Zoned steam vent and oil resistant formable paper-based packaging structure for hot food hamburger wraps and methods of making and using
By setting a PHA coating pattern on the food contact side of hot food hamburger packaging paper, dividing functional areas and forming an exposed cellulose continuous phase, the problems of oil resistance and vapor release in the high oil contact area of hot food hamburger packaging paper are solved, and a stable packaging structure and shape maintenance are achieved.
Patent Information
- Application Number
- CN202611363585.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-09-04
AI Technical Summary
Existing hot food hamburger packaging paper has difficulty achieving continuous oil resistance in high oil contact areas while effectively venting steam on the periphery. Furthermore, the steam venting end is unstable after folding and labeling, increasing the complexity of the manufacturing process.
A PHA coating pattern is provided on the food contact side of the paper-based packaging structure to divide it into a first functional area and a second functional area. The first functional area forms a continuous PHA barrier phase, and the second functional area forms an exposed cellulose continuous phase, ensuring that water vapor is transferred through the exposed cellulose surface and that at least one end is connected to the outside after folding.
It achieves continuous oil-blocking protection in high oil contact areas, ensures effective water vapor discharge, maintains the stability and shape integrity of the packaging structure, and reduces the complexity of preparation.
Smart Images

Figure CN122852990B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of paper-based food packaging materials, bio-based barrier coatings, and patterned coatings, and relates to a partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot food hamburgers, as well as its preparation and application methods. Background Technology
[0002] Hot hamburgers, such as beef burgers, cheeseburgers, and fried chicken burgers, continue to release grease, sauces, and water vapor after being served. If the packaging paper lacks sufficient barrier properties, grease and sauces can easily seep through the paper fiber network via capillary action, causing oil seepage through the paper back, hand contamination, and outer packaging contamination. When a dense film with high coverage forms on the food contact side, water vapor can easily accumulate and condense between the hamburger and the paper surface, causing the hamburger bun to become soggy, collapse, or deform, and increasing the adhesion of bread crumbs to the packaging paper. Therefore, the paper-based packaging structure used for hot hamburger wraps needs to maintain stable oil resistance at the main pressure-bearing and high-oil contact areas of the hamburger, while also retaining a paper base area on its outer perimeter that can transfer water vapor and remain effective after folding and labeling.
[0003] To improve the oil and water resistance of paper-based food packaging, existing technologies have employed polyhydroxyalkanoates (PHA) or other biodegradable polymers to form paper-based coatings. US5451456A discloses a technique for coating or impregnating paper and other fibrous structures with PHA aqueous latex; WO2017151595A1 discloses an aqueous dispersion containing biodegradable polymer particles and stabilizers, listing paper coating as one of its applications; WO2020036843A1 discloses applying an aqueous PHA dispersion to the food contact surface of a biodegradable substrate to improve water and oil resistance; WO2021256381A1 discloses coated paper containing poly(3-hydroxybutyrate-3-hydroxyhexanoate) copolyester (PHBH) and an adhesive; CN120759147B discloses a PHA oil-resistant and moisture-permeable coating for hamburger paper, which balances oil resistance, moisture permeability, and flexibility through a compositional gradient in the coating thickness direction. The key technical aspects of the above solutions lie in the composition of the coating material, water-based dispersion, film quality, interlayer bonding, or thickness-direction structure. When this type of material is directly applied to single-sheet hot food hamburger packaging paper, if the coating coverage of the food contact surface is increased in a continuous or nearly uniform manner, the open paper surface available for water vapor to pass outward through the paper thickness will decrease accordingly; if the coating coverage is generally reduced, it will be difficult to ensure that a stable and continuous oil-resistant area is formed in the main pressure-bearing and high-oil contact areas of the hamburger.
[0004] To balance oil resistance and water vapor transmission, WO2013008938A1 discloses a coating formed using an acid-containing copolymer and filler, enabling food packaging paper to maintain air permeability and moisture permeability while possessing water resistance, oil resistance, and release properties. JP4520138B2 discloses a method for obtaining food packaging paper with both oil resistance and water vapor permeability by combining parameters such as base paper structure, water-soluble polymer coating, and moisture permeability. EP0676920B1 discloses applying a coating that reduces porosity to a porous membrane used for modified atmosphere packaging of fruits and vegetables according to a predetermined pattern and coating amount to regulate the transmission of oxygen and carbon dioxide. These solutions demonstrate that barrier and transmission properties can be coordinated through paper structure, coating formulation, coating amount, or coating pattern, but their technical focus remains on the overall performance of the packaging paper or the gas transmission rate of the modified atmosphere membrane. For single-sheet wrapping paper that needs to be folded around a hot hamburger and secured with a label, having only a predetermined overall moisture permeability or partial open area cannot guarantee that the open paper surface will extend continuously from the outer perimeter of the hamburger to the edge of the paper, nor can it guarantee that it will retain an end that is connected to the outside of the packaging after forming multiple folds and being labeled.
[0005] Existing technologies also handle water vapor in hot food packaging through water-absorbing vapor-conveying layers or specialized vapor-venting components. CN114438824B discloses a method of setting a waterproof vapor-conveying layer formed by heating and foaming on the outer surface of a paper substrate, and setting a water-absorbing layer on the inner surface, so that water vapor generated by hot food is absorbed and transported outward; US4874620A discloses the use of slits and unlaminated areas in the inner layer of a microwaveable packaging bag to form interlayer vapor-venting channels to release pressure and steam inside the packaging; US4355757A discloses a vapor-venting structure formed by tangents, folds, vent holes, and a support plate at the bottom of a food heating carton. These solutions can provide absorption, transport, or emission points for water vapor, but typically require double-sided functional layers, foam pores, interlayer channels in the bag wall, vent holes, slits, or a carton support structure. When this type of structure is used in single-sheet hamburger wrappers that require quick folding and labeling, it increases the requirements for preparation and folding coordination. If the venting location falls in the main contact area of oil and sauce, or is covered by folds and labels after folding, it may also weaken the oil-blocking effect or reduce the effectiveness of venting after the packaging is formed.
[0006] Therefore, the existing technology still needs further improvement: forming a continuous oil-blocking area on the same food contact side to bear the load of the main oil and sauce of the hot hamburger, and a continuous open paper base area for transmitting water vapor; making the continuous open paper base area form multiple continuous paths that pass through different folding areas and reach different paper edges, so as to reduce the risk of simultaneously closing all the ends of the paths in the same fold or when fixing the label; and ensuring that after the paper is folded and the label is fixed, at least one end of the path is still located on the outer surface of the packaging and connected to the outside, thereby taking into account oil blocking, steam venting, and shape maintenance during the hot hamburger wrapping process. Furthermore, if the above functions can be achieved without relying on double-sided functional layers, through-hole steam venting holes, steam venting cuts, interlayer steam venting channels, or complex multi-layer structures, the manufacturing complexity of the paper base packaging structure and its coordination requirements with the folding operation can also be reduced. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for hot food hamburger wrapping, as well as its preparation and usage methods. It aims to solve the problems that existing hot food hamburger wrapping paper cannot simultaneously maintain continuous oil blocking in the main high-oil contact area, steam venting in the thickness direction of the outer paper sheet, and stable exposure of the steam venting end after folding and labeling.
[0008] This invention provides a PHA coating pattern on the food contact side of a fiber-based paper, and divides the paper-based packaging structure into a first functional area and a second functional area located around the periphery of the first functional area and extending to the paper edge. The first functional area corresponds to the main pressure-bearing area, sauce concentration area, or high-oil contact projection at the bottom of a hot hamburger. During the drying process, PHA particles merge with each other to form a continuous PHA barrier phase in the planar direction of the paper surface. The second functional area is provided with a PHA-covered area, and the exposed cellulose continuous pathway forms a continuous exposed cellulose surface between the inner starting boundary of the pathway and the corresponding paper edge.
[0009] The paper-based packaging structure has at least two folded areas defined by a predetermined wrapping pattern. At least two continuous exposed cellulose pathways in the maximum exposed cellulose connectivity region pass through different folded areas and reach different paper edges. During the wrapping process, the different folded areas are folded along corresponding predetermined folding positions to form different paper layers, such that when the edge of a component located in one folded area is covered by the corresponding paper layer or a packaging label, the edge of a component located in another folded area will not necessarily be closed simultaneously by the same paper layer.
[0010] The exposed cellulose continuous pathway and its edge end have a defined positional relationship relative to the predetermined folding overlap area and the predetermined area of the packaging fixation label. After the paper-based packaging structure is folded around the hot food hamburger and the packaging fixation label is set, at least one exposed cellulose edge end forms a visible exposed area on the outer surface of the packaging body, located outside the coverage of other paper layers and the packaging fixation label, and communicating with the outside of the packaging body.
[0011] The term "vapor exhaust" in this invention refers to the outward transmission of water vapor released from the hot hamburger through the exposed cellulose surface of the second functional area, the interconnected cellulose fiber network within the thickness of the fiber base paper, and the outer surface opposite the food contact side. It then diffuses to the outside of the packaging body through the exposed cellulose maintaining external connectivity to the corresponding area at the edge. The term "shape retention" in this invention refers to reducing oil migration and condensation, slowing down the softening, collapse, and crumb adhesion of the hamburger bun, thus maintaining good structural stability and shape integrity of the wrapped hot hamburger.
[0012] The paper-based packaging structure includes a fiber-based paper and a polyhydroxyalkanoate coating pattern disposed on the food contact side of the fiber-based paper. The food contact side includes a first functional area and a second functional area that do not overlap with each other. The first functional area is defined by a closed boundary and spaced apart from the edge of the fiber-based paper. The second functional area is located on the outer periphery of the first functional area and extends to the edge of the fiber-based paper.
[0013] The polyhydroxyalkanoate coating pattern forms a continuous polyhydroxyalkanoate barrier phase in the first functional region, and the planar projected area of the largest polyhydroxyalkanoate connected domain in the continuous polyhydroxyalkanoate barrier phase accounts for C1≥70% of the planar projected area of the first functional region. The second functional region includes a polyhydroxyalkanoate covered area and an exposed cellulose continuous phase formed from the exposed cellulose surface of the fiber base paper, and the planar projected area of the largest exposed cellulose connected domain in the exposed cellulose continuous phase accounts for C2≥30% of the planar projected area of the second functional region.
[0014] The paper-based packaging structure has at least two folded areas, a predetermined folded overlap area, and a predetermined area for fixing the packaging label, all defined by a predetermined package pattern. The at least two folded areas are located within the second functional area. The maximum exposed cellulose connectivity includes at least two continuous exposed cellulose pathways extending from the outer periphery of the first functional area to the edge of the fiber-based paper. Each of these continuous exposed cellulose pathways forms an exposed cellulose edge at its arrival edge. The at least two continuous exposed cellulose pathways pass through different folded areas and reach different edges of the fiber-based paper.
[0015] The exposed cellulose continuous pathway, the exposed cellulose to the edge end, the predetermined folding overlap area, and the predetermined packaging fixing label area have a fixed layout position relationship, such that after the paper-based packaging structure is folded according to the predetermined package pattern and a packaging fixing label is set in the predetermined packaging fixing label area, at least one of the exposed cellulose to the edge end is located on the outer surface of the formed packaging body and communicates with the outside of the packaging body.
[0016] In some embodiments, the food contact side has an effective food contact side area A. t The effective area A of the food contact side t It is composed of the first functional area and the second functional area; the planar projected area A1 of the first functional area occupies the effective area A of the food contact side. t The percentage is 15%–60%, and the dry weight per unit area (q1) of polyhydroxyalkanoate in the first functional region is 3.0–8.0 g / m². 2 The planar projected area of the polyhydroxyalkanoate-covered region within the second functional zone accounts for 15% to 60% of the planar projected area of the second functional zone, and the area-weighted average dry mass (q2) of the polyhydroxyalkanoate within the second functional zone is 0.10 to 1.75 g / m². 2 And q1>q2.
[0017] In some embodiments, the second functional area has an inner starting boundary of the passage, which is the outer boundary of the first functional area, or the outer edge of a continuous polyhydroxyalkanoate oil-blocking boundary band disposed in the inner periphery of the second functional area, connected to and surrounding the first functional area. The minimum effective width of each of the exposed cellulose continuous passages is 1.0–6.0 mm, the continuous length of the exposed cellulose to the edge end along the paper edge direction is not less than 1.0 mm, and the minimum effective width perpendicular to the paper edge direction is not less than 1.0 mm.
[0018] In some embodiments, the paper sheet region within the second functional area corresponding to the exposed cellulose continuity forms a continuous paper sheet entity, which extends continuously from the food contact side along the thickness direction of the fiber base paper to the outer surface opposite the food contact side, and includes a network of interconnected cellulose fibers.
[0019] In some embodiments, the paper-based packaging structure does not have vent holes or vent cuts penetrating the fiber-based paper, and does not have interlayer venting channels.
[0020] When performing registration, structural inspection, or folding state restoration on the finished product layout, if the finished product has positioning marks, the predetermined fold line, predetermined fold overlap area, and predetermined area for packaging label fixing can be determined using the positioning marks; if the finished product does not have positioning marks, translation, rotation, and proportional registration can be performed with the geometric center of the finished product as the origin, through the actual paper edge of the finished product, the boundary of the first functional area, and the polyhydroxyalkanoate coating pattern. The positioning and registration methods are used to restore and detect the positional relationship of the layout, and are not considered as necessary physical components for forming the first functional area, the second functional area, and the continuous exposed cellulose pathway.
[0021] When quantitatively detecting the external connectivity after folding, if the visible exposed area formed by the exposed cellulose to the edge end on the outer surface of the packaging has a continuous visible length along the paper edge direction of not less than 1.0 mm and an exposed width perpendicular to the paper edge direction of not less than 1.0 mm, and is located outside the coverage of other paper layers and packaging fixing labels, it is determined that the exposed cellulose to the edge end meets the corresponding size and exposure position conditions.
[0022] As a mass distribution parameter, the spatial concentration factor K of the PHA coating pattern is determined according to K=q1 / q t Calculate, where q1 is the dry mass of PHA per unit area in the first functional region, q t The effective area A of the food contact side t The average dry mass per unit area of the internal PHA. In some embodiments, K ≥ 1.20. K is used to characterize the degree to which PHA is concentrated in the first functional region, and is not used as a condition for determining the validity of the structure of the invention independently of C1, C2 and the pathway topology. The first functional region is used to block the release of oil and sauce from hot hamburgers, and the second functional region is used to allow water vapor to pass outward through the thickness of the fiber base paper via the exposed cellulose continuous phase.
[0023] In some implementations, the planar projected area A1 of the first functional area occupies an area A of the effective food contact side. t The proportion ranges from 15% to 60%, and can be 15%, 20%, 25%, 30%, 36%, 40%, 45%, 50%, 55%, or 60%. The effective area A between the geometric center of the first functional area and the food contact side... t The distance between the geometric centers can be considered as the effective area A of the food contact side. t 0%, 2%, 5%, 8%, 10%, 12%, 15%, 18%, or 20% of the length of the shorter side of the minimum circumscribed rectangle; in some embodiments, the effective area A of the geometric center of the first functional area and the food contact side. t The geometric centers coincide. The second functional area is located on the outer periphery of the first functional area and extends from the outer boundary of the first functional area to the edge of the fiber-based paper.
[0024] The PHA film coverage F1 of the first functional region can be 85%, 88%, 90%, 92%, 94%, 95%, 96%, 97%, 98%, 99%, or 100%; the proportion of the largest connected domain within the PHA phase R1 can be 80%, 82%, 85%, 88%, 90%, 92%, 95%, 97%, 98%, 99%, or 100%. The area proportion of the largest PHA connected domain in the first functional region C1 is determined by both F1 and R1, and is ≥70%; in some embodiments, it is 80% to 100%. When the first functional region uses a solid plate, a high-coverage micro-dot plate, or an application unit that can merge with each other after drying, the PHA particles merge with each other to form a specified continuous PHA barrier phase for receiving oils, cheese, and sauces.
[0025] The planar projection area coverage of the second functional area, PHA coverage, can be 15%, 18%, 20%, 25%, 30%, 34%, 40%, 45%, 50%, 55%, 58%, or 60%. The sum of the planar projection area coverage of the PHA coverage area and the exposed cellulose surface is 100%.
[0026] When the planar projected area coverage of the second functional region PHA is 15%–60%, the cellulose exposure rate E2 of the second functional region is 40%–85%, and can be 40%, 42%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or 85%. For control structures used for boundary comparison that do not meet the above coverage conditions, their E2 can be outside this range. The maximum connected domain ratio R2 within the exposed cellulose phase can be 60%, 65%, 70%, 75%, 80%, 85%, 90%, 92%, 95%, 96%, 98%, or 100%. The maximum exposed cellulose connected domain area ratio C2 of the second functional region is determined by both E2 and R2, and is ≥30%; in some embodiments, it is 40%–85%.
[0027] The predetermined fold line coordinates can define two, three, or four fold regions within the second functional area. In the implementation with four fold regions, the four fold regions correspond to the top, right, bottom, and left edges of the fiber-based paper, respectively; in the implementation with two fold regions, the two fold regions can correspond to adjacent edges, opposite edges, or other combinations of different edges, respectively.
[0028] The second functional area is set with a PHA coverage area, and each continuous exposed cellulose passage forms a continuous exposed cellulose surface between the inner starting boundary of the passage and the corresponding paper edge; the PHA coverage area is used to control the spatial distribution of PHA in the outer area while maintaining the continuous exposed paper surface.
[0029] In some embodiments, the minimum effective width of each exposed cellulose continuous pathway is 1.0–6.0 mm, and can be 1.0 mm, 1.5 mm, 2.0 mm, 3.0 mm, 4.0 mm, 5.0 mm, or 6.0 mm. 0.20 mm, 0.50 mm, 8.0 mm, 10.0 mm, 12.0 mm, and 15.0 mm are used for boundary controls.
[0030] The continuous length of exposed cellulose along the paper edge direction to the edge end can be 1.0mm, 2.0mm, 3.0mm, 4.0mm, 5.0mm, 6.0mm, 8.0mm, 10.0mm, 12.0mm, 15.0mm, or 20.0mm; the minimum effective width perpendicular to the paper edge direction can be 1.0mm, 1.5mm, 2.0mm, 3.0mm, 4.0mm, 5.0mm, or 6.0mm.
[0031] In the four-way redundancy implementation, four continuous exposed cellulose pathways are provided, each extending along two intersecting directions to one of four different paper edges, and these four pathways pass through four different folding regions. When one or more edges are obscured by folding or labeling, the edges located in other folding regions and other paper edges still constitute the visible area on the outer surface of the packaging, thus forming multi-directional folding tolerance.
[0032] In some implementations, the dry mass q1 of PHA per unit area within the first functional region is 3.0–8.0 g / m². 2 It can be 3.0g / m 2 4.0g / m 2 4.5g / m 2 4.8g / m 2 5.0g / m 2 5.5g / m 2 6.0g / m 2 6.5g / m 2 7.0g / m 2 7.5g / m 2 Or 8.0g / m 2 .
[0033] In some implementations, the area-weighted average dry mass per unit area (q2) of PHA within the second functional zone is 0.10–1.75 g / m². 2 It can be 0.10g / m 2 0.15g / m 2 0.20g / m 2 0.25g / m 2 0.30g / m 2 0.35g / m 2 0.40g / m2 0.50g / m 2 0.60g / m 2 0.70g / m 2 0.80g / m 2 1.00g / m 2 1.25g / m 2 1.50g / m 2 Or 1.75g / m 2 .
[0034] Effective area A of food contact side t The average dry mass per unit area of internal PHA, q t According to q t =fq1+(1-f)q2, where f is the area of the first functional area's planar projection relative to the effective area A on the food contact side. t The proportion.
[0035] The spatial concentration factor K is calculated according to K=q1 / q t Calculation. In some implementations, K ≥ 1.20, and can be 1.20, 1.25, 1.50, 2.00, 2.26, 2.46, 2.55, 2.59, 3.00, 3.70, 4.00, 5.00, 5.50, or 6.00.
[0036] When the continuous PHA oil-blocking boundary zone is set within the second functional area, its area and PHA mass are both included in the second functional area. q2 is the area-weighted average dry mass of PHA per unit area, including the continuous PHA oil-blocking boundary zone, the ordinary pattern area of the second functional area, and the exposed cellulose continuous pathway area.
[0037] Area of the first functional area, q1, q2, q t Together with K, they constitute the spatial distribution relationship of PHA material. K is used to distinguish between concentrated distribution of PHA to the first functional area and uniform distribution across the entire width, but K does not deviate from the continuity of PHA in the first functional area, the continuity of exposed cellulose in the second functional area, the different folding areas, and the multi-paper edge pathway relationship to produce technical effects independently.
[0038] The inner periphery of the second functional area near the first functional area can be provided with a continuous PHA oil-blocking boundary band that is connected to and surrounds the first functional area. The area of the continuous PHA oil-blocking boundary band is included in the second functional area and constitutes part of the PHA coverage area within the second functional area. The width of the continuous PHA oil-blocking boundary band can be 0.5mm, 1.0mm, 2.0mm, 3.0mm, 4.0mm, 5.0mm, 6.0mm, 8.0mm, 10.0mm, 12.0mm, or 15.0mm.
[0039] The inner starting boundary of the passage is the outer boundary of the first functional area, or the outer edge of the continuous PHA oil-blocking boundary band. When the continuous PHA oil-blocking boundary band is set, each exposed cellulose continuous passage extends continuously from the outer edge of the continuous PHA oil-blocking boundary band to the corresponding paper edge, passing through different folding areas and reaching different paper edges; the continuous PHA oil-blocking boundary band is located outside the planar projection range of the exposed cellulose continuous passage.
[0040] The film-forming polymer component forming the continuous PHA barrier phase and the PHA-covered region within the second functional area includes one or more PHAs, and the film-forming polymer component may further include a polymeric stabilizing component. In some embodiments, the proportion of PHA to the total mass of the film-forming polymer component is not less than 90%, and the proportion may be 90%, 92%, 95%, 96%, 96.8%, 97.0%, 97.1%, 97.4%, 98%, 99%, or 100%. In BIOTEN 1030, BIOTEN 1031, BIOTEN 1032, and BIOTEN 1033, the proportion of PHA to the total mass of the film-forming polymer component is 96.8% to 97.4%. The PHA is selected from one or more of poly(3-hydroxybutyrate) (PHB), poly(3-hydroxybutyrate-3-hydroxyvalerate) copolyester (PHBV), poly(3-hydroxybutyrate-4-hydroxybutyrate) copolyester (P34HB), and poly(3-hydroxybutyrate-3-hydroxyhexanoate) copolyester (PHBH). Different PHAs adjust the drying process according to the comonomer content, melting peak temperature, molecular weight and particle aggregation behavior, but the continuous barrier phase of PHA in the first functional zone, the exposed continuous cellulose phase in the second functional zone, the folded area and the determination method of the edge end are consistent.
[0041] This invention uses water-based coatings containing PHA particles for patterned coating. The mass fraction of PHA in the water-based coating can be 18%, 19%, 20%, 21%, or 22% based on the total mass of the water-based coating. The coating coverage of the first functional area can be 85%, 88%, 90%, 92%, 95%, 97%, 98%, 99%, or 100%. The coverage of the PHA-covered area in the second functional area can be 15%, 18%, 20%, 25%, 30%, 34%, 35%, 40%, 45%, 50%, 55%, 58%, or 60%.
[0042] The same patterned coating plate includes a high-coverage pattern for a first functional area, a PHA-covered pattern for a second functional area, and at least two continuous uncoated line patterns; when a continuous PHA oil-blocking boundary band is set, it also includes a continuous wet-coated oil-blocking band pattern. The at least two continuous uncoated line patterns correspond to folded areas defined by different predetermined folding line coordinates and different predetermined cutting line coordinates, respectively.
[0043] The coating speed is 5–500 m / min, and the drying medium temperature of the continuous drying system is set to 60–190 °C. The highest value among the main melting peak temperatures of each PHA contained in the water-based coating, measured by differential scanning calorimetry during the second heating phase, is recorded as the highest main melting peak temperature T. m,max Before the patterned wet-coated fiber-based paper enters the final high-energy drying zone where PHA particles soften and coalesce, the residual moisture content should not exceed 5% of the initial coating moisture content; the percentage of residual moisture to initial coating moisture content can be 0.5%, 1.0%, 2.0%, 3.0%, 4.0%, or 5.0%. The peak temperature of the paper surface on the food contact side should be higher than the highest main melting peak temperature T. m,max The paper surface peak temperature is 5–13°C higher than the highest main melting peak temperature T. m,max The temperature difference can be 5℃, 6℃, 7℃, 8℃, 9℃, 10℃, 11℃, 12℃, or 13℃. This ensures that the temperature of the paper surface on the food contact side is continuously not lower than the highest main melting peak temperature T. m,max The coating time is 1.0–3.0 s, which can be 1.0 s, 1.5 s, 2.0 s, 2.5 s, or 3.0 s. The specific coating speed, drying medium setting temperature, paper surface peak temperature, and high-temperature holding time depend on the basis weight of the base paper, the type of PHA, and the highest main melting peak temperature T. m,max The dry mass per unit area of the regional PHA and the paper web running speed were determined.
