were 185℃ in the first intensive mixing and 180℃ in the second intensive mixing) to obtain the foamed layer material. This foamed layer material was then processed using a four-roll calender (e.g.,...). Figure 9 The material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 185℃, roll 2 at 185℃, roll 3 at 180℃ and roll 4 at 175℃) and cooled (the first two pairs of cooling rolls are circulated with 5℃ low-temperature cold water, and the last pair of cooling rolls are circulated with 23℃ room temperature water) to obtain the foaming layer. The material temperature is monitored in real time throughout steps S1' and S2' at 170-175℃.
[0088] S3'. The foaming layer is bonded to the fabric side of the first bonding layer for the second time to obtain the second bonding layer.
[0089] S4'. Obtaining the surface layer: By weight, 100 parts of PVC resin (SG-3 type PVC resin), 99 parts of plasticizer (di(2-propylheptyl) phthalate), 5 parts of stabilizer (calcium zinc stabilizer), 3 parts of pigment (carbon black, index number P.BK.7) and 5 parts of calcium powder (heavy calcium carbonate powder) are mixed (stirring speed 1700 r / min, stirring time 10 min). After intensive mixing (stirring speed 750 r / min, intensive mixing time 360 s), the surface layer material is obtained. The surface layer material is heated to 177-183℃ and then bonded to the surface of the second bonding layer to be foamed for the third time (roller bonding, roller pressure 20 MPa). After cooling by cooling rollers (the first two pairs of cooling rollers are circulated with 5℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 23℃ room temperature water), a semi-finished product is obtained.
[0090] S5'. A water-based treatment agent is applied to the surface of the semi-finished product using a gravure roller coating method for surface treatment. The first layer uses water-based treatment agent A, which is applied using a 120-mesh anilox roller at a speed of 20 m / min through a 6-m long oven at 130°C. The second layer uses water-based treatment agent B, which is applied using a 130-mesh anilox roller at a speed of 20 m / min through a 15-m long oven at 110°C. Then, cooling is performed (the first two pairs of cooling rollers are circulated with 5°C low-temperature cold water, and the last pair of cooling rollers are circulated with 23°C room temperature water). This improves the product's feel. Then, foaming is performed (four drying ovens are set up in sequence in the foaming furnace, each oven is 6m long, and the water-treated semi-finished product passes through linearly and continuously. Each section is independently temperature controlled, with the temperature T1 set at 170-210-210-140℃, the foaming time being 2.4min, and the material conveying speed in the foaming furnace during the foaming process being 10m / min). After cooling (the first two pairs of cooling rollers are circulated with 5℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 23℃ room temperature water), and then rolled up, PVC artificial leather is obtained.
[0091] Example 3 This embodiment provides a method for preparing PVC artificial leather, including the following steps: S1'. Obtaining the base fabric layer: Apply a layer of thermosetting adhesive (two-component polyurethane adhesive) to the base fabric (knitted fabric), and dry it (drying is done by setting the temperature and time to 170℃, 0.3min and 180℃, 0.3min respectively) to make the adhesive semi-cured to form the base fabric layer. Obtaining the backing layer: The backing layer components (by weight, including 100 parts of PVC resin (SG-3 type PVC resin), 100 parts of plasticizer (di(2-propylheptayl) phthalate), 2 parts of stabilizer (barium zinc stabilizer), 0.5 parts of pigment (carbon black, index number P.BK.7), 2 parts of AC foaming agent (azodicarbonamide), and 25 parts of calcium powder (heavy calcium carbonate powder)) are stirred and mixed (stirring speed 1300 r / min, stirring time 600 s), internally mixed (internal mixing speed 800 r / min, internal mixing time 340 s), and plasticized (the front and rear roll temperatures of the two-roll mill are both 185℃ in the first open mill and the front and rear roll temperatures of the two-roll mill are both 185℃ in the second open mill) to obtain the backing layer material. Then, the backing layer material is processed using a four-roll calender (e.g., Figure 9 As shown, the material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 185℃, roll 2 at 185℃, roll 3 at 180℃ and roll 4 at 175℃), and then cooled (the cooling rolls are arranged in pairs, with a total of three pairs; the first two pairs of cooling rolls are circulated with 8℃ low-temperature cold water, and the last pair of cooling rolls is circulated with 24℃ room temperature water) and then bonded to the base fabric layer for the first time to obtain the first bonding layer.
