Uvioresistant hot oxygen double aging modified asphalt and preparation method thereof
By using a composite microparticle modification method to disperse aminated titanium dioxide and encapsulate antioxidants in modified asphalt, the aging problem of modified asphalt under ultraviolet light and heat-oxygen environments was solved, improving its aging resistance and service life.
Patent Information
- Application Number
- CN202611281024.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-08-24
AI Technical Summary
When existing modified asphalt ages under ultraviolet light and heat-oxygen conditions, the molecular bonds break, leading to reduced flexibility and weakened adhesion, resulting in aggregate spalling and mixture breakage, thus shortening the service life of roads.
A composite microparticle modification method is used to form UV- and heat- and oxygen-resistant modified asphalt by dispersing aminated titanium dioxide on a core and coating it with an organic shell to encapsulate antioxidants.
It improves the resistance of modified asphalt to ultraviolet radiation and thermal oxidation, prolongs the release time of antioxidants, enhances compatibility with base asphalt and SBS, improves dispersion uniformity, and extends the service life of roads.
Smart Images

Figure CN122854822B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of modified asphalt preparation technology, and particularly relates to a UV-resistant, heat-oxidative dual-aging modified asphalt and its preparation method. Background Technology
[0002] Modified asphalt is a high-performance material used in road maintenance. When used, modified asphalt is mixed with aggregates in a specific ratio to form a mixture. An asphalt film forms on the aggregate surface, which, after paving and compaction, fills and bonds to road defects, achieving efficient repair. However, during use, the surface of the mixture is exposed to ultraviolet radiation for extended periods. The ultraviolet energy breaks the chemical bonds in the asphalt molecules, inducing photo-oxidation reactions and generating free radicals. This triggers an oxidation chain reaction, causing lightweight components to gradually transform into heavy components through dehydrogenation and cross-linking. The flexibility of the asphalt film is significantly reduced, and its adhesion to the aggregate weakens. Ultimately, repeated wheel rolling leads to problems such as aggregate spalling and mixture breakage, shortening the road's service life.
[0003] Chinese patent application CN110872442A discloses an asphalt anti-UV aging modifier, which is prepared by the following method: adding nano-titanium dioxide powder to water and shaking, adding dopamine hydrochloride and stirring, adding buffer solution to adjust the pH value, continuing stirring, filtering and drying to obtain preliminarily modified nano-titanium dioxide; then adding it together with a hindered amine light stabilizer to an organic solvent, reacting under heating and reflux conditions, cooling, and then filtering, washing and drying to obtain the asphalt anti-UV aging modifier. Although the polydopamine layer reduces the high surface energy of titanium dioxide, the catechol hydroxyl and amino functional groups in the polydopamine layer have significant polarity, which is incompatible with the weakly polar colloidal environment of the asphalt as a whole. Titanium dioxide has insufficient wettability in asphalt and is prone to weak agglomeration or sedimentation segregation in asphalt, resulting in uneven spatial distribution of ultraviolet shielding effect. In addition, the ultraviolet aging modifier in this application does not contain antioxidants. Under high temperature and aerobic environment, carbon-carbon double bonds and alkanes in asphalt are easily oxidized to generate carbonyl and sulfoxide groups, which leads to hardening of the asphalt film and easy separation from the aggregate under vehicle rolling. Summary of the Invention
[0004] This invention provides a UV-resistant and heat-oxidation dual-aging modified asphalt and its preparation method. The asphalt is prepared by mixing base asphalt and SBS, and then adding composite microparticles. The composite microparticles include a core, an organic shell, and an antioxidant encapsulated in the pores of the organic shell. In the core, titanium dioxide is dispersed and fixed on silica, inhibiting titanium dioxide agglomeration and allowing titanium dioxide to fully exert its UV resistance, thus improving the UV aging resistance of this invention. The encapsulation of pores increases the effective release time of the antioxidant and reduces its self-oxidation loss, enabling long-term utilization of the antioxidant and improving the heat oxidation resistance of this invention.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing UV- and heat-oxidation resistant modified asphalt includes the following steps: S1. Aminated titanium dioxide and epoxidized silica are dispersed in DMF (N,N-dimethylformamide), deionized water is added and reacted, and after modification by MPS (γ-methacryloyloxypropyltrimethoxysilane) and drying, the core is obtained; S2. A coating solution is sprayed onto the core, the mixture is heated to react, dispersed in an antioxidant solution, impregnated, and dried to obtain composite microparticles. The coating solution is prepared by mixing LMA (lauryl methacrylate), PEG (polyethylene glycol), HEMA (2-hydroxyethyl methacrylate), EGDMA (ethylene glycol dimethacrylate), an initiator, and a solvent. The antioxidant solution is prepared by mixing an antioxidant with acetone. S3. Mix the base asphalt and SBS (styrene-butadiene-styrene triblock copolymer), add the composite microparticles and mix well to obtain UV-resistant heat and oxygen dual-aging modified asphalt.
[0006] This invention incorporates composite microparticles into a mixture of asphalt and SBS to obtain UV- and heat-oxidation-resistant modified asphalt. The composite microparticles comprise a core, an organic shell encapsulating the core, and an antioxidant encapsulated within the pores of the organic shell. During preparation, firstly, under the facilitation of deionized water, the primary amino groups on aminated titanium dioxide and the epoxy groups on epoxidized silica undergo a ring-opening reaction to form a core precursor. Subsequently, carbon-carbon double bonds are introduced onto the core precursor through the hydrolysis and condensation reaction of MPS. Under the thermal initiation of an initiator, LMA, HEMA, EGDMA, and the carbon-carbon double bonds on the core surface undergo a free radical copolymerization reaction, forming an organic shell with PEG as a pore-forming template outside the core. After PEG removal, pores are formed on the organic shell. The swelling effect of acetone on the organic shell allows antioxidant molecules to diffuse into the pores. After drying, the organic shell shrinks, and the antioxidant is encapsulated within the pores, yielding the composite microparticles.
