A hanging polar pendant group-containing biphenyl type epoxy resin cured product, a method for producing the same, and use thereof

By using a biphenyl-type epoxy resin structure with suspended polar side groups, the contradiction between rigidity and density in traditional epoxy resins is resolved, resulting in a significant improvement in the tensile and compressive properties of cured epoxy resins. This forms a denser cross-linked network, meeting the high-performance requirements of extreme working conditions.

CN122854548BActive Publication Date: 2026-11-24SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611338151.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-24
Estimated Expiration
2046-08-31

AI Technical Summary

Technical Problem

Traditional high-performance epoxy resins present a contradiction between improving rigidity and density, making it difficult to achieve a comprehensive improvement in the mechanical properties of the material, especially in terms of insufficient resistance to compressive deformation and high yield strength under complex alternating stress fields.

Method used

The biphenyl-type epoxy resin structure with suspended polar side groups provides high rigidity through the biphenyl backbone and suspends polar side groups at specific sites to form a dense hydrogen bond network, fills free volume, and enhances intermolecular forces. The preparation method includes gradient temperature curing and specific monomer reaction.

Benefits of technology

It significantly improves the tensile and compressive properties of epoxy resin cured products, enhances the elastic modulus and compressive strength, forms a denser cross-linked network, and achieves a comprehensive improvement in mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122854548B_ABST
    Figure CN122854548B_ABST
Patent Text Reader

Abstract

This invention provides a biphenyl-type epoxy resin cured product with suspended polar side groups, its preparation method, and its applications, belonging to the field of advanced materials technology. This invention prepares an epoxy resin cured product by curing an epoxy resin monomer and a curing agent as shown in Formula 1. This cured product utilizes the rigid anchoring effect of the biphenyl backbone, combined with the space-filling effect of the polar side groups and hydrogen bonding, to form a denser cross-linked network. Compared with epoxy resin cured products with diphenylmethane and pure biphenyl structures, the cured product of this invention significantly improves its tensile modulus, compressive strength, and compressive modulus, while also achieving substantial improvements. This provides a new design concept for the development of high-performance epoxy resin materials for extreme working conditions. Formula 1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of advanced materials technology, specifically relating to a biphenyl-type epoxy resin cured product with suspended polar side groups, its preparation method, and its uses. Background Technology

[0002] High-performance epoxy resins, with their outstanding mechanical properties, thermal stability, and chemical corrosion resistance, have been widely used in aerospace, deep-sea exploration, transportation equipment, sporting goods, electronic products, and electronic packaging, serving as indispensable key matrix materials for extreme service environments. As high-end equipment continues to evolve towards lightweight design, the industry is setting increasingly stringent standards for the elastic modulus and compressive strength of epoxy resin matrices.

[0003] Traditional high-performance epoxy resins (such as tetrafunctional resin systems with diphenylmethane as the backbone) can form dense cross-linked networks after curing, possessing basic rigidity and mechanical strength. However, they have inherent defects: on the one hand, their intrinsic flexibility not only limits further improvement in the overall rigidity of the system, but also makes it difficult to meet the stringent requirements for compressive deformation resistance and high yield strength under complex alternating stress fields; on the other hand, the large-volume rigid aromatic ring structures introduced into the resin backbone often disrupt the regularity of the close packing of polymer chains, drastically increasing the steric hindrance within the cross-linked system. This "rigid support" in the microscopic topology is usually accompanied by the generation of a large amount of unfilled "free volume," leading to a looser micro-cross-linked network and severely weakening intermolecular interactions. Therefore, macroscopically, the improvement in the material's elastic modulus and compressive strength is far less than theoretically expected, and it is even impossible to achieve a comprehensive balance of mechanical properties.

[0004] In summary, traditional high-performance epoxy resins generally suffer from an intrinsic contradiction between "high rigidity of the skeleton" and "high density of the cross-linked network". How to resolve this contradiction and achieve synergistic regulation of steric hindrance and microscopic intermolecular forces, thereby breaking through the mechanical modulus and compressive strength, is a technical problem that urgently needs to be solved in the field of polymer materials. Summary of the Invention

[0005] The purpose of this invention is to provide a biphenyl-type epoxy resin cured product with suspended polar side groups, its preparation method, and its uses.

[0006] This invention provides a cured epoxy resin product, which is obtained by curing epoxy resin monomers and a curing agent. The structure of the epoxy resin monomer is as follows: R1 and R2 are independently -O(CH2). n1 CH3、-COO(CH2) n2 CH3、-OCO(CH2) n3 CH3、-CO(CH2) n4CH3 or -CONH-(CH2) n5 CH3, n1, n2, n3, n4, n5 are independently selected from integers from 0 to 3.

[0007] Furthermore, the structure of the epoxy resin monomer is as follows: The n1, n2, n3, n4, and n5 are independently selected from 0 or 1.

[0008] Furthermore, the structure of the epoxy resin monomer is as follows: .

[0009] Furthermore, the molar ratio of the epoxy resin monomer to the curing agent is (1~10):(0.05~2).

[0010] Furthermore, the molar ratio of the epoxy resin monomer to the curing agent is 1:0.5.

[0011] Furthermore, the curing agent is selected from at least one of amine curing agents, acid anhydride curing agents, phenolic curing agents, and imidazole curing agents.

[0012] Further, the amine curing agent is selected from at least one of 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, m-phenylenediamine, m-phenylenediamine, diaminodiphenyl ether, 4,4'-diaminobenzophenone, 4,4'-diaminobenzoylaniline, diethyltoluenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, isophoronediamine, polyetheramine; the anhydride curing agent is selected from methylhexahydrophthalic anhydride, methyl... The curing agent is selected from at least one of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, pyromellitic anhydride, methylnadic anhydride, and dodecenylsuccinic anhydride; the phenolic curing agent is selected from at least one of phenolic resin, cresol phenolic resin, cashew phenol-modified phenolic resin, bisphenol A phenolic resin, and o-cresol epoxy resin; the imidazole curing agent is selected from at least one of 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 2-phenylimidazole, and imidazoline derivatives.

[0013] The present invention also provides a method for preparing epoxy resin cured products, comprising the following steps: mixing epoxy resin monomer and curing agent, degassing and then curing to obtain epoxy resin cured products.

[0014] Furthermore, the curing process is a gradient temperature curing process.

[0015] Furthermore, the gradient temperature curing process is as follows: 100~120℃ for 1~3h, 140~160℃ for 2~4h, and 180~200℃ for 2~4h.

[0016] Furthermore, the method for preparing the epoxy resin monomer includes the following steps: dissolving benzidine (… The reaction of imidazole curing agents and epoxy halogenated propane is carried out. After cooling, a ring-closing agent is added, and the mixture is stirred, cooled, filtered, washed, and extracted until the solution pH is 6-8. After standing and separating into layers, the epoxy halogenated propane phase is retained. After removing the epoxy halogenated propane, the epoxy resin monomer is obtained.

[0017] Further, the epoxy halopropane is selected from at least one of epichlorohydrin and epibromopropane; the ring-closing agent is an alkali metal hydroxide; the alkali metal hydroxide is selected from at least one of sodium hydroxide, potassium hydroxide, and lithium hydroxide; the reaction temperature is 80~120℃, and the time is 10~15h; the molar ratio of the biphenyl diamine, epoxy halopropane, and ring-closing agent is (0.05~0.15):(1~2):(0.3~0.6), preferably 0.1:0.5:0.45; the mass of the imidazole curing agent is 0.5~1.5wt% of the biphenyl diamine, preferably 1wt%.

[0018] The present invention also provides the use of epoxy resin cured products in the preparation of equipment for aerospace, deep-sea exploration, transportation equipment, sporting goods, electronic products, electronic packaging and other fields.

[0019] Furthermore, the device is a high-compression-performance component.

[0020] This invention yields a biphenyl-structured epoxy resin cured product containing polar side groups. Compared to diphenylmethane-structured and pure biphenyl-structured (without polar side groups) epoxy resin cured products, it exhibits significantly improved tensile and compressive properties, effectively enhancing the elastic modulus and compressive strength of the epoxy resin cured product, thus achieving a substantial improvement in the overall mechanical properties of the epoxy resin cured product. Furthermore, compared to diphenylmethane-structured epoxy resin cured products, the epoxy resin cured product of this invention forms a denser cross-linked network structure. This is mainly attributed to the synergistic effect of the epoxy resin molecular topology: the biphenyl backbone imparts extremely high inherent stiffness to the system, while the polar side groups suspended at specific sites fill the free volume generated by the cross-linking of the rigid skeleton through a "space-filling effect," simultaneously forming a dense hydrogen bond network with the polar groups within the network, significantly enhancing intermolecular forces.

[0021] Experiments have shown that the cured product (DMBE-DDM) obtained by curing epoxy resin (DMBE) and 4,4-diaminodiphenylmethane (DDM) of this invention, compared with epoxy resin cured products with diphenylmethane structure and pure biphenyl structure, exhibits the following improvements: tensile strength increased by 5.3% and 7.7%, tensile modulus increased by 29.5% and 17.2%, compressive yield strength increased by 32.2% and 28%, compressive modulus increased by 59.3% and 25.4%, and specified yield strength increased by 23.7% and 13.7%, respectively. This directly and fully demonstrates that epoxy resin cured products with biphenyl structure have improved tensile and compressive properties compared to epoxy resin cured products with diphenylmethane structure. Introducing methoxy side groups into the biphenyl structure further enhances the tensile and compressive properties of the epoxy resin cured product, especially showing a significant advantage in improving the compressive modulus and compressive strength.

[0022] This invention breaks through the technical bottleneck of traditional epoxy resin modification strategies that rely on high-rigidity aromatic ring skeletons, which struggle to balance the rigidity of the resin main chain and the density of the crosslinking network. It achieves a synergistic improvement of both properties at the molecular structure level, through the "synergistic effect of main chain rigidity and side group polarization." While ensuring the high modulus of the cured product, it also improves the compressive strength, providing a new design solution for the development of high-performance epoxy resin matrices and their curing materials for extreme working conditions.

[0023] Obviously, based on the above description of the present invention, and according to common technical knowledge and conventional methods in the field, various other modifications, substitutions or alterations can be made without departing from the basic technical concept of the present invention.

[0024] The following detailed embodiments further illustrate the above-described content of the present invention. However, this should not be construed as limiting the scope of the present invention to the following embodiments. All technologies implemented based on the above-described content of the present invention fall within the scope of the present invention. Attached Figure Description

[0025] Figure 1 It is the 1H NMR spectrum of epoxy resin (DMBE).

[0026] Figure 2 The following are the mechanical property test results of different epoxy resin cured products: (a) Tensile strength and tensile modulus of AG80-DDM, BZAE-DDM and DMBE-DDM; (b) Compressive yield strength, compressive modulus and specified yield strength of AG80-DDM, BZAE-DDM and DMBE-DDM.

[0027] Figure 3 These are the XRD test results of AG80-DDM and DMBE-DDM. Detailed Implementation

[0028] The raw materials and equipment used in this invention are all known products, obtained by purchasing commercially available products.

[0029] Example 1: Preparation and Characterization of Cured Epoxy Resin 1.1 Preparation of epoxy resin monomer (DMBE) 3,3-Dimethoxybenzidine (DMB, 0.1 mol) was added to a 500 mL flask, followed by 2-methylimidazole (1 wt% of DMB) and epichlorohydrin (1.5 mol). The reaction was carried out at 100 °C for 12 h, then cooled to 45 °C, and sodium hydroxide granules (0.45 mol) were added. The mixture was stirred for another 4 h, cooled, filtered, and washed with deionized water until a clear solution was obtained. The solution was then extracted until the pH reached 7. After standing and separating the layers, the epichlorohydrin phase was retained. The epichlorohydrin phase was concentrated using a rotary evaporator to remove the epichlorohydrin, yielding the epoxy resin monomer (DMBE). The structural formula of DMBE is as follows: .