[0044] During preparation, according to a predetermined packaging pattern, a first functional area, a second functional area located on the outer periphery of the first functional area and extending to a predetermined cutting line, at least two folded areas located within the second functional area, a predetermined folded overlap area, and a predetermined area for fixing the packaging label are determined on the food contact side of the fiber-based paper. At least two continuous uncoated lines are also determined, each passing through a different folded area and extending to a different predetermined cutting line. The continuous uncoated lines, the predetermined folded overlap area, and the predetermined area for fixing the packaging label have a fixed positional relationship, such that after cutting along the predetermined cutting line, at least two of the continuous uncoated lines form continuous exposed cellulose pathways reaching different paper edges. After folding the resulting paper-based packaging structure and setting the packaging label, at least one exposed cellulose edge end formed by the continuous exposed cellulose pathway at the corresponding paper edge is located on the outer surface of the formed packaging and communicates with the outside.
[0045] A water-based coating containing PHA particles is patterned and applied to a portion of the first and second functional areas, while retaining the continuous uncoated lines, to obtain patterned wet-coated fiber-based paper.
[0046] The patterned wet-coated fiber base paper is dried so that the PHA particles in the first functional area merge to form a continuous PHA barrier phase with C1≥70%, and the second functional area forms a PHA covered area and an exposed cellulose continuous phase formed by the exposed cellulose surface corresponding to the continuous uncoated lines with C2≥30%, thus obtaining the patterned dried fiber base paper.
[0047] The patterned dry fiber base paper is cut along the predetermined cutting line, so that at least two of the continuous uncoated lines form continuous exposed cellulose pathways that pass through different folded areas and reach different paper edges, and the exposed cellulose is formed at the edge ends of the corresponding paper edges.
[0048] In some embodiments, the amount of water-based coating applied and the coverage of the coating pattern are controlled so that the dry mass q1 of PHA per unit area in the first functional area after drying is 3.0–8.0 g / m². 2 The planar projection area of the PHA-covered area in the dried second functional zone is 15% to 60% of the planar projection area of the second functional zone, and the area-weighted average dry mass q2 of PHA within the dried second functional zone is 0.10 to 1.75 g / m². 2 And q1>q2.
[0049] In some embodiments, the lateral leveling of the wet coating is controlled so that the continuous uncoated line remains continuous between the outer boundary of the first functional area or the outer edge of the continuous PHA oil barrier boundary band and the corresponding predetermined cutting line, and the paper area corresponding to the continuous uncoated line extends continuously from the food contact side along the thickness direction of the fiber base paper to the outer surface.
[0050] The patterned coating is applied using flexographic coating, direct gravure coating, rotary screen coating, silkscreen coating, or digital coating.
[0051] The present invention also provides a method of using the paper-based packaging structure, the method comprising the following steps: folding the paper-based packaging structure with the food contact side facing the hot hamburger, folding the paper-based packaging structure around the hot hamburger according to the predetermined packaging pattern; setting a packaging fixing label in the predetermined area of the packaging fixing label, such that at least one of the exposed cellulose edges is located on the outer surface of the formed hot hamburger packaging and communicates with the outside of the hot hamburger packaging.
[0052] In some embodiments, the hot hamburger forms a hot hamburger orthographic projection on the food contact side, and the overlap area between the hot hamburger orthographic projection and the first functional area accounts for 92% to 100% of the area of the hot hamburger orthographic projection, and at least a portion of the second functional area is located on the outer periphery of the hot hamburger orthographic projection.
[0053] In some embodiments, the surface temperature of the center of the bottom of the hot hamburger when it initially contacts the paper-based packaging structure is 65–90°C. This temperature range is used to illustrate the verification conditions for a 65°C single-layer beef hamburger, a 70°C double-layer cheeseburger, and a 90°C fried chicken hamburger, and does not constitute the only applicable temperature range for the paper-based packaging structure.
[0054] In use, the food contact side of the paper-based packaging structure faces the hot hamburger, so that the main high-oil contact projection of the bottom of the hot hamburger falls into the first functional area, and at least a part of the second functional area is located on the outer periphery of the hot hamburger's frontal projection; fold different folding areas according to the folding sequence determined by the predetermined package pattern, and set the packaging fixing label in the predetermined area of the packaging fixing label.
[0055] In some embodiments, after folding and labeling, at least one exposed cellulose end forms a visible exposed area on the outer surface of the package outside the coverage of other paper layers and the package fixing label. The visible exposed area has a continuous visible length of not less than 1.0 mm along the paper edge direction, an exposed width of not less than 1.0 mm perpendicular to the paper edge direction, and communicates with the outside of the package.
[0056] The water vapor released from the hot hamburger is transferred outward through the exposed cellulose surface of the second functional area, the interconnected cellulose fiber network within the thickness of the fiber base paper, and the outer surface opposite the food contact side.
[0057] In the four-way redundancy implementation, the paper-based packaging structure has four folded areas corresponding to four different paper edges, and four continuous exposed cellulose pathways passing through the four folded areas and reaching the four different paper edges. When the folded paper layer or packaging fixing label obscures one or more of the edge ends, the edge ends in other directions can still constitute the visible area of the outer surface of the packaging and maintain external communication.
[0058] The long, narrow stuffed foods and the rectangular stuffed foods are used to illustrate the adaptability of the partitioned structure to different food shapes.
[0059] Compared with the prior art, the use of this invention can achieve the following significant beneficial effects:
[0060] The PHA continuous barrier phase in the first functional area and the exposed cellulose continuous phase in the second functional area form a spatial division of labor on the same food contact side, so that the main high oil contact projection of hot hamburgers can be continuously protected against oil, and water vapor located on its periphery can be transferred outward through the cellulose fiber network that is interconnected within the exposed cellulose surface and the thickness of the fiber base paper, thereby reducing oil penetration through the back of the paper, condensation, soft bread, and crumb adhesion.
[0061] The pre-designed package layout defines at least two folding areas within the second functional area, with at least two continuous exposed cellulose pathways passing through different folding areas and reaching different paper edges. The continuous exposed cellulose pathways, the exposed cellulose edge ends, the pre-defined folding overlap areas, and the pre-defined packaging labeling area have defined positional relationships. After folding and labeling, at least one of the exposed cellulose edge ends can be located outside other paper layers and the packaging labeling and connected to the outside, reducing the risk of simultaneously closing all exposed cellulose edge ends in the same fold or packaging labeling.
[0062] The proportion of the maximum PHA connected domain area in the first functional area (C1), the proportion of the maximum exposed cellulose connected domain area in the second functional area (C2), the spatial concentration coefficient (K), the minimum effective width of the pathway, the folded area traversed by the pathway, the paper edge reached, and the dimensions to the edge end can be detected through regional sampling, chemical imaging, image connectivity analysis, and folded state imaging.
[0063] The high-coverage pattern in the first functional area, the PHA-covered pattern in the second functional area, the continuous uncoated lines, and the continuous PHA oil-blocking boundary band during setup can be formed in one step using the same water-based coating, the same patterned coating plate, and the same coating unit, and the PHA particles can be agglomerated through continuous drying. In embodiments without double-sided functional layers, vent holes or vent cuts penetrating the fiber base paper, and interlayer venting channels, water vapor can be directly transferred using the exposed cellulose surface of the second functional area and the interconnected cellulose fiber network inside the fiber base paper.
[0064] PHA is concentrated in the first functional zone where continuous oil blocking is required, while the second functional zone retains the exposed cellulose continuous phase and has a PHA pattern with a lower coverage, thereby reducing the average amount of PHA used on the food contact side while maintaining oil blocking, vapor venting and folding tolerance. Attached Figure Description
[0065] Figure 1 This is a schematic diagram of the mechanism of a partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure used for wrapping hot hamburgers.
[0066] In the figure, 1-first functional region; 2-polyhydroxyalkanoate continuous barrier phase; 3-second functional region; 4-exposed cellulose continuous phase; 5-exposed cellulose continuous pathway; 6-water vapor thickness transfer region; 7-exposed cellulose to the edge end; 8-water vapor escaping outward. Detailed Implementation
[0067] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention. Unless otherwise stated, the raw materials used in this embodiment are commercially available industrial products or can be prepared by conventional methods. Unless otherwise specified, performance testing methods are performed according to the "Main Test Standards" and corresponding test methods in this specific embodiment.
[0068] like Figure 1 As shown, a hot hamburger is placed above the first functional area 1. The first functional area 1 contains a continuous polyhydroxyalkanoate barrier phase 2 to collect grease and sauce from the bottom of the hamburger and reduce their migration to the back of the paper. A second functional area 3 is located around the outer periphery of the first functional area 1. The second functional area 3 retains an exposed cellulose continuous phase 4 and forms multiple exposed cellulose continuous pathways 5 extending towards different paper edges. Water vapor released from the hot hamburger enters the paper interior through the exposed cellulose continuous phase 4, passes through the interconnected cellulose fiber network in the water vapor thickness transfer area 6, and is transferred outwards. After the exposed cellulose continuous pathways 5 reach the paper edge, they form exposed cellulose edge-to-edge 7. After the paper-based packaging structure is folded and fixed, at least one exposed cellulose edge-to-edge 7 is located outside the coverage area of other paper layers and the packaging label, forming a visible exposed area communicating with the outside of the packaging, allowing the escaping water vapor 8 to continue to transfer to the outside of the packaging.
[0069] Unless otherwise stated, percentages relating to the composition of raw materials, coatings, and food products represent mass fractions; percentages relating to the proportion of planar projected area, coverage, connected component proportion, overlap rate, success rate, failure rate, and integrity rate represent the corresponding area or quantity proportions. q1, q2, q t The dry weight per unit area of all other PHAs is calculated based on the oven-dry PHA weight, excluding polymer-type stabilizing components; the dry weight per unit area of total non-volatile matter includes PHAs, polymer-type stabilizing components, and other non-volatile substances in water-based coatings. Samples were conditioned for 24 hours at 23±1℃ and 50±2% relative humidity (RH) before structural and performance tests were conducted.
[0070] The total nonvolatile matter content of PHA aqueous dispersions was determined according to International Organization for Standardization (ISO) 3251:2019. 1.000 ± 0.010 g of sample was weighed and placed in a pre-weighed aluminum weighing dish. The sample was dried in a UF55 forced-air drying oven at 105 ± 2 °C for 60 min, then cooled in a desiccator for 30 min before weighing. This drying process was repeated for 30 min each time until the difference between two consecutive weighings was ≤ 0.5 mg. Each sample was measured in triplicate, and the average value was taken.
[0071] The PHA mass fraction in the PHA aqueous dispersion was determined using the methanololysis-gas chromatography-flame ionization detector (GC-FID) method specified in this instruction manual. The difference between the total non-volatile matter content and the PHA mass fraction was recorded as the non-PHA non-volatile matter mass fraction. The mass fraction of the polymeric stable component was determined based on the oven-dry feed mass during the preparation of the aqueous dispersion and verified using a detection or mass balance method capable of distinguishing between the polymeric stable component and other non-PHA non-volatile matter. The proportion of PHA to the total mass of the film-forming polymer component was calculated using the following formula:
[0072] PHA ratio = PHA mass fraction / (PHA mass fraction + polymeric stabilizing component mass fraction + other film-forming polymer mass fraction) × 100%.
[0073] The aqueous dispersion used in this embodiment does not contain any film-forming polymers other than PHA and the polymeric stabilizing component; therefore, the mass fraction of other film-forming polymers is 0.
[0074] The PHA ratio in each batch should not be less than 90%; the batch control range for BIOTEN 1030, BIOTEN 1031, BIOTEN 1032 and BIOTEN1033 is 96.8% to 97.4%.
[0075] The pH of the PHA aqueous dispersion was determined according to ISO 976:2013. A benchtop pH meter with a composite glass electrode and three-point calibration was used for calibration at 25.0 ± 0.5 °C using standard buffer solutions with pH values of 4.01, 7.00, and 10.01. The electrode was immersed in the sample, and the result was recorded when the reading changed by ≤0.02 within 30 seconds. Each sample was measured in triplicate, and the average value was taken.
[0076] The cumulative distribution particle size D of PHA aqueous dispersion 90 PHA was determined using a Zetasizer Ultra particle size and Zeta potential analyzer according to ISO 22412:2025. Based on the measured PHA mass fraction obtained by gas chromatography-flame ionization detector (GC-FID), the sample was diluted to a PHA mass fraction of 0.050 ± 0.005% using deionized water filtered through a 0.22 μm membrane. After equilibration at 25.0 ± 0.1 °C for 2 min, dynamic light scattering (DLS) was performed in 173° backscatter mode. The cumulative 90% particle size of the intensity-weighted particle size distribution was used as the Dsize. 90 Each sample was measured in triplicate and the average value was taken.
[0077] The apparent viscosity of the coating was measured using a DV2Plus rotational viscometer with an ultra-low viscosity adapter (ULA) rotor. The sample volume was 16.0 mL, the measurement temperature was 25.0 ± 0.1 ℃, the rotation speed was 30 rpm, and the rotor was started after 10 min of constant temperature and the reading was taken at 60 s. The measuring torque was maintained at 10% to 90% of the instrument's full scale. Each sample was measured in parallel three times and the average value was taken.
[0078] The density of the coating was determined according to ISO 2811-1:2023 using a BYK-Gardner 1140 50mL certified ISO density cup at 25.0±0.1℃. Before measurement, both the density cup and the coating were kept at a constant temperature for 30 minutes, and the mass of the empty cup was recorded. The cup was then filled with coating and capped, allowing excess coating to drain through the overflow hole. The outer surface was wiped clean before weighing. Each sample was measured in triplicate, and the average value was taken.
[0079] Main raw materials, standardized samples and auxiliary materials.
[0080] Table 1. Main raw materials, standardized samples and auxiliary materials.
[0081]
[0082] BIOTEN 1030 is an aqueous dispersion of PHB, with a total non-volatile content of 40±1%, of which PHB mass fraction is 38.8±1.0% and polymeric stabilizing component mass fraction is 1.2±0.2%; pH is 7.5±0.5, and cumulative distribution particle size D... 90 The apparent viscosity at 25℃ is 200–500 mPa·s, ≤300 nm. The molar fraction of 3-hydroxybutyric acid structural units in the PHB is 100%. The main melting peak temperature during the second heating phase, measured by differential scanning calorimetry, is 174 ± 2℃, and the apparent number-average molecular weight M0 is [missing value]. n It is (2.4±0.2)×10 5 g / mol, apparent weight-average molecular weight M w It is (5.2±0.4)×10 5 g / mol, with a dispersion coefficient of 2.17 ± 0.15.
[0083] BIOTEN 1031 is an aqueous dispersion of PHBV, with a total non-volatile content of 40±1%, of which the mass fraction of PHBV is 38.8±1.0% and the mass fraction of polymeric stabilizing components is 1.2±0.2%; the pH is 7.5±0.5, and the cumulative distribution particle size D is... 90The apparent viscosity at 25℃ is 300–700 mPa·s, ≤300 nm. The molar fraction of 3-hydroxyvalerate structural units in the PHBV is 14.0 ± 0.8%, with the remainder being 3-hydroxybutyrate structural units. The main melting peak temperature during the second heating, determined by differential scanning calorimetry, is 150 ± 3℃, and the apparent number-average molecular weight M0 is [not specified]. n It is (2.2±0.2)×10 5 g / mol, apparent weight-average molecular weight M w It is (4.8±0.4)×10 5 g / mol, with a dispersion coefficient of 2.18 ± 0.15.
[0084] BIOTEN 1032 is an aqueous dispersion of P34HB with a total non-volatile content of 40±1%, of which P34HB mass fraction is 38.8±1.0% and polymeric stabilizing component mass fraction is 1.2±0.2%; pH is 7.5±0.5, and cumulative distribution particle size D... 90 The apparent viscosity at 25℃ is 250–650 mPa·s, ≤300 nm. The molar fraction of 4-hydroxybutyric acid structural units in P34HB is 16.0 ± 0.8%, with the remainder being 3-hydroxybutyric acid structural units. The main melting peak temperature during the second heating, determined by differential scanning calorimetry, is 148 ± 3℃, and the apparent number-average molecular weight M0 is [not specified]. n It is (1.8±0.2)×10 5 g / mol, apparent weight-average molecular weight M w It is (3.9±0.4)×10 5 g / mol, with a dispersion coefficient of 2.17 ± 0.18.
[0085] BIOTEN 1033 is an aqueous dispersion of PHBH, with a total non-volatile content of 40±1%, of which the mass fraction of PHBH is 38.8±1.0% and the mass fraction of polymeric stabilizing components is 1.2±0.2%; the pH is 7.5±0.5, and the cumulative distribution particle size D is... 90 The apparent viscosity at 25℃ is 200–600 mPa·s, ≤300 nm. The molar fraction of 3-hydroxyhexanoic acid structural units in the PHBH is 10.0 ± 0.5%, with the remainder being 3-hydroxybutyric acid structural units. The main melting peak temperature during the second heating, measured by differential scanning calorimetry, is 127 ± 3℃, and the apparent number-average molecular weight M0 is [not specified]. n It is (2.1±0.2)×10 5 g / mol, apparent weight-average molecular weight M w It is (4.5±0.4)×10 5 g / mol, with a dispersion coefficient of 2.14 ± 0.16.
[0086] BIOTEN 1030, BIOTEN 1031, BIOTEN 1032, and BIOTEN 1033 all use polyvinyl alcohol (PVA)-based polymer stabilizers. With 100 parts by weight of PHA dry solids, the polymer stabilizer comprises 3.0 ± 0.3 parts by weight. With the total mass of PHA and the polymer stabilizer comprising 100%, the batch-controlled proportion of PHA is 96.8%–97.4%. These four aqueous dispersions do not contain other film-forming polymers.
[0087] The molar content of PHA comonomers was determined by proton nuclear magnetic resonance spectroscopy. Following the centrifugation and washing procedures used in preparing the methanolysis calibration PHA solid according to this instruction manual, PHA particles were separated from the corresponding aqueous dispersion. After washing three times with deionized water, the particles were vacuum dried to constant weight at 60±2℃ and an absolute pressure ≤20 kPa. 20.0±1.0 mg of dried PHA was weighed, added to 0.70 mL of deuterated chloroform, dissolved at 50±2℃, and cooled to 25±1℃ before analysis.
[0088] The proton resonance frequency of the hydrogen nuclear magnetic resonance spectrometer was 400 MHz, the test temperature was 25 ± 1 °C, the spectral width was -1 to 12 ppm, the number of acquisitions was 64, the relaxation delay was 10 s, and tetramethylsilane was used as the chemical shift reference. The molar content of the 3-hydroxyvalerate structural unit in PHBV was calculated based on the integrated area of the terminal methyl peak of 3-hydroxyvalerate in the range of 0.85–0.95 ppm and the methyl peak of 3-hydroxybutyrate in the range of 1.20–1.35 ppm; the molar content of the 4-hydroxybutyrate structural unit in P34HB was calculated based on the integrated area of the oxygen-linked methylene peak of 4-hydroxybutyrate in the range of 4.05–4.15 ppm and the methylene peak of 3-hydroxybutyrate in the range of 5.15–5.30 ppm; the molar content of the 3-hydroxyhexanoate structural unit in PHBH was calculated based on the integrated area of the terminal methyl peak of 3-hydroxyhexanoate in the range of 0.85–0.95 ppm and the methyl peak of 3-hydroxybutyrate in the range of 1.20–1.35 ppm. Each integral area was corrected according to the number of hydrogen atoms represented by the corresponding characteristic peak. Each sample was measured in triplicate, and the average value was taken.
[0089] The melting peak temperature of PHA was determined according to ISO 11357-3:2025. 5.0–8.0 mg of vacuum-dried PHA solid was weighed and placed in a sealed aluminum crucible, using an empty aluminum crucible as a reference. The nitrogen flow rate was 50 ± 5 mL / min. The sample was first heated from -50℃ to 200℃ at a rate of 10℃ / min and held for 3 min, then cooled to -50℃ at a rate of 10℃ / min and held for 3 min, followed by a second heating to 200℃ at a rate of 10℃ / min. The peak temperature of the endothermic melting peak in the second heating curve was taken as the main melting peak temperature; when multiple endothermic melting peaks existed, all peak temperatures were recorded, and the endothermic melting peak with the largest peak area was taken as the main melting peak.
[0090] Apparent number-average molecular weight M of PHA n Apparent weight-average molecular weight M w The dispersion coefficient was determined by gel permeation chromatography according to ISO 16014-1:2019 and ISO 16014-3:2019. Vacuum-dried PHA solid was added at 3.0 mg / mL to chromatographically pure chloroform, and dissolved by shaking at 25±2℃ for 12 h. The solution was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) membrane. Two PLgel 5 μm MIXED-C columns were used in series at a column temperature of 35±1℃, a chloroform flow rate of 1.0 mL / min, and an injection volume of 100 μL. Detection was performed using a differential refractive index detector, and a calibration curve was established using narrow-distribution polystyrene standards. The obtained M... n and M w The dispersion factor is relative to the apparent molecular weight of polystyrene standards, and is calculated according to M. w / M n calculate.
[0091] The amount of polymeric stabilizing component added is calculated based on the oven-dry mass of the aqueous dispersion during preparation. When the aqueous dispersion contains no other non-volatile substances besides PHA and the polymeric stabilizing component, the difference between the total non-volatile content and the PHA mass fraction measured by GC-FID is used for verification. If other non-PHA non-volatile substances are present, the mass fraction of these non-PHA non-volatile substances is subtracted from the difference before verification. The difference between the calculated value and the verified value should not exceed 0.3 percentage points.
[0092] Before use, calculate the amount of aqueous dispersion and deionized water to be added based on the measured PHA mass fraction in the aqueous dispersion. Dilute the corresponding aqueous dispersion to the PHA mass fraction specified in each embodiment, stir for 15 minutes at 400±20 rpm, and filter through a 100μm filter before sending it to the coating unit. The required mass of aqueous dispersion is calculated by dividing the product of the total mass of the target coating and the target PHA mass fraction by the measured PHA mass fraction in the aqueous dispersion.
[0093] Standardized food samples are prepared under the following conditions, and the same batch of samples is used for the same round of comparison.
[0094] M-65 mayonnaise is composed of 8% pasteurized egg yolks, 22% deionized water, 4% vinegar, 1% salt, and 65% soybean oil. First, mix the egg yolks, deionized water, vinegar, and salt. Then, add the soybean oil while stirring at 800 rpm and continue emulsifying for 5 minutes. Store at 4°C and restore to 23±1°C before use.
[0095] HB-98, HB-105, and HB-110 were prepared using the same batch of hamburger bun dough, shaped in round molds with inner diameters of 98mm, 105mm, and 110mm, respectively, baked at 190±3℃ for 12 minutes, and cooled for 2 hours. The total weights of the three types of bread were 75±2g, 80±3g, and 85±3g, respectively, with a moisture content of 33±2% for all three.
[0096] SB-160 is made from the same batch of sandwich bread dough, shaped in a 160mm×100mm rectangular mold, baked at 190±3℃ for 18min and cooled for 2h, and horizontally cut into upper and lower slices. The total weight is 70±2g, the moisture content is 36±2%, and the combined projected size is 160mm×100mm.
[0097] WP-180 is prepared using the same batch of tortilla dough, rolled to a thickness of 4.0±0.5mm, cut into 180mm×70mm pieces, and baked on a hot plate at 220±5℃ for 45 seconds on each side. The resulting tortilla dough weighs 70±2g and has a moisture content of 34±2%.
[0098] C-20, C-22, and C-30 were prepared from the same batch of processed cheddar cheese. The processed cheddar cheese contained 45±2% water, 25±2% fat, and 18±2% protein; the masses of the three samples were 20.0±0.5g, 22.0±0.5g, and 30.0±1.0g, respectively.
[0099] BP-100 and BP-90 were prepared using ground beef from the same batch with a fat content of 20±1%. The raw weights were 105±2g and 95±2g, respectively. After cooking according to the general conditions for food packaging testing, the cooked weights were 100±2g and 90±2g, respectively.
[0100] CP-140 and CS-120 were prepared using the same batch of skinless chicken and fried according to the general conditions for food packaging testing, resulting in an oil absorption rate of 10±1% after cooking, with cooked weights of 140±3g and 120±3g, respectively. GC-80 was prepared using the same batch of skinless chicken breast, and a sample weighing 80±2g was selected after cooking according to the general conditions for food packaging testing.
[0101] V-40 is prepared by mixing lettuce and cabbage from the same batch at a mass ratio of 1:1. Lettuce and cabbage are washed separately, drained of surface water, and shredded. 20±1g of each is weighed, and the total mass after mixing is 40±2g.
[0102] The packaging label is a round pressure-sensitive label with a diameter of 35mm, and the basis weight is 80g / m³. 2 The label consists of a kraft paper face, a water-based acrylic pressure-sensitive adhesive layer, and a silicone release paper. It is used after conditioning for 24 hours at 23±1℃ and RH 50±2%. When labeling, remove the release paper and apply the pressure-sensitive adhesive layer to the folded, overlapping area on the outside of the packaging corresponding to the predetermined area coordinates of the label fixing area, pressing with a normal force of 20±2N for 2 seconds. The label fixing area does not come into direct contact with the food.
[0103] In the same round of application examples, the food components and packaging labels used were taken from the same formulation, preparation or die-cutting batch.
[0104] Main preparation and analysis / testing equipment.
[0105] Table 2. Main preparation and analysis equipment.
[0106]
[0107] The laboratory rotary screen coating uses the VCML Lab / Pilot Coater rotary screen coating module, while the industrial direct gravure coating uses the EXPERTCOAT 1000 direct gravure coating unit. Both sets of equipment use their respective matching continuous drying systems.