[0007] During core preparation, the amino groups grafted onto the aminated titanium dioxide inhibit titanium dioxide agglomeration due to steric hindrance, which facilitates the dispersion and fixation of the aminated titanium dioxide on the epoxidized silica, improving the dispersion uniformity of titanium dioxide and enabling it to fully exert its UV resistance properties. The long-chain alkyl groups introduced by LMA in the organic shell improve the compatibility of the composite particles with the matrix asphalt and SBS, promoting the uniform dispersion of the composite particles in the matrix asphalt and SBS mixture, further enhancing the dispersion uniformity of titanium dioxide and improving the UV aging resistance of the present invention. The antioxidant is encapsulated in the pores, increasing the diffusion resistance of the antioxidant, prolonging the release time of the antioxidant, and reducing the direct contact between the antioxidant and external oxygen, inhibiting the ineffective loss of the antioxidant due to its own oxidation, and realizing the long-term utilization of the antioxidant.
[0008] Furthermore, the aminated titanium dioxide is prepared by the following method: TEOS (tetraethyl orthosilicate) and 94-96 wt% ethanol solution are mixed, titanium dioxide is added and dispersed, ammonia is added dropwise to adjust the pH to 8.3-8.7, the reaction is carried out for 2-3 hours, filtered, washed with ethanol solution and anhydrous ethanol, and then dispersed in 94-96 wt% ethanol solution. Acetic acid solution is added dropwise to adjust the pH to 4-5, APTES (γ-aminopropyltriethoxysilane) is added and reacted for 1.5-2 hours, filtered, washed with deionized water and DMF to obtain aminated titanium dioxide.
[0009] A silicon-oxygen network is formed on titanium dioxide through the hydrolysis and condensation reaction of TEOS. Subsequently, a condensation reaction occurs between the hydrolysis product of APTES and the silanol groups of the silicon-oxygen network, and amino groups containing primary amino groups are covalently grafted onto the silicon-oxygen network to obtain aminated titanium dioxide, which provides a functional group basis for the covalent attachment of aminated titanium dioxide to epoxide silicon dioxide.
[0010] Furthermore, the epoxidized silica is prepared by the following method: silica is dispersed in toluene, heated to 108-112℃ and refluxed to remove water for 20-30 min, cooled to 75-80℃ and GPTMS (γ-glycidyl etheroxypropyltrimethoxysilane) is added, the mixture is heated to 108-112℃ and refluxed for 3-4 h, filtered, and washed with toluene and DMF to obtain epoxidized silica.
[0011] Under anhydrous conditions, the reaction between the methoxy group of GPTMS and the silanol group of silica promotes the covalent grafting of epoxy groups onto silica, resulting in epoxidized silica. This provides a functional group basis for the subsequent dispersion and fixation of aminated titanium dioxide through the ring-opening reaction of primary amines and epoxy groups.
[0012] Further, in step S1, aminated titanium dioxide and epoxidized silicon dioxide are dispersed in DMF, deionized water is added, the temperature is raised to 55-59℃, and the reaction is carried out for 2.5-3 hours. After filtration, the mixture is washed with DMF and anhydrous ethanol and then mixed with the pre-hydrolyzed solution for 3-4 hours. After filtration, the mixture is washed with deionized water and anhydrous ethanol and then dried under reduced pressure to obtain the core-loaded solution. The pre-hydrolyzed solution is prepared by adding acetic acid solution dropwise to a 94-96 wt% ethanol solution to adjust the pH to 4-5, adding MPS and mixing for 2-3 hours to obtain the pre-hydrolyzed solution.
[0013] During the preparation of the core, the amino groups inhibit the aggregation of aminated titanium dioxide under steric hindrance, which is beneficial for the dispersion and fixation of aminated titanium dioxide on epoxidized silica to obtain the core precursor. Under pH 4-5 conditions, the hydrolysis products of MPS undergo a condensation reaction with the residual silanol groups on the core precursor, introducing carbon-carbon double bonds into the core precursor to obtain the core. The carbon-carbon double bonds can participate in the free radical copolymerization reaction of LMA, HEMA and EGDMA under the thermal initiation conditions of the initiator, so that the organic shell is connected to the core through covalent bonds, inhibiting the peeling of the organic shell during the mixing of the organic shell and the matrix bitumen and preventing the sudden release of antioxidants.
[0014] Furthermore, during the preparation of the pre-hydrolyzed solution, after adjusting the pH value to 4-5, MPS and MTMS (methyltrimethoxysilane) are added and reacted for 2-3 hours.
[0015] MTMS can react with the residual silanol groups on the core surface to generate silanyl methyl end capping structures, reducing the impact of the introduction of amino groups on the hydrophobicity of the core surface. This facilitates the uniform spreading of the coating solution on the core surface, thereby forming a uniform and complete organic shell. This reduces the burst release of antioxidants caused by local thinning of the organic shell, enabling longer-lasting and more controllable release of antioxidants and slowing down the ineffective consumption of antioxidants in aerobic environments.