[0092] S2'. By weight, 100 parts of PVC resin (SG-3 type PVC resin), 100 parts of plasticizer (di(2-propylheptayl) phthalate), 2 parts of stabilizer (barium zinc stabilizer), 0.5 parts of pigment (titanium dioxide, index number PW6), 2 parts of AC foaming agent (azodicarbonamide), 25 parts of calcium powder (heavy calcium carbonate powder), and 20 parts of flame retardant (antimony trioxide) are mixed for the first time (mixing speed 1600 r / min, mixing time 2.5 min) to obtain the first mixture. The first mixture is heated to T1=88℃ and then foamed with 6 parts of microspheres. The agent (average particle size 120μm) was mixed a second time (mixing speed 1700r / min, mixing time 6min) to obtain a second mixture. The mixture was then heated to T2=115℃ and subjected to intensive mixing (intensive mixing speed 700r / min, intensive mixing time 340s, with hammering every 90-110s to check for material sticking). Plasticization was then performed (the front and rear roll temperatures of the two-roll mill were 185℃ in the first sizing and 180℃ in the second sizing to obtain the foamed layer material). This foamed layer material was then processed using a four-roll calender (e.g.,...). Figure 9The material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 185℃, roll 2 at 185℃, roll 3 at 180℃ and roll 4 at 175℃) and then cooled (the first two pairs of cooling rolls are circulated with 8℃ low-temperature cold water, and the last pair of cooling rolls are circulated with 24℃ room temperature water) to obtain the foaming layer. The material temperature is monitored in real time throughout steps S1' and S2' at 170-175℃.
[0093] S3'. The foaming layer is bonded to the fabric side of the first bonding layer for the second time to obtain the second bonding layer.
[0094] S4'. Obtaining the surface layer: By weight, 100 parts of PVC resin (SG-3 type PVC resin), 85 parts of plasticizer (di(2-propylheptayl) phthalate), 5 parts of stabilizer (calcium zinc stabilizer), 1 part of pigment (titanium dioxide, index number PW6), and 5 parts of calcium powder (heavy calcium carbonate powder) are mixed (stirring speed is 1700 r / min, stirring time is 10 min). After intensive mixing (stirring speed is 750 r / min, intensive mixing time is 360 s), the surface layer material is obtained. The surface layer material is heated to 177-183℃ and then bonded to the surface of the second bonding layer to be foamed for the third time (roller bonding, roller pressure is 20 MPa). After cooling by cooling rollers (the first two pairs of cooling rollers are circulated with 8℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 24℃ room temperature water), a semi-finished product is obtained.
[0095] S5'. A water-based treatment agent is applied to the surface of the semi-finished product using a gravure roller coating method for surface treatment. The first layer uses water-based treatment agent A, applied using a 100-mesh anilox roller at a speed of 20 m / min through a 6-m long oven at 140°C. The second layer uses water-based treatment agent B, applied using a 130-mesh anilox roller at a speed of 20 m / min through a 15-m long oven at 120°C. Then, cooling is performed (the first two pairs of cooling rollers are circulated with 8°C low-temperature cold water, and the last pair of cooling rollers are circulated with 24°C room temperature water). This improves the product's feel. Then, foaming is performed (four drying ovens are set up in sequence in the foaming furnace, each oven is 6m long, and the water-treated semi-finished product passes through linearly and continuously. Each section is independently temperature controlled, with the set temperatures T1 being 170-210-210-140℃, the foaming time being 2.5min, and the material conveying speed in the foaming furnace during the foaming process being 9.6m / min). After cooling (the first two pairs of cooling rollers are circulated with 8℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 24℃ room temperature water), the product is rolled up to obtain PVC artificial leather.