[0108] The VCML Lab / Pilot Coater is equipped with an unwinding mechanism, a base paper support and traction mechanism, a tension control mechanism, a replaceable rotary screen coating module, a polyurethane doctor blade, a feed trough, a circulation pump, feed and return pipelines, a gap adjustment mechanism, a hot air drying module, a short-wave infrared drying module, a cooling roller, and a winding mechanism. The effective coating width used in this embodiment is ≤300mm. Before use, ensure the rotary screen axis is parallel to the transverse direction of the base paper, that the base paper passes straight through the rotary screen coating position, and that the feed trough, circulation pump, coating area, and return pipeline form a closed-loop circulation. Set the rotary screen, doctor blade, gap, and circulation flow rate according to step 2 below. Calibrate the actual wet transfer coefficient to 0.85±0.03 based on the wet mass difference before and after coating, and verify it using the pattern size, q1, q2, and the continuity of the exposed cellulose continuous pathway.
[0109] The EXPERTCOAT 1000 is equipped with an automatic unwinding and rewinding mechanism, a web guiding and tension control mechanism, guide rollers, a direct gravure coating unit, a doctor blade angle and loading pressure adjustment mechanism, a feed circulation mechanism, a main drive encoder and PLC data acquisition module, a segmented hybrid continuous drying system, and cooling rollers. This embodiment uses a 1000mm wide paper web. Before use, the roller axes are made parallel to each other. The coating speed, paper web tension, feed circulation flow rate, doctor blade angle, and loading pressure are set according to the corresponding embodiment. The actual wet transfer coefficient is calibrated using the wet mass difference before and after coating. The actual wet transfer coefficients for Embodiments 9 and 10 are 0.80±0.03 and 0.75±0.03, respectively, and are verified using registration position, regional PHA areal density, and the continuity of exposed cellulose pathways.
[0110] The continuous drying section of the VCML Lab / Pilot Coater consists of a hot air pre-drying module, a short-wave infrared drying module, and a cooling roller; the continuous drying section of the EXPERTCOAT 1000 consists of segmented hot air drying zones, a high-energy drying zone at the end, and a cooling roller arranged sequentially along the paper web running direction. Each drying module is linked to the paper web conveying speed. Before use, the hot air temperature, air velocity, nozzle-to-paper distance, and infrared thermometer reading are checked. The infrared thermometer emissivity is set to 0.95, and the paper surface temperature is verified using a contact surface thermocouple.
[0111] The peak paper temperature described in this specification refers to the highest temperature reached on the food-contact surface of the paper web as it passes through the continuous drying system. The peak paper temperature is set based on the second heating main melt peak temperature of the corresponding batch of PHA measured according to ISO 11357-3:2025 and the aggregation state of the PHA particles. For water-based coatings containing two or more types of PHA, the highest value among the main melt peak temperatures of each PHA is used as the temperature setting benchmark. In this embodiment, calculated based on the nominal main melt peak temperature of each brand, the peak paper temperature is 5–13°C higher than the highest nominal main melt peak temperature of the corresponding single PHA or mixed PHA.
[0112] The high-temperature holding time described in this specification refers to the time during which the surface temperature of the food contact side of the paper web remains continuously at or above the corresponding PHA main melting peak temperature. In Examples 9 and 10, when P34HB was used, the time during which the paper surface temperature remained continuously ≥150°C was separately recorded for process control under high-speed industrial conditions.
[0113] During laboratory and pilot-scale coating, a Fluke 62 MAX+ infrared thermometer was used for mobile measurements, and a testo925 contact surface thermocouple was used for low-speed calibration. During industrial coating, fixed CTfast LT25 infrared temperature measurement points were installed at the outlet of each hot air drying zone, the inlet of the final high-energy drying zone, the interior of the final high-energy drying zone, and the outlet. The sensor emissivity was set to 0.95, and the sampling frequency was 100Hz. Each temperature measurement point was calibrated using low-speed paper web and contact surface thermocouples before formal operation; the calibration temperature difference should be ≤2℃.
[0114] The linear velocity of the industrial paper web is measured by an EXPERTCOAT 1000 main drive encoder and recorded as data in the PLC at a frequency of 10Hz. The paper surface temperature profile is established based on the location of the temperature measurement points, the temperature at each measurement point, and the synchronous linear velocity data. The high-temperature holding time is calculated based on the start and end points of the paper surface temperature profile exceeding the specified temperature threshold and the synchronous linear velocity. The peak paper surface temperature, high-temperature holding time, residual moisture content, and finished product C1 are used as the combined drying endpoint control values for PHA particle agglomeration and continuous film formation.
[0115] The TA-100-FINAT fixed-weight pressure roller has a steel core roller and a silicone rubber coating with a Shore A hardness of 80. Its nominal total mass is 2 kg, the effective width of the roller surface is 50 mm, and the outer diameter is 85 mm. Before use, verify the roller's quality, surface integrity, and rotational flexibility. During rolling, the handle is only used for horizontal traction; no additional downward pressure is applied. Roll back and forth once at a speed of 50 ± 5 mm / s.
[0116] The auxiliary observation components used in the central hot oil breakthrough test include a rigid support frame, a horizontally fixed 8mm thick optical glass plate, and a vertical imaging system. The effective observation area of the optical glass plate completely covers the 100mm × 100mm sample and its 50mm diameter oil-receiving area. A Nikon D7500 camera is fixed below the optical glass plate, with its lens optical axis perpendicular to the optical glass plate and facing the back of the standard oil absorption indicator paper. With uniform illumination, images are continuously acquired at 1 frame / s. Before each test, a millimeter ruler is placed on the plane of the standard oil absorption indicator paper to calibrate the pixel size, fix the focal length, exposure, and illumination conditions, and confirm the recognition capability with a calibration pattern of equivalent diameter 1.0mm; the timing for image acquisition begins at the start of corn oil addition.
[0117] Main testing standards.
[0118] The following standards, published by the International Organization for Standardization (ISO) and the Technological Association of the Pulp and Paper Industries (TAPPI), are used for the testing of this invention.
[0119] Table 3. Main test standards.
[0120]
[0121] Parameter definition and planar structure determination.
[0122] Effective area A of food contact side t A is the total planar projected area of the paper-based packaging structure when unfolded and folded, facing the food side. Process positioning holes, inspection and clamping holes, and cutting waste edges that do not participate in the wrapping are not included in A. t .
[0123] The first and second functional areas do not overlap and together constitute the effective area of the food contact side. The planar projected areas of the first and second functional areas are denoted as A1 and A2, respectively, and satisfy the following:
[0124] A t =A1+A2.
[0125] The second functional area is divided into a general PHA coverage area, a continuous PHA oil-barrier boundary zone area, and an exposed cellulose area. The planar projected areas of the general PHA coverage area, the continuous PHA oil-barrier boundary zone area, and the exposed cellulose area are denoted as A, respectively. 2p A 2β and A 2o And satisfy:
[0126] A2=A 2p +A 2β +A 2o .
[0127] The ordinary PHA coverage area and the continuous PHA oil-blocking boundary zone do not overlap and together constitute the second functional area PHA coverage area. The planar projected area of the second functional area PHA coverage area is denoted as A. 2c And satisfy:
[0128] A 2c =A 2p +A 2β .
[0129] The planar projection area coverage of the second functional area, PHA, is A. 2c / A2×100%, the cellulose exposure rate E2 in the second functional zone is A 2o / A2×100%, the sum of the two is 100%.
[0130] The ordinary PHA coverage area is the PHA coverage area within the second functional zone, excluding the continuous PHA oil barrier boundary zone area.
[0131] The continuous PHA oil barrier boundary zone is the PHA coverage area located on the outer periphery of the first functional area, connected to the continuous PHA barrier of the first functional area, and surrounding the first functional area.
[0132] The exposed cellulose region is the area within the second functional area located outside the coverage of the PHA recognition pixel. It includes continuous exposed cellulose pathways, exposed cellulose to edge ends, and other exposed cellulose surfaces that may or may not be connected to the maximum exposed cellulose connectivity region. The exposed cellulose region simultaneously meets the following criteria: it is determined to be an exposed cellulose pixel according to the micro-Raman calibration and full-area optical image classification methods specified in this specification; and it is defined within a 25cm radius. 2 When the sampling area was determined using the methanolysis-gas chromatography-flame ionization detector method, the PHA mass was less than 0.10 mg, which translates to a PHA dry mass per unit area of less than 0.04 g / m². 2 .
[0133] The predetermined fold line coordinates define at least two folded areas within the second functional area. These folded areas are zones designated for folding purposes based on the predetermined package pattern, and can simultaneously include a general PHA coverage area, a continuous PHA oil-blocking boundary zone, and an exposed cellulose area. The folded areas are not counted repeatedly as additional areas beyond A2.
[0134] The origin of the coordinate system is the geometric center of the finished product, with the machine direction as the x-axis and the horizontal direction as the y-axis. Unless otherwise specified, the geometric center of the first functional area coincides with the origin, and the long side of the rectangular first functional area is parallel to the x-axis. The first functional area is determined by registering the finished product coordinates with the closed boundary of the high-coverage pattern of the first functional area in the coating pattern. The PHA recognition pixels within the closed boundary are used to calculate F1, R1, and C1. The second functional area is the region between the outer perimeter of the closed boundary and the actual edge of the finished product paper. When positioning marks are set on the finished product, the finished product coordinate registration is completed using the positioning marks; when no positioning marks are set, the origin of the coordinate system is the geometric center of the finished product, and translation, rotation, and proportional registration are performed through the actual edge of the finished product paper, the high-coverage pattern of the first functional area, and the PHA coating pattern.
[0135] The coordinates of the predetermined fold line, fold area, predetermined fold overlap area, predetermined area for packaging label fixing, and predetermined cutting line are determined based on the predetermined package pattern, coating pattern, and finished product dimensions. When positioning marks are set on the finished product, a pattern coordinate system is established using the positioning marks; when no positioning marks are set, the geometric center of the finished product is used as the origin of the coordinate system, and translation, rotation, and proportional registration are performed through the actual paper edge of the finished product, the high-coverage pattern of the first functional area, and the PHA coating pattern. After the finished product is cut, the edge formed by the actual cut is used as the paper edge.
[0136] The folded regions traversed by the continuous exposed cellulose pathway are determined by superimposing the pathway skeleton diagram with the registered coordinates of the folded regions. When a continuous exposed cellulose pathway enters a folded region from its inner starting boundary and extends continuously within that folded region to the corresponding paper edge, the pathway is determined to have traversed the folded region.
[0137] Two continuous pathways of exposed cellulose pass through different folded regions, meaning that the two pathways enter folded regions defined by different predetermined fold line coordinates and reach different paper edges corresponding to the different folded regions.
[0138] The PHA continuous barrier phase, the PHA-covered area in the second functional region, and the exposed cellulose continuous phase are classified using bright-field and cross-polarized full-area optical image results calibrated by micro Raman pixel determination results, and jointly determined by eight-neighbor connectivity analysis.
[0139] Micro Raman spectroscopy was performed using a 532 nm laser, a 10x objective lens, a laser power of 3.0 ± 0.3 mW on the sample surface, a 600 gr / mm grating, an integration time of 1.0 s, and two accumulations. After baseline subtraction using asymmetric least squares, the spectra were integrated within the PHA carbonyl characteristic region (1720–1760 cm⁻¹). -1 The characteristic range of cellulose is 1070–1120 cm. -1 According to R=S PHA / (S) PHA +S cellulose Calculate the strength ratio.
[0140] The reference strength ratio R of the base paper was obtained using the same batch of uncoated base paper. base The 6.0±0.2 g / m² sample was prepared on the same batch of base paper using the same type or combination of PHAs as the test sample. 2 Full-width continuous membrane obtains full-film reference intensity ratio R film Press R norm =(RR base ) / (R film -R base Normalize R. norm Raman surface scan pixels with a value ≥0.50 are marked as PHA coverage calibration pixels, R norm Raman surface scan pixels with a value <0.50 are marked as exposed cellulose calibration pixels.
[0141] The local bright-field and cross-polarized images corresponding to the Raman calibration field of view were acquired using a Leica DM6 M local materials microscope. These images were used to verify the local morphology and field of view boundaries of the Raman surface scanning area and were not directly used as input images for the binary classification linear discriminant model. The full-area optical images of the first and second functional areas were acquired using the Nikon D7500 full-area optics and vertical imaging system listed in Table 2. With the food-contact side of the finished product facing the lens, bright-field red, green, and blue (RGB) images and cross-polarized RGB images were acquired segment by segment along the x and y axes in the finished product coordinate system. The x and y coordinates of the center of each field of view in the finished product coordinate system were recorded. The focal length and shooting distance were adjusted and fixed so that the output pixel size of each field of view was no greater than 20μm × 20μm, with 10% overlap between adjacent fields of view. After flat field correction, geometric registration, and overlapping area fusion, the stitched image was resampled to a 20μm × 20μm full-area imaging pixel size. Brightfield images, cross-polarized images, and Raman calibration fields of view were registered at the pixel level using the same pre-designed coordinate system, the same pixel size, and the same cropping boundary. All optical feature vectors of the binary classification linear discriminant model were extracted from full-area optical images obtained from a Nikon D7500.
[0142] The bright-field RGB image is converted to the International Commission on Illumination (CIELAB) color space. For each 20μm × 20μm full-area imaging pixel, the feature vector is extracted according to the following formula:
[0143] x=[L* / 100, a* / 128, b* / 128, I CP / (I BF +10 -6 ), σ L / 100] T .
[0144] Where L*, a*, and b* are the parameters of the pixel in the CIELAB color space; I BF For bright field RGB images according to I BF = (0.299R) RGB +0.587G RGB +0.114B RGB The gray intensity is calculated as () / 255; I CP The grayscale intensity of a cross-polarized RGB image calculated using the same formula; σ L L* represents the standard deviation within a 5×5 pixel window centered on that pixel.
[0145] The first functional region acquires nine 2mm × 2mm Raman surface scanning fields at the center, four quarter positions, and four adjacent boundary positions. The second functional region selects no fewer than twelve 2mm × 2mm Raman surface scanning fields in the ordinary PHA coverage area, the continuous PHA oil-blocking boundary zone, the middle of the exposed cellulose continuous pathway, the exposed cellulose to the edge, the area adjacent to the predetermined fold line coordinates, and other exposed cellulose areas. The Raman surface scanning step size is 20μm, and each Raman surface scanning pixel is registered one-to-one with a 20μm × 20μm pixel at the same coordinates in the full-area optical image.
[0146] For each base paper batch and each PHA or PHA combination, a binary linear discriminant model is established for PHA-covered pixels and exposed cellulose pixels, respectively. The model is directly used across base paper batches or PHA types. Using R... norm The judgment result is used as a category label. The fields of view are grouped according to the Raman plane scanning field of view. 80% of the field of view is used to build a classification model, and the remaining 20% of the field of view is used for independent verification.
[0147] The classification model employs linear discriminant analysis with a shared covariance matrix. The feature mean vectors for the PHA-covered class and the exposed cellulose class are denoted as μ. PHA and μ cell The shared covariance matrix is denoted as Σ, and the prior probabilities of both classes are both 0.50.
[0148] For the feature vector x of the pixel to be classified, the discrimination score is calculated according to the following formula:
[0149] g j (x) = x T Σ -1 μ j -0.5μ j T Σ -1 μ j +ln(0.50).
[0150] Where j represents either PHA-covered or exposed cellulose. The PHA coverage discrimination probability is calculated using the following formula:
[0151] P PHA =exp[g PHA (x)] / {exp[g PHA (x)]+exp[g cell (x)]}.
[0152] P PHA Pixels with a full-area imaging resolution ≥0.50 are considered PHA-covered pixels. PHAPixels with a value <0.50 across the entire imaging area are classified as exposed cellulose pixels. Classification and binary image output are performed by running a macro script in ImageJ 1.54f based on the above formulas and decision parameters, without requiring manual pixel-by-pixel correction by the analyst.
[0153] The overall classification accuracy of independently verified pixels should be ≥95%. If the overall classification accuracy is below 95%, the registration status of bright-field and cross-polarized images, the Raman calibration field of view coverage, and the flat-field correction results should be re-examined, and a new classification model should be established. The validated model is used for full-area classification of the first and second functional areas of the corresponding base paper batch and PHA type or PHA combination.
[0154] When determining whether a single finished product forms the specified structure, a complete imaging analysis is performed on the first and second functional areas of the finished product. The coverage rate, area ratio, path width, and edge dimensions are determined based on the detection results of the single finished product. The structural parameters reported in the examples and comparative examples are the average values of the detection results of the middle sections of three independent batches of finished products. Only isolated noise with an equivalent diameter less than 40 μm is removed from the binary image; no connectivity bridging, artificial line filling, hole filling, or boundary smoothing is performed. The first and second functional areas are marked with eight-neighbor connected components on the final binary image, and F1, R1, C1, E2, R2, and C2 are obtained according to the described area calculation method.
[0155] The PHA recognition pixel area within the first functional region is divided by the total area of the first functional region to obtain the PHA film coverage rate F1 of the first functional region; the maximum PHA connected region area within the first functional region is divided by the total area of the first functional region to obtain the maximum PHA connected region area ratio C1 of the first functional region; the ratio obtained by dividing the maximum PHA connected region area within the first functional region by the total area of PHA recognition pixels within the first functional region is denoted as the maximum connected region ratio R1 within the PHA phase, and satisfies:
[0156] C1 = F1 × R1 / 100.
[0157] The area of PHA-identified pixels within the second functional region divided by the total area of the second functional region yields the planar projection area coverage of the PHA-covered region in the second functional region; the area of exposed cellulose-identified pixels within the second functional region divided by the total area of the second functional region yields the cellulose exposure rate E2 in the second functional region; the area of the largest exposed cellulose connected region within the second functional region divided by the total area of the second functional region yields the proportion of the largest exposed cellulose connected region within the second functional region C2; the proportion obtained by dividing the area of the largest exposed cellulose connected region within the second functional region by the total area of exposed cellulose-identified pixels within the second functional region is denoted as the proportion of the largest connected region within the exposed cellulose phase R2, and satisfies:
[0158] C2 = E2 × R2 / 100.
[0159] The PHA recognition pixels within the second functional area are further divided into a normal PHA coverage area and a continuous PHA oil-blocking boundary zone area based on the map coordinates and the position of the finished image. When there is a deviation between the actual finished product boundary and the map coordinates, the boundary of the finished product PHA recognition pixels shall prevail.
[0160] The exposed cellulose continuous pathway is determined using the eight-neighbor path of the largest exposed cellulose connected domain. The inner starting boundary of the pathway is the outer boundary of the first functional area, or the outer edge of the continuous PHA oil-blocking boundary band; when there is a continuous path consisting entirely of exposed cellulose identification pixels from the inner starting boundary of the pathway to the paper edge, it is determined that an exposed cellulose continuous pathway is formed.
[0161] The minimum effective width of the exposed cellulose continuous pathway is calculated using skeletonization and Euclidean distance transformation. The minimum effective width of the exposed cellulose continuous pathway is defined as the minimum diameter of the largest circle of equal diameter that can be continuously traversed along the complete path from the inner boundary of the pathway to the edge of the paper.
[0162] The folded regions traversed by the continuous exposed cellulose pathway are determined by superimposing the pathway skeleton diagram with the coordinates of the predetermined fold lines. When a continuous exposed cellulose pathway enters a folded region from the inner starting boundary of the pathway and extends continuously within the folded region to the corresponding paper edge, it is determined that the pathway traverses the folded region.
[0163] Two continuous pathways of exposed cellulose pass through different folded regions, meaning that the two pathways enter folded regions defined by different predetermined fold line coordinates and reach different paper edges corresponding to the different folded regions.
[0164] When the area ratio of the largest PHA connected domain in the first functional region C1 is ≥70%, and the second functional region simultaneously contains an exposed cellulose continuous phase with a PHA-covered area and an area ratio of the largest exposed cellulose connected domain C2 ≥30%, and at least two exposed cellulose continuous pathways in the largest exposed cellulose connected domain pass through different folded areas and reach different paper edges, the partitioned exhaust and oil-blocking conformal planar structure is determined to be formed. The PHA coverage rate and spatial concentration coefficient K of the second functional region are recorded separately as material spatial distribution parameters; the PHA coverage rate of the second functional region is 15% to 60%, and K ≥ 1.20 are respectively used as control ranges in some implementation methods, and are not necessary conditions for determining the validity of the planar structure independently of C1, C2, and the pathway topology.
[0165] Determining the external connectivity status after folding:
[0166] Whether the paper-based packaging structure meets the requirements for folded use shall be determined according to the following multi-view imaging detection method for external connectivity after folding.
[0167] Before testing, the paper-based packaging structure to be tested is fully unfolded with the food contact side facing the scanning surface. An Expression 13000XL flatbed scanner is used to acquire an unfolded image at a scanning resolution of 600 dpi and 24-bit color mode. When positioning marks are set on the finished product, a layout coordinate system is established based on the positioning marks; when no positioning marks are set, the geometric center of the finished product is used as the origin of the coordinate system. The actual paper edge of the finished product, the high-coverage pattern of the first functional area, and the PHA coating pattern are translated, rotated, and proportionally registered. The coordinates of the predetermined fold line, the fold area, the predetermined fold overlap area, and the predetermined area coordinates of the packaging fixing label are superimposed onto the unfolded image.
[0168] Based on the registered layout coordinates and the microscopic image, the continuous pathway contours of exposed cellulose are determined, and the boundaries of each exposed cellulose to the edge are marked in the unfolded image. The marked boundary of each exposed cellulose to the edge includes at least the actual paper edge position it reaches, the start and end coordinates along the paper edge direction, and the contour extending from the paper edge into the paper interior.
[0169] Following the food placement and folding sequence specified in the corresponding application example, fold along the predetermined folding line coordinates, and affix the packaging fixing label to the position corresponding to the predetermined area coordinates. After the label is pressed, without moving the label, reopening the folds, or adjusting the relative positions of the paper layers, place the package with the seam facing upwards at the center of a manually rotated platform with an angle scale. Multi-view imaging is performed in an environment of 23±1℃ and 50±5% relative humidity.
[0170] Multi-view imaging was performed using a Nikon D7500 camera and a 60mm macro lens. The camera was mounted on a fixed bracket, with the distance from the lens optical axis to the geometric center of the packaging being 500±5mm. Illumination was provided by a surface light source with a color temperature of 5500K, and the illuminance on the test surface was 1000±100lx. Orthogonal polarizers were used on both the lens and the light source to reduce reflections from the paper and labels. The camera was operated in manual exposure mode with an ISO of 200, an aperture of f / 8, a shutter speed of 1 / 60s, and a white balance of 5500K. The camera focal length, shooting distance, exposure conditions, and illumination conditions remained constant throughout the experiment.
[0171] For each package, a top view, a bottom view, and eight side views surrounding the package are captured sequentially. The rotation angles of the eight side views are 0°, 45°, 90°, 135°, 180°, 225°, 270°, and 315°, respectively. At 0° rotation, the top edge of the unfolded package faces the camera; the other angles are determined according to the clockwise direction of the top view. The lens optical axes of the top and bottom views are perpendicular to the main load-bearing planes at the top and bottom of the package, respectively.
[0172] During each photograph, place the millimeter ruler near the local paper surface where the end to be measured is located. The height difference between the millimeter ruler and the local paper surface to be measured should be ≤1.0mm, and it should not obstruct the exposed cellulose to the edge of the paper. If the millimeter ruler cannot be placed directly, use a calibration image obtained before photographing at the same distance and on the same local plane to perform pixel size conversion.
[0173] Geometrically register the exposed cellulose to the edge contour marked in the unfolded image before folding with the actual paper edge, paper corner, crease intersection, and outer contour of the packaging label in each view after folding. Select a view where the angle between the local paper surface where the end to be measured is ≤15° and the lens imaging plane for dimensional measurement; if the view does not exist, perform perspective correction using four geometric feature points on the local paper surface to be measured before dimensional measurement.
[0174] The registered image was measured using ImageJ 1.54f. The continuous visible length outside the coverage area of other paper layers and packaging labels was measured along the actual paper edge direction reached by the edge to be measured; the minimum exposed width of the visible area was measured along a direction perpendicular to the actual paper edge and pointing inwards from the paper.
[0175] A cell with exposed cellulose at its edge is considered to maintain communication with the outside of the packaging when all of the following conditions are met:
[0176] First, the area where the exposed cellulose reaches the edge can be directly observed from the outside of the packaging without moving the packaging to fix the label, opening the folds, or changing the relative positions of the paper layers.
[0177] Second, the area where the exposed cellulose reaches the edge itself constitutes part of the outer surface of the packaging, rather than the internal area of the packaging that can only be observed through the gap between the two layers of paper;
[0178] Third, the visible exposed area formed by the exposed cellulose to the edge is outside the coverage of other paper layers formed by folding and the packaging fixing label;
[0179] Fourth, the continuous visible length of the exposed cellulose to the edge end along the paper edge direction is ≥1.0mm, and the minimum exposed width perpendicular to the paper edge direction is ≥1.0mm.
[0180] The number of exposed cellulose ends meeting the above conditions in a package is denoted as the number of externally connected ends of the package. When the number of externally connected ends is ≥1, it is determined that at least one of the externally connected ends of the package is successfully connected to the outside; when the number of externally connected ends is 0, it is determined that all externally connected ends of the package have failed to be sealed.
[0181] The average number of externally connected terminals is calculated using the following formula:
[0182] Average number of externally connected ends = Sum of the total number of externally connected ends of all packages / Total number of packages.
[0183] The success rate of connecting at least one edge end to the outside world is calculated according to the following formula:
[0184] Success rate of at least one external connection end = number of packages with ≥1 external connection end / total number of packages × 100%.
[0185] The failure rate of complete edge closure is calculated using the following formula:
[0186] Failure rate of complete edge closure = number of packages with zero external connection ends / total number of packages × 100%.
[0187] The image of each package was determined by two analysts who were unaware of the sample number and structural type. If the two analysts agreed on the number of externally connected ends, that determination was adopted; if they disagreed, a third analyst who was unaware of the sample number and structural type reviewed the image, and the result of at least two of the three analysts agreeing was taken as the final result.
[0188] Regional PHA surface density and water vapor transfer test.
[0189] The areal density of the PHA region was determined using the methanol hydrolysis-gas chromatography-flame ionization detector (GC-FID) method. When judging a single finished sheet, equal-area samples were cut from the center and four quarter-positions of the first functional area of the finished sheet, with a total area of 25 cm² for the five samples. 2 The five samples were combined for measurement, and the total mass of PHA was divided by 0.0025m. 2 The q1 of the finished product is obtained.
[0190] When determining q2 for a single finished product, based on the area ratio of the ordinary PHA-covered area, the continuous PHA oil-blocking boundary zone area, and the exposed cellulose area within the second functional area of the finished product, samples are cut from each area according to the corresponding ratio and combined to form a total area of 25cm². 2 The total mass of PHA measured in the composite sample was divided by 0.0025m. 2 The q2 of the finished product was obtained. When it was impossible to form a composite sample in proportion, q was measured separately. 2p q 2β and q 2o And according to q2=(A 2p ×q 2p +A 2β ×q 2β +A 2o ×q 2o ) / A2 calculation.
[0191] The second functional area is divided into a general PHA coverage area, a continuous PHA oil-blocking boundary zone area, and an exposed cellulose area. The general PHA coverage area was cut from four directions and one corner of five different finished products, each measuring 25.0 cm. 2 Samples were measured separately, and the average value was taken to obtain the dry mass q of PHA per unit area in the area covered by ordinary PHA. 2p .
[0192] Samples of the continuous PHA oil-blocking boundary zone were cut from another 10 finished sheets along the continuous PHA oil-blocking boundary zone and combined into 3 composite samples with the same area ratio. The total area of each composite sample was 25.0 cm². 2 After separate measurements, the average value was taken to obtain the dry mass q of PHA per unit area in the continuous PHA oil-blocking boundary zone. 2β .
[0193] Exposed cellulose areas were extracted from the 10 finished sheets, including continuous exposed cellulose pathways, exposed cellulose extending to the edges, and other exposed cellulose areas. These were then combined into three composite samples according to the area ratio of each area within the total exposed cellulose area, with each composite sample having a total area of 25.0 cm². 2 The dry mass q per unit area of PHA in the exposed cellulose region was obtained by measuring the values of each region. 2o .
[0194] Before sampling, PHA coverage in areas with ordinary PHA coverage and continuous PHA oil-blocking boundary zones was confirmed using micro-Raman spectroscopy. In exposed cellulose areas, micro-Raman spectroscopy was used to confirm the absence of a continuous PHA film before sampling. The limit of quantification for the GC-FID method was 0.10 mg PHA; when 25.0 cm⁻¹… 2 When the PHA mass in the composite sample from the exposed cellulose region is less than 0.10 mg, report q. 2o <0.04g / m 2 .
[0195] The area-weighted average dry mass per unit area of PHA in the second functional area, q2, is calculated according to the following formula:
[0196] q2=(A 2p ×q 2p +A 2β ×q 2β +A 2o ×q 2o ) / A2.
[0197] When using a structure without a continuous PHA oil barrier boundary zone, A 2β Take 0. When q 2o When the value is below the method limit of quantitation, in order to maintain a consistent calculation method between the examples and comparative examples, q is used in the calculation of q2. 2oTreat it as 0, but record the single test result as q. 2o <0.04g / m 2 This calculation convention does not imply that the exposed cellulose area is absolutely free of PHA.
[0198] Examples 1-12 and Comparative Examples 2-13 each prepared three independent coated batches; Comparative Example 1 and the uncoated base paper control were sampled from three independent base paper batches; Comparative Example 14 directly used the three independent coated batches corresponding to Example 1. q1 and q2 in the examples and comparative examples were taken as the average of the results of the three independent batches.
[0199] Average dry mass q of PHA per unit area within the effective area of the food contact side t Calculate q using the following formula: t =(A1×q1+A2×q2) / A t .
[0200] The spatial concentration factor K is calculated using the following formula: K = q1 / q t .
[0201] For GC-FID analysis, the sample was placed in a VO29 vacuum drying oven and dried to constant weight at 60±2℃ and absolute pressure ≤20kPa, and the sampling area was accurately recorded. The sample was then placed in a pressure-resistant reaction tube with a polytetrafluoroethylene-lined sealing cap, and 2.0 mL of chloroform and 2.0 mL of methanol solution containing 3% sulfuric acid and 1.00 mg / mL benzoic acid as an internal standard were added. The reaction was carried out in a Reacti-Therm™ TS-18821 thermostatic heating and stirring module at 100±1℃ for 4 h in a sealed environment. After cooling to room temperature, 1.0 mL of water was added, the mixture was shaken for 30 s, allowed to stand for separation, and the organic phase was separated and dried with anhydrous sodium sulfate.
[0202] The chromatographic column was an HP-INNOWax capillary column with dimensions of 30m × 0.25mm × 0.25μm; the injection port temperature was 250℃, the flame ionization detector temperature was 280℃, the carrier gas was helium, the constant flow rate was 1.0mL / min, the injection volume was 1.0μL, and the split ratio was 20:1; the column temperature program was 60℃ for 2 min, increased to 180℃ at 10℃ / min, then increased to 240℃ at 5℃ / min and held for 8 min.
[0203] To prepare the PHA solid for calibration, place the corresponding BIOTEN brand PHA aqueous dispersion in a 50 mL centrifuge tube and centrifuge for 20 min at 20±2℃ and 10000×g using a Centrifuge 5910 Ri refrigerated centrifuge with an FA-6×50 fixed-angle rotor. Discard the supernatant. Add an equal volume of deionized water to redisperse the supernatant, and repeat the centrifugation and washing process three times. Place the resulting precipitate in a VO29 vacuum drying oven and dry it to constant weight at 60±2℃ and an absolute pressure ≤20 kPa.
[0204] A methanololysis calibration series using the same PHA solid was prepared with PHA masses of 0.10 mg, 0.20 mg, 0.50 mg, 2.0 mg, 5.0 mg, 10.0 mg, 20.0 mg, and 30.0 mg, respectively, prepared using the same method. A mixed calibration series was prepared using the same PHA dry solid ratio as in the examples. Before analysis of each batch of samples, the methanololysis product of the corresponding PHA calibration sample was injected. The absolute value of the retention time deviation was ≤0.10 min to identify the source peaks of each PHA, and the areas of all PHA source peaks were summed. The method quantitation limit was set to the value of the correlation coefficient R of the calibration curve. 2 The lowest calibration point is defined as ≥0.995, with a spiked recovery rate of 95%–105% and a relative deviation of ≤5% for parallel determinations; the limit of quantitation for this method is 0.10 mg PHA. Blank correction is performed using uncoated base paper from the same batch.
[0205] Used to calculate the area-weighted equivalent water vapor transmission rate (WVTR) in the unfolded state. t The water vapor transmission rate data for each local material condition were obtained according to the desiccant cup method of ISO 2528:2017, using a W3 / 031 water vapor transmission rate tester and a standard test area of 33 cm². 2 A moisture permeability cup was used. For the spatially non-uniform pattern of paper-based packaging structures, the water vapor permeability per unit area of each local material state was determined using the same batch area replication sample method.
[0206] When preparing each batch of paper-based packaging structures, the same batch of fiber-based paper, the same PHA water-based coating, and the same drying heat history were used. Simultaneously, replica samples of the first functional area, the second functional area (ordinary pattern), the exposed cellulose continuous pathway, and the boundary zone with a continuous PHA oil-blocking boundary were prepared. Each type of replica sample had a size ≥100mm × 100mm and met the following conditions:
[0207] The first functional area replication sample uses the same pattern, PHA unit area dry mass q1, film coverage and drying conditions as the first functional area of the corresponding embodiment.
[0208] The second functional area common pattern replication sample uses the same periodic pattern, local layout coverage, and PHA unit area dry mass q as the second functional area common pattern area in the corresponding embodiment. 2p and drying conditions;
[0209] The cellulose continuous pathway replication sample was prepared using uncoated fiber-based paper from the same batch, and its PHA dry mass per unit area q 2o =0;
[0210] The boundary zone replica sample uses the same local PHA unit area dry mass q as the continuous PHA oil-blocking boundary zone in the corresponding embodiment. 2β and drying conditions.
[0211] Circular specimens with a diameter of 74 mm were cut from each replicated sample, with the food contact side facing the high-humidity side, resulting in an effective test area of 33 cm². 2 Anhydrous calcium chloride was placed in the cup, and the distance between the sample and the desiccant surface was 10±1 mm. The test temperature was 38±0.5℃, and the relative humidity on the high-humidity side was 90±2%. The sample edge was sealed with room-temperature curing butyl sealant. Mass was recorded every 2 hours after the start of the test (6 hours), obtaining at least 6 consecutive data points. Edge leakage blank correction was performed using the same empty cup. The linear regression correlation coefficient R between mass and time was calculated. 2 ≥0.995.
[0212] The local water vapor transmission rates WVTR1 and WVTR were measured in the first functional region, the ordinary pattern area of the second functional region, the exposed cellulose area, and the continuous PHA oil barrier boundary zone. 2p WVTR 2o and WVTR 2β And calculate the area-weighted equivalent water vapor transmission rate WVTR2 of the second functional area according to the following formula: WVTR2 = (A 2p ×WVTR 2p +A 2o ×WVTR 2o +A 2β ×WVTR 2β ) / A2;
[0213] The unfolded area-weighted equivalent water vapor transmission rate (WVTR) of the paper-based packaging structure is calculated using the following formula: t WVTR t =f×WVTR1+(1-f)×WVTR2.
[0214] The projected area of the continuous PHA oil barrier boundary zone is denoted as A. 2β When a structure without a continuous PHA oil barrier boundary zone is adopted, A 2β Take 0.
[0215] Exposed cellulose to the edge is considered part of the exposed cellulose region and is not weighted repeatedly as an independent material state. The area-weighted equivalent water vapor transmission rate (WVTR) in the unfolded state is used. t The water vapor transmission rate is calculated based on the local test results of the replicated samples in each region of the unfolded state and the proportion of their planar projected area. It is not the water vapor transmission rate directly measured on the folded complete package.
[0216] For samples that did not form a first functional zone, circular specimens with a diameter of 74 mm were cut from the center of the food contact side and each of the four quadrants. The average local water vapor transmission rate at the five locations was reported, without region weighting. The average of the five independent specimens was taken for each local water vapor transmission rate.
[0217] Oil-blocking and encapsulation performance tests.
[0218] Oil resistance grades were determined according to TAPPI T 559 cm-22, with samples taken from the center of the first functional zone; samples that did not form a first functional zone were taken from the nominal central area of Example 1. The highest test solution number that did not form dark spots was recorded, and this grade was designated as the oil resistance grade. Given that this method primarily evaluates the oil repellency or wicking resistance of paper and paperboard surfaces, and that its applicability to film-like barriers or non-fluorinated treatments requires evaluation in conjunction with specific materials, this specification uses this grade only as an auxiliary evaluation of surface repulsion ability. Continuous film structures are evaluated separately using the hot oil breakthrough method.
[0219] The central hot oil breakthrough method is as follows: Cut a 100mm × 100mm sample with the center of the first functional area as the sample center, with the food contact side facing upwards; when the short side of the first functional area is less than 100mm, still cut it as 100mm × 100mm, but the oil-receiving area with a diameter of 50mm is completely located within the first functional area. Place Whatman Grade 1 standard oil absorption indicator paper under the sample, and place both on a horizontally fixed optical glass plate with a thickness of 8mm. Fix the Nikon D7500 vertical imaging system under the optical glass plate, so that the lens optical axis is perpendicular to the optical glass plate and facing the back of the standard oil absorption indicator paper, and continuously acquire images of the back of the standard oil absorption indicator paper at 1 frame / s. Place a PTFE limiting ring with an inner diameter of 50mm and a height of 5mm at the center of the first functional area, and add 5.0 ± 0.05g of corn oil at a temperature of 80 ± 2℃ using a glass syringe within 5 ± 1s. The breakthrough point is when the first oil penetration spot with an equivalent diameter ≥ 1.0mm appears on the back of the standard oil absorption indicator paper. The upper limit of observation is 1800 s. If no specified oil spot appears within the 1800 s observation period, it is recorded as 1800 s.
[0220] The hot oil penetration method for creases is as follows: Before cutting, all samples are marked with the machine direction, and a test crease line is set through the center of the first functional area and parallel to the machine direction, so that the food contact side is on the outside of the fold. After folding the sample 180° along the test crease line, a TA-100-FINAT fixed-weight pressure roller is used to roll it back and forth once along the test crease line at a speed of 50±5mm / s; the nominal mass of the pressure roller is 2kg, the effective width of the roller surface is 50mm, the outer diameter is 85mm, and the Shore A hardness of the silicone rubber coating is 80. The sample is unfolded and left to stand for 60s, and then the oil-receiving area is centered on the center of the test crease line, and the test is performed according to the central hot oil penetration method.
[0221] In the oil stain diffusion area test, corn oil and tomato sauce were preheated to 80±2℃, mixed at a mass ratio of 4:1, and stirred at 300 rpm for 60 s. 5.0±0.05 g of the mixture was added to the same limiting ring, and after 30 min, the remaining mixture was removed, and surface liquid was gently blotted with lint-free paper. The back of the paper was scanned using a flatbed scanner with a resolution of 600 dpi and a grayscale depth of 8 bits. The mean grayscale value μ0 and standard deviation σ0 were obtained from the same batch of paper that had not been exposed to the liquid. Grayscale values ≤ μ0 - 3σ0 and connected areas ≥ 0.785 mm² were considered. 2 The pixel area is identified as an oil spot, and the total area is calculated according to the calibration scale.
[0222] The overlap rate of food projection was determined using an imaging method perpendicular to the plane of the paper-based packaging structure. The optical axis of the lens of the vertical imaging system was perpendicular to the plane of the paper-based packaging structure, the shooting distance was 500±5mm, and a 100mm calibration ruler was set in the image; the image was acquired within 3 seconds after the hot food was first placed on the unfolded paper-based packaging structure.
[0223] When setting positioning marks, the positioning marks are 0.2mm wide linear marks, set on the outer surface opposite the food contact side, or on the surface where the effective area A of the food contact side is not included. t Process waste edges removed during finished product cutting. Positioning marks must not be placed on the effective area A of the food contact side. t Inside. When no positioning marks are set, the boundary of the first functional area is determined by the registration relationship between the actual paper edge, the geometric center of the finished product, the high-coverage pattern of the first functional area and the PHA coating pattern and the layout coordinates.
[0224] The orthographic projection of the food is determined by edge segmentation and verified by two operators. The overlap rate is calculated by dividing the area of the intersection between the orthographic projection of the food and the first functional area by the area of the orthographic projection of the food. The allowable deviation of the target overlap rate is ±1 percentage point.
[0225] After the specified wrapping time, open the package and remove the food. Within 60 seconds, fully unfold the paper-based packaging structure without wiping the back of the paper. Scan the paper with the back facing the scanning surface at 600 dpi and 8-bit grayscale. Obtain μ0 and σ0 from the same batch of paper that has not been in contact with the food. The grayscale value should be ≤μ0-3σ0 and the connected area should be ≥0.785 mm². 2 The rules are used to statistically analyze the total area of dark spots that show through the oil.
[0226] The percentage of condensation area was observed by photographing the food-contact side within 10 seconds of opening the package and removing the food. Calibration images were created using dry paper, water-wetted paper, corn oil-wetted paper, and tomato sauce-contaminated paper from the same batch as the test samples, respectively, for dry paper, water-wetted paper, oil-wetted paper, and sauce-contaminated paper. All four types of calibration images were acquired using the same camera, lens, shooting distance, exposure, 5500K illumination, and cross-polarization conditions as the test samples.
[0227] Convert the image to the CIELAB color space. For each pixel, extract the feature vector x. c =[L*, a*, b*, σ] L H L ] T Where L*, a*, and b* are the pixel parameters in the CIELAB color space; σ L H is the standard deviation of L* within a 5×5 pixel window centered on that pixel; L To quantize the L* within the window into 16 gray levels, a gray-level co-occurrence matrix is established with a pixel distance of 1 and directions of 0°, 45°, 90° and 135°, and the texture entropy is obtained by averaging the values of the four directions.
[0228] A four-class linear discriminant model with a shared covariance matrix is adopted. The mean vectors of the four classes of calibration pixels are denoted as μ. k The shared covariance matrix is denoted as Σ, and the prior probabilities for all four classes are all 0.25. The discrimination scores for each class are calculated using the following formula:
[0229] g k (x) c )=x c T Σ -1 μ k -0.5μ k T Σ -1 μ k +ln(0.25).
[0230] Calculate the posterior probabilities of each class according to the following formula: p k =exp[g k (x) c )] / ∑ j exp[gj (x) c )].
[0231] L* decreases by ≥8 relative to the average L* of the same batch of dry paper calibration images, and the posterior probability p of the wetness class. water ≥0.80 and connected area ≥1.0mm 2 Droplets and continuous wet areas are counted as condensation areas. Pixels identified as oily or sauce-contaminated are not included in the condensation area. The proportion of the projected area of the condensation area to the projected area of the food contact area is the percentage of the visible condensation area.
[0232] In each round of analysis, 20% of the calibration images are grouped and independently validated. The accuracy rate for water-wetting category identification should be ≥95%; if it is lower than 95%, calibration images are reacquired and the model is rebuilt. Linear discriminant calculation, connected component filtering, and area statistics are performed by running a macro script written according to the above formulas and decision parameters in ImageJ 1.54f.
[0233] The bottom bread texture retention rate was determined using a paired sample method, without repeated compression of the same piece of bread before and after wrapping. For each parallel test, two bottom breads from the same batch with a weight difference ≤1.0g and a thickness difference ≤0.5mm were selected. One was used as a control immediately at the start of wrapping, and the other was used for the actual wrapping. The texture analyzer used a 50mm diameter flat-bottomed cylindrical probe with a trigger force of 5g. The speeds were 1mm / s before testing, 1mm / s during testing, and 5mm / s after testing. The bread was compressed to 70% of its original thickness. The bottom bread texture retention rate was calculated by dividing the peak force after wrapping by the peak force before wrapping of the paired sample.
[0234] Food debris adhesion rate was measured by photographing the paper-based packaging structure after it was unfolded 180°. Calibration images were created using clean paper surfaces from the same batch of the test sample, bread crumbs or fried crust fragments from the corresponding food products, corn oil-soaked paper, and sauce-contaminated paper, respectively, for clean paper surfaces, food debris, oil-soaked paper, and sauce-contaminated paper. The calibration images were acquired using the same camera, lens, shooting distance, exposure, 5500K illumination, and cross-polarization conditions as the test samples.
[0235] For each pixel, extract the feature vector x. d =[L*, a*, b*, σ] L H L G Sobel ] T Where L*, a*, and b* are the pixel parameters in the CIELAB color space; σ L and H L Determined according to the classification method based on the proportion of visible condensation area; G SobelThis is the normalized average gradient magnitude calculated by the Sobel operator within a 5×5 pixel window centered on this pixel.
[0236] A four-class linear discriminant method with the same shared covariance matrix as the visible condensation area proportion was adopted, with the prior probabilities of all four classes set to 0.25. The posterior probability p of the debris class was obtained using the same discriminant function and posterior probability calculation method. crumb p crumb Pixels with a resolution of ≥0.80 are classified as debris recognition pixels. Condensation areas formed according to the visible condensation area ratio determination method, as well as pixels classified as oily or sauce-contaminated and their adjacent areas extending outward by 1 pixel, are not included in the debris connectivity statistics.
[0237] Eight-neighbor connectivity analysis was performed on the pixels used for debris recognition, and the connected areas were calculated to be ≥1.0 mm². 2 The total area of the connected regions of debris. The proportion of the total area of the connected regions of debris to the projected area of food contact is the food debris adhesion rate. In each round of analysis, 20% of the calibration images are reserved for independent verification according to the calibration image group. The accuracy of debris identification should be ≥95%; if it is lower than 95%, the calibration images are re-acquired and the model is rebuilt.
[0238] It can be seen that the proportion of condensation area, the bottom bread texture retention rate, and the food debris adhesion rate are used together to evaluate the degree of wetness, collapse, and surface damage of hamburger buns during the wrapping process, serving as evaluation indicators for the shape retention of hot hamburgers.
[0239] Oil stains at folds are defined as the number of independent oil spots on the back of the paper with an equivalent diameter ≥1.0mm located within a 10mm radius of the intersection of the actual fold or crease line after the package is unfolded. Oil spots that are in contact with each other and have a minimum connection width ≥0.5mm are counted as one oil spot. Paper integrity is defined as no delamination occurring after the paper-based packaging structure is unfolded, and no tears with a length ≥10mm or a single area ≥100mm². 2 The proportion of the effective area of adhesion to the total area of the paper-based packaging structure was calculated. All image analyses were performed using ImageJ 1.54f, and the analysts verified the analyses without knowing the sample numbers.
[0240] General conditions for food packaging.
[0241] Food packaging tests were conducted in an environment of 23±1℃ and RH 50±5%, with continuous recording using a temperature and humidity recorder. Beef patties were formed from ground beef with a fat content of 20±1%. The raw BP-100 patty weighed 105±2g, and the raw BP-90 patty weighed 95±2g. They were heated on a plate at 180±5℃ for 3 minutes on each side until the center temperature reached 75±2℃. After resting for 60 seconds, cooked beef patties weighing 100±2g and 90±2g were obtained, respectively. CP-140 fried chicken cutlets and CS-120 fried chicken strips were fried in corn oil at 175±3℃ until the center temperature reached 75±2℃. After draining the oil for 60 seconds, their weights were 140±3g and 120±3g, respectively, with an oil absorption rate controlled at 10±1%. GC-80 roasted chicken breast was heated on a plate at 180±5℃ until the center temperature reached 75±2℃ and then rested for 60 seconds.
[0242] Unless otherwise specified in Application Examples 7 and 8, before each wrapping, the paper-based packaging structure shall be placed on the folding template with the food contact side facing upwards, and the actual paper edge of the finished product and the boundary of the first functional area shall be aligned with the layout coordinates of the folding template. The coordinate lines on the folding template are used to indicate the coordinates of the predetermined fold lines, and it is not required that creases or printed fold lines be actually formed on the paper-based packaging structure.
[0243] Once the center of the bottom surface of the food reaches the temperature specified in the corresponding application example, it is transferred from the temperature measuring position to the paper-based packaging structure within 5 seconds, and the time from food placement to completion of packaging does not exceed 20 seconds.
[0244] When folding inwards on all four sides, fold the two sides along the predetermined folding line coordinates corresponding to 15mm outside the left and right edges of the food's orthographic projection. Then, fold sequentially along the predetermined folding line coordinates corresponding to 15mm outside the bottom and top edges of the food's orthographic projection, so that the top paper layer overlaps by 20±5mm. When folding inwards on both sides, fold the two sides along the position corresponding to 10mm outside the long side of the food, and make the top paper layer overlap by 25±5mm. The long roll is wrapped in the order of folding inwards on both sides, folding up at the bottom, and folding back at the top.
[0245] When fixation is required, peel off the release paper of the packaging fixation label, place the adhesive layer with the outside of the paper-based packaging structure, and attach it to the folded and overlapping area corresponding to the predetermined area coordinates of the packaging fixation label, and press it with a normal force of 20±2N for 2s.
[0246] In Application Examples 2-8, all packages were tested and included in the statistics according to their initial state after the operator first completed folding and labeling. Samples were not screened based on the food orthographic projection overlap rate, the amount of exposed cellulose to the edge, the state of the exposed end, or the state of external connection. Furthermore, the packages were not refolded, the labels were not moved, or the relative positions of the paper layers were not adjusted after the packaging was completed.
[0247] Application Examples 2-6 were completed by following the predetermined folding line coordinates, predetermined folding sequence, and predetermined area coordinates for the packaging label. Three independent packages were tested for each sample. Comparative examples without a continuous exposed cellulose pathway reaching the paper edge or without an exposed cellulose continuous phase were tested using the same food placement, folding position, folding sequence, fold overlap width, and labeling conditions. Application Examples 2-6 did not calculate the success rate of external connectivity to the edge.
[0248] Application Example 7 completes the wrapping by rotating the paper-based packaging structure in the specified direction, without changing the folding or label position based on the edge position. Application Example 8 does not provide a folding template with coordinate lines, food positioning marks, label positioning templates, or access status indicators. Application Examples 7 and 8 calculate the edge-to-external connectivity success rate and edge-to-edge closure failure rate for all completed packaging units.