[0016] Further, in step S2, the core is placed in a fluidized bed and a nitrogen flow is introduced for aeration. The coating solution is sprayed in under the conditions of an inlet air temperature of 80-85℃ and an outlet air temperature of 75-78℃. The reaction is carried out for 4-5 hours. After cooling, the core is dispersed in a 60-65wt% ethanol solution and soaked and washed for 3-4 hours. After filtration, the core is washed with anhydrous ethanol and acetone and then dispersed in an antioxidant solution for 3-4 hours. After filtration, the core is dried under reduced pressure to obtain composite microparticles. In the coating solution, the solvent is butyl acetate and n-butanol, and the initiator is AIBN (azobisisobutyronitrile).
[0017] The organic shell is washed sequentially with 60-65 wt% ethanol aqueous solution and anhydrous ethanol to remove PEG and form pores in situ. Then, acetone is used to replace the water and ethanol in the pores, which facilitates the diffusion of antioxidant molecules into the pores of the swollen organic shell. Finally, the acetone is removed by vacuum drying, the volume of the organic shell shrinks, the pores shrink and the antioxidant is physically confined, thus achieving the encapsulation of the antioxidant.
[0018] Furthermore, the molecular weight of the PEG is 400-700 g / mol.
[0019] Furthermore, in step S3, the base asphalt and SBS are mixed at 168-172℃, cooled to 85-90℃, composite microparticles are added and mixed, and then cooled to obtain UV-resistant heat-oxidation dual-aging modified asphalt.
[0020] A UV-resistant, heat- and oxygen-resistant modified asphalt, prepared by the above-mentioned method for preparing UV-resistant, heat- and oxygen-resistant modified asphalt, comprises the following raw materials in parts by weight: 400-410 parts of base asphalt, 18-22 parts of SBS, and 8-10 parts of composite microparticles; wherein the composite microparticles comprise the following raw materials in parts by weight: 30-35 parts of core carrier, 12-14 parts of LMA, 3-4 parts of PEG, 2-3 parts of HEMA, 0.7-1 parts of EGDMA, 0.2-0.3 parts of initiator, and 7-8 parts of antioxidant, wherein the antioxidant is Irganox 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid).
[0021] Furthermore, the core comprises the following raw materials in parts by weight: 24-28 parts titanium dioxide, 15-19 parts silicon dioxide, 8-10 parts TEOS, 1.2-1.5 parts APTES, 1-1.2 parts GPTMS, 0-1 parts MTMS, and 4-5 parts MPS.
[0022] The present invention has the following beneficial effects: This invention involves mixing composite microparticles with a mixture of base asphalt and SBS to obtain UV-resistant, heat- and oxygen-resistant modified asphalt. The composite microparticles comprise a core, an organic shell coating the core, and an antioxidant encapsulated within the pores of the organic shell. In the preparation of the composite microparticles, aminated titanium dioxide is first covalently linked to epoxidized silica via a ring-opening reaction. Subsequently, a carbon-carbon double bond is introduced through MPS to obtain the core. During the ring-opening reaction, the steric hindrance of the amino groups promotes the dispersion and fixation of the aminated titanium dioxide on the epoxidized silica, inhibiting titanium dioxide agglomeration and facilitating the full utilization of the titanium dioxide's UV resistance. The carbon-carbon double bonds on the core and LMA in the coating solution undergo a free radical copolymerization reaction under the initiation of an initiator. An organic shell containing long-chain alkyl groups, using PEG as a pore-forming template, is constructed outside the core. After washing to remove PEG, pores are introduced into the organic shell. The swelling effect of acetone on the organic shell allows the antioxidant to diffuse into the pores. After drying, the pores shrink, thus encapsulating the antioxidant, prolonging its release time, reducing direct contact between the antioxidant and external oxygen, and inhibiting the ineffective loss of the antioxidant due to its own oxidation, thereby achieving long-term utilization of the antioxidant. The long-chain alkyl groups can improve the compatibility of the composite particles with the matrix asphalt and SBS, enhance the dispersion uniformity of the composite particles, and further improve the dispersion uniformity of titanium dioxide. Attached Figure Description
[0023] Figure 1 The infrared spectrum of the nucleus prepared in Example 5; Figure 2 The nitrogen adsorption-desorption isotherm is obtained by drying the composite microparticles prepared in Example 5 in an environment of 40°C and 10 kPa for 8 hours before immersion in an antioxidant solution. Detailed Implementation
[0024] Preparation Example 1 Mix 8g TEOS and 200g 96wt% ethanol solution, stir at 300rpm for 10min, add 28g titanium dioxide with a particle size of 100nm, sonicate at 100W for 15min, adjust the pH to 8.3 by adding 10wt% ammonia dropwise, stir at 300rpm for 3h, filter, wash twice with 50wt% ethanol solution, wash twice with anhydrous ethanol, add to 200g 96wt% ethanol solution, stir at 800rpm for 15min, adjust the pH to 4 by adding 10wt% acetic acid solution dropwise, add 1.2g APTES, stir at 200rpm for 2h, filter, wash twice with deionized water, wash twice with DMF to obtain aminated titanium dioxide; add 19g silica with a particle size of 10μm to 200g toluene, sonicate at 100W for 15min, heat to 110℃, stir and reflux at 300rpm for 20min, cool to 80℃, add 1.1g GPTMS was heated to 110℃ and refluxed at 300 rpm for 4 h. After filtration, the mixture was washed twice with toluene and twice with DMF to obtain epoxidized silica. Aminated titanium dioxide and epoxidized silica were added to 400 g of DMF and stirred at 800 rpm for 20 min. 10 g of deionized water was added, and the mixture was heated to 58℃ and stirred at 200 rpm for 2.8 h. After filtration, the mixture was washed twice with DMF and four times with anhydrous ethanol to obtain the core-loaded precursor.