[0096] Example 4 This embodiment provides a method for preparing PVC artificial leather, including the following steps: S1'. Obtaining the base fabric layer: Apply a layer of thermosetting adhesive (two-component polyurethane adhesive) to the base fabric (knitted fabric), and dry it (drying is done by setting the temperature and time to 170℃, 0.3min and 180℃, 0.3min respectively) to make the adhesive semi-cured to form the base fabric layer. Obtaining the backing layer: The backing layer components (by weight, including 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptaethyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (barium zinc stabilizer), 0.8 parts of pigment (carbon black, index number P.BK.7), 2 parts of AC foaming agent (azodicarbonamide), and 50 parts of calcium powder (heavy calcium carbonate powder)) are stirred and mixed (stirring speed 1700 r / min, stirring time 500 s), internally mixed (internal mixing speed 750 r / min, internal mixing time 360 s), and plasticized (the front and rear roll temperatures of the two-roll mill are both 185℃ in the first open mill and the front and rear roll temperatures of the two-roll mill are both 185℃ in the second open mill) to obtain the backing layer material. Then, the backing layer material is processed using a four-roll calender (e.g., Figure 9 As shown, the material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 190℃, roll 2 at 190℃, roll 3 at 185℃ and roll 4 at 180℃), and then cooled (the cooling rolls are arranged in pairs, with a total of three pairs; the first two pairs of cooling rolls are circulated with 0℃ low-temperature cold water, and the last pair of cooling rolls is circulated with 25℃ room temperature water) and then bonded to the base fabric layer for the first time to obtain the first bonding layer.
[0097] S2'. By weight, 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (calcium-zinc stabilizer), 0.8 parts of pigment (titanium dioxide, index number PW6), 2 parts of AC foaming agent (azodicarbonamide), 50 parts of calcium powder (heavy calcium carbonate powder), and 18 parts of flame retardant (antimony trioxide) are mixed for the first time (mixing speed 1500 r / min, mixing time 3 min) to obtain the first mixture. The first mixture is then heated to T1=1. After reaching 00℃, a second mixing was performed with 5 parts of microsphere foaming agent (average particle size 115μm) (mixing speed 1500r / min, mixing time 5.5min) to obtain a second mixture. The mixture was then heated to T2=115℃ and subjected to intensive mixing (intensive mixing speed 700r / min, intensive mixing time 360s, with hammering every 90-110s to check for material sticking) and plasticizing (temperatures of the front and rear rolls of the two-roll mill were 185℃ in the first intensive mixing and 180℃ in the second intensive mixing) to obtain the foamed layer material. This foamed layer material was then processed using a four-roll calender (e.g., Figure 9 The material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 185℃, roll 2 at 185℃, roll 3 at 180℃ and roll 4 at 175℃) and then cooled (the first two pairs of cooling rolls are circulated with 0℃ cold water, and the last pair of cooling rolls are circulated with 25℃ room temperature water) to obtain the foaming layer. The material temperature is monitored in real time throughout steps S1' and S2' at 170-175℃.
[0098] S3'. The foaming layer is bonded to the fabric side of the first bonding layer for the second time to obtain the second bonding layer.
[0099] S4'. Obtaining the surface layer: By weight, 100 parts of PVC resin (SG-3 type PVC resin), 99 parts of plasticizer (di(2-propylheptyl) phthalate), 5 parts of stabilizer (calcium zinc stabilizer), 3 parts of pigment (carbon black (index number P.BK.7)) and 5 parts of calcium powder (heavy calcium carbonate powder) are mixed (stirring speed 1700 r / min, stirring time 10 min). After intensive mixing (stirring speed 750 r / min, intensive mixing time 360 s), the surface layer material is obtained. The surface layer material is heated to 177-183℃ and then bonded to the surface of the second bonding layer to be foamed for the third time (roller bonding, roller pressure 20 MPa). After cooling by cooling rollers (the first two pairs of cooling rollers are circulated with 0℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 25℃ room temperature water), a semi-finished product is obtained.
[0100] S5'. A water-based treatment agent is applied to the surface of the semi-finished product using a gravure roller coating method for surface treatment. The first layer uses water-based treatment agent A, applied using a 100-mesh anilox roller at a speed of 20 m / min through a 6-m long oven at 135°C. The second layer uses water-based treatment agent B, applied using a 130-mesh anilox roller at a speed of 20 m / min through a 15-m long oven at 115°C. Cooling is then performed (the first two pairs of cooling rollers are circulated with 0°C cold water, and the last pair is circulated with 25°C room temperature water). This process is then repeated. To improve the feel of the product, it is then foamed (during foaming, four drying ovens are set up in sequence in the foaming furnace, each oven is 6m long, and the water-based semi-finished product passes through linearly and continuously, with independent temperature control for each section. The set temperatures T1 are 170-208-208-140℃, the foaming time is 50s, and the material conveying speed in the foaming furnace during the foaming process is 28.8m / min). After that, it is cooled by cooling rollers (the first two pairs of cooling rollers are filled with 0℃ low-temperature cold water, and the last pair of cooling rollers are filled with 25℃ room temperature water), and then rolled up to obtain PVC artificial leather.
[0101] Example 5 This embodiment provides a method for preparing PVC artificial leather, including the following steps: S1'. Obtaining the base fabric layer: Apply a layer of thermosetting adhesive (two-component polyurethane adhesive) to the base fabric (knitted fabric), and dry it (drying is done by setting the temperature and time to 170℃, 0.3min and 180℃, 0.3min respectively) to make the adhesive semi-cured to form the base fabric layer. Obtaining the backing layer: The backing layer components (by weight, including 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptaethyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (barium zinc stabilizer), 0.8 parts of pigment (carbon black, index number P.BK.7), 2 parts of AC foaming agent (azodicarbonamide), and 50 parts of calcium powder (heavy calcium carbonate powder)) are stirred and mixed (stirring speed 1700 r / min, stirring time 500 s), internally mixed (internal mixing speed 750 r / min, internal mixing time 340 s), and plasticized (the front and rear roll temperatures of the two-roll mill are both 185℃ in the first open mill and the front and rear roll temperatures of the two-roll mill are both 185℃ in the second open mill) to obtain the backing layer material. Then, the backing layer material is processed using a four-roll calender (e.g., Figure 9As shown, the material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 at 190℃, roll 2 at 190℃, roll 3 at 185℃ and roll 4 at 180℃), and then cooled (the cooling rolls are arranged in pairs, with a total of three pairs; the first two pairs of cooling rolls are circulated with 0℃ low-temperature cold water, and the last pair of cooling rolls is circulated with 25℃ room temperature water) and then bonded to the base fabric layer for the first time to obtain the first bonding layer.
[0102] S2'. By weight, 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (calcium-zinc stabilizer), 0.8 parts of pigment (titanium dioxide, index number PW6), 2 parts of AC foaming agent (azodicarbonamide), 50 parts of calcium powder (heavy calcium carbonate powder), and 18 parts of flame retardant (antimony trioxide) are mixed for the first time (mixing speed 1500 r / min, mixing time 3 min) to obtain the first mixture. The first mixture is then heated to T1=100℃. Then, it is mixed a second time with 5 parts of microsphere foaming agent (the average particle size of the microsphere foaming agent is 115μm) (mixing speed is 1500r / min, mixing time is 5.5min) to obtain a second mixture. The mixture is then heated to T2=115℃ and subjected to intensive mixing (intensive mixing speed is 700r / min, intensive mixing time is 340s, during which the hammer is used every 90-110s to observe for any sticking). Plasticization is then performed (the front and rear roll temperatures of the two-roll mill are 185℃ in the first intensive mixing and 180℃ in the second intensive mixing) to obtain the foamed layer material. The foamed layer material is then processed using a four-roll calender (e.g., Figure 9 The material is calendered (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with the temperature of roll 1 being 185℃, roll 2 being 185℃, roll 3 being 180℃ and roll 4 being 175℃), and then cooled (the first two pairs of cooling rolls are circulated with 0℃ low-temperature cold water, and the last pair of cooling rolls are circulated with 25℃ room temperature water) to obtain the foaming layer. The material temperature is monitored in real time throughout steps S1' and S2' at 170-175℃.
[0103] S3'. The foaming layer is bonded to the fabric side of the first bonding layer for the second time to obtain the second bonding layer.
[0104] S4'. Obtaining the surface layer: By weight, 100 parts of PVC resin (SG-3 type PVC resin), 99 parts of plasticizer (di(2-propylheptyl) phthalate), 5 parts of stabilizer (calcium zinc stabilizer), 3 parts of pigment (carbon black (index number P.BK.7)) and 5 parts of calcium powder (heavy calcium carbonate powder) are mixed (stirring speed 1700 r / min, stirring time 10 min). After intensive mixing (stirring speed 750 r / min, intensive mixing time 360 s), the surface layer material is obtained. The surface layer material is heated to 177-183℃ and then bonded to the surface of the second bonding layer to be foamed for the third time (roller bonding, roller pressure 20 MPa). After cooling by cooling rollers (the first two pairs of cooling rollers are circulated with 0℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 25℃ room temperature water), a semi-finished product is obtained.
[0105] S5'. A water-based treatment agent is applied to the surface of the semi-finished product using a gravure roller coating method for surface treatment. The first layer uses water-based treatment agent A, applied using a 100-mesh anilox roller at a speed of 20 m / min through a 6-m long oven at 135°C. The second layer uses water-based treatment agent B, applied using a 130-mesh anilox roller at a speed of 20 m / min through a 15-m long oven at 115°C. Cooling is then performed (the first two pairs of cooling rollers are circulated with 0°C cold water, and the last pair is circulated with 25°C room temperature water). To improve the product's feel, foaming is then performed (during foaming, four drying ovens are set up in sequence inside the foaming furnace, each oven being 6m long. The water-treated semi-finished product passes through linearly and continuously, with independent temperature control for each section. The set temperatures T1 are 170-208-208-140℃, and the foaming time is 2.4min. During the foaming process, the material conveying speed inside the foaming furnace is 10m / min). After cooling (the first two pairs of cooling rollers are circulated with 0℃ low-temperature cold water, and the last pair of cooling rollers are circulated with 25℃ room temperature water), the product is rolled up to obtain PVC artificial leather.
[0106] Comparative Example 1 This comparative example provides a method for preparing PVC artificial leather, which differs from Example 1 only in that the microsphere foaming agent is replaced with an equal mass of chemical foaming agent (AC foaming agent) in S2'.
[0107] Comparative Example 2 This comparative example provides a method for preparing PVC artificial leather, which differs from Example 4 only in that the microsphere foaming agent is replaced with an equal mass of chemical foaming agent (AC foaming agent) in S2'.
[0108] Comparative Example 3 This comparative example provides a method for preparing PVC artificial leather, which differs from Example 5 only in that the microsphere foaming agent is replaced with an equal mass of chemical foaming agent (AC foaming agent) in S2'.
[0109] Comparative Example 4 This comparative example provides a method for preparing PVC artificial leather, which differs from Example 1 only in step S2': By weight, 100 parts of PVC resin (SG-3 type PVC resin), 105 parts of plasticizer (60 parts of di(2-propylheptyl) phthalate, 40 parts of diisooctyl sebacate, and 5 parts of dioctyl azelate), 2.6 parts of stabilizer (calcium-zinc stabilizer), 0.8 parts of pigment (titanium dioxide, index number PW6), 2 parts of AC foaming agent (azodicarbonamide), 50 parts of calcium powder (heavy calcium carbonate powder), 18 parts of flame retardant (antimony trioxide), and 5 parts of microsphere foaming agent (the average particle size of the microsphere foaming agent is 115 μm, the outer shell is acrylonitrile-vinylidene chloride copolymer, the inner layer is isobutane gas, and the initial foaming temperature is 182-204℃) are mixed (mixing speed is 1500 r / min, mixing time is 8.5 min) to obtain a mixture.
[0110] Comparative Example 5 This comparative example provides a method for preparing PVC artificial leather by calendering, which differs from Example 1 only in step S2': The process includes: second mixing (mixing speed 1500 r / min, mixing time 500 s), internal mixing (internal mixing speed 700 r / min, internal mixing time 360 s), plasticizing (temperature of the front and rear rolls of the two-roll mill is 190℃ in the first open mill and 185℃ in the second open mill), and calendering (passing through roll 1, roll 2, roll 3 and roll 4 in sequence, with roll 1 temperature 190℃, roll 2 temperature 190℃, roll 3 temperature 187℃ and roll 4 temperature 182℃). The material temperature is monitored in real time throughout steps S1 and S2 at 185℃.
[0111] Experimental Example 1 The foamed layer samples obtained in Example 1 and Comparative Example 1 were each evaluated for odor by six testers to assess the odor. The odor evaluation procedure was performed according to the following requirements: Odor evaluation results: Odor evaluation results are divided into 1 to 6 levels, as shown in Table 1. If the evaluation level is between two levels, a half-level evaluation can be used. For example, if it is between level 1 and level 2, the evaluation level is 1.5.
[0112] The odor rating test results of the foamed layer samples obtained in Example 1 and Comparative Example 1 are shown in Table 2. The average value in the table is the value obtained after removing the highest and lowest values from multiple tests.
[0113] Table 1
[0114] Table 2
[0115] The results show that the foamed layer sample prepared in Example 1 of the present invention has no interfering odor, while the foamed layer sample prepared in Comparative Example 1 using AC foaming agent has an irritating interfering odor. This indicates that the irritating odor of the foamed layer sample prepared by combining microsphere foaming agent and chemical foaming agent is effectively improved.
[0116] Experimental Example 2 The uniformity of the PVC artificial leather samples prepared in Examples 1, 4, and 5, and Comparative Examples 1-3, were observed under a microscope. The results are as follows: Figures 1-6 As shown. The PVC artificial leather samples of Example 4 and Comparative Example 2, prepared after a foaming time of 50 s, were observed under a microscope. Figure 1 and Figure 4 PVC artificial leather samples prepared after a foaming time of 2.8 min in Examples 1 and Comparative Example 1. Figure 2 and Figure 5 PVC artificial leather samples prepared after a foaming time of 2.4 min in Examples 5 and 3. Figure 3 and Figure 6 The foaming layer state: The PVC artificial leather samples prepared in Examples 1, 4 and 5 of the present invention under different foaming times have dense and relatively uniform pores, and the shape of the pores does not change much and the shape is mostly round; however, the PVC artificial leather samples obtained in Comparative Examples 1 to 3 have irregular pore changes, uneven sizes and connected pores under different foaming times.
[0117] Comparative Examples 4 and 5, prepared with a foaming time of 2.4 min, had their cell uniformity observed under a microscope. The results are as follows: Figure 7 and Figure 8 As shown. Microscopic observation of the foaming state: Compared to Example 5, in Comparative Example 4, the plasticizer in the foaming layer was directly mixed with the microsphere foaming agent, causing the microsphere shell to swell and soften. Combined with the mechanical shear force during the mixing process, the shell ruptured prematurely before foaming, causing the gas inside the microspheres to escape. This prevented volume expansion during subsequent heating, resulting in foaming failure of the microsphere foaming agent. Only a small amount of chemical foaming agent was effective. Under the same foaming process, the cell effect was not obvious, and the appearance was almost identical to no foaming agent effect. Compared to Example 5, in Comparative Example 5, the microsphere foaming agent reached the initial foaming temperature during the calendering process, resulting in slight foaming of the foaming layer material during calendering. However, due to the small space between the rollers during calendering, the microsphere foaming agent could not produce volume expansion, leading to foaming failure. Only a small amount of AC had a foaming effect, resulting in an indistinct cell effect in the product, and the appearance was almost identical to no foaming agent effect.
[0118] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A method for preparing a foamed layer, characterized in that, Includes the following steps: S1. The first PVC resin, the first chemical foaming agent, the first plasticizer, the first stabilizer, the first pigment, the first calcium powder, and the flame retardant are mixed for the first time to obtain the first mixture, and then the first mixture is mixed with the microsphere foaming agent for the second time to obtain the second mixture; The first mixture, by mass, comprises the following components: 100 parts of first PVC resin, 72-105 parts of first plasticizer, 1-3 parts of first stabilizer, 0.5-1.0 parts of first pigment, 20-50 parts of first calcium powder, 18-25 parts of flame retardant, and 1-8 parts of first chemical foaming agent; The first plasticizer is composed of di(2-propylheptyl) phthalate, diisooctyl sebacate and dioctyl azelate in a mass ratio of (50-65):(20-45):(2-8). The first calcium powder includes at least one of heavy calcium carbonate powder and light calcium carbonate powder; The mass ratio of microsphere foaming agent to first PVC resin in S1 is (5-8):100; The structure of the microsphere foaming agent includes an outer shell and an inner layer. The outer shell is an acrylonitrile-vinylidene chloride copolymer, and the inner layer is isobutane gas. The average particle size of the microsphere foaming agent is 100-120 μm; S2. The second mixture is calendered to obtain the foaming layer; S3. The layer to be foamed is foamed to obtain the foamed layer; The temperature of the material in S1 and S2 is lower than the initial foaming temperature of the microsphere foaming agent.
2. The method for preparing the foamed layer according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The rotation speed of the first mixing is 1300-1700 r / min, and the time of the first mixing is 1-3 min; (2) The rotation speed of the second mixing is 1300-1700 r / min, and the time of the second mixing is 3-7 min; (3) The initial foaming temperature of the microsphere foaming agent is 182-188℃; (4) The second mixing process further includes heating the first mixture to T1; (5) The process before calendering also includes heating the second mixture to T2; (6) The temperature of the material in S1 and S2 is 165-175℃; (7) The S2 step, after calendering, also includes a first cooling step; (8) The foaming step in S3 includes sequentially performing a first heating stage, a second heating stage, a third heating stage and a fourth heating stage; the temperature of the first heating stage is 160-180℃, the temperature of the second heating stage is 200-210℃, the temperature of the third heating stage is 200-210℃, and the temperature of the fourth heating stage is 130-150℃. (9) The foaming time in S3 is 50s-240s; (10) S3 also includes a second cooling and winding step after foaming.