[0249] After the specified settling time, two operators worked in parallel: within 5 seconds, they opened the package and removed the food, and within 10 seconds, they acquired images of the condensation on the food contact side; one operator removed the bottom bread from the package within 20 seconds and began texture testing within 30 seconds, while the other operator fully unfolded the paper-based packaging structure without wiping the back of the paper, and completed a back scan within 60 seconds, subsequently measuring the debris adhesion rate, oil penetration point at folds, and paper integrity rate. One parallel test for each sample corresponded to a set of independent food items and a paired control bread item before packaging.
[0250] A general preparation process for a partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure used for hot food hamburger wraps.
[0251] Step 1: Condition the fiber-based paper at 23±1℃ and RH 50±2% for 24 hours. Establish a layout coordinate system with the geometric center of the paper as the origin, the machine direction as the x-axis, and the transverse direction as the y-axis. Within this layout coordinate system, determine the outer contour of the paper-based packaging structure, the closed boundary of the first functional area, the second functional area, the PHA coverage area, the exposed cellulose continuous pathway, the continuous PHA oil-blocking boundary zone when present, the coordinates of the predetermined folding line, the folded area defined by the predetermined folding line coordinates, the coordinates of the predetermined folding overlap area, the coordinates of the predetermined area for fixing the packaging label, and the coordinates of the predetermined cutting line.
[0252] Unless otherwise specified, four straight, continuous exposed cellulose pathways are provided, leading to the top, right, bottom, and left edges of the paper, respectively. The centerlines of these four pathways coincide with the x-axis or y-axis, and extend from the outer boundary of the first functional area or the outer edge of the continuous PHA oil-blocking boundary zone to the corresponding predetermined cutting line coordinates. The four pathways pass through the upper, right, lower, and left folding areas defined by different predetermined folding line coordinates.
[0253] Unless otherwise specified, the coordinates of the predetermined fold line are set at a position 15mm outward from the outer edge of the orthographic projection of the hot food hamburger in the corresponding application example, and the overlap width of the top paper layer after folding is 20±5mm; the coordinates of the predetermined area of the packaging fixing label are located at the center of the coordinates of the predetermined fold overlap area and are adapted to the packaging fixing label with a diameter of 35mm.
[0254] The coordinates of the exposed cellulose continuous pathway, the predetermined fold line coordinates, the predetermined fold overlap area coordinates, the predetermined area coordinates of the packaging fixed label, and the predetermined cutting line coordinates are mapped according to the predetermined package pattern, so that at least two exposed cellulose edges formed by cutting are located in different fold areas and reach different paper edges.
[0255] Examples 11, 12, 12, and 13 are as follows: Figure 1 Based on the basic partitioning structure shown, and according to the respective pathway topologies described below, the branches are set to the edge branches and the blind-end branches that do not reach the paper edge. A 5.0 mm wide PHA closed area is maintained between the blind-end branches and the corresponding paper edge. By adjusting the internal blind-end compensation area connected to the maximum exposed cellulose connectivity region and the ordinary PHA coverage area, the four samples are made to have the same or the same control range of second functional area PHA coverage, cellulose exposure rate, maximum exposed cellulose connectivity region area ratio, and q2.
[0256] Step 2: Dilute the corresponding BIOTEN brand PHA aqueous dispersion with deionized water to the specified mass fraction. After stirring and filtration, feed it into the feed tank of the VCML Lab / Pilot Coater. Maintain the coating temperature at 25±1℃ and the feed circulation flow rate at 2.0±0.2L / min. According to ISO 2811-1:2023, determine the density of each diluted coating at 25℃ using a BYK-Gardner 1140 50mL certified ISO density cup, and control the density to 1.00±0.02g / cm³. 3 .
[0257] The VCML Lab / Pilot Coater's rotary screen coating module uses a 325-mesh nickel rotary screen with a screen thickness of 100±5μm and a photosensitive layer thickness of 30±3μm. The polyurethane squeegee has a Shore A hardness of 75±3, a squeegee angle of 30±2°, a loading pressure of 0.20±0.02MPa, and a gap between the rotary screen and the base paper of 0.10±0.02mm. The actual wet transfer coefficient of the rotary screen is calibrated to 0.85±0.03 based on the difference in wet mass before and after coating.
[0258] Local theoretical PHA unit area dry mass q PHA Calculate q according to the following formula: PHA =V×η×ρ×C×F.
[0259] Local theoretical total nonvolatile matter dry mass per unit area q NV Calculate q according to the following formula: NV =V×η×ρ×S×F.
[0260] Where V is the nominal mesh or cell volume of the corresponding solid area, dot, short line, grid, or boundary zone coating unit, η is the actual wet transfer coefficient, ρ is the coating density, C is the mass fraction of PHA in the coating, S is the total non-volatile matter mass fraction measured according to ISO 3251:2019, and F is the coverage of the corresponding pattern. The theoretical dry mass per unit area of polymeric stable components and other non-PHA non-volatile substances is calculated according to q. NV -q PHA calculate.
[0261] In this specification, q1, q2 and q t All figures refer to the dry mass of PHA per unit area, excluding polymer-type stable components. The dry mass of PHA per unit area in the test area and the PHA coverage in the second functional area are adjusted to meet specified values by adjusting V, the local pattern coverage, and the center distance of the ordinary pattern.
[0262] A patterned coating plate containing a high-coverage pattern in the first functional area, a normal PHA coverage pattern in the second functional area, and at least two continuous uncoated line patterns is used to allow the fiber-based paper to pass through the rotary screen coating module in one pass; when a continuous PHA oil-blocking boundary band is set, the patterned coating plate also includes a continuous wet coating band pattern.
[0263] A continuous wet coating strip is disposed in the inner periphery of the second functional area near the first functional area, connected to the wet coating layer in the first functional area and surrounding the first functional area. A continuous uncoated line extends continuously from the outer boundary of the first functional area or the outer edge of the continuous wet coating strip, passing through folded areas defined by different predetermined fold line coordinates and reaching different predetermined cutting line coordinates, to obtain patterned wet-coated fiber base paper.
[0264] The ordinary PHA covering pattern and the continuous wet coating strip in the second functional area together constitute the PHA covering area of the second functional area, and the planar projection area of the PHA covering area accounts for 15% to 60% of the planar projection area of the second functional area.
[0265] The standard layout of the dimensions in this specification is as follows: 20% dots are arranged in a square with a diameter of 0.50 mm and a center-to-center distance of 1.00 mm; 12% dots are arranged in a square with a diameter of 0.40 mm and a center-to-center distance of 1.02 mm; 10% dots are arranged in a square with a diameter of 0.40 mm and a center-to-center distance of 1.12 mm; 15% dots are arranged in a square with a diameter of 0.40 mm and a center-to-center distance of 0.92 mm; 5% dots are arranged in a square with a diameter of 0.20 mm and a center-to-center distance of 0.79 mm; 60% high-coverage dots are arranged in a square with a diameter of 0.80 mm and a center-to-center distance of 0.92 mm; 40% dots are arranged in a square with a diameter of 0.50 mm and a center-to-center distance of 0.70 mm.
[0266] 15% of the discontinuous short lines are line segments with a length of 1.00 mm and a width of 0.30 mm, arranged in the same direction as 2.00 mm × 1.00 mm rectangular units. 25% of the grid is an orthogonal grid with a line width of 0.27 mm and a pitch of 2.00 mm; 65% of the grid is an orthogonal grid with a line width of 0.41 mm and a pitch of 1.00 mm; 70% of the grid is an orthogonal grid with a line width of 0.45 mm and a pitch of 1.00 mm.
[0267] 95% of the high-coverage micro-dots consist of uncoated micropores with a diameter of 0.20 mm and a center-to-center distance of 0.79 mm set within a continuous solid area; 90% of the high-coverage micro-dots consist of uncoated micropores with a diameter of 0.30 mm and a center-to-center distance of 0.84 mm set within a continuous solid area; and 85% of the high-coverage micro-dots consist of uncoated micropores with a diameter of 0.30 mm and a center-to-center distance of 0.69 mm set within a continuous solid area. The area coverage rate of the map is calculated based on computer-aided design area and controlled within ±0.5 percentage points of the nominal value.
[0268] Step 3: The patterned wet-coated fiber base paper is fed into a continuous drying system that is compatible with the coating equipment.
[0269] Examples 1-8, Examples 11-12, and Comparative Examples 2-13 used the continuous drying module of VCML Lab / Pilot Coater. The paper was first pre-dried at a specified hot air temperature for 20±1s, with a hot air velocity of 2.0±0.2m / s and a nozzle-to-paper distance of 80±5mm, so that the residual moisture before entering the short-wave infrared drying module was ≤5% of the initial coating water content. Then, the paper was dried by the short-wave infrared drying module until it reached the coagulation temperature of the corresponding PHA particles and maintained for a specified time.
[0270] Examples 9 and 10 employ the EXPERTCOAT 1000 segmented hybrid continuous drying system. According to the effective length of the hot air zone, the set temperature of the hot air, the hot air speed, the distance from the nozzle to the paper surface, the paper web running speed, and the end high-energy drying conditions specified in the corresponding examples, the residual moisture before entering the end high-energy drying zone is ≤5% of the initial coating water content, and the paper surface reaches the specified peak temperature and is maintained for the specified time.
[0271] The initial quality of the transferred wet coating is determined based on the difference in wet weight before and after coating. A complete, repeating coating unit is used as the testing unit, and the quality of the wet coating transferred to this testing unit after coating is denoted as m. w The mass fraction of PHA in the coating is denoted as C, and the mass fraction of total nonvolatile matter measured according to ISO 3251:2019 is denoted as S. Then, the initial mass of PHA transferred to this detection unit is m. PHA,0 Initial non-volatile mass m NV,0 and initial coating water volume m water,0 Calculate m according to the following formulas respectively: PHA,0 =m w ×C;m NV,0 =m w ×S;m water,0 =m w ×(1-S).
[0272] Where C≤S, SC corresponds to the mass fraction of polymer-type stable components and other non-PHA non-volatile substances in the waterborne coating. The residual moisture ratio is calculated according to m water,r / m water,0 Calculated by multiplying by 100%, where m water,r This refers to the residual moisture in the paper web before it enters the final high-energy drying zone.
[0273] In Examples 9 and 10, HPIR-R reflective high-performance infrared moisture sensors were used to measure the residual moisture content of the paper web online before it entered the high-energy drying zone. Measurement tracks were formed at the center of the left, middle, and right coating channels, respectively. Online data was collected at a frequency of 100Hz, and the 1-second moving average was used as the residual moisture measurement value at the corresponding time.
[0274] For each industrial coating batch, three recording intervals were obtained at 5 min, 15 min, and 25 min after the start of stable operation, with each recording interval lasting 60 s.
[0275] The online moisture sensor is calibrated offline by gravimetric method after each change of base paper batch, PHA water-based coating batch, or major drying parameters. During calibration, the paper web speed is reduced to 30 m / min, and a complete repeat coating unit is cut from each of the left, middle, and right coating channels, and placed in a pre-weighed aluminum-plastic composite bag and sealed within 2 seconds. After weighing the wet sample, the sample is placed in a forced-air drying oven at 105±2℃ and dried to constant weight. The difference between the wet sample mass and the constant-weight sample mass is the residual moisture content (m). water,r And calculate the residual moisture ratio according to the following formula: Residual moisture ratio = m water,r / m water,0 ×100%.
[0276] The online moisture sensor output value was corrected using offline gravimetric measurements, and the correlation coefficient R of the calibration curve was calculated. 2The residual moisture content should be ≥0.995, and the relative deviation between online and offline measurements should be ≤5%. During high-speed operation, the average value of the online measurements from the left, middle, and right coating lanes is used as the residual moisture result. When the residual moisture content is ≤5%, the paper web is considered to have reached the moisture requirement for entering the final high-energy drying zone.
[0277] Step 3: The patterned wet-coated fiber base paper is fed into a continuous drying system. The lateral leveling of the wet coating and the agglomeration of PHA particles are controlled so that the first functional area forms a continuous PHA barrier phase, the second functional area forms a PHA covered area and an exposed continuous cellulose phase, and the continuous uncoated line remains continuous between the starting boundary of the passage and the corresponding predetermined cutting line coordinates.
[0278] When setting up a continuous wet coating strip, the continuous wet coating strip is dried to form a continuous PHA oil-blocking boundary strip that is connected to and surrounds the first functional area (PHA). The continuous PHA oil-blocking boundary strip constitutes part of the PHA coverage area of the second functional area, and its outer edge forms the inner boundary of the passage.
[0279] Step 4: Cut the patterned dry fiber base paper according to the predetermined cutting line coordinates that are fixedly aligned with the patterned coating plate and the predetermined folding line coordinates, so that at least two continuous exposed cellulose pathways pass through different folding areas and reach different paper edges, forming exposed cellulose at the edge ends of the corresponding paper edges.
[0280] Examples 1-12 and Comparative Examples 2-13 each prepared three independent coating batches, with at least 100 finished sheets produced continuously from each batch; Comparative Example 1 and the uncoated base paper control were sampled from the three independent base paper batches; Comparative Example 14 extracted paper-based packaging structures from the three coating batches of Example 1, without preparing separate material batches. At least five finished sheets were extracted from the starting section, middle section, and ending section of each coating batch to verify the layout size, dry mass per unit area of the PHA region, PHA coverage of the second functional area, C1, C2, number of exposed cellulose to the edge, number of different folded areas traversed by the pathway, number of different paper edges reached by the pathway, minimum effective width of continuous pathways, and cutting registration deviation.
[0281] When the finished product satisfies C1≥70%, the second functional region simultaneously contains a PHA-covered area and C2≥30% exposed cellulose continuous phase, and at least two exposed cellulose continuous pathways in the maximum exposed cellulose connectivity domain pass through different folded areas and reach different paper edges, the finished product is determined to form a partitioned exhaust and oil-blocking conformal planar structure. The PHA coverage rate and spatial concentration coefficient K of the second functional region are recorded as PHA material spatial distribution parameters; the PHA coverage rate of the second functional region is 15%~60% and K≥1.20 are respectively used as control ranges in some implementation methods, and are not used as independent judgment conditions that deviate from C1, C2 and pathway topology.
[0282] The finished product forming the planar structure is further verified by physical folding and labeling. Folding is performed according to the position corresponding to the predetermined folding line coordinates, and a packaging fixing label is set at the position corresponding to the predetermined area coordinates of the packaging fixing label; when at least one exposed cellulose to the edge forms a visible exposed area on the outer surface of the packaging body that is outside the coverage of other paper layers and the packaging fixing label and is connected to the outside of the packaging body, the packaging body is determined to meet the requirements for folding and use.
[0283] Example
[0284] Unless otherwise stated, the upper folded area, right folded area, lower folded area, and left folded area in the following embodiments and comparative examples all refer to the paper base area defined by the predetermined fold line coordinates in the predetermined packaging pattern. The predetermined fold line coordinates, predetermined cutting line coordinates, predetermined fold overlap area coordinates, and predetermined area coordinates for the packaging fixed label are all layout design coordinates, and it is not required that the food contact side of the paper base packaging structure form indentations, printed fold lines, or other physical fold lines. When positioning marks are set on the finished product, the positioning marks are set on the outer surface opposite to the food contact side or on the process waste edge removed during cutting; when no positioning marks are set, the geometric center of the finished product is used as the coordinate origin, and the actual paper edge of the finished product, the high-coverage pattern of the first functional area, and the PHA coating pattern are translated, rotated, and proportionally registered to restore the layout coordinates.
[0285] Example 1: Using a quantitative method of 40 g / m 2 The food-contact grade bleached kraft paper has a finished size of 300mm × 300mm. The first functional area is a centered 180mm × 180mm square, which accounts for 36% of the effective area of the food contact side. The first functional area uses 100% solid wood.
[0286] The second functional area uses a 20% dot pattern and features four continuous exposed cellulose pathways that extend along the x and y axes to the four paper edges, with a minimum effective width of 4.0 mm. These four continuous exposed cellulose pathways pass through the upper, right, lower, and left folded areas, respectively, and reach the upper, right, lower, and left paper edges.
[0287] The nominal mesh volume of the first functional area of the round wire mesh is 35.3 cm³. 3 / m 2 The nominal mesh volume of the second functional area is 8.8 cm³. 3 / m 2 The PHBV waterborne coating has a PHBV mass fraction of 20%, an apparent viscosity of 185 mPa·s at 25℃, and is applied by rotary screen coating at a speed of 10 m / min.
[0288] The first functional zone q1 is 6.0 g / m2 The second functional area q2 is 0.30 g / m 2 q t 2.352 g / m 2 K is 2.55. After pre-drying with hot air at 90℃ for 20s, the peak temperature of the paper surface reaches 160℃ and is maintained for 2s.
[0289] The finished product has a PHA film coverage rate (F1) of 95% in the first functional zone, a maximum connected domain ratio (R1) of 98% within the PHA phase, and a C1 ratio of 93.1%. In the second functional zone, the PHA coverage rate is 30%, the cellulose exposure rate (E2) is 70%, and the maximum connected domain ratio (R2) within the exposed cellulose phase is 96% and a C2 ratio of 67.2%. No continuous PHA oil-blocking boundary zone was established.
[0290] Example 2: Using 35g / m 2 Food-grade bleached kraft paper, finished size 300mm×300mm. The first functional area is a centered 180mm×150mm rectangle, the area of which accounts for 30% of the effective area of the food contact side, and the first functional area uses 100% solid wood.
[0291] The second functional area uses 15% discontinuous short lines and is equipped with four continuous exposed cellulose pathways that reach the four paper edges along the x and y axes, with a minimum effective width of 4.0 mm. The four pathways pass through the upper, right, lower, and left folded areas and reach the corresponding paper edges.
[0292] The nominal mesh volume of the first functional area of the round wire mesh is 32.4 cm³. 3 / m 2 The nominal mesh volume of the short line in the second functional area is 9.8 cm³. 3 / m 2 The P34HB waterborne coating has a P34HB mass fraction of 20%, an apparent viscosity of 160 mPa·s at 25℃, and is applied by rotary screen coating at a speed of 12 m / min.
[0293] The first functional zone q1 is 5.5g / m 2 The second functional region q2 is 0.25 g / m 2 q t It is 1.825 g / m 2 K is 3.01. After pre-drying with hot air at 85℃ for 20 seconds, the peak temperature of the paper surface reaches 155℃ and is maintained for 2 seconds.
[0294] The finished product F1 is 97%, R1 is 99%, and C1 is 96.0%; the second functional area PHA coverage is 25%, E2 is 75%, R2 is 97%, and C2 is 72.8%. No continuous PHA oil-blocking boundary zone was set.
[0295] Example 3: Using 45g / m2 Food-grade bleached kraft paper, finished size 300mm×300mm. The first functional area is a centered 180mm×200mm rectangle, accounting for 40% of the effective area of the food contact side, and the first functional area uses 95% high-coverage micro-dots.
[0296] The second functional area uses a 25% grid and features four continuous exposed cellulose pathways that extend along the x and y axes to the four paper edges, with a minimum effective width of 3.0 mm. These four pathways pass through four different folded areas and reach four different paper edges.
[0297] The nominal mesh volume of the first functional area of the round wire mesh is 34.4 cm³. 3 / m 2 The nominal mesh volume of the second functional area is 9.2 cm³. 3 / m 2 The PHBH waterborne coating has a PHBH mass fraction of 18%, an apparent viscosity of 140 mPa·s at 25℃, and is applied by rotary screen coating at a speed of 10 m / min.
[0298] The first functional area q1 is 5.0 g / m 2 The second functional area q2 is 0.35 g / m 2 q t It is 2.210 g / m 2 K is 2.26. After pre-drying with hot air at 85℃ for 20s, the peak temperature of the paper surface reaches 140℃ and is maintained for 2s.
[0299] The finished product F1 coverage is 94%, R1 is 96%, and C1 is 90.2%; the second functional area PHA coverage is 32%, E2 is 68%, R2 is 92%, and C2 is 62.6%. No continuous PHA oil-blocking boundary zone was set.
[0300] Example 4: Using 50g / m 2 Food-grade bleached kraft paper, finished size 300mm×300mm. The first functional area is a centered 150mm×150mm square, accounting for 25% of the effective area of the food contact side, and uses 100% solid wood.
[0301] The second functional area uses 10% dots and is equipped with four continuous exposed cellulose pathways that reach the four paper edges along the x and y axes, with a minimum effective width of 5.0 mm. The four pathways pass through four different folded areas and reach four different paper edges.
[0302] The nominal mesh volume of the first functional area of the round wire mesh is 40.1 cm³. 3 / m 2 The nominal mesh volume of the second functional area is 10.7 cm³. 3 / m 2 The PHB waterborne coating has a PHB mass fraction of 22% and an apparent viscosity of 210 mPa·s at 25℃. It is applied by rotary screen coating at a speed of 8 m / min.
[0303] The first functional zone q1 is 7.5g / m 2 The second functional region q2 is 0.20 g / m 2 q t It is 2.025 g / m 2 K is 3.70. After pre-drying with hot air at 100℃ for 20 seconds, the peak temperature of the paper surface reaches 180℃ and is maintained for 1 second.
[0304] The finished product F1 coverage is 96%, R1 is 99%, and C1 is 95.0%; the second functional area PHA coverage is 22%, E2 is 78%, R2 is 98%, and C2 is 76.4%. No continuous PHA oil-blocking boundary zone was set.
[0305] Example 5: PHBV aqueous dispersion and P34HB aqueous dispersion were mixed at a PHA dry solids mass ratio of 1:1, and the total PHA mass fraction was adjusted to 20% with deionized water. The apparent viscosity at 25°C was 175 mPa·s.
[0306] Using 40g / m 2 Food-contact grade bleached kraft paper, finished size 300mm×300mm, with the first functional area accounting for 36% of the effective area of the food contact side, and the pattern is the same as in Example 1. The second functional area uses 20% dots and has four exposed cellulose continuous pathways with a minimum effective width of 4.0mm, passing through four different folding areas and reaching four different paper edges.
[0307] The nominal mesh volume of the first functional area of the round wire mesh is 32.4 cm³. 3 / m 2 The nominal mesh volume of the second functional area is 11.8 cm³. 3 / m 2 Rotary screen coating was performed at a speed of 10 m / min, with the first functional zone q1 being 5.5 g / m. 2 The second functional area q2 is 0.40 g / m 2 q t It is 2.236 g / m 2 K is 2.46.
[0308] After pre-drying with hot air at 85℃ for 20 seconds, the peak temperature of the paper surface reaches 155℃ and is maintained for 2 seconds. The finished product has an F1 content of 96%, an R1 content of 98%, and a C1 content of 94.1%; the PHA coverage rate in the second functional area is 34%, E2 is 66%, R2 is 94%, and C2 is 62.0%. No continuous PHA oil-blocking boundary zone was set.
[0309] Example 6: Using 30g / m 2 Food contact grade bleached kraft paper, finished size 300mm×300mm, the first functional area is a centered 180mm×180mm square, the area accounts for 36% of the effective area of the food contact side.
[0310] The first functional area uses a 100% solid color, while the second functional area uses 12% dots. Four continuous exposed cellulose pathways, each with a minimum effective width of 2.0 mm, are set along the x and y axes, reaching the four paper edges respectively. The inner periphery of the second functional area near the first functional area has a width of 2.0 mm and an area of 1456 mm². 2 Furthermore, a continuous PHA oil-blocking boundary zone is connected to the first functional area PHA continuous barrier, and the continuous PHA oil-blocking boundary zone is in the form of a closed loop.
[0311] The nominal mesh volume of both the first functional zone and the boundary zone of the round wire mesh is 28.2 cm³. 3 / m 2 The nominal mesh volume of the ordinary dots in the second functional area is 4.0 cm³. 3 / m 2 The P34HB waterborne coating has a P34HB mass fraction of 20%, an apparent viscosity of 150 mPa·s at 25℃, and is applied by rotary screen coating at a speed of 15 m / min.
[0312] The first functional zone q1 is 4.8 g / m 2 The second functional region q2 is 0.20 g / m 2 q2 is the area-weighted average value including the boundary zone, the ordinary dotted region, and the exposed cellulose continuous pathway region. t It is 1.856 g / m 2 K is 2.59.
[0313] After pre-drying with hot air at 80℃ for 20 seconds, the peak temperature of the paper surface reaches 155℃ and is maintained for 2 seconds. The finished product has a F1 content of 93%, R1 content of 95%, and C1 content of 88.4%; the coverage rate of the second functional area PHA is 18%, E2 content of 82%, R2 content of 98%, and C2 content of 80.4%.
[0314] Example 7: Using 60g / m 2 Food-grade bleached kraft paper, finished size 300mm×300mm. The first functional area is a centered 225mm×240mm rectangle, accounting for 60% of the effective area of the food contact side, and the first functional area uses 90% high-coverage micro-dots.
[0315] The second functional area features 60% high-coverage dots and four continuous exposed cellulose pathways extending along the x and y axes to the four paper edges, with a minimum effective width of 1.0 mm. These four pathways pass through four different folded areas and reach four different paper edges.
[0316] The nominal mesh volume of the first functional area of the round wire mesh is 19.6 cm³. 3 / m 2 The nominal mesh volume of the second functional area is 17.2 cm³. 3 / m 2 The P34HB waterborne coating has a P34HB mass fraction of 20%, an apparent viscosity of 170 mPa·s at 25℃, and is applied by rotary screen coating at a speed of 12 m / min.
[0317] The first functional zone q1 is 3.0 g / m 2 The second functional area q2 is 1.75 g / m 2 q t 2.500g / m 2 K is 1.20. After pre-drying with hot air at 85℃ for 20 seconds, the peak temperature of the paper surface reaches 155℃ and is maintained for 2 seconds.
[0318] The finished product coverage is 90% for F1, 90% for R1, and 81.0% for C1; the second functional area has a PHA coverage of 58%, E2 of 42%, R2 of 80%, and C2 of 33.6%. No continuous PHA oil-blocking boundary zone was set.
[0319] Example 8: Using 40g / m 2 Food-grade bleached kraft paper, finished size 280mm×280mm. The first functional area is a centered 120mm×98mm rectangle, the area of which accounts for 15.00% of the effective area of the food contact side, and the first functional area uses 100% solid paper.
[0320] The second functional area uses 15% dots and is equipped with four continuous exposed cellulose pathways that extend along the x and y axes to the four paper edges, with a minimum effective width of 6.0 mm. The four pathways pass through four different folded areas and reach four different paper edges.
[0321] The nominal mesh volume of the first functional area of the round wire mesh is 47.1 cm³. 3 / m 2 The nominal mesh volume of the second functional area is 11.8 cm³. 3 / m 2 The P34HB waterborne coating has a P34HB mass fraction of 20%, an apparent viscosity of 165 mPa·s at 25℃, and is applied by rotary screen coating at a speed of 10 m / min.
[0322] The first functional zone q1 is 8.0 g / m2 The second functional area q2 is 0.30 g / m 2 q t It is 1.455 g / m 2 K is 5.50. After pre-drying with hot air at 90℃ for 20 seconds, the peak temperature of the paper surface reaches 155℃ and is maintained for 3 seconds.
[0323] The finished product F1 is 98%, R1 is 98%, and C1 is 96.0%; the second functional area PHA coverage is 20%, E2 is 80%, R2 is 95%, and C2 is 76.0%. No continuous PHA oil-blocking boundary zone was set.
[0324] Example 9: Using the P34HB pattern from Example 2, a pattern with a width of 1000mm and a basis weight of 35g / m² was prepared. 2 The food contact grade bleached kraft paper is divided into 3 coating channels with an effective width of 300mm, with 50mm of cutting waste left on each side, and the repeating length in the machine direction is 300mm.
[0325] Each repeated coating unit simultaneously features a solid pattern in the first functional area, a discontinuous short line pattern in the second functional area, and four continuous uncoated lines. After coating, each repeated coating unit is cut into 300mm × 300mm finished products according to the predetermined cutting line coordinates that are fixedly aligned with the coating pattern and the predetermined fold line coordinates. This allows the four continuous uncoated lines to form continuous exposed cellulose pathways that pass through four different folding areas and reach four different paper edges.
[0326] The coating was performed using an EXPERTCOAT 1000 machine equipped with a direct gravure coating unit and a segmented hybrid continuous drying system. The P34HB waterborne coating was obtained by diluting BIOTEN 1032 with deionized water, with a P34HB mass fraction of 20.0±0.2%, a total non-volatile matter mass fraction of 20.6±0.3%, and an apparent viscosity of 180 mPa·s at 25°C. The waterborne coating was filtered through a 100 μm filter before being fed into the feed circulation system at a flow rate of 25±2 L / min and a paper web running speed of 150 m / min.
[0327] The nominal cell volume of the solid area in the first functional zone of the intaglio printing is 34.4 cm³. 3 / m 2 The nominal cell volume of the 15% discontinuous short line pattern in the second functional area is 10.4 cm³. 3 / m 2 The doctor blade angle is 55±2°, the loading pressure is 0.18±0.02MPa, the paper web tension is 60±5N / m, and the actual wet transfer coefficient is 0.80±0.03.
[0328] In Example 9, three independent industrial coating batches were performed. Each batch was run continuously for 30 minutes after the speed increase and process parameters stabilized. The average paper web speeds recorded by the main drive encoder during the stable operating range of the three batches were 149.8±0.5 m / min, 150.1±0.6 m / min, and 150.0±0.5 m / min, respectively.
[0329] The segmented hybrid continuous drying system consists of a first hot air drying zone, a second hot air drying zone, a third hot air drying zone, and a final high-energy drying zone, arranged sequentially along the paper web's running direction. The effective length of each of the three hot air drying zones is 12.0 m, with set hot air temperatures of 100±3℃, 120±3℃, and 140±3℃ respectively, a hot air velocity of 18±2 m / s for all zones, and a nozzle-to-paper surface distance of 80±5 mm for all zones. The effective length of the final high-energy drying zone is 6.0 m, with a set hot air temperature of 175±3℃, a hot air velocity of 20±2 m / s, a nozzle-to-paper surface distance of 70±5 mm, and a surface power density of 38±3 kW / m². 2 Short-wave infrared radiation-assisted heating.
[0330] With the inlet of the first hot air drying zone as the paper web running direction position 0m, the average temperature curves of the food contact side of the paper surface constructed during the stable operation of three batches are as follows: 0m 25℃, 12m 71℃, 24m 92℃, 36m 110℃, 36.5m 137℃, 37.0m 150℃, 38.0m 153℃, 39.0m 155℃, 40.0m 155℃, 41.0m 153℃, and 42.0m 150℃.
[0331] The peak paper surface temperatures of the three batches were 154.8℃, 155.2℃, and 155.0℃, respectively. Based on the data from fixed temperature measurement points, the temperature changes between adjacent temperature measurement points, and the synchronous linear velocity data, the times for the paper surface temperature to remain ≥150℃ were calculated to be 2.00s, 2.04s, and 1.98s, respectively. All of these meet the control conditions of a peak paper surface temperature of 155±3℃ and a paper surface temperature maintained at ≥150℃ for 2.0±0.2s.
[0332] Based on the effective area of the food contact side, the average wet coating transfer amount is 9.125 g / m². 2 The initial coating water content was 7.25 ± 0.15 g / m². 2 The average residual moisture content of the three batches before entering the final high-energy drying zone was 0.31 g / m³. 2 0.33g / m 2 and 0.31g / m 2 These accounted for 4.3%, 4.6%, and 4.3% of the initial coating water, respectively.
[0333] The total effective length of the three hot air drying zones and the final high-energy drying zone is 42.0 m. Based on the actual average linear velocity of the three batches, the total residence time of the paper web in the continuous drying system is 16.82 s, 16.79 s, and 16.80 s, respectively. After leaving the final high-energy drying zone, the paper web is cooled by cooling rollers at a temperature of 20 ± 2 ℃. The paper surface temperature before winding for all three batches is 32 ± 3 ℃ and does not exceed 35 ℃.
[0334] The first functional zone q1 is 5.5g / m 2 The second functional region q2 is 0.25 g / m 2 q t It is 1.825 g / m 2 K is 3.01. The finished product F1 is 97%, R1 is 99%, and C1 is 96.0%; the second functional area PHA coverage is 25%, E2 is 75%, R2 is 97%, and C2 is 72.8%. No continuous PHA oil-blocking boundary zone was set.
[0335] Fixed infrared temperature data and online residual moisture data are acquired at a frequency of 100Hz, while the main drive encoder linear speed data is acquired at a frequency of 10Hz.
[0336] Example 10: Using a quantitative method of 35 g / m 2 The food contact grade bleached kraft paper has three coating channels with an effective width of 280mm on a paper width of 1000mm, with 80mm cutting waste edges retained on both the left and right sides, and the repeating plate length in the machine direction is 280mm.
[0337] Each repeat coating unit is cut into 280mm × 280mm finished products according to predetermined cutting line coordinates. The first functional area is a centered 120mm × 98mm rectangle, which occupies 15% of the effective area on the food contact side and uses a 100% solid pattern. The second functional area is set with a 15% dot pattern and four continuous uncoated lines extending along the x-axis and y-axis, reaching different predetermined cutting line coordinates, with a minimum effective width of 6.0mm.
[0338] Four continuous uncoated lines pass through four folded areas defined by different predetermined fold line coordinates, and after cutting, they form continuous exposed cellulose pathways that reach four different paper edges.
[0339] The coating was applied using an EXPERTCOAT1000 machine equipped with a high-volume direct gravure coating unit and a segmented hybrid continuous drying system. The P34HB waterborne coating was obtained by diluting BIOTEN 1032 with deionized water, with a P34HB mass fraction of 20.0±0.2%, a total non-volatile matter mass fraction of 20.6±0.3%, and an apparent viscosity of 180 mPa·s at 25°C. The waterborne coating was filtered through a 100 μm filter before being fed into the feed circulation system at a flow rate of 40±3 L / min and a paper web running speed of 500 m / min.
[0340] The nominal pit volume of the first functional area is 53.3 cm³. 3 / m 2 The nominal cavity volume of the dotted pattern in the second functional area is 7.0 cm³. 3 / m 2 The doctor blade angle is 55±2°, the loading pressure is 0.20±0.02MPa, the paper web tension is 75±5N / m, and the actual wet transfer coefficient is 0.75±0.03.
[0341] In Example 10, three independent industrial coating batches were performed. Each batch was run continuously for 30 minutes after the speed increase and process parameters stabilized. The average paper web speeds recorded by the main drive encoder during the stable operating range of the three batches were 499.6±1.4 m / min, 500.4±1.6 m / min, and 500.1±1.5 m / min, respectively.
[0342] The segmented hybrid continuous drying system consists of six hot air drying zones and one end high-energy drying zone arranged sequentially along the paper web's running direction. The six hot air drying zones each have an effective length of 12.0 m, with set hot air temperatures of 100±3℃, 115±3℃, 130±3℃, 140±3℃, 150±3℃, and 160±3℃ respectively, a hot air velocity of 22±2 m / s, and a nozzle-to-paper surface distance of 60±5 mm. The end high-energy drying zone has an effective length of 28.0 m, a set hot air temperature of 185±3℃, a hot air velocity of 25±2 m / s, a nozzle-to-paper surface distance of 60±5 mm, and uses a surface power density of 55±5 kW / m². 2 Short-wave infrared radiation-assisted heating.
[0343] With the inlet of the first hot air drying zone as the paper web running direction position 0m, the average temperature curves of the food contact side of the paper surface constructed during the stable operation of three batches are as follows: 0m 25℃, 12m 56℃, 24m 73℃, 36m 88℃, 48m 101℃, 60m 112℃, 72m 120℃, 73m 138℃, 74m 147℃, 75m 150℃, 80m 153℃, 86m 155℃, 94m 154℃, and 100m 150℃.
[0344] The peak paper surface temperatures of the three batches were 154.8℃, 155.2℃, and 155.1℃, respectively. Based on data from fixed temperature measurement points, temperature changes between adjacent measurement points, and synchronous linear velocity data, the times for the paper surface temperature to remain ≥150℃ were calculated to be 3.00s, 3.04s, and 2.98s, respectively. These all meet the control conditions of a peak paper surface temperature of 155±3℃ and a continuous paper surface temperature ≥150℃ for 3.0±0.2s. The paper surface temperature reaches 150℃ 3.0m after the entrance of the high-energy drying zone at the end, and the effective length for continuous ≥150℃ is 25.0m.
[0345] Based on the effective area of the food contact side, the average wet coating transfer amount is 6.665 g / m². 2 The initial coating water content was 5.29 ± 0.12 g / m². 2 The average residual moisture content of the three batches before entering the final high-energy drying zone was 0.22 g / m³. 2 0.23g / m 2 and 0.21g / m 2 These accounted for 4.2%, 4.3%, and 4.0% of the initial coating water, respectively.
[0346] The total effective length of the six hot air drying zones and the final high-energy drying zone is 100.0 m. Based on the actual average linear velocity of the three batches, the total residence time of the paper web in the continuous drying system is 12.01 s, 11.99 s, and 12.00 s, respectively. After leaving the final high-energy drying zone, the paper web is cooled by cooling rollers at a temperature of 15 ± 2 ℃. The paper surface temperature before winding for all three batches is 30 ± 3 ℃ and does not exceed 35 ℃.
[0347] The first functional zone q1 is 8.0 g / m 2 The second functional region q2 is 0.157 g / m 2 q t It is 1.333 g / m 2 K is 6.00. Finished product F1 is 98%, R1 is 98%, and C1 is 96.0%; the second functional area PHA coverage is 20%, E2 is 80%, R2 is 95%, and C2 is 76.0%. No continuous PHA oil-blocking boundary zone was set.
[0348] Fixed infrared temperature data and online residual moisture data are acquired at a frequency of 100Hz, while the main drive encoder linear speed data is acquired at a frequency of 10Hz.
[0349] Example 11: The same base paper, first functional area, PHBV waterborne coating, coating equipment, and drying conditions as in Example 1 were used. The PHBV mass fraction in the PHBV waterborne coating was 20.0 ± 0.2%, and the total non-volatile matter mass fraction was 20.6 ± 0.3%. Except for the pathway topology, blind-end branches, and matching compensation area in the second functional area, the remaining layout parameters were the same as in Example 1.
[0350] The second functional area adopts a pathway topology matching composite layout with a PHA planar projection area coverage of 30.0±0.5%. The maximum exposed cellulose connectivity domain is set with four branches with a minimum effective width of 4.0 mm. The upper and right branches pass through the upper and right folded areas defined by the corresponding predetermined fold line coordinates, and reach the upper and right paper edges, respectively; the lower and left branches terminate at positions 5.0 mm from the lower and left paper edges, respectively, and are separated from the corresponding paper edges by the PHA closed area, forming two blind-end branches.
[0351] By adjusting the blind-end compensation area connected to the maximum exposed cellulose connectivity region and the ordinary PHA coverage area, the PHA coverage area, total cellulose exposure area, maximum exposed cellulose connectivity region area, and q2 of the second functional area are made to be within the same control range as in Examples 12, 12, and 13. No continuous PHA oil-blocking boundary zone was set.
[0352] The first functional zone q1 is 6.02 g / m 2 The second functional area q2 is 0.30 g / m 2 q t It is 2.359 g / m 2 K is 2.55. F1 is 95.0%, R1 is 98.0%, and C1 is 93.1%; the coverage of the second functional area PHA is 30.0%, E2 is 70.0%, R2 is 96.0%, and C2 is 67.2%. The maximum exposed cellulose connected domain forms two exposed cellulose ends, which pass through different folding areas and reach the top and right edges of the paper, respectively.
[0353] Example 12: Using the same base paper, first functional area, PHBV waterborne coating, coating equipment, drying conditions, second functional area PHA coverage area, total cellulose exposed area, and maximum exposed cellulose connected domain area as in Example 11.
[0354] The second functional area has four branches with a minimum effective width of 4.0 mm, each representing the maximum exposed cellulose connectivity. These four branches extend outward from the upper, right, lower, and left boundaries of the first functional area, passing through the upper, right, lower, and left folded areas defined by different predetermined folding line coordinates, and reaching the upper, right, lower, and left paper edges, respectively. By adjusting the compensation area and PHA coverage area within the second functional area, the PHA coverage rate, E2, R2, C2, and q2 of the second functional area are made to be within the same control range as in Examples 11, 12, and 13. No continuous PHA oil-blocking boundary zone was established.
[0355] The first functional zone q1 is 5.99 g / m 2 The second functional area q2 is 0.30 g / m 2 q t It is 2.348 g / m 2 K is 2.55. F1 is 95.0%, R1 is 98.0%, and C1 is 93.1%; the coverage of the second functional area PHA is 30.0%, E2 is 70.0%, R2 is 96.0%, and C2 is 67.2%. The maximum exposed cellulose connected domain forms four exposed cellulose to the edge ends, and the four ends pass through four different folding areas and reach four different paper edges.
[0356] According to the aforementioned structural determination method, in Examples 1-12, C1 is 81.0%-96.0%, C2 is 33.6%-80.4%, the area ratio of the first functional region is 15%-60%, and q1 is 3.0-8.0 g / m². 2 q2 is 0.157~1.75g / m 2 K ranges from 1.20 to 6.00, and the measured PHA coverage rate in the second functional area is 18% to 58%.
[0357] Examples 1-10 and Example 12 each form four continuous exposed cellulose pathways that pass through four different folding regions and reach four different paper edges; Example 11 forms two continuous exposed cellulose pathways that pass through two different folding regions and reach two different paper edges. The minimum effective width of the continuous pathway in each complete example is 1.0-6.0 mm.
[0358] Comparative Example 1: Using the same 40 g / m³ as in Example 1 2 Food-grade bleached kraft paper, without PHA application, was directly cut to 300mm × 300mm pieces. The total dry mass of PHA in this sample was 0, and no continuous PHA barrier phase was formed in the first functional region; the cellulose exposure rate on the food contact side was 100%, and the proportion of the largest connected domain within the exposed cellulose phase was 100%. Due to q t If the value is 0, K is not applicable. This sample is used to evaluate the performance without a PHA barrier structure.
[0359] Comparative Example 2: Using the same base paper and PHBV water-based coating as Example 1, a 90% high-coverage micro-dot pattern was used to uniformly cover the entire food contact side. The nominal mesh volume of the cylinder screen was 15.4 cm³. 3 / m 2 The coating was applied at a speed of 10 m / min, and pre-dried at 90°C for 20 s and held at a peak temperature of 160°C for 2 s as described in Example 1, resulting in an average dry coating weight of 2.352 g / m² across the entire width of the PHBV coating. 2 Furthermore, the total dry weight of PHA was the same as in Example 1. When sampling was performed at the central and peripheral regions as in Example 1, both q1 and q2 were 2.352 g / m³. 2 q t 2.352 g / m 2 K is 1.00. The PHA coverage on the contact side of the finished food is 90%, and the proportion of the largest connected domain within the PHA phase is 92%; the cellulose exposure rate is 10%, and the proportion of the largest connected domain within the exposed cellulose phase is 20%. The finished product does not form a continuous pathway consisting of the exposed cellulose continuous phase in the second functional area, which passes through different folding regions to different paper edges. This sample is used to evaluate the effect of uniform distribution of the same total PHA and the lack of a planar partitioned continuous network.
[0360] Comparative Example 3: Except for the coating pattern, the same 40 g / m² coating was used as in Example 1. 2 The processing conditions were as follows: food contact grade bleached kraft paper, PHBV water-based coating, 300mm×300mm finished size, rotary screen coating equipment, coating speed of 10m / min, 90℃ hot air pre-drying for 20s, and maintaining a peak paper surface temperature of 160℃ for 2s. A full-width 40% dot pattern was used, with a 4.0mm wide uncoated path at the x and y axis positions. The area outside the uncoated path was filled with square dots with a diameter of 0.50mm and a center-to-center distance of 0.69mm, resulting in a dot coverage of 41.1% for this area, while maintaining the full-width area coverage calculated according to the computer-aided design (CAD) layout at 40%.
[0361] The four uncoated pathways pass through four different folded areas and reach four different paper edges. The nominal mesh volume of the dotted area is 34.6 cm³. 3 / m 2 The average dry coating weight of PHA on the whole paper is 2.352 g / m². 2 .
[0362] When sampling from the nominal central and peripheral regions, both q1 and q2 are 2.352 g / m². 2K is 1.00. The PHA film coverage in the central nominal region is 40%, and the proportion of the largest connected domain within the PHA phase is 15%, with no continuous PHA barrier phase formed. This sample is used to evaluate the impact of having multi-directional edge-to-edge pathways but with PHA fully dispersed and no continuous barrier phase formed in the central region.
[0363] Comparative Example 4: Using the same 40 g / m³ as in Example 1 2 Food-grade bleached kraft paper, PHBV water-based coating, 300mm×300mm finished size, rotary screen coating equipment, coating speed of 10m / min, pre-drying with hot air at 90℃ for 20s, and maintaining a peak paper surface temperature of 160℃ for 2s. The first functional area is a centered 180mm×180mm square, with an area ratio of 36.0% and q1 of 4.0g / m². 2 Three PHA grid connected regions that are not connected to each other are set; the PHA recognition pixel areas of the three connected regions account for 45%, 35% and 20% of the total PHA recognition pixel area of the first functional area, respectively, and the first functional area C1 accounts for 31.5%.
[0364] The second functional area uses a dot pattern with a PHA planar projection area coverage of 45.0%, and sets up four continuous exposed cellulose pathways with a minimum effective width of 4.0 mm, passing through four different folded areas and reaching four different paper edges. The q2 of the second functional area is 1.425 g / m². 2 q t It is 2.352 g / m 2 K was 1.70 and C2 was 49.5%. This sample was used to evaluate the effect when the second functional region has a connected structure but the first functional region PHA continuity is insufficient.
[0365] Comparative Example 5: Except for the closed window layout of the second functional area, the same 40g / m² was used as in Example 1. 2 The processing conditions included food-contact grade bleached kraft paper, PHBV water-based coating, a finished product size of 300mm × 300mm, rotary screen coating equipment, a coating speed of 10m / min, pre-drying with hot air at 90℃ for 20s, and maintaining a peak paper surface temperature of 160℃ for 2s. The central region adopted the same PHBV continuous structure as in Example 1, with a central region q1 of 6.0 g / m³. 2 The PHA film coverage rate was 95%, and the proportion of the largest connected domain within the PHA phase was 98%.
[0366] The second functional zone divides the exposed cellulose area into 12 non-interconnected closed windows by a continuous PHA background line. The total area of these closed windows accounts for 70% of the area of the second functional zone, with the largest closed window accounting for 12.0% of the total exposed cellulose area. Each closed window does not contact the first functional zone, the paper edge, or other closed windows, and does not form a continuous pathway of exposed cellulose extending from the periphery of the first functional zone to the paper edge. The PHA coverage of the second functional zone is 30%, and q2 is 0.30 g / m². 2 q t It is 2.352 g / m 2 K was 2.55 and C2 was 8.4%. This sample was used to evaluate the performance when the total exposed cellulose area remained essentially consistent but was segmented into isolated windows.
[0367] Comparative Example 6: Using the same base paper and PHBV water-based coating as Example 1, a 100% solid cylinder screen with a nominal mesh volume of 35.3 cm³ was used. 3 / m 2 The coating was applied at a speed of 10 m / min and pre-dried with hot air at 90°C for 20 s and held at the peak paper temperature of 160°C for 2 s as described in Example 1, resulting in a 6.0 g / m² coating on the entire food contact side. 2 A continuous PHBV membrane. The nominal central region and peripheral regions have q1, q2, and q... t Both are 6.0 g / m 2 K is 1.00. The PHA film coverage on the food contact side is 100%, and the maximum connected domain ratio within the PHA phase is 100%. The cellulose exposure rate is 0, and the maximum connected domain ratio and continuous pathway width within the exposed cellulose phase are not applicable. This sample does not form a second functional area of exposed cellulose continuous phase or an exposed cellulose continuous pathway reaching the paper edge. This sample is used to evaluate the oil-blocking and condensation performance of full-width high dry weight continuous films.
[0368] Comparative Example 7: Using the same 60 g / m³ as in Example 7 2 Food-grade bleached kraft paper, P34HB water-based coating, 300mm×300mm finished product size, rotary screen coating equipment, and corresponding drying conditions. The area ratio of the first functional zone is 60%, and the q1 of the first functional zone is 3.0g / m². 2 The second functional area uses a 65% grid, with q2 being 2.0 g / m². 2 q t 2.600 g / m 2 K is 1.15.
[0369] A continuous exposed cellulose pathway with a minimum effective width of 1.0 mm is set along the x-axis and y-axis, passing through four different folded areas and reaching four different paper edges.
[0370] The first functional region C1 has a content of 81.0%; the second functional region has a content of 35% for E2, 75% for R2, and 26.3% for C2. This sample was used to evaluate the combined boundary state when the PHA distribution is nearly uniform and accompanied by an insufficient proportion of the area of the peripheral maximum exposed cellulose connected domain.
[0371] Comparative Example 8: Using the same 60 g / m³ as in Example 7 2 Food-grade bleached kraft paper, P34HB water-based coating, 300mm×300mm finished product size, rotary screen coating equipment, and corresponding drying conditions. The first functional area is a centered 250mm×252mm rectangle, accounting for 70% of the area, with q1 of 4.0g / m². 2 The second functional area q2 is 0.10 g / m 2 q t 2.830 g / m 2 K is 1.41, and the first functional area C1 is 68.0%.
[0372] The second functional zone uses 5% dots and features four continuous exposed cellulose pathways that pass through four different folding areas and reach four different paper edges, with a minimum effective width of 0.20 mm. The second functional zone has E2 at 95%, R2 at 100%, and C2 at 95.0%.
[0373] The sample has a continuous cellulose phase with exposed periphery, but the C1 content in the first functional region is less than 70%, which is used to evaluate the effect of insufficient PHA continuity in the first functional region.
[0374] Comparative Example 9: Using the same 35 g / m³ as in Example 2 2 Food-grade bleached kraft paper, P34HB water-based coating, 300mm×300mm finished product size, rotary screen coating equipment, and corresponding drying conditions. The first functional area is a centered 180mm×200mm rectangle, accounting for 40% of the area, using 100% solid paper, with q1 of 12.0g / m². 2 The second functional area q2 is 4.00 g / m 2 q t 7.200g / m 2 K is 1.67, and the PHA coverage rate of the second functional area is 80%.
[0375] Four continuous exposed cellulose pathways, each with a minimum effective width of 15.0 mm, pass through four different folded regions and reach four different paper edges. The first functional zone, C1, has a coverage of 100%; the second functional zone has coverage of 20% for E2, 60% for R2, and 12.0% for C2. This sample was used to evaluate performance when the peripheral effective continuous exposed area is insufficient.
[0376] Comparative Example 10: Using the same 35 g / m³ as in Example 2 2Food-grade bleached kraft paper, P34HB water-based coating, 300mm×300mm finished product size, rotary screen coating equipment, and corresponding drying conditions. The first functional area is a centered 150mm×120mm rectangle, accounting for 20% of the area, with q1 of 1.5g / m². 2 The second functional area q2 is 0.25 g / m 2 q t 0.500g / m 2 K is 3.00, and the first functional area C1 is 68.0%.
[0377] The second functional area uses 5% dots and sets up four continuous exposed cellulose pathways that pass through four different folding areas and reach four different paper edges, with a minimum effective width of 0.20 mm and C2 of 95.0%.
[0378] This sample was used to evaluate the performance when the PHA areal density was low and the continuous barrier area of the first functional region was insufficient.
[0379] Comparative Example 11: Using the same 60 g / m³ as in Example 7 2 Food-grade bleached kraft paper, P34HB water-based coating, 300mm×300mm finished product size, rotary screen coating equipment, and corresponding drying conditions. The first functional area is a centered 225mm×240mm rectangle, accounting for 60% of the area, using 100% solid paper, with q1 of 12.0g / m². 2 The second functional area q2 is 2.00 g / m 2 q t 8.000g / m 2 K is 1.50, and the PHA coverage rate of the second functional area is 70%.
[0380] Four 10.0 mm wide exposed cellulose continuous pathways pass through four different folded regions and reach four different paper edges. The first functional area C1 is 100%; the second functional area E2 is 30%, R2 is 80%, and C2 is 24.0%. This sample is used to evaluate the performance when the total area of exposed cellulose on the periphery is present but the maximum continuous open area is insufficient.
[0381] Comparative Example 12: The same base paper, first functional area, PHBV waterborne coating, PHA coverage area, total exposed cellulose area, maximum exposed cellulose connected area, coating equipment, and drying conditions as in Example 11 were used. Only the upper branch passed through the upper fold area defined by the predetermined fold line coordinates and reached the upper paper edge; the other three branches extended toward the right paper edge, lower paper edge, and left paper edge, respectively, but all terminated at a position 5.0 mm from the corresponding paper edge and were separated from the corresponding paper edge by the PHA closed area.
[0382] The first functional zone q1 is 6.01 g / m2 The second functional area q2 is 0.30 g / m 2 q t It is 2.356 g / m 2 K is 2.55; C1 is 93.1% and C2 is 67.2%. This sample forms only one exposed cellulose end, which passes through a folded area and reaches a paper edge.
[0383] Comparative Example 13: Using the same base paper, first functional area, PHBV waterborne coating, PHA coverage area, total exposed cellulose area, maximum exposed cellulose connectivity area, coating equipment, and drying conditions as Example 11. Two branches extend upward from the upper boundary of the first functional area, centered at x=-30mm and x=30mm respectively, both passing through the upper folded area defined by the same set of predetermined fold line coordinates and reaching the upper paper edge; the two edge ends are separated by a PHA coverage area with a width ≥2.0mm along the paper edge direction. The other two branches extend towards the right and lower paper edges respectively, but both terminate at a position 5.0mm from the corresponding paper edge and are separated from the corresponding paper edge by a PHA closed area.
[0384] The first functional zone q1 is 6.00 g / m 2 The second functional area q2 is 0.30 g / m 2 q t It is 2.352 g / m 2 K was 2.55; C1 was 93.1% and C2 was 67.2%. The sample formed two exposed cellulose ends, but both ends passed through the same folding area and reached the same paper edge.
[0385] Comparative Example 14: Paper-based packaging structures obtained directly from three independent coating batches of Example 1, without preparing additional material batches, were used. The base paper, finished product dimensions, PHA material, structure of the first and second functional areas, and parameters q1, q2, and q... t The parameters K, C1, C2, number of pathways, pathway width, and preparation conditions are the same as in Example 1.
[0386] In the hot food packaging test of the corresponding application example, the food composition, initial contact temperature, folding position corresponding to the predetermined folding line coordinates, folding sequence, folding overlap width, packaging label position, and testing conditions were all the same as those of the sample from Example 1. Only the food placement position was adjusted so that the measured overlap rate between the food's orthographic projection and the first functional area was 55±1%. This comparative example was used to evaluate the impact on paper back oil penetration, corner oil penetration, condensation, and food shape retention when the packaging structure remained unchanged but the main high-oil contact projection of the food was not aligned with the first functional area as required.
[0387] Comparative Example 1 does not form a continuous PHA barrier phase; Comparative Examples 2 and 6 do not form the specified second functional area exposed cellulose continuous phase; Comparative Examples 3 and 4 do not form the specified PHA continuous barrier phase in the first functional area; Comparative Example 5 does not form a continuous exposed cellulose pathway leading to the paper edge; Comparative Example 7 has a C2 of less than 30% and a K of 1.15, which is only recorded as the material spatial distribution state; Comparative Examples 8 and 10 both have a C1 of less than 70%; Comparative Examples 9 and 11 both have a C2 of less than 30%; Comparative Example 12 has only one pathway passing through a folded area and reaching a paper edge; Comparative Example 13 has two edge ends, but both ends pass through the same folded area and reach the same paper edge. The paper-based packaging structure of Comparative Example 14 is the same as that of Example 1, except that the overlap between the food orthographic projection and the first functional area is insufficient.
[0388] Application example.
[0389] The layout adjustments and sample preparation for Application Examples 2-8 were performed according to the following rules. When the finished product size needed to be changed, the outer contour of the paper-based packaging structure, the boundary of the first functional area, the boundary of the second functional area, the coordinates of the predetermined fold line, the center line of the passage, the coordinates of the predetermined cutting line, the coordinates of the predetermined fold overlap area, and the coordinates of the predetermined area for fixing the packaging label were adjusted proportionally. Dots, grids, discontinuous short lines, and high-coverage micro-dots were regenerated within the adjusted functional area according to the original unit size and original local layout coverage of the source sample, and q1, q2, and K were kept at the set values of the source sample by adjusting the mesh or cell volume. Except for the rounded rectangle remaking in Application Example 4, the basic outline form and passage topology of the first functional area were not changed. The samples obtained from the remade plates were all used as independent package samples for the corresponding application examples.
[0390] Application Example 2 uniformly adopts a 300mm×300mm pattern; for Examples 8 and 10 with source dimensions of 280mm×280mm, the macroscopic layout coordinates are adjusted according to 300 / 280, that is, 1.0714 times.
[0391] Application Example 3 uniformly adopts a 330mm×330mm format; the coordinates of the macroscopic map with a source size of 300mm×300mm are adjusted by a factor of 1.100, and the coordinates of Examples 8 and 10 with a source size of 280mm×280mm are adjusted by a factor of 330 / 280, i.e., 1.1786.
[0392] Application Example 4 uses a uniform 320mm×300mm template and is adjusted according to the rules for remaking the first functional area of the rounded rectangle specified in this application example.
[0393] Application Examples 5 and 6 use the original finished product size of the source samples. Specifically, Examples 8 and 10 use a 280mm × 280mm pattern, while the remaining samples use a 300mm × 300mm pattern.
[0394] In Application Example 7, the 65℃ and 90℃ batches use a 300mm×300mm pattern, and the 70℃ batch uses a 330mm×330mm pattern. The macroscopic map coordinates of the 300mm×300mm source map are adjusted by a factor of 1.100.
[0395] Application Example 8 uses a 300mm × 300mm form factor. The statistical inclusion and prohibition of subsequent adjustments for all packaging bodies in Application Examples 2–8 shall be implemented in accordance with the aforementioned general conditions for food packaging.
[0396] Application Example 1: Comprehensive evaluation of material-level oil resistance and water vapor transfer.
[0397] This application example is a material-level test and does not involve food placement, folding, or labeling. Examples 1-12 and Comparative Examples 1-13 were sampled from original-size finished products or replicated samples from the same batch. Comparative Example 14 uses the same batch, pattern, and material structure as Example 1, and its material-level results are based on the test results of Example 1.
[0398] Five independent parallel samples were used for each of the following tests: central hot oil breakthrough, crease hot oil breakthrough, 30-minute oil stain area, and oil resistance test grade. For samples with a first functional zone, the center of the first functional zone was used as the sampling center; for samples without a first functional zone, the nominal central area of Example 1 was used as the sampling center.
[0399] The samples forming the first and second functional regions were used to determine and calculate the area-weighted equivalent water vapor transmission rate (WVTR) in the unfolded state using the aforementioned batch-replicated sample method. t Five parallel specimens were used for each local material condition, with an effective test area of 33 cm². 2 For samples that did not form a first functional zone, the five-point average local water vapor transmission rate was reported, without regional weighting. All results were the average of parallel samples.
[0400] Table 4. Comprehensive evaluation results of material-grade oil resistance and water vapor transfer.
[0401]
[0402] Note: For samples that have not formed a first functional zone, the water vapor transmission performance column in Table 4 reports the five-point average local water vapor transmission rate, which is not used as the area-weighted equivalent water vapor transmission rate (WVTR) in the developed state. t .
[0403] Analysis: The results show that the continuous PHA barrier phase in the first functional zone affects oil resistance in the center and at the creases, while the openness of the second functional zone affects moisture permeability. Example 1 and Comparative Examples 2 and 3 have the same total PHA content; the latter two, due to near-uniform distribution or discontinuity in the central region, experienced earlier hot oil breakthrough. Comparative Example 6 showed strong oil resistance in the center of the continuous film, but decreased moisture permeability. Although Comparative Example 5 lacked an edge-to-edge pathway, its material-level oil resistance and WVTRt were close to those of Example 1, indicating that the application examples only evaluate material performance in the unfolded state and cannot replace verification of external connectivity after folding. Because multiple groups simultaneously changed q1, q2, C1, and C2, the results should not be attributed to a single parameter.
[0404] Application Example 2: Instant wrapping of a single-layer beef burger at 65℃.
[0405] The single-layer beef burger consists of an HB-98 bun (75±2g), a BP-100 cooked beef patty (100±2g), a C-20 cheese slice (20.0±0.5g), ketchup (12±1g), and M-65 mayonnaise (13±1g), for a total weight of 220±10g. The ketchup and mayonnaise are evenly spread on a 60mm diameter circular area on the top surface of the bottom bun, with the beef patty and cheese slice placed in the center. The surface temperature of the center of the hot burger's bottom layer upon initial contact with the paper-based packaging structure is 65±2℃.
[0406] Samples with a first functional area were positioned using vertical imaging to adjust the food's position so that the overlap between the food's orthographic projection and the first functional area reached the values listed in Table 5, with an allowable deviation of ±1 percentage point. Samples without a first functional area were placed at the nominal center of the paper. Comparative Example 14 used the same paper-based packaging structure as Example 1, only adjusting the food's position to achieve an overlap rate of 55±1%.
[0407] Each sample was folded inwards on all four sides and labeled according to general food packaging conditions, and then tested after standing for 15 minutes. For each sample, three individual hamburgers and three paired buns were tested, and the results were averaged.
[0408] In Tables 5 to 9, “—” indicates that the corresponding sample did not form the first functional area as defined in this document, and therefore the overlap rate between the food orthographic projection and the first functional area is not calculated; other properties of such samples are still tested according to the prescribed nominal central placement method.
[0409] Table 5. Results of wrapping a single-layer beef burger at 65℃.
[0410]
[0411] Analysis: Under the single-layer beef burger condition at 65℃, the complete embodiment balances low paper back oil permeation, low condensation, and high texture retention. Examples 8 and 10 have high q1, C1, and C2 and low q2; Example 7 has high oil permeation, condensation, and debris adhesion because q1 is at the lower limit, q2 is at the upper limit, and C2 is close to the lower limit. Comparative Example 1 lacks a continuous PHA barrier phase, resulting in significant oil permeation; Comparative Example 6 lacks an exposed cellulose continuous phase, which, although providing good oil barrier properties, results in severe condensation; Comparative Example 14, by reducing the food overlap rate to 55%, increases oil permeation and decreases texture retention, indicating that both material structure and correct alignment affect overall performance.
[0412] Application Example 3: 70℃ Double-Layer Cheeseburger with High Oil Load.
[0413] The double cheeseburger consists of 85±3g of HB-110 bun, two 90±2g BP-90 cooked beef patties, two 20.0±0.5g C-20 cheese slices, and 25±2g of sauce, for a total weight of 330±15g. The sauce is a 1:1 mixture of tomato sauce and M-65 mayonnaise, evenly spread on a 70mm diameter circular area on the top surface of the bottom bun. The surface temperature of the center of the hot burger bottom when it first contacts the paper-based packaging structure is 70±2℃.
[0414] Samples with a first functional area were positioned using vertical imaging to adjust the food's position so that the overlap between the food's orthographic projection and the first functional area reached the values listed in Table 6, with an allowable deviation of ±1 percentage point. Samples without a first functional area were placed at the nominal center position of the paper. Comparative Example 14 used the same material structure as the sample from Example 1, but only the food position was adjusted to achieve an overlap rate of 55 ± 1%.
[0415] Each sample was folded inwards on all four sides and labeled according to general food packaging conditions. After standing for 20 minutes, the oil penetration area on the back of the paper, the oil penetration points at the folded corners, the percentage of visible condensation area, and the texture retention rate of the bottom bread were measured. For each sample, three independent hamburgers and three paired bottom breads before packaging were tested, and the results were averaged.
[0416] Table 6 Results of high-oil-load wrapping of double-layer cheeseburgers at 70℃.
[0417]
[0418] Analysis: Under the high oil load of a 70℃ double-layer cheeseburger, the differences are amplified. Examples 8 and 10 maintain low oil permeability, no corner oil permeability, and low condensation, indicating that a balance is formed between higher C1, lower q2, and higher C2. Example 7 shows increased oil permeability, corner oil points, and condensation due to low q1, high q2, and C2 of 33.6%. Comparative Examples 4 and 10 have insufficient oil resistance due to insufficient continuity in the first functional zone; Comparative Examples 6, 9, and 11 have strong oil resistance, but severe condensation due to insufficient continuous open paper surface; Comparative Example 14 has an overlap rate of 55%, increased oil permeability, and decreased texture retention, indicating that zoning structure and food alignment are equally important under high oil load.
[0419] Application Example 4: Extended Applicability Verification of 62℃ Long Strip Fried Chicken Rolls.
[0420] This application example illustrates the applicability of the partitioned structure to long, hot food wrapping conditions.
[0421] Specific adjustment instructions for the samples: All samples in this application example are re-made according to the 320mm×300mm template. For samples with a first functional area, the first functional area is adjusted to a rounded rectangle with the x-axis as the major axis, and adjusted according to A=L×W-(4-π)r. 2 Calculate the area of the rounded rectangle to ensure that the area ratio of the first functional area is consistent with that of the source sample; for samples that do not form a first functional area, reconstruct their original uncoated, full-width pattern or full-width continuous film structure according to the outer contour of 320mm×300mm, without adding a first functional area.
[0422] The exposed cellulose continuous pathway extends from the outer boundary of the rounded rectangle or the outer edge of the continuous PHA oil-blocking boundary band along the x and y axes to the corresponding paper edge. The minimum effective width of the pathway, the boundary band width, and the pathway topology are maintained as set in the source sample. Periodic dots, grids, and micro-dots are regenerated in the new functional area according to the original unit size and the original local coverage. The mesh volume is adjusted to maintain the set values of q1, q2, and K as set in the source sample.
[0423] Comparative Example 4 still forms three unconnected PHA connected regions within the first functional area of the rounded rectangle. The PHA recognition pixel areas of the three connected regions account for 45%, 35%, and 20% of the total PHA recognition pixel area of the first functional area, respectively. Comparative Example 5 forms 12 unconnected exposed cellulose closed windows in the second functional area. The total area of the windows accounts for 70% of the area of the second functional area, and the largest window area accounts for 12.0% of the total exposed cellulose area. None of the windows contact the first functional area, the paper edge, or other windows.
[0424] The orthographic projection of the fried chicken roll was defined as a rounded rectangle of 180mm × 70mm with a corner radius of 20mm. For samples with a first functional area, the food position was adjusted using vertical imaging to achieve the overlap rate between the food's orthographic projection and the first functional area, as listed in Table 7, with an allowable deviation of ±1 percentage point. Samples without a first functional area were placed in the center. Comparative Example 14 used the same material structure as the adjusted Example 1, only adjusting the food position to achieve an overlap rate of 55±1%. All three packages of each sample were tested in their initial state after the first fold and labeling, and the average value was included.
[0425] The fried chicken roll consisted of 70±2g of WP-180 wrap dough, 120±3g of CS-120 fried chicken strips, 40±2g of V-40 vegetables, and 20±2g of M-65 mayonnaise, for a total weight of 250±15g. The mayonnaise was evenly spread along a 160mm×40mm area at the center of the wrap dough's long axis, with the fried chicken strips and vegetables laid out along the long axis. The initial contact surface temperature was 62±2℃. The wrapping method involved folding inwards on both sides, folding upwards at the bottom, and folding back at the top. A 35mm diameter packaging label was used to secure the top folded area. After standing for 15 minutes, the oil penetration area on the back of the paper, the percentage of visible condensation, the debris adhesion rate, and the paper integrity rate were recorded. Three independent fried chicken rolls were tested for each sample.
[0426] Table 7. Results of wrapping long strip fried chicken rolls at 62℃.
[0427]
[0428] Analysis: In the long fried chicken roll test, the complete embodiment maintained low oil permeability, low condensation, and over 95% paper integrity under the remade pattern, indicating that the structure is suitable for long food products. Comparative Example 1 lacked a continuous PHA barrier phase, resulting in increased oil permeability and breakage; in Comparative Example 5, the exposed cellulose was divided into isolated windows, leading to increased condensation and debris; Comparative Examples 6, 9, and 11 had insufficient open paper surfaces, resulting in high condensation despite oil resistance; Comparative Example 14 experienced increased oil permeability and decreased integrity due to food misalignment. The overlap rate of some embodiments was 85%–90%, and these samples are only used to illustrate the adaptation trend and are not used to evaluate overlap conditions of 92%–100%.
[0429] Application Example 5: Extended Applicability Verification of 45℃ Hot Sandwiches.
[0430] This application example illustrates the applicability of the partitioned structure to rectangular hot food wrapping conditions. The hot sandwich consists of SB-160 sandwich bread, GC-80 grilled chicken breast (80±2g), C-30 cheese (30±1g), and sauce (10±1g); the bread combination weighs 70±2g, the food's orthographic projection size is 160mm×100mm, and the total weight is 190±10g. The sauce is a 1:1 mixture of tomato sauce and M-65 mayonnaise by weight, evenly spread over a 140mm×80mm area of the lower bread layer. The surface temperature of the sandwich bottom upon initial contact with the paper-based packaging structure is 45±2℃.
[0431] The long side of the food's orthographic projection is parallel to the x-axis. For samples with a first functional area, the food position is adjusted using vertical imaging to achieve the overlap rate between the food's orthographic projection and the first functional area as listed in Table 8, with an allowable deviation of ±1 percentage point. Samples without a first functional area are placed at the nominal center position of the paper. Comparative Example 14 uses the same material structure as Example 1, only adjusting the food position to achieve an overlap rate of 55±1%.
[0432] Each sample was folded inwards on both sides and labeled according to general food packaging conditions. After standing for 10 minutes, the oil penetration area on the back of the paper, the percentage of visible condensation area, the texture retention rate of the bottom bread, and the crumb adhesion rate were measured. Three independent sandwiches and three paired bottom breads were tested for each sample.
[0433] Table 8 Results of wrapping hot sandwiches at 45℃.
[0434]
[0435] Analysis: Under 45°C hot sandwich conditions, the complete examples maintained low oil permeability, low condensation, and 85%–94% texture retention, indicating that the partitioned structure is suitable for rectangular foods. Comparative Example 1 lacked a PHA barrier, resulting in significant oil permeability; Comparative Example 5, due to the exposure of cellulose, was divided into isolated windows, leading to increased condensation and debris; Comparative Examples 6, 9, and 11 had insufficient continuous open paper surfaces, resulting in strong oil resistance but poor condensation and texture; Comparative Example 14 showed increased oil permeability and debris after misalignment. Most examples had an overlap rate below 92%; these samples were used to illustrate shape expansion and trend consistency, and were not used to evaluate 92%–100% usage conditions.
[0436] Application Example 6: High-temperature wrapping of fried chicken burgers at 90℃.
[0437] The fried chicken burger consists of an HB-105 burger bun (80±3g), a CP-140 fried chicken fillet (140±3g), a C-22 cheese slice (22.0±0.5g), and 18±2g of sauce, for a total weight of 260±15g. The sauce is a 1:1 mixture of ketchup and M-65 mayonnaise, evenly spread on a 70mm diameter circular area on the top surface of the bottom bun. The nominal diameter of the bottom projection of the food is 105±3mm, and the surface temperature of the center of the hot burger bottom when it initially contacts the paper-based packaging structure is 90±2℃.
[0438] Samples with a first functional area were positioned using vertical imaging to adjust the food's position so that the overlap between the food's orthographic projection and the first functional area reached the values listed in Table 9, with an allowable deviation of ±1 percentage point. Samples without a first functional area were placed at the nominal center position of the paper. Comparative Example 14 used the same material structure as Example 1, but adjusted the food's position to achieve an overlap rate of 55 ± 1%.
[0439] Each sample was folded inwards on all four sides and labeled according to general food packaging conditions. After standing for 15 minutes, the oil penetration area on the back of the paper, the oil penetration points at the folded corners, the percentage of visible condensation area, and the texture retention rate of the bottom bread were measured. For each sample, three independent fried chicken hamburgers and three paired bottom breads were tested.
[0440] Table 9. Results of high-temperature wrapping of fried chicken burgers at 90℃.
[0441]
[0442] Analysis: 90℃ fried chicken burgers have high oil and steam loads. Examples 8 and 10 show low rates of oil penetration through the paper back, oil spots at the corners, and condensation, resulting in high texture retention. Example 7 exhibits the weakest performance due to low q1, high q2, and C2 being close to the lower limit. Comparative Examples 1, 3, 4, and 10 show increased oil penetration and oil spots at the corners due to insufficient continuity in the first functional area. Comparative Examples 6, 9, and 11, while showing strong oil resistance due to insufficient open paper surface, exhibit high condensation and low texture retention. Comparative Example 14, with a 55% overlap, shows oil penetration increasing to 25.0 cm. 2 The texture retention rate dropped to 48%. At high temperatures, the oil-blocking structure, exhaust passage, and alignment all affect performance.
[0443] Application Example 7: Topology comparison of multi-directional to-edge paths and verification of folding and rotation tolerance.
[0444] Specific sample adjustment instructions: In this application example, Examples 11, 12, 12, and 13 are selected as pathway topology matching samples, and Comparative Example 5 is selected as the isolated window reference sample. The pathway topology matching samples use the same or similarly controlled base paper, PHA material, first functional area, q1, q2, and q... tK, F1, R1, C1, E2, R2, C2, and the minimum effective width of the pathway are varied, only the amount of exposed cellulose to the edge ends, the number of different folded areas traversed by the pathway, and the number of different paper edges reached are changed. Comparative Example 5 shows the first functional area structure, q1, q2, q... t The samples were identical to those with K and the pathway topology matching, but the exposed cellulose region of the second functional area was segmented into isolated windows that were not connected to the paper edge.
[0445] This application example uses the 65°C single-layer beef burger specified in Application Example 2, the 70°C double-layer cheeseburger specified in Application Example 3, and the 90°C fried chicken burger specified in Application Example 6. The composition, initial contact temperature, and resting time of each food item are performed in accordance with the corresponding application example.
[0446] Each sample was rotated relative to the layout coordinate system of the folding template in four directions (0°, 90°, 180°, and 270°) under each hamburger condition. Three independent packages were set up in each rotation direction, for a total of 12 packages. Each package was folded according to the folding sequence and folding overlap width specified in the corresponding application example, and a packaging fixing label was set at the position corresponding to the coordinate of the predetermined folding line. The folding position or label position was not changed according to the position of the exposed cellulose to the edge.
[0447] Within 30 seconds after the packaging label is pressed together, the first image acquisition is completed using the aforementioned multi-view imaging detection method for the external connectivity status after folding. The number of external connectivity ends for each package is recorded, and the average number of external connectivity ends, the success rate of external connectivity at at least one edge end, and the failure rate of closure at all edge ends are calculated. During the image acquisition process, the packaging label is not moved, the folds are not opened, and the relative positions of the paper layers are not changed.
[0448] After image acquisition, the packaging body is kept in its initial state with the seams facing upwards and left to stand. The corresponding indicators of paper back oil penetration, corner oil penetration, visible condensation, bottom bread texture retention, and debris adhesion are measured according to the standing time and testing methods specified in Application Examples 2, 3, and 6, respectively.
[0449] Table 10. Structural parameters of the pathway topology control samples.
[0450]
[0451] In the table, “—” indicates that there is no continuous exposed cellulose pathway reaching the edge of the paper in Comparative Example 5, so the minimum effective width of the continuous pathway is not calculated.
[0452] Table 11. Validation results of the pathway topology for a single-layer beef burger at 65℃.