[0025] Preparation Example 2 Mix 9g TEOS and 200g of 94wt% ethanol solution, stir at 300rpm for 10min, add 24g of titanium dioxide with a particle size of 100nm, sonicate at 100W for 15min, adjust the pH to 8.5 by adding 10wt% ammonia dropwise, stir at 300rpm for 2.5h, filter, wash twice with 50wt% ethanol solution, wash twice with anhydrous ethanol, add to 200g of 94wt% ethanol solution, stir at 800rpm for 15min, adjust the pH to 4.5 by adding 1.3g of TEOS solution, and then add 1.3g of ethanol solution. APTES was stirred at 200 rpm for 1.5 h, filtered, washed twice with deionized water, and washed twice with DMF to obtain aminated titanium dioxide. 15 g of silica with a particle size of 10 μm was added to 200 g of toluene, ultrasonically dispersed at 100 W for 15 min, heated to 108 °C, stirred and refluxed at 300 rpm for 30 min, cooled to 75 °C, 1.2 g of GPTMS was added, heated to 108 °C, stirred and refluxed at 300 rpm for 3.5 h, filtered, washed twice with toluene, and washed twice with DMF to obtain epoxidized silica. Aminated titanium dioxide and epoxidized silica were added to 400 g of DMF, stirred at 800 rpm for 20 min, 10 g of deionized water was added, heated to 55 °C, stirred at 200 rpm for 2.5 h, filtered, washed twice with DMF, and washed four times with anhydrous ethanol to obtain the core-loaded precursor.
[0026] Preparation Example 3 Mix 10g TEOS and 200g 95wt% ethanol solution, stir at 300rpm for 10min, add 26g titanium dioxide with a particle size of 100nm, sonicate at 100W for 15min, adjust the pH to 8.7 by adding 10wt% ammonia dropwise, stir at 300rpm for 2h, filter, wash twice with 50wt% ethanol solution, wash twice with anhydrous ethanol, add to 200g 95wt% ethanol solution, stir at 800rpm for 15min, adjust the pH to 5 by adding 10wt% acetic acid solution dropwise, and add 1.5g... APTES was stirred at 200 rpm for 1.8 h, filtered, washed twice with deionized water, and washed twice with DMF to obtain aminated titanium dioxide. 18 g of silica with a particle size of 10 μm was added to 200 g of toluene, ultrasonically dispersed at 100 W for 15 min, heated to 112 °C, stirred and refluxed at 300 rpm for 25 min, cooled to 78 °C, 1 g of GPTMS was added, heated to 112 °C, stirred and refluxed at 300 rpm for 3 h, filtered, washed twice with toluene, and washed twice with DMF to obtain epoxidized silica. Aminated titanium dioxide and epoxidized silica were added to 400 g of DMF, stirred at 800 rpm for 20 min, 10 g of deionized water was added, heated to 59 °C, stirred at 200 rpm for 3 h, filtered, washed twice with DMF, and washed four times with anhydrous ethanol to obtain the core-loaded precursor.
[0027] Example 1 The pH was adjusted to 4 by adding 5 wt% acetic acid solution to 400 g of 95 wt% ethanol solution. 4 g of MPS and 1 g of MTMS were added, and the mixture was stirred at 300 rpm for 2 h to obtain a pre-hydrolyzed solution. The core-loaded precursor was added to the pre-hydrolyzed solution, and the mixture was stirred at 300 rpm for 3.5 h. The mixture was filtered, washed twice with deionized water and twice with anhydrous ethanol, and dried at 40 °C and 10 kPa for 5 h to obtain the core-loaded solution.
[0028] Mix 13g LMA, 3g PEG (molecular weight 400g / mol), 95g butyl acetate, and 17g n-butanol. Heat to 60℃ and stir at 300rpm for 15min. Cool to room temperature, add 2.3g HEMA, 0.7g EGDMA, and 0.25g AIBN, and stir at 300rpm for 15min to obtain the coating solution. Add 8g Irganox 3114 to 200g acetone and stir at 300rpm for 25min to obtain the antioxidant solution. Place 35g of the core carrier in a fluidized bed, circulate nitrogen gas, adjust the inlet air temperature to 80℃ and the outlet air temperature to 75℃, spray the coating solution through a nozzle and maintain the temperature for 5h. After cooling to room temperature, add to 300g of... The composite microparticles were dispersed in a 60wt% ethanol solution by ultrasonication at 100W for 15 min, soaked and washed at 300rpm for 4 h, filtered, washed twice with anhydrous ethanol and three times with acetone, added to an antioxidant solution, stirred and soaked at 400rpm for 3 h, filtered, and dried at 40℃ and 10kPa for 8 h to obtain composite microparticles.
[0029] Mix 405g of base asphalt (preferably AH-70 asphalt) and 18g of SBS (preferably YH-791 linear SBS), heat to 168℃, stir at 1000rpm for 20min, stir at 3000rpm for 25min, cool to 85℃, slowly add 8g of composite microparticles while stirring at 1000rpm, stir at 1000rpm for 10min after addition, and cool to room temperature to obtain UV-resistant heat-oxygen dual-aging modified asphalt.
[0030] The nucleus-loaded precursor used in this embodiment was prepared in Preparation Example 1.
[0031] Example 2 The pH was adjusted to 4 by adding 5 wt% acetic acid solution to 400 g of 95 wt% ethanol solution. 5 g of MPS and 0.8 g of MTMS were added, and the mixture was stirred at 300 rpm for 2 h to obtain a pre-hydrolyzed solution. The core-loaded precursor was added to the pre-hydrolyzed solution, and the mixture was stirred at 300 rpm for 3.5 h. The mixture was filtered, washed twice with deionized water, and washed twice with anhydrous ethanol. The mixture was then dried at 40 °C and 10 kPa for 5 h to obtain the core-loaded solution.
[0032] Mix 13g LMA, 3.5g PEG (molecular weight 400g / mol), 95g butyl acetate, and 17g n-butanol, heat to 60℃, stir at 300rpm for 15min, cool to room temperature, add 2g HEMA, 0.8g EGDMA, and 0.25g AIBN, stir at 300rpm for 15min to obtain the coating solution; add 7.5g Irganox 3114 to 200g acetone, stir at 300rpm for 25min to obtain the antioxidant solution; place 35g of the core carrier in a fluidized bed, circulate nitrogen gas, adjust the inlet air temperature to 80℃ and the outlet air temperature to 75℃, spray the coating solution through a nozzle and keep warm for 5h, cool to room temperature, and then add to 300g of... The composite microparticles were dispersed in a 60wt% ethanol solution by ultrasonication at 100W for 15 min, soaked and washed at 300rpm for 4 h, filtered, washed twice with anhydrous ethanol and three times with acetone, added to an antioxidant solution, stirred and soaked at 400rpm for 3 h, filtered, and dried at 40℃ and 10kPa for 8 h to obtain composite microparticles.
[0033] Mix 400g of base asphalt (preferably AH-70 asphalt) and 19g of SBS (preferably YH-791 linear SBS), heat to 168℃, stir at 1000rpm for 20min, stir at 3000rpm for 25min, cool to 85℃, slowly add 9g of composite microparticles while stirring at 1000rpm, stir at 1000rpm for 10min after addition, and cool to room temperature to obtain UV-resistant heat-oxidation dual-aging modified asphalt.
[0034] The nucleus-loaded precursor used in this embodiment was prepared in Preparation Example 1.
[0035] Example 3 To adjust the pH to 5, add 5wt% acetic acid solution dropwise to 400g of 94wt% ethanol solution. Add 4.5g MPS and 0.9g MTMS, and stir at 300rpm for 3h to obtain a pre-hydrolyzed solution. Add the core-loaded precursor to the pre-hydrolyzed solution, stir at 300rpm for 3h, filter, wash twice with deionized water and twice with anhydrous ethanol, and dry at 40℃ and 10kPa for 5h to obtain the core-loaded solution.
[0036] 12g LMA, 4g PEG (molecular weight 600g / mol), 95g butyl acetate, and 17g n-butanol were mixed, heated to 60℃, stirred at 300rpm for 15min, cooled to room temperature, and 2.5g HEMA, 1g EGDMA, and 0.3g AIBN were added. The mixture was stirred at 300rpm for 15min to obtain the coating solution. 8g Irganox 3114 was added to 200g acetone and stirred at 300rpm for 25min to obtain the antioxidant solution. 33g of the core was placed in a fluidized bed, and nitrogen gas was introduced for aeration. The inlet air temperature was adjusted to 82℃ and the outlet air temperature to 76℃. The coating solution was sprayed through a nozzle and kept at this temperature for 4.5h. After cooling to room temperature, it was added to 300g of... The composite microparticles were dispersed in a 62wt% ethanol solution by ultrasonication at 100W for 15 min, soaked and washed at 300rpm for 3.5 h, filtered, washed twice with anhydrous ethanol and three times with acetone, added to an antioxidant solution, stirred and soaked at 400rpm for 3.5 h, filtered, and dried at 40℃ and 10kPa for 8 h to obtain the composite microparticles.
[0037] Mix 408g of base asphalt (preferably AH-70 asphalt) and 20g of SBS (preferably YH-791 linear SBS), heat to 172℃, stir at 1000rpm for 20min, stir at 3000rpm for 25min, cool to 90℃, slowly add 10g of composite microparticles while stirring at 1000rpm, stir at 1000rpm for 10min after addition, and cool to room temperature to obtain UV-resistant heat-oxidation dual-aging modified asphalt.
[0038] The nucleus-carrying precursor used in this embodiment was prepared in Preparation Example 2.
[0039] Example 4 To adjust the pH to 5, add 5 wt% acetic acid solution dropwise to 400 g of 94 wt% ethanol solution. Add 4.5 g MPS and 1 g MTMS, and stir at 300 rpm for 3 h to obtain a pre-hydrolyzed solution. Add the core-loaded precursor to the pre-hydrolyzed solution, stir at 300 rpm for 3 h, filter, wash twice with deionized water and twice with anhydrous ethanol, and dry at 40 °C and 10 kPa for 5 h to obtain the core-loaded solution.
[0040] 13.5g LMA, 3.5g PEG (molecular weight 600g / mol), 95g butyl acetate, and 17g n-butanol were mixed, heated to 60℃, stirred at 300rpm for 15min, cooled to room temperature, and 3g HEMA, 0.8g EGDMA, and 0.3g AIBN were added. The mixture was stirred at 300rpm for 15min to obtain the coating solution. 7.2g Irganox 3114 was added to 200g acetone and stirred at 300rpm for 25min to obtain the antioxidant solution. 32g of the core was placed in a fluidized bed, and nitrogen gas was introduced for aeration. The inlet air temperature was adjusted to 82℃ and the outlet air temperature to 76℃. The coating solution was sprayed through a nozzle and kept at this temperature for 4.5h. After cooling to room temperature, it was added to 300g of... The composite microparticles were dispersed in a 62wt% ethanol solution by ultrasonication at 100W for 15 min, soaked and washed at 300rpm for 3.5 h, filtered, washed twice with anhydrous ethanol and three times with acetone, added to an antioxidant solution, stirred and soaked at 400rpm for 3.5 h, filtered, and dried at 40℃ and 10kPa for 8 h to obtain the composite microparticles.