3. A method for preparing PVC artificial leather, characterized in that, Includes the following steps: S1'. Obtain the base fabric layer and the backing fabric layer and perform the first bonding to obtain the first connecting layer; S2'. The first PVC resin, the first chemical foaming agent, the first plasticizer, the first stabilizer, the first pigment, the first calcium powder, and the flame retardant are mixed for the first time to obtain the first mixture. Then the first mixture is mixed with the microsphere foaming agent for the second time to obtain the second mixture. The second mixture is calendered to obtain the foaming layer. The first mixture, by mass, comprises the following components: 100 parts of first PVC resin, 72-105 parts of first plasticizer, 1-3 parts of first stabilizer, 0.5-1.0 parts of first pigment, 20-50 parts of first calcium powder, 18-25 parts of flame retardant, and 1-8 parts of first chemical foaming agent; The first plasticizer is composed of di(2-propylheptyl) phthalate, diisooctyl sebacate and dioctyl azelate in a mass ratio of (50-65):(20-45):(2-8). The first calcium powder includes at least one of heavy calcium carbonate powder and light calcium carbonate powder; The mass ratio of microsphere foaming agent to first PVC resin in S2' is (5-8):100; The structure of the microsphere foaming agent includes an outer shell and an inner layer. The outer shell is an acrylonitrile-vinylidene chloride copolymer, and the inner layer is isobutane gas. The average particle size of the microsphere foaming agent is 100-120 μm; The temperature of the material in S1' and S2' is lower than the initial foaming temperature of the microsphere foaming agent; S3'. The foaming layer is bonded to the fabric side of the first connecting layer for the second time to obtain the second connecting layer; S4'. Obtain the surface layer, and bond the surface layer to the surface of the foaming layer of the second connecting layer for the third time to obtain a semi-finished product; S5'. The semi-finished product is foamed to obtain the PVC artificial leather.
4. The method for preparing PVC artificial leather according to claim 3, characterized in that, The step of heating the surface layer is also included before the third bonding in S4'. And / or, the third bonding step includes roll bonding; And / or, the third bonding process may include a cooling step.
5. The method for preparing PVC artificial leather according to claim 3 or 4, characterized in that, S5' further includes performing a water-based treatment on the surface layer of the semi-finished product before foaming.
6. The method for preparing PVC artificial leather according to claim 3 or 4, characterized in that, At least one of the following conditions must be met: (1) The base fabric layer in S1' includes at least one of knitted fabric and non-woven fabric; (2) The fabric layer in S1' comprises, by weight, the following components: 100 parts of second PVC resin, 72-105 parts of second plasticizer, 1-3 parts of second stabilizer, 0.5-1.0 parts of second pigment, 1-2 parts of second chemical foaming agent, and 20-50 parts of second calcium powder, wherein the second calcium powder includes at least one of heavy calcium carbonate powder and light calcium carbonate powder; (3) The S4' middle layer, by mass, includes the following components: 100 parts of third PVC resin, 80-100 parts of third plasticizer, 3-5 parts of third stabilizer, 1-3 parts of third pigment, and 2-5 parts of third calcium powder, wherein the third calcium powder includes at least one of heavy calcium carbonate powder and light calcium carbonate powder.
7. The method for preparing PVC artificial leather according to claim 6, characterized in that, At least one of the following conditions must be met: (1) The second plasticizer and the third plasticizer each independently include one or more of di(2-propylheptyl) phthalate, diisooctyl sebacate, and dioctyl azelate; (2) The second PVC resin and the third PVC resin each independently include at least one of SG-3 type PVC resin and SG-5 type PVC resin; (3) The second stabilizer and the third stabilizer each independently include at least one of calcium-zinc stabilizer and barium-zinc stabilizer; (4) The second chemical foaming agent includes at least one of azodicarbonamide and modified sodium bicarbonate.
Citation Information
Patent Citations
High-permeability PVC artificial leather and application thereof
CN110373910A
Foaming agent regulation and control method for low-density high-performance polyurethane sole stock solution