Anti-sloughing lubricant for drilling fluid and its production process

By compounding polymer hydration fluid, lubricating phase and multi-scale plugging material, the problem of plugging and lubrication of drilling fluid anti-collapse lubricant in complex formations is solved, achieving high efficiency of wellbore stability and lubrication effect. It is suitable for drilling fluid applications in long horizontal sections, extended reach wells and deep complex formations.

CN122855040BActive Publication Date: 2026-11-20XIANYANG FENGHUA MUD MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611358760.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-20
Estimated Expiration
2046-09-03

AI Technical Summary

Technical Problem

Existing drilling fluid anti-collapse lubricants are prone to instability in high temperature, high salinity, high solid phase and shear environment, making it difficult to effectively enter nano- or micron-sized pore throats. Furthermore, component compatibility issues lead to poor storage stability and field application performance, failing to meet the anti-collapse, plugging and lubrication requirements of long horizontal sections, extended reach wells and deep complex formations.

Method used

Polymer hydration solution is formed using polyanionic cellulose and polyacrylamide. Potassium humate, potassium chloride, and sodium borate are added to enhance adsorption and inhibition. A lubricating phase is formed by combining polyether polyol, fatty acid soap, and nonionic emulsifier. Sulfonated asphalt powder, graphite powder, and flake mica powder are further added to form a multi-scale plugging effect. The oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase is used to support potassium magnesium aluminum silicate composite nanosheets and boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres to enhance the plugging and lubrication effect.

Benefits of technology

It improves the suspension stability, viscosity enhancement and colloid protection of drilling fluid, and filtration control capabilities, enhances the adsorption and inhibition effect on the wellbore, reduces frictional resistance, forms multi-scale plugging and lubrication drag reduction effects, and improves wellbore stability and anti-collapse performance under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application belongs to the technical field of drilling fluid treating agent, and particularly relates to a drilling fluid anti-sloughing lubricant and a production process thereof.The process takes deionized water, polyionic cellulose, polyacrylamide, potassium humate, potassium chloride, sodium borate, polyether polyol, fatty acid soap, nonionic emulsifier, sulfonated asphalt powder, graphite powder and flaky mica powder as basic components, and adds oxygen vacancy cerium-zirconium-yttrium composite oxide solid solution phase loaded potassium-magnesium-aluminum silicate composite nanosheet and boron-modified titanium nitride-fluorine-containing calcium phosphate gradient-coated nanobeads, and is prepared through hydration, dispersion, shearing and filtration.The obtained anti-sloughing lubricant has shale inhibition, micro-fracture plugging, filtration loss reduction and lubrication and drag reduction effects, and is suitable for a water-based drilling fluid system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of drilling fluid treatment agent technology, specifically relating to anti-collapse lubricants for drilling fluids and their production process. Background Technology

[0002] Drilling fluid is a crucial engineering fluid for maintaining wellbore safety and improving drilling efficiency during the drilling of oil and gas wells, geothermal wells, and unconventional energy wells. Its main functions include carrying cuttings, cooling the drill bit, balancing formation pressure, stabilizing the wellbore, and reducing frictional resistance between the drill string and the wellbore. In mudstone, brittle shale, formations with well-developed bedding, and formations with high content of water-sensitive clay minerals, free water in water-based drilling fluids can easily enter the formation interior along shale pores, microfractures, and bedding planes, causing clay mineral hydration, expansion, dispersion, and strength reduction. This can lead to complex situations such as wellbore collapse, diameter reduction, blockage, stuck drill string, tripping difficulties, and wellbore enlargement. Especially during drilling long horizontal sections, extended reach wells, and deep, complex formations, the large contact area between the drill string and the wellbore and the high frictional resistance place higher demands on the drilling fluid's anti-collapse properties, plugging properties, lubrication, and system stability. Therefore, developing composite drilling fluid treatment agents that combine anti-collapse suppression, micro-crack sealing, filtration loss reduction, and lubrication drag reduction functions has become an important technical direction for improving drilling safety and construction efficiency in complex formations.