[0041] Mix 402g of base asphalt (preferably AH-70 asphalt) and 22g of SBS (preferably YH-791 linear SBS), heat to 172℃, stir at 1000rpm for 20min, stir at 3000rpm for 25min, cool to 90℃, slowly add 8g of composite microparticles while stirring at 1000rpm, stir at 1000rpm for 10min after addition, and cool to room temperature to obtain UV-resistant heat-oxidation dual-aging modified asphalt.
[0042] The nucleus-loaded precursor used in this embodiment was prepared in Preparation Example 2.
[0043] Example 5 The pH was adjusted to 4.5 by adding 5wt% acetic acid solution to 400g of 96wt% ethanol solution. Then, 4.8g of MPS and 0.8g of MTMS were added, and the mixture was stirred at 300rpm for 2.5h to obtain a pre-hydrolyzed solution. The core-loading precursor was added to the pre-hydrolyzed solution, and the mixture was stirred at 300rpm for 4h. The mixture was filtered, washed twice with deionized water, and twice with anhydrous ethanol. The mixture was then dried at 40℃ and 10kPa for 5h to obtain the core-loading solution.
[0044] 14g LMA, 3g PEG (molecular weight 700g / mol), 95g butyl acetate, and 17g n-butanol were mixed, heated to 60℃, stirred at 300rpm for 15min, cooled to room temperature, and 2.5g HEMA, 1g EGDMA, and 0.2g AIBN were added. The mixture was stirred at 300rpm for 15min to obtain the coating solution. 7g Irganox 3114 was added to 200g acetone and stirred at 300rpm for 25min to obtain the antioxidant solution. 30g of the core was placed in a fluidized bed, and nitrogen gas was introduced for aeration. The inlet air temperature was adjusted to 85℃ and the outlet air temperature to 78℃. The coating solution was sprayed through a nozzle and kept at this temperature for 4h. After cooling to room temperature, it was added to 300g of... The composite microparticles were dispersed in a 65 wt% ethanol solution by ultrasonication at 100 W for 15 min, soaked and washed at 300 rpm for 3 h, filtered, washed twice with anhydrous ethanol and three times with acetone, added to an antioxidant solution, stirred and soaked at 400 rpm for 4 h, filtered, and dried at 40℃ and 10 kPa for 8 h to obtain composite microparticles.
[0045] Mix 410g of base asphalt (preferably AH-70 asphalt) and 19g of SBS (preferably YH-791 linear SBS), heat to 170℃, stir at 1000rpm for 20min, stir at 3000rpm for 25min, cool to 88℃, slowly add 9g of composite microparticles while stirring at 1000rpm, stir at 1000rpm for 10min after addition, and cool to room temperature to obtain UV-resistant heat-oxidation dual-aging modified asphalt.
[0046] The nucleus-carrying precursor used in this embodiment was prepared in Preparation Example 3.
[0047] Example 6 The pH was adjusted to 4.5 by adding 5 wt% acetic acid solution dropwise to 400 g of 96 wt% ethanol solution. 4.8 g of MPS was added, and the mixture was stirred at 300 rpm for 2.5 h to obtain a pre-hydrolyzed solution. The core-loaded precursor was added to the pre-hydrolyzed solution, stirred at 300 rpm for 4 h, filtered, washed twice with deionized water, washed twice with anhydrous ethanol, and dried at 40 ℃ and 10 kPa for 5 h to obtain the core-loaded solution.
[0048] 14g LMA, 3g PEG (molecular weight 700g / mol), 95g butyl acetate, and 17g n-butanol were mixed, heated to 60℃, stirred at 300rpm for 15min, cooled to room temperature, and 2.5g HEMA, 1g EGDMA, and 0.2g AIBN were added. The mixture was stirred at 300rpm for 15min to obtain the coating solution. 7g Irganox 3114 was added to 200g acetone and stirred at 300rpm for 25min to obtain the antioxidant solution. 30g of the core was placed in a fluidized bed, and nitrogen gas was introduced for aeration. The inlet air temperature was adjusted to 85℃ and the outlet air temperature to 78℃. The coating solution was sprayed through a nozzle and kept at this temperature for 4h. After cooling to room temperature, it was added to 300g of... The composite microparticles were dispersed in a 65 wt% ethanol solution by ultrasonication at 100 W for 15 min, soaked and washed at 300 rpm for 3 h, filtered, washed twice with anhydrous ethanol and three times with acetone, added to an antioxidant solution, stirred and soaked at 400 rpm for 4 h, filtered, and dried at 40℃ and 10 kPa for 8 h to obtain composite microparticles.
[0049] Mix 410g of base asphalt (preferably AH-70 asphalt) and 19g of SBS (preferably YH-791 linear SBS), heat to 170℃, stir at 1000rpm for 20min, stir at 3000rpm for 25min, cool to 88℃, slowly add 9g of composite microparticles while stirring at 1000rpm, stir at 1000rpm for 10min after addition, and cool to room temperature to obtain UV-resistant heat-oxidation dual-aging modified asphalt.
[0050] The nucleus-carrying precursor used in this embodiment was prepared in Preparation Example 3.
[0051] The present invention also includes comparative examples and related experiments.
[0052] Comparative Example 1 The difference between this comparative example and Example 5 is that APTES was not added during the preparation of the core-loaded precursor. The remaining operation steps and reaction conditions were the same as in Example 5, resulting in UV-resistant heat-oxidation dual-aging modified asphalt.
[0053] Comparative Example 2 The difference between this comparative example and Example 5 is that MPS was not added to the pre-hydrolyzed solution. The remaining operation steps and reaction conditions are the same as in Example 5, resulting in UV-resistant heat-oxygen dual-aging modified asphalt.
[0054] Comparative Example 3 The difference between this comparative example and Example 5 is that PEG was not added to the coating solution. The remaining operation steps and reaction conditions are the same as in Example 5, resulting in UV-resistant heat-oxidation dual-aging modified asphalt.
[0055] Comparative Example 4 The difference between this comparative example and Example 5 is that the LMA in the coating solution is replaced with methyl methacrylate in an equal molar amount of double bonds. The remaining operation steps and reaction conditions are the same as in Example 5, resulting in UV-resistant heat-oxidation dual-aging modified asphalt.
[0056] Heat and oxygen aging test Referring to JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering", modified asphalt samples prepared in each example and comparative example were taken. The penetration P1 at 25°C was measured. A rotating thin-film oven test was conducted at 163°C. After aging for 85 minutes, the residue was poured into a PAV standard sample tray while still hot and placed in a pressure aging apparatus. The temperature was raised to 100°C and the pressure was increased to 2 MPa. The pressure was maintained for 20 h, 30 h, and 40 h, respectively. After depressurization, the samples were removed, cooled to room temperature, and scraped off. The penetration P2 at 25°C of each aged sample was measured according to the following formula:
[0057] The penetration retention rate was calculated, and the results are shown in Table 1.
[0058] Table 1
[0059] UV resistance test The UV-resistant thermo-oxidative dual-aging modified asphalt samples prepared in each example and comparative example were heated to a fluid state and poured into molds for molding. After demolding, test pieces with a thickness of 1.0 mm were obtained. The penetration P3 (mm) of each test piece at 25℃ was measured. Referring to JT / T1333-2020 "Evaluation Method for UV Aging of Road Asphalt Materials", UVA-340 was selected as the UV light source, and the irradiance was set to 0.76 W / m²@340 nm. The test pieces were subjected to 8 hours of light irradiation (black panel temperature 60℃) and 16 hours of dark room irradiation (black panel temperature 45-50℃) cycles. After a cumulative irradiation of 480 hours, the penetration P4 (mm) of the test pieces at 25℃ was measured according to the following formula:
[0060] The penetration retention rate was calculated, and the results are shown in Table 2.
[0061] Table 2
[0062] The contact angle of the coating liquid prepared in Example 5 with the cores prepared in Example 6 was tested. The contact angle between the coating liquid and the core prepared in Example 5 was 5.23°, and the contact angle between the coating liquid and the core prepared in Example 6 was 11.12°. This indicates that the introduction of MTMS can further reduce the surface energy of the core and improve its affinity for the oily coating liquid, which is beneficial for the coating liquid to uniformly cover the core during fluidized bed spraying. According to Table 1, the modified asphalt prepared in Example 5 has better heat and oxygen aging resistance than that prepared in Example 6. This indicates that the introduction of MTMS can improve the uniformity of the organic shell layer, avoid premature release of antioxidants due to local thinning of the organic shell layer, and improve the heat and oxidation resistance of the present invention.
[0063] Depend on Figure 1 It can be seen that at a wavenumber of 2930 cm⁻¹ -1 3400cm -1 1560cm -1 Characteristic peaks appeared in the vicinity, indicating that APTES was covalently grafted onto the core. According to Table 2, the UV resistance of the modified asphalt prepared in Example 5 was significantly better than that of Comparative Example 1. This indicates that the introduction of APTES is beneficial for the dispersion and fixation of aminated titanium dioxide on the surface of modified silica, inhibiting titanium dioxide agglomeration, improving the dispersibility of titanium dioxide, and enabling titanium dioxide to exert its UV resistance.
[0064] Depend on Figure 1 It can be seen that at a wavenumber of 1700 cm⁻¹ -1 The presence of significant characteristic peaks nearby indicates that the core surface contains ester groups, further proving that MPS was covalently grafted onto the core. According to Table 1, the heat oxidation resistance of the modified asphalt prepared in Example 5 is better than that in Comparative Example 2, indicating that the introduction of MPS can introduce carbon-carbon double bonds on the core surface. These carbon-carbon double bonds can participate in the formation of the organic shell, improve the bonding strength between the organic shell and the core, inhibit the cracking of the organic shell under shear stress, and thus inhibit the premature release of antioxidants and reduce the ineffective loss of antioxidants.
[0065] Depend on Figure 2 It can be seen that a clear hysteresis loop is formed between the adsorption line and the desorption line, indicating that the introduction of PEG has created open pores in the organic shell. According to Table 1, the long-term heat oxidation resistance of the modified asphalt prepared in Example 5 is better than that in Comparative Example 3, indicating that the introduction of PEG into the coating liquid is beneficial to creating pores in the organic shell for antioxidant penetration, realizing the effective encapsulation of antioxidant in functional microparticles, delaying the release time of antioxidant, avoiding premature mixing of antioxidant into the matrix asphalt, and reducing the ineffective loss of antioxidant.
[0066] According to Tables 1 and 2, the modified asphalt prepared in Example 5 has better UV resistance than that in Comparative Example 4. This indicates that the introduction of LMA can introduce long-chain alkyl groups on the surface of the organic shell, which is beneficial for the uniform dispersion of composite particles in the mixture of base asphalt and SBS, inhibits the agglomeration of composite particles, and thus helps titanium dioxide to exert its UV resistance.
Claims
1. A method for preparing UV- and heat-oxidative dual-aging modified asphalt, characterized in that, Includes the following steps: S1. Aminated titanium dioxide and epoxidized silica are dispersed in N,N-dimethylformamide, deionized water is added and reacted, and after modification with γ-methacryloxypropyltrimethoxysilane, the mixture is dried to obtain the core. The aminated titanium dioxide was prepared by the following method: tetraethyl orthosilicate and 94-96 wt% ethanol solution were mixed, titanium dioxide was added and dispersed, ammonia was added dropwise to adjust the pH to 8.3-8.7, the reaction was carried out for 2-3 hours, filtered, washed with ethanol solution and anhydrous ethanol, and then dispersed in 94-96 wt% ethanol solution. Acetic acid solution was added dropwise to adjust the pH to 4-5, γ-aminopropyltriethoxysilane was added and reacted for 1.5-2 hours, filtered, washed with deionized water and N,N-dimethylformamide to obtain aminated titanium dioxide; The epoxidized silica is prepared by the following method: silica is dispersed in toluene, heated to 108-112℃ and refluxed to remove water for 20-30 min, cooled to 75-80℃ and γ-glycidoxypropyltrimethoxysilane is added, heated to 108-112℃ and refluxed for 3-4 h, filtered, and washed with toluene and N,N-dimethylformamide to obtain epoxidized silica; The core was prepared by dispersing aminated titanium dioxide and epoxidized silica in N,N-dimethylformamide, adding deionized water, heating to 55-59°C, reacting for 2.5-3 hours, filtering, washing with N,N-dimethylformamide and anhydrous ethanol, mixing with a pre-hydrolyzed solution, reacting for 3-4 hours, filtering, washing with deionized water and anhydrous ethanol, and drying under reduced pressure to obtain the core. The pre-hydrolyzed solution was prepared by adding acetic acid solution dropwise to a 94-96 wt% ethanol solution to adjust the pH to 4-5, adding γ-methacryloyloxypropyltrimethoxysilane, and reacting for 2-3 hours to obtain the pre-hydrolyzed solution. S2. Spray coating liquid onto the core, heat to react, disperse in antioxidant solution for impregnation, dry to obtain composite microparticles; The coating solution is prepared by mixing lauryl methacrylate, polyethylene glycol, 2-hydroxyethyl methacrylate, ethylene glycol dimethacrylate, an initiator, and a solvent; the antioxidant solution is prepared by mixing an antioxidant with acetone. The composite microparticles are prepared by the following method: placing the core in a fluidized bed and passing nitrogen gas through it for aeration; spraying a coating liquid under the conditions of inlet air temperature of 80-85℃ and outlet air temperature of 75-78℃; reacting for 4-5 hours; cooling and then dispersing in a 60-65wt% ethanol solution for soaking and washing for 3-4 hours; filtering; washing with anhydrous ethanol and acetone; dispersing in an antioxidant solution for soaking for 3-4 hours; filtering; and drying under reduced pressure to obtain the composite microparticles. In the coating solution, the solvent is butyl acetate and n-butanol, and the initiator is azobisisobutyronitrile; S3. Mix the base asphalt and styrene-butadiene-styrene triblock copolymer, add composite microparticles and mix well to obtain UV-resistant heat and oxygen dual-aging modified asphalt. In step S3, the base asphalt and styrene-butadiene-styrene triblock copolymer are mixed at 168-172°C, cooled to 85-90°C, and then composite microparticles are added and mixed. After cooling, ultraviolet heat and oxygen dual aging resistant modified asphalt is obtained.
2. The method for preparing UV-resistant, heat-oxidative dual-aging modified asphalt according to claim 1, characterized in that, During the preparation of the pre-hydrolyzed solution, after adjusting the pH value to 4-5, γ-methacryloyloxypropyltrimethoxysilane and methyltrimethoxysilane are added and reacted for 2-3 hours.
3. The method for preparing UV-resistant, heat-oxidative dual-aging modified asphalt according to claim 1, characterized in that, The molecular weight of the polyethylene glycol is 400-700 g / mol.
4. A UV- and heat-oxidative dual-aging modified asphalt, characterized in that, The modified asphalt, prepared by any one of claims 1-3, comprises the following raw materials in parts by weight: 400-410 parts of base asphalt, 18-22 parts of styrene-butadiene-styrene triblock copolymer, and 8-10 parts of composite microparticles; wherein the composite microparticles comprise the following raw materials in parts by weight: 30-35 parts of core carrier, 12-14 parts of lauryl methacrylate, 3-4 parts of polyethylene glycol, 2-3 parts of 2-hydroxyethyl methacrylate, 0.7-1 parts of ethylene glycol dimethacrylate, 0.2-0.3 parts of initiator, and 7-8 parts of antioxidant, wherein the antioxidant is Irganox 3114.
5. The UV-resistant, heat- and oxygen-resistant modified asphalt according to claim 4, characterized in that, The core comprises the following raw materials in parts by weight: 24-28 parts titanium dioxide, 15-19 parts silicon dioxide, 8-10 parts tetraethyl orthosilicate, 1.2-1.5 parts γ-aminopropyltriethoxysilane, 1-1.2 parts γ-glycidoxypropyltrimethoxysilane, 0-1 part methyltrimethoxysilane, and 4-5 parts γ-methacryloyloxypropyltrimethoxysilane.
Citation Information
Patent Citations
Asphalt ultraviolet-aging-resistant modifier and preparation method thereof, and modified asphalt and preparation method thereof
CN110872442A
Preparation and application of latent nonionic self-emulsifying epoxy curing agent
CN101885832A