[0030] 1.2 Preparation of epoxy resin cured product (DMBE-DDM) The DMBE and 4,4-diaminodiphenylmethane (DDM) were mixed in a molar ratio of 1:0.5, and the mixture was degassed under vacuum. Then, the mixture was cured by gradient temperature increase under the following conditions: 110℃ for 2 hours, 150℃ for 3 hours, and 190℃ for 3 hours to obtain the epoxy resin cured product (DMBE-DDM).

[0031] 1.3 Characterization of epoxy resin monomer (DMBE) (1) Characterization method: Nuclear magnetic resonance spectroscopy (NMR) was performed on a Bruker AV III HD 400MHz using DMSO-d6 as solvent.

[0032] (2) Characterization results: such as Figure 1 The 1H NMR spectrum of DMBE shown is presented in this example, indicating the successful synthesis of DMBE. 1 HNMR (400MHz, DMSO, DMBE) δ7.18-7.10 (m, 6H), δ3.90-3.82 (s, 6H), δ3.45-3 .42(d,4H), δ3.22-3.17(d,4H), δ3.06(s,4H), δ2.69(s,4H), δ2.51(s,4H). Comparative Example 1: Preparation of epoxy resin cured product (AG80-DDM) Referring to Example 1, section 1.2, the only difference is that DMBE is replaced with 4,4-diaminodiphenylmethane tetraglycidylamine (AG80). .

[0033] Comparative Example 2: Preparation of Cured Epoxy Resin 2.1 Preparation of epoxy resin monomer (BZAE) Referring to Example 1, 1.1, the only difference is that DMB is replaced with benzidine (BZA); the structural formula of BZA is: .

[0034] 2.2 Preparation of epoxy resin cured product (BZAE-DDM) Referring to section 1.2 of Example 1, the only difference is that DMBE is replaced with BZAE.

[0035] Experiment Example 1: Mechanical Property Testing 1.1 Experimental Methods Tensile strength and tensile modulus testing: The material was subjected to tensile testing using a universal testing machine in accordance with ASTM D638 standard at a rate of 1 mm / min.

[0036] Compression yield strength, compression modulus, and specified yield strength tests: The material was subjected to compression tests using a universal testing machine in accordance with GB / T 2567-2021 standard, at a rate of 2 mm / min.

[0037] 1.2 Experimental Results like Figure 2 As shown in Table 1, compared to AG80-DDM, both BZAE-DDM and DMBE-DDM with biphenyl structures exhibit improved tensile modulus, compressive yield strength, compressive modulus, and specified yield strength. However, the improvement in mechanical properties of BZAE-DDM with a pure biphenyl backbone is limited, while the mechanical properties of DMBE-DDM with suspended methoxy side groups are further improved.

[0038] Compared to AG80-DDM, DMBE-DDM showed a 5.3% increase in tensile strength, while BZAE-DDM and DMBE-DDM showed increases of 10.5% and 29.5% in tensile modulus, respectively. Their compressive yield strengths increased by 3.3% and 32.2%, respectively, their compressive modulus increased by 27.1% and 59.3%, respectively, and their specified yield strengths increased by 8.8% and 23.7%, respectively. Compared to BZAE-DDM, DMBE-DDM showed a 7.7% increase in tensile strength, a 17.2% increase in tensile modulus, a 28% increase in compressive yield strength, a 25.4% increase in compressive modulus, and a 13.7% increase in specified yield strength.

[0039] This indicates that, compared to epoxy resins with a diphenylmethane structure, epoxy resins with a biphenyl structure exhibit improved tensile and compressive properties. Furthermore, epoxy resins obtained by introducing methoxy side groups onto the biphenyl structure further enhance tensile and compressive properties, exhibiting superior tensile strength, tensile modulus, compressive yield strength, compressive modulus, and specified yield strength. In particular, DMBE-DDM shows a significant increase in compressive yield strength and compressive modulus compared to AG80-DDM and BZAE-DDM, significantly improving the compressive strength of the epoxy resin.

[0040] The above experimental results show that, compared with epoxy resin cured products with diphenylmethane structure and pure biphenyl structure, the epoxy resin cured product with biphenyl structure containing methoxy side groups of the present invention has significantly improved tensile and compressive properties, and significantly enhanced comprehensive mechanical properties.

[0041] Table 1 Mechanical properties of different cured products Experiment Example 2: XRD Test 2.1 Experimental Methods X-ray diffraction was performed using Ultima IV, with a detection range of 5–90° and a step size of 0.02°.

[0042] 2.2 Experimental Results like Figure 3 As shown, both AG80-DDM and DMBE-DDM exhibit broad diffuse diffraction peaks in the range of 2θ = 15° to 30°, indicating that both epoxy resins form typical, completely amorphous cross-linked networks lacking long-range geometric order after curing. Specifically, the diffraction peak maximum of AG80-DDM occurs at 2θ = 18.6°, while the diffraction peak of DMBE-DDM shifts significantly to higher angles, reaching 2θ = 23.1°. According to the Bragg equation (nλ = 2d sinθ) for amorphous polymers, the increase in diffraction angle (2θ) directly corresponds to a significant reduction in the average interchain spacing in the cross-linked network. This suggests that the highly conjugated biphenyl structure promotes the close arrangement of local chain segments, and the electron-rich methoxy groups also participate in the formation of a dense intermolecular hydrogen bond network, both contributing to the formation of a dense cross-linked network.

[0043] In summary, compared with diphenylmethane and pure biphenyl structure epoxy resin cured products (AG80-DDM and BZAE-DDM), the methoxy-containing biphenyl structure epoxy resin cured product (DMBE-DDM) prepared in this invention exhibits significantly improved tensile strength, tensile modulus, compressive yield strength, compressive modulus, and specified yield strength, thus significantly enhancing the overall mechanical properties of epoxy resin cured products. Particularly in terms of compressive properties, compared with AG80-DDM and BZAE-DDM, DMBE-DDM shows a substantial increase in compressive yield strength and compressive modulus, with compressive yield strength increasing by 32.2% and 28%, respectively, and compressive modulus increasing by 59.3% and 25.4%, respectively. This invention achieves improved compressive strength while maintaining high modulus of the cured product, providing a new design solution for the development of high-performance epoxy resin matrices and their cured materials for extreme operating conditions.

Claims

1. A cured epoxy resin product, characterized in that, It is obtained by curing epoxy resin monomers and a curing agent, and the structure of the epoxy resin monomers is as follows: The molar ratio of the epoxy resin monomer to the curing agent is (1~10):(0.05~2).

2. The epoxy resin cured product according to claim 1, characterized in that, The curing agent is selected from at least one of amine curing agents, acid anhydride curing agents, phenolic curing agents, and imidazole curing agents.

3. The epoxy resin cured product according to claim 2, characterized in that, The amine curing agent is selected from at least one of 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, m-phenylenediamine, m-phenylenediamine, diaminodiphenyl ether, 4,4'-diaminobenzophenone, 4,4'-diaminobenzoylaniline, diethyltoluenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, isophoronediamine, and polyetheramine; the anhydride curing agent is selected from methylhexahydrophthalic anhydride, The curing agent is selected from at least one of methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, pyromellitic anhydride, methylnadic anhydride, and dodecenylsuccinic anhydride; the phenolic curing agent is selected from at least one of phenolic resin, cresol phenolic resin, cashew phenol-modified phenolic resin, and bisphenol A phenolic resin; the imidazole curing agent is selected from at least one of 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 2-phenylimidazole, and imidazoline derivatives.

4. The method for preparing the epoxy resin cured product according to any one of claims 1 to 3, characterized in that, The process includes the following steps: mixing epoxy resin monomers and curing agents, degassing, and then curing to obtain cured epoxy resin.

5. The use of the epoxy resin cured product according to any one of claims 1 to 3 in the preparation of equipment for aerospace, deep-sea exploration, transportation equipment, sporting goods, electronic products, and electronic packaging.

Citation Information

Patent Citations

  • Difunctional biphenyl compounds, preparation, and uses

    EP3749637A1

  • Curable epoxy composition, film obtained using same, layered film, prepreg, layered body, cured product, and composite

    WO2016067330A1