[0003] Existing drilling fluid anti-collapse lubricants are typically formulated using humates, asphalt-based materials, potassium salts, polymer coating agents, graphite powder, mica powder, fatty acid salt lubricants, or polyether lubricants. Humates and potassium salts can inhibit shale hydration to some extent, polymers can improve filter cake density and cuttings coating, sulfonated asphalt, graphite powder, and mica powder can provide some sealing effect on formation microfractures and pore throats, and fatty acid salts and polyether components can reduce friction between the drill string and the wellbore. However, traditional systems still have several shortcomings: firstly, conventional sealing materials have large particle sizes, making it difficult to effectively penetrate nano- or micron-sized pore throats, resulting in insufficient continuity and density of the sealing layer; secondly, single organic lubricants are prone to adsorption decay, emulsification instability, or lubricating film damage under high temperature, high salinity, high solids, and shear conditions, leading to decreased lubrication performance. In addition, there may be compatibility issues among certain inorganic salts, alkaline components, and fatty acid soaps, which can easily lead to precipitation, flocculation, decreased viscosity, or loss of effective components, affecting product storage stability and field application performance. Summary of the Invention

[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide an anti-collapse lubricant for drilling fluid and its production process.

[0005] A first aspect of the present invention provides a production process for an anti-collapse lubricant for drilling fluids, comprising the following steps: S1. By weight, add 18.0-26.0 parts of deionized water to a reactor and stir at room temperature. Add 1.0-3.0 parts of polyanionic cellulose and stir. Then add 0.8-2.5 parts of polyacrylamide and continue stirring to obtain a polymer hydration solution. Add 8.0-14.0 parts of potassium humate, 2.0-6.0 parts of potassium chloride, and 0.5-2.0 parts of sodium borate to the polymer hydration solution and stir to obtain a basic anti-collapse dispersion. Mix 5.0-10.0 parts of polyether polyol, 3.0-6.0 parts of fatty acid soap, and 1.5-4.0 parts of nonionic emulsifier and stir to obtain a lubricating phase. Add the lubricating phase to the basic anti-collapse dispersion and stir to obtain a composite lubricating anti-collapse solution.

[0006] S2. Add 10.0-18.0 parts of sulfonated asphalt powder, 4.0-8.0 parts of graphite powder, and 3.0-7.0 parts of flake mica powder to the composite lubricating anti-collapse fluid in sequence, stir and disperse to obtain a sealing slurry; add 2.0-6.0 parts of oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase supported potassium magnesium aluminum silicate composite nanosheets and 1.5-5.0 parts of boron modified titanium nitride-fluorinated calcium phosphate gradient coated nanospheres to the sealing slurry, shear and disperse, add 0.1-0.5 parts of defoamer and 0.05-0.3 parts of corrosion inhibitor, continue stirring, and filter.