[0453]
[0454] Table 12. Validation results of pathway topology for a 70℃ double-layer cheeseburger.
[0455]
[0456] Table 13. Validation results of the pathway topology for 90℃ fried chicken burgers.
[0457]
[0458] Analysis: Application Example 7 uses a topological comparison based on matching main material parameters to directly evaluate the effect of the number of ends and directional dispersion. In Example 12, the four ends pass through four folded areas and reach four paper edges, resulting in the highest success rate for external connectivity across the three food products. Example 11, with its two-way ends, is second best. Comparative Example 13, although having two ends, is located in the same folded area and on the same paper edge, leading to a lower success rate. Comparative Example 12, with only one end, has an even higher failure rate. Comparative Example 5, lacking any edge-to-edge pathways, fails entirely. In this design, simply increasing the number of ends cannot replace directional dispersion; the pathways must also pass through different folded areas and reach different paper edges.
[0459] Application Example 8: Simulating random parcel delivery without specific training in stores and open fault tolerance verification at the edge.
[0460] This application example selects Examples 11, 12, 5, 12, and 13 to evaluate the impact of the number of edge points, the number of folded areas traversed, and the direction of the paper edge reached on actual package tolerance, without specific training in first functional area positioning, identification of exposed cellulose continuous pathway locations, and avoidance of packaging label fixing. This application example does not evaluate the operator's mastery of ordinary paper folding and basic food packaging operations.
[0461] The operators were divided into three groups: a skilled and normal group of 4 people, all of whom had at least 6 months of experience in manually wrapping similar paper and operated at the normal working speed; an inexperienced group of 4 people, all of whom had no experience in wrapping similar paper and only received instructions on ordinary four-sided inward folding actions that did not involve the first functional area, passageway position and label avoidance; and a skilled and fast group of 4 people, all of whom had at least 6 months of experience in manually wrapping similar paper and operated at the daily peak period speed.
[0462] Each operator completed 5 wraps for each of the five samples. Each sample was wrapped 60 times by 12 operators, for a total of 300 wraps for all five samples. The samples were randomly numbered, and the order in which each operator received the five samples was arranged in a balanced random manner. The operators were only instructed to "wrap the samples as you would normally wrap a hot hamburger and affix a fixed label to the top of each package."
[0463] The 65°C single-layer beef burger as specified in Application Example 2 was used for packaging. The paper-based packaging structure had the food contact side facing the operator, and no coordinate-lined folding templates, food positioning marks, first functional area boundary indicators, passageway location indicators, label positioning templates, or passageway avoidance requirements were provided. The packaging time started from the operator's first contact with the paper-based packaging structure and ended when the packaging label was pressed shut. The orthographic projection position of the food was recorded within 3 seconds after the burger was initially placed; the first multi-view image acquisition of the external connectivity state after folding was completed within 30 seconds after the packaging label was pressed shut.
[0464] Each package was kept in the state it was in after the operator first completed folding and labeling, without reopening the folds, moving the fixed labels, or changing the relative positions of the paper layers. All 60 packages for each sample were included in the statistics, and the average wrapping time, average food orthographic overlap rate, proportion of overlap rates above 92%, average number of external connection ends, success rate of external connection to at least one edge end, and failure rate of sealing all edge ends were calculated.
[0465] After image acquisition, each package was kept in its initial state and left to stand for 15 minutes. The oil penetration area on the back of the paper, the percentage of visible condensation area, the bottom bread texture retention rate, and the debris adhesion rate were measured according to the method in Application Example 2. The paper integrity rate was measured according to the aforementioned method.
[0466] Table 14 Overall results of random parcels in simulated stores without specific training.
[0467]
[0468] Table 15. Parcel fault tolerance results for different operator groups.
[0469]
[0470] Analysis: Application Example 8 did not provide functional area positioning, pathway prompts, or label avoidance requirements. The wrapping time and food overlap rate were similar across samples, with differences in external connectivity primarily stemming from pathway topology. The success rates of Examples 12 and 11 were 96.7% and 90.0%, respectively. Comparative Example 13, with both ends concentrated in the same folding area and paper edge, had a success rate of 71.7%. Comparative Example 12, with only one end, had a success rate of 45.0%. Comparative Example 5, lacking edge pathways, failed entirely, exhibiting high condensation and low texture retention. The inexperienced group performed poorly, indicating that under simulated conditions, multi-directional redundancy can reduce but not eliminate operational bias.
[0471] Experimental Results and Analysis:
[0472] The continuous oil-blocking structure in the first functional area is aligned with the orthographic projection of the food.
[0473] The average dry mass q of PHA per unit area on the food contact side of Examples 1, 2, and 3 t Both are 2.352 g / m 2 In Example 1, PHA was concentrated in the first functional region, resulting in q1 reaching 6.0 g / m². 2 A continuous PHA barrier phase was formed; in Comparative Example 2, the same total amount of PHA was approximately uniformly distributed to the food contact side, and in Comparative Example 3, the same total amount of PHA was distributed as full-width dots. The central hot oil breakthrough times for the three examples were 1180s, 145s, and 42s, respectively, and the oil spot areas at 30 min were 1.1 cm², respectively. 2 10.8cm 2 and 23.6cm 2 This comparison shows that, under the condition of the same total amount of PHA, the concentrated distribution of PHA and its planar continuity within the first functional area directly affect the oil-blocking performance of the main high-oil contact area.
[0474] Comparative Example 14 used the same batch, layout, material structure, and preparation conditions as Example 1, with the only difference being the reduction of the overlap between the food's orthographic projection and the first functional area from 100% to 55%. In tests of a single-layer beef burger at 65°C, a double-layer cheeseburger at 70°C, and a fried chicken burger at 90°C, the oil-permeable area on the back of Comparative Example 14 was 8.9 cm². 2 17.0cm 2 and 25.0cm 2 The samples from Example 1 were 0.7 cm. 2 1.6cm 2 and 2.8cm 2 This comparison shows that the compliance of the paper-based packaging structure with regulations and the correct alignment of the main high-oil contact projection of the food with the first functional area are two interrelated conditions that can be detected separately.
[0475] In the complete embodiment, the area ratio of the first functional area is 15% to 60%. This area ratio needs to be determined in conjunction with q1, C1, the continuous open structure of the second functional area, and the orthographic projection size of the food, and cannot be evaluated in isolation from other structural parameters.
[0476] The second functional area features a continuously open structure and a coordinated oil-blocking and steam-exhausting mechanism.
[0477] The first functional area structure, q1, q2, and q of Example 1 and Comparative Example 5 t Similar to K, the central hot oil breakthrough times were 1180s and 1160s, respectively, and the oil spot area at 30 minutes was 1.1cm. 2 and 1.2cm 2The main difference between the two is that: in Example 1, the C2 is 67.2%, and continuous exposed cellulose pathways leading to different paper edges are formed; in Comparative Example 5, the exposed cellulose area is divided into isolated windows, with a C2 of only 8.4%, and no continuous pathways leading to the paper edges exist. In each hot food wrapping scenario, the visible condensation area ratio of Comparative Example 5 is higher than that of Example 1, indicating that a similar total exposed cellulose area cannot replace the edge pathways formed by a continuously open paper surface.
[0478] Comparative Example 6 formed 6.0 g / m² on the entire food contact side. 2 The continuous PHBV membrane did not experience a central hot oil breakthrough during the 1800s observation period, but the average local water vapor permeability at five points was only 260 g / (m²). 2 • 24h). In different hot food applications, the visible condensation area ratio of Comparative Example 6 was 29%–57%, and the bottom bread texture retention rate was 42%–71%. The area-weighted equivalent water vapor transmission rate (WVTR) in the unfolded state of Examples 1, 2, 6, 8, 9, and 10 is shown. t 1580~2210g / (m 2 •24h), while maintaining low levels of oil penetration and condensation on the back of the paper. This result indicates that a full-width continuous barrier film can improve oil blocking performance but restricts water vapor transfer; the combination of continuous oil blocking in the first functional area and continuous openness in the second functional area can create spatial synergy between the two types of performance.
[0479] PHA spatial allocation parameter K and its evidence boundary:
[0480] The spatial concentration factor K in the complete embodiment is 1.20 to 6.00. K is used to characterize the degree to which PHA is concentrated in the first functional area, so that there is a comparable quality distribution index between different areas of the first functional area and different average PHA usage in the whole paper.
[0481] In Example 7, K was 1.20 and C2 was 33.6%, while in Comparative Example 7, K was 1.15 and C2 was 26.3%; q2 and q... t The PHA coverage and C2 of the second functional zone change simultaneously. Therefore, this set of data is only used to illustrate the overall change when the PHA distribution is nearly uniform and accompanied by a continuous decrease in the open area of the second functional zone. It cannot be concluded from this that an increase in K from 1.15 to 1.20 will independently produce a performance mutation. K needs to be evaluated together with the area of the first functional zone, q1, q2, C1, C2 and pathway topology.
[0482] Multi-directional edge access and folding tolerance:
[0483] Comparative Example 12 forms one edge-to-edge end that passes through a folded area and reaches a paper edge; Comparative Example 13 forms two edge-to-edge ends, but both ends pass through the same folded area and reach the same paper edge; Example 11 forms two edge-to-edge ends that pass through different folded areas and reach different paper edges; Example 12 forms four edge-to-edge ends that pass through four different folded areas and reach four different paper edges. The materials and main planar structural parameters of the above samples are within the same control range, and the main variables are the number of edge-to-edge ends, the number of folded areas traversed by the path, and the direction of the paper edge reached.
[0484] In Application Example 7, under conditions of 65°C and 70°C, the success rates of external connectivity to at least one edge of Examples 12, 11, 13, and 12 were 100.0%, 91.7%, 66.7%, and 41.7%, respectively; under conditions of 90°C, they were 91.7%, 83.3%, 58.3%, and 33.3%, respectively. In the simulated store test without specific training in Application Example 8, the external connectivity success rates of the four were 96.7%, 90.0%, 71.7%, and 45.0%, respectively, with average package times ranging from 17.5 to 17.9 seconds.
[0485] The above results indicate that increasing the number of edges can improve folding tolerance, but the dispersion of the folding areas traversed by the edges and the direction of the paper edges reached is equally important. When at least two paths traverse different folding areas and reach different paper edges, the likelihood of the same fold or packaging fixing label simultaneously closing all ends is reduced; when four paths traverse four folding areas and reach four different paper edges, a four-way redundant structure is formed, and higher untrained package stability is achieved under the test conditions of this application.
[0486] Feasibility of material systems, industrial processes, and application scenarios:
[0487] PHB, PHBV, P34HB, PHBH, and the combination of PHBV / P34HB can all form the specified first and second functional areas under the corresponding process conditions. In this embodiment, the main melting peak temperature of PHB in BIOTEN 1030 during the second heating is 174±2℃, while Example 4 uses a paper peak temperature of 180℃. In BIOTEN 1031, the molar fraction of 3-hydroxyvalerate structural unit of PHBV is 14.0±0.8%, and the main melting peak temperature is 150±3℃, while the corresponding embodiment uses a paper peak temperature of 160℃. In BIOTEN 1032, the molar fraction of 4-hydroxybutyric acid structural unit of P34HB is 16.0±0.8%, and the main melting peak temperature is 148±3℃, while the corresponding embodiment uses a paper peak temperature of 155℃. In BIOTEN 1033, the molar fraction of 3-hydroxyhexanoic acid structural unit of PHBH is 10.0±0.5%, and the main melting peak temperature is 127±3℃, while Example 3 uses a paper peak temperature of 140℃. Based on the nominal main melting peak temperature of each grade, the above paper peak temperature is 5 to 13°C higher than the highest nominal main melting peak temperature of the corresponding single PHA or mixed PHA, which is used to promote the softening of PHA particles and interfacial cohesion after moisture removal.
[0488] Examples 9 and 10 were performed using direct gravure coating at speeds of 150 m / min and 500 m / min, respectively. In Example 9, the total continuous drying residence time was 16.79–16.82 s, and the time for the paper surface temperature to remain ≥150°C was 1.98–2.04 s. In Example 10, the total continuous drying residence time was 11.99–12.01 s, and the time for the paper surface temperature to remain ≥150°C was 2.98–3.04 s. The resulting C1 values were 96.0% and 96.0%, respectively, and the C2 values were 72.8% and 76.0%, respectively, indicating that the patterned coating, continuous drying, and registration-cutting structure can be achieved under laboratory, pilot-scale, and high-speed industrial coating conditions.
[0489] In the complete embodiment, the minimum effective width of the exposed cellulose continuous pathway is 1.0–6.0 mm. The pathway width and the width of the continuous PHA oil-blocking boundary band are determined based on the food size, the position corresponding to the predetermined fold line coordinates, the coating and cutting registration capability, and the oil load.
[0490] A 65°C single-layer beef burger, a 70°C double-layer cheeseburger, and a 90°C fried chicken burger were used to verify the applicability of the paper-based packaging structure under different hot food burger conditions; a 62°C long fried chicken wrap and a 45°C hot sandwich were used to illustrate the adaptability of the partitioned structure to the shapes of long and rectangular stuffed foods. Different application scenarios simultaneously change the type, quality, fat content, sauce amount, orthographic projection size of the food, and wrapping time; therefore, performance differences between scenarios are not solely attributed to temperature.
[0491] The influence trend of changes in PHA content and spatial distribution on experimental results:
[0492] In the examples and comparative examples using P34HB, the dry mass q1 per unit area of the first functional region PHA was set to 1.5 g / m². 2 4.0g / m 2 5.5g / m 2 8.0g / m 2 and 12.0g / m 2 The central hot oil breakthrough time of the corresponding samples generally increased from 190s to 430s, 1040–1060s, 1680–1710s, and 1800s, respectively, while the oil spot area over 30 minutes generally increased from 8.7cm². 2 Reduced to 4.6cm 2 1.3~1.4cm 2 0.5cm 2 and 0.2~0.3cm 2 The results indicate that, in the compared samples, as q1 increases and the overall connectivity of the first functional region (PHA) improves, the central hot oil breakthrough time generally lengthens, and the oil spot diffusion area generally decreases. Since q1, C1, the area of the first functional region, q2, C2, and drying conditions all vary simultaneously, these results only represent a comprehensive trend and cannot prove the independent quantitative effect of q1 when other conditions remain constant.
[0493] In the complete embodiment, the area-weighted average dry mass per unit area (q2) of the second functional area (PHA) is 0.157–1.75 g / m². 2 q2 is 0.157–0.40 g / m 2 In the complete embodiment, WVTR t 1390~2210g / (m 2 •24h); q2 is 1.75g / m 2 In Example 7, WVTR t Reduced to 820g / (m 2 •24h). q2 is 2.00~4.00g / m 2 In the comparative example, WVTR t 420–760 g / (m 2 •24h), and showed a higher proportion of visible condensation area in hot food applications. This change indicates that as the dry mass per unit area of the second functional zone PHA and the coverage of PHA increase, the exposed cellulose area and its continuous openness generally decrease, and the water vapor transfer capacity decreases accordingly. The specific upper limit of q2 still needs to be determined in conjunction with the pattern topology of the second functional zone, C2, and the continuous pathway of exposed cellulose.
[0494] In the complete embodiment, K ranges from 1.20 to 6.00. An increase in K indicates that PHA is more concentrated in the first functional region, at lower q... t Under these conditions, a relatively high q1 can still be obtained; when K approaches 1, the spatial distribution of PHA on the food contact side tends to be uniform. The results of Example 7 and Comparative Example 7 show that when K decreases from 1.20 to 1.15, accompanied by an increase in q2 and PHA coverage in the second functional area, and a decrease in C2, the overall oil blocking-vapor exhaust performance decreases. Since K, q2, and C2 change simultaneously, K cannot be evaluated independently of the area of the first functional area, q1, q2, C1, C2, and the pathway topology.
[0495] In the examples, the PHA mass fraction in the water-based coatings was 18%–22%, and the proportion of PHA to the total mass of the film-forming polymer components was 96.8%–97.4%. The PHA mass fraction in the coatings was primarily used to coordinate with the mesh or cell volume, wet transfer coefficient, and localized coverage to form specified values q1 and q2. Since the existing examples did not employ a single-variable design where all other conditions were identical except for the PHA mass fraction in the coatings, the independent performance gains of the PHA mass fraction within the 18%–22% range were not quantitatively ranked.
[0496] In summary, this invention constructs a first functional area and a second functional area located on the periphery of the first functional area and extending to the paper edge on the same food contact side of the fiber-based paper. The first functional area forms a continuous PHA barrier phase with C1 ≥ 70%, while the second functional area simultaneously forms a PHA-covered area and an exposed cellulose continuous phase with C2 ≥ 30%. The maximum exposed cellulose connectivity includes at least two continuous exposed cellulose pathways that pass through different folding areas and reach different paper edges. After the paper-based packaging structure is folded according to a predetermined packaging pattern and a packaging fixing label is set, at least one exposed cellulose edge is located on the outer surface of the packaging body and communicates with the outside. This reduces oil penetration through the back of the paper, condensation inside the packaging, soft bread, and crumb adhesion through continuous oil blocking in the main high-oil contact area, water vapor transmission on the continuously open outer paper surface, and folding tolerance in multiple directions to the edge pathways.
[0497] In some implementations, the area of the first functional zone accounts for 15% to 60% of the effective area of the food contact side, and the dry mass q1 of PHA per unit area in the first functional zone is 3.0 to 8.0 g / m². 2 The planar projected area of the PHA coverage area in the second functional zone accounts for 15% to 60% of the total planar projected area of the second functional zone. The area-weighted average dry mass per unit area of PHA within the second functional zone, q2, is 0.10 to 1.75 g / m². 2 Furthermore, q1 > q2; the minimum effective width of the exposed cellulose continuous pathway is 1.0–6.0 mm. These ranges are used to further define the spatial distribution, regional continuity, and industrial preparation conditions of the PHA material.
[0498] Those skilled in the art should understand that the above embodiments are merely exemplary and not intended to limit the scope of the invention. The scope of protection of the present invention is defined by the appended claims. Any modifications, equivalent substitutions, improvements, etc., made to the technical solutions of the present invention within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot hamburgers, characterized in that, Includes a fiber-based paper and a polyhydroxyalkanoate coating pattern disposed on the food contact side of the fiber-based paper; The food contact side includes a first functional area and a second functional area that do not overlap with each other. The first functional area is defined by a closed boundary and is spaced apart from the edge of the fiber-based paper. The second functional area is located on the outer periphery of the first functional area and extends to the edge of the fiber-based paper. The polyhydroxyalkanoate coating pattern forms a continuous polyhydroxyalkanoate barrier phase in the first functional region, and the planar projected area of the largest polyhydroxyalkanoate connected domain in the continuous polyhydroxyalkanoate barrier phase accounts for ≥70% of the planar projected area of the first functional region; The second functional region includes a polyhydroxyalkanoate-covered area and an exposed cellulose continuous phase formed by the exposed cellulose surface of the fiber-based paper, wherein the planar projected area of the largest exposed cellulose connected domain in the exposed cellulose continuous phase accounts for C2≥30% of the planar projected area of the second functional region; The paper-based packaging structure has at least two folding areas, a predetermined folding overlap area, and a predetermined area for fixing the packaging label, all defined by a predetermined package pattern. The at least two folding areas are located within the second functional area. The maximum exposed cellulose connectivity includes at least two continuous exposed cellulose pathways extending from the outer periphery of the first functional area to the edge of the fiber-based paper. Each of the continuous exposed cellulose pathways forms exposed cellulose to the edge end at the edge it reaches. The at least two continuous exposed cellulose pathways pass through different folded areas and reach different edges of the fiber-based paper. The exposed cellulose continuous pathway, the exposed cellulose to the edge end, the predetermined folding overlap area, and the predetermined packaging fixing label area have a fixed layout position relationship, such that after the paper-based packaging structure is folded according to the predetermined package pattern and a packaging fixing label is set in the predetermined packaging fixing label area, at least one of the exposed cellulose to the edge end is located on the outer surface of the formed packaging body and communicates with the outside of the packaging body.
2. The partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot hamburgers according to claim 1, characterized in that, The dry mass per unit area of polyhydroxyalkanoate in the first functional region is higher than the area-weighted average dry mass per unit area of polyhydroxyalkanoate in the second functional region.
3. The partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot hamburgers according to claim 1, characterized in that, The fiber-based paper has four paper edges, and the predetermined wrapping pattern defines four folded areas that correspond to the four paper edges and are located within the second functional area. The maximum exposed cellulose connectivity includes four continuous exposed cellulose pathways, which pass through the four folded areas and reach the four paper edges.
4. The partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot hamburgers according to claim 1, characterized in that, The inner periphery of the second functional area is provided with a continuous polyhydroxyalkanoate oil barrier boundary band, which is connected to the continuous polyhydroxyalkanoate barrier and continuously surrounds the first functional area along the entire outer periphery. The outer edge of the continuous polyhydroxyalkanoate oil barrier boundary band constitutes the inner starting boundary of the exposed cellulose continuous pathway.
5. The partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot hamburgers according to claim 1, characterized in that, The paper-based packaging structure does not have vent holes or vent cuts that penetrate the fiber-based paper, nor does it have interlayer venting channels.
6. A method for preparing the partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for hot food hamburger wrapping as described in claim 1, characterized in that, Includes the following steps: Step 1: Based on the predetermined package design, determine a first functional area, a second functional area located around the periphery of the first functional area and extending to a predetermined cutting line, at least two folding areas located within the second functional area, a predetermined folding overlap area, and a predetermined area for fixing the packaging label on the food contact side of the fiber-based paper. Also determine at least two continuous uncoated lines that pass through different folding areas and extend to different predetermined cutting lines. The continuous uncoated lines, the predetermined folding overlap area, and the predetermined area for fixing the packaging label have a fixed positional relationship, such that after cutting along the predetermined cutting line, at least two of the continuous uncoated lines form continuous exposed cellulose pathways that reach different paper edges. After folding the resulting paper-based packaging structure and setting the packaging label, at least one exposed cellulose edge end formed by the continuous exposed cellulose pathway at the corresponding paper edge is located on the outer surface of the formed packaging and communicates with the outside. Step 2: Apply a water-based coating containing polyhydroxyalkanoate particles in a patterned manner to a portion of the first functional area and the second functional area, while retaining the continuous uncoated lines, to obtain a patterned wet-coated fiber-based paper. Step 3: Dry the patterned wet-coated fiber base paper, so that the polyhydroxyalkanoate particles in the first functional area merge with each other to form a continuous polyhydroxyalkanoate barrier phase, and so that the second functional area forms a polyhydroxyalkanoate covered area and an exposed cellulose continuous phase formed by the exposed cellulose surface corresponding to the continuous uncoated lines, to obtain the patterned dry fiber base paper. Step 4: Cut the patterned dry fiber base paper along the predetermined cutting line so that at least two continuous uncoated lines form continuous exposed cellulose pathways that pass through different folded areas and reach different paper edges, and form the exposed cellulose to the edge end at the corresponding paper edge.
7. The preparation method according to claim 6, characterized in that, The same water-based coating, the same patterned coating plate, and the same coating unit are used for patterned coating in the first functional area and the second functional area. The same patterned coating plate includes a coating pattern corresponding to the first functional area, a coating pattern corresponding to the second functional area, and an uncoated line pattern corresponding to at least two consecutive uncoated lines. The fiber-based paper undergoes patterning of the water-based coating in a single pass through the coating unit, and is continuously dried to form the polyhydroxyalkanoate continuous barrier phase, the polyhydroxyalkanoate covered area, and the exposed cellulose continuous phase.
8. The preparation method according to claim 6, characterized in that, The highest value among the main melting peak temperatures of the second heating phases of each polyhydroxyalkanoate contained in the water-based coating, measured by differential scanning calorimetry, is recorded as the highest main melting peak temperature T. m,max Before the patterned wet-coated fiber-based paper enters the final high-energy drying zone, the residual moisture content is ensured to be no more than 5% of the initial coating moisture content; and the paper surface temperature on the food contact side is continuously maintained at or above the highest main melting peak temperature T. m,max The time is 1.0 to 3.0 seconds.
9. A method of using the partitioned steam venting and oil-blocking shape-preserving paper-based packaging structure for wrapping hot hamburgers according to claim 1, characterized in that, Includes the following steps: With the food-contact side of the paper-based packaging structure facing the hot hamburger, fold the paper-based packaging structure around the hot hamburger according to the predetermined wrapping pattern; A packaging fixing label is provided in the predetermined area of the packaging fixing label, such that at least one of the exposed cellulose ends is located on the outer surface of the formed hot food hamburger package and communicates with the outside of the hot food hamburger package.
10. The method of use according to claim 9, characterized in that, The hot hamburger forms a frontal projection of the hot hamburger on the food contact side, and the overlap area between the frontal projection of the hot hamburger and the first functional area accounts for 92% to 100% of the area of the frontal projection of the hot hamburger. At least a portion of the second functional area is located on the outer periphery of the frontal projection of the hot hamburger.
Citation Information
Patent Citations
A high-permeability paper material for vapor packaging, its manufacturing method and application
CN114438824B
Bio-based PHA oil-blocking and moisture-permeable coating for hamburger paper, coated paper and preparation method
CN120759147B
Controlled atmosphere container for respiring produce and method of retarding maturation of packaged respiring produce
EP0676920B1
Oil-resistant paper
JP4520138B2
Venting carton and blank therefor
US4355757A