[0007] In this invention, the formation process of the anti-collapse lubricant for drilling fluid involves polymer hydration, dispersion of salt-inhibiting components, emulsification of the lubricating phase, dispersion of sheet-like plugging materials, and compounding of two inorganic modified materials (oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase supported on potassium-magnesium-aluminum silicate composite nanosheets and boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres). After adding polyanionic cellulose to deionized water, the polyanionic cellulose molecular chains gradually absorb water and unfold, forming a hydration network with thickening, protective, and filtration control functions. Then, after adding partially hydrolyzed polyacrylamide, the partially hydrolyzed polyacrylamide forms an entangled structure with the aqueous phase, improving the viscoelasticity and suspension stability of the continuous phase of the system, resulting in a polymer-hydrated fluid. After potassium humate enters the polymer hydration fluid, its aromatic structure and oxygen-containing functional groups such as carboxyl and phenolic hydroxyl groups enhance adsorption on the surface of shale and clay particles. Potassium chloride provides potassium ions to reduce the hydration dispersion tendency of clay minerals. The borate species formed by the hydrolysis of sodium borate form complexes and cross-links with the oxygen-containing functional groups in potassium humate, improving the strength of the adsorption film on the shale surface, thus obtaining the basic anti-collapse dispersion. After polyether polyol, fatty acid soap, and nonionic emulsifier are mixed to form a lubricating phase, the nonionic emulsifier reduces the oil-water interfacial tension, allowing the lubricating phase to be uniformly dispersed in the basic anti-collapse dispersion. The polyether polyol provides hydration lubrication and interfacial drag reduction, while the fatty acid soap forms an adsorption lubricating film on the wellbore and metal surface, resulting in a composite lubricating anti-collapse fluid. When sulfonated asphalt powder, water-dispersed graphite powder, and flake mica powder are added to a composite lubricating anti-collapse fluid, the sulfonated asphalt powder provides flexible plugging and softening point plugging, the water-dispersed graphite powder provides low-shear lubrication and interlayer sliding, and the flake mica powder provides sheet-like bridging and tile-like plugging. These three components form a plugging slurry. After the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase, loaded with potassium-magnesium-aluminum silicate composite nanosheets, enters the system, it relies on its sheet-like structure to penetrate micro-cracks and pore throats and adsorb onto the shale surface. The oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase enhances interfacial bonding and high-temperature stability. Boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres play a role in hard bearing, micro-rolling, and inorganic film formation at the friction interface. An antifoaming agent suppresses foam generated during shear dispersion, and an anticorrosive agent improves storage stability, ultimately forming a drilling fluid anti-collapse lubricant with functions of anti-collapse, plugging, filtration loss reduction, and lubrication drag reduction.

[0008] According to a preferred embodiment of the present invention, in step S1, the nonionic emulsifier is selected from at least one of lauryl alcohol polyoxyethylene ether, isotretinoin polyoxyethylene ether, and oleyl alcohol polyoxyethylene ether.

[0009] According to a preferred embodiment of the present invention, in step S2, the defoamer is selected from at least one of polyether-modified silicone defoamer, dimethyl silicone oil emulsion, and mineral oil defoamer; the preservative is selected from at least one of 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, 1,2-benzisothiazolin-3-one, and 2-bromo-2-nitro-1,3-propanediol.

[0010] According to a preferred embodiment of the present invention, the preparation method of the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium-magnesium-aluminum silicate composite nanosheets includes: A1. Dissolve 90.0-110.0 parts by weight of sodium silicate in 600.0-700.0 parts by weight of deionized water and stir at room temperature to obtain a silicate solution; dissolve 38.0-46.0 parts by weight of aluminum nitrate nonahydrate and 32.0-40.0 parts by weight of magnesium nitrate hexahydrate in 250.0-350.0 parts by weight of deionized water to obtain a magnesium aluminum salt solution; while stirring, add the magnesium aluminum salt solution dropwise to the silicate solution, and adjust the pH to 10.0-10 with ammonia. 8. Stir and age at 70-80℃ to obtain magnesium aluminum silicate precursor slurry. Add 16.0-23.0 parts of potassium chloride and continue stirring to obtain potassium-containing magnesium aluminum silicate precursor slurry. Transfer the potassium-containing magnesium aluminum silicate precursor slurry to a hydrothermal reactor and hydrothermally react at 150-170℃. Cool to room temperature, centrifuge, and collect precipitate A. Wash precipitate A with deionized water, then wash with anhydrous ethanol, and vacuum dry to obtain potassium-containing magnesium aluminum silicate composite nanosheets.

[0011] A2. Add 80.0-100.0 parts of potassium magnesium aluminum silicate composite nanosheets to 500.0-650.0 parts of deionized water and disperse ultrasonically to obtain a nanosheet dispersion; dissolve 10.0-14.0 parts of cerium nitrate hexahydrate, 7.0-11.0 parts of zirconium oxynitrate hydrate, 2.0-4.0 parts of yttrium nitrate hexahydrate, and 45.0-65.0 parts of urea in 250.0-350.0 parts of deionized water to obtain a cerium-zirconium-yttrium salt solution; add the cerium-zirconium-yttrium salt solution to the nanosheets. The nanosheets were reacted in a dispersion at 85-95℃, centrifuged, and precipitate B was collected. Precipitate B was washed with deionized water and then with anhydrous ethanol, and dried under vacuum at 70-90℃ to obtain potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors. The potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors were ground, placed in an air atmosphere, and heated to 520-580℃ and held. Then, the atmosphere was switched to a hydrogen-nitrogen mixed gas atmosphere and held at 480-520℃. After cooling to room temperature, the nanosheets were pulverized and sieved.

[0012] In this invention, the formation process of potassium-magnesium-aluminum silicate composite nanosheets supported by the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase includes the generation of potassium-magnesium-aluminum silicate composite nanosheets and the loading of the cerium-zirconium-yttrium composite oxide solid solution phase and the construction of oxygen vacancies. Sodium silicate is dissolved in deionized water to form an alkaline silicate solution, and aluminum nitrate nonahydrate and magnesium nitrate hexahydrate are dissolved in deionized water to form a magnesium-aluminum salt solution. When the magnesium-aluminum salt solution is added dropwise to the silicate solution, aluminum species participate in the construction of the silicon-oxygen network in the form of aluminum-oxygen coordination units, and magnesium species couple with silicon-oxygen tetrahedral sheets in the form of magnesium-oxygen octahedra. Ammonia water is used to adjust the alkalinity of the system to allow the magnesium-aluminum components to fully deposit and undergo condensation and rearrangement with silicate ions to form a magnesium-aluminum silicate precursor slurry. After the addition of potassium chloride, potassium ions are distributed in the interlayer and surface sites of the magnesium aluminosilicate precursor through adsorption, exchange, and hydrothermal recrystallization. The hydrothermal reaction further promotes the ordered rearrangement of silicon-oxygen tetrahedra, magnesium-oxygen octahedra, and aluminum-oxygen coordination units, transforming the precursor from an amorphous or low-order gel into sheet-like potassium-containing magnesium aluminosilicate composite nanosheets. After washing and drying, the obtained potassium-containing magnesium aluminosilicate composite nanosheets retain hydroxyl groups and potential sites on their surface, providing heterogeneous nucleation sites for subsequent cerium-zirconium-yttrium precursor deposition. Cerium nitrate hexahydrate, zirconium oxynitrate hydrate, yttrium nitrate hexahydrate, and urea are dissolved in deionized water to form a cerium-zirconium-yttrium salt solution. After the cerium-zirconium-yttrium salt solution is added to the nanosheet dispersion, urea slowly hydrolyzes under heating conditions, releasing alkaline substances. This causes cerium, zirconium, and yttrium ions to gradually hydrolyze and co-deposit on the surface of the potassium-containing magnesium aluminosilicate composite nanosheets as the alkalinity of the system increases, forming cerium-zirconium-yttrium precursor-loaded potassium-containing magnesium aluminosilicate composite nanosheets. When the precursor is heated in an air atmosphere, the hydroxide and aqueous hydroxyl precursor dehydrate, decompose, and transform into a cerium-zirconium-yttrium composite oxide solid solution phase. Subsequently, it is kept at a temperature in a hydrogen-nitrogen mixed atmosphere, where the cerium species undergoes a partial valence state transformation, and oxygen vacancy defects are generated on the crystal lattice surface, ultimately forming an oxygen vacancy cerium-zirconium-yttrium composite oxide solid solution phase supporting potassium magnesium aluminum silicate composite nanosheets.

[0013] According to a preferred embodiment of the present invention, in step A1, the temperature of vacuum drying is 70-90°C.

[0014] According to a preferred embodiment of the present invention, in step A2, the time for holding the temperature at 520-580°C is 2-4 hours, and the time for holding the temperature at 480-520°C is 2-4 hours.

[0015] According to a preferred embodiment of the present invention, the preparation method of the boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres includes: B1, adding 90.0-110.0 parts by weight of nano-titanium dioxide, 6.0-10.0 parts by weight of boric acid and 140.0-180.0 parts by weight of melamine into a ball mill jar and ball milling to obtain a boron-nitrogen-titanium composite precursor; under an ammonia atmosphere, heating the boron-nitrogen-titanium composite precursor to 760-800℃ for heat treatment, then heating it to 900-940℃ for reaction, cooling it to room temperature, grinding it, washing it with deionized water, and drying it to obtain boron-modified titanium nitride nanocore material.

[0016] B2. Add 80.0-100.0 parts of boron-modified titanium nitride nanomaterial to 450.0-550.0 parts of deionized water and disperse ultrasonically to obtain a core material dispersion; dissolve 58.0-94.0 parts of calcium nitrate tetrahydrate in 150.0-220.0 parts of deionized water to obtain a calcium source solution; dissolve 18.0-26.0 parts of ammonium dihydrogen phosphate in 120.0-180.0 parts of deionized water to obtain a phosphorus source solution; dissolve 1.7-3.2 parts of ammonium fluoride in 50... A fluorine source solution was obtained by adding 0-90.0 parts of deionized water; under stirring, the phosphorus source solution and fluorine source solution were added to the core material dispersion, the pH was adjusted to 9.8-10.6 with ammonia, and then the calcium source solution was added dropwise to maintain the pH at 9.8-10.6. The reaction was stirred, aged, centrifuged, and precipitate C was collected; precipitate C was washed with deionized water and then with anhydrous ethanol, and dried under vacuum at 60-80℃; under a nitrogen atmosphere, it was heat-treated at 460-500℃, pulverized, and sieved.

[0017] In this invention, the formation process of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres includes the generation of boron-modified titanium nitride nanocore material and the in-situ deposition of the fluorinated calcium phosphate coating layer. Nano-titanium dioxide, boric acid, and melamine are ball-milled to form a uniformly contacted boron-nitrogen-titanium composite precursor, wherein nano-titanium dioxide serves as the titanium source, boric acid as the boron source, and melamine as the organic nitrogen source. During heat treatment of the boron-nitrogen-titanium composite precursor under an ammonia atmosphere, melamine gradually decomposes, releasing nitrogen-containing active fragments, which, together with ammonia, provide an active nitrogen source. Boric acid dehydrates to generate boron-containing oxides, which, under the action of ammonia and nitrogen-containing decomposition products, partially transform into a boron nitride phase, tightly composited with the titanium nitride phase. With continued heating, the titanium-oxygen bonds in the nano-titanium dioxide are gradually replaced by active nitrogen, transforming into a titanium nitride phase, resulting in a boron-modified titanium nitride nanocore material composed of a titanium nitride phase and a boron nitride phase. After grinding, washing, and drying, the core material develops a small amount of hydroxylated titanium oxide layer and polar sites on its surface, which is beneficial for the subsequent heterogeneous nucleation of calcium, phosphorus, and fluorine components. After dispersing the boron-modified titanium nitride nanocore material in deionized water, a phosphorus source solution formed by dissolving ammonium dihydrogen phosphate and a fluorine source solution formed by dissolving ammonium fluoride are added to the core material dispersion. Ammonia water is used to adjust the alkaline environment, causing phosphate and fluoride ions to adsorb onto the hydroxylated sites on the core material surface. Subsequently, a calcium source solution formed by dissolving calcium nitrate tetrahydrate is added dropwise. Calcium ions react with phosphate and fluoride ions on the core material surface, forming an initial coating layer of fluorinated calcium phosphate controlled by the calcium-to-phosphorus and fluorine-to-phosphorus molar ratios. As the stirring reaction and aging proceed, the fluorinated calcium phosphate layer gradually rearranges, solidifies, and coats the outer surface of the boron-modified titanium nitride nanocore material from amorphous deposits. After washing, drying, and heat treatment in a nitrogen atmosphere, the amorphous fluorinated calcium phosphate on the surface is further dehydrated, solidified, and initially crystallized to form boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres consisting of a boron-modified titanium nitride core, a transition hydroxylation interface, and a fluorinated calcium phosphate outer layer.

[0018] According to a preferred embodiment of the present invention, in step B1, the heat treatment time at 760-800°C is 1.5-2.5 hours, and the reaction time at 900-940°C is 3-5 hours.

[0019] According to a preferred embodiment of the present invention, in step B2, the heat treatment time at 460-500°C is 1.5-2.5 hours.

[0020] A second aspect of the present invention provides an anti-collapse lubricant for drilling fluid prepared according to the production process of the aforementioned anti-collapse lubricant for drilling fluid.

[0021] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention utilizes polyanionic cellulose and polyacrylamide to form a polymer hydration solution in deionized water, thereby providing the drilling fluid anti-collapse lubricant with good suspension stability, thickening and protective properties, and basic filtration control. Potassium humate, potassium chloride, and sodium borate, upon entering the polymer hydration solution, enhance the adsorption and inhibition of shale and clay particle surfaces, reduce the hydration and dispersion tendency of clay minerals, and form a stable wellbore adsorption film. The lubricating phase formed by polyether polyol, fatty acid soap, and nonionic emulsifier can be uniformly dispersed in the basic anti-collapse dispersion, improving the system's spreading ability on the wellbore and drill string surfaces, and reducing frictional and adhesion resistance during drilling.

[0022] (2) The present invention, by adding sulfonated asphalt powder, graphite powder and flake mica powder, forms a multi-scale plugging system. Sulfonated asphalt powder has flexible plugging and filtration loss reduction effects, and can fill micro-cracks and pores in the well wall; graphite powder has layered slip characteristics, which can reduce friction between solid particles and between the drill string and the well wall; flake mica powder can form sheet-like bridging and overlapping plugging structures on the well wall surface, improving the density and erosion resistance of the filter cake. The above components work together to give the drilling fluid anti-collapse lubricant good plugging, filtration loss reduction and lubrication drag reduction effects in shale formations, which can reduce problems such as well wall spalling, diameter reduction, stuck drill bit and increased friction.

[0023] (3) The oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium-containing magnesium-aluminum silicate composite nanosheets in this invention have a sheet-like structure, potassium-containing inhibitory effect, and oxygen-vacancy interfacial activity. They can enter the micropore throat and enhance the bonding with the shale surface, improving wellbore stability and anti-collapse effect under high temperature conditions. Boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres have hard bearing, interfacial film formation, and particle rolling effects, which can improve the strength of the lubricating film and reduce wear. The defoamer can reduce shear dispersion and foam during field use, and the corrosion inhibitor can improve the product storage stability. The drilling fluid anti-collapse lubricant prepared in this way has the properties of shale inhibition, microcrack sealing, filtration control, lubrication drag reduction, and storage stability. Detailed Implementation

[0024] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0025] Example 1: This example provides a production process for an anti-collapse lubricant for drilling fluids, the steps of which include: S1. Add 22.0g of deionized water to a reactor equipped with a mechanical stirrer. Stir at 500rpm at 25℃. Slowly add 2.0g of polyanionic cellulose over a period of 5 minutes. Continue stirring for 40 minutes after addition to ensure complete hydration of the polyanionic cellulose. Then add 1.65g of polyacrylamide and continue stirring for 40 minutes to obtain a polymer hydrated solution. Add 11.0g of potassium humate, 4.0g of potassium chloride, and 1.25g of sodium borate to the polymer hydrated solution sequentially. After stirring for 5 minutes, and then stirring for another 30 minutes after all the ingredients have been added, a basic anti-collapse dispersion is obtained. Separately, 7.5 g of polyether polyol, 4.5 g of fatty acid soap and 2.75 g of nonionic emulsifier are added to a premixed container and stirred at 500 rpm for 30 minutes at 50°C to obtain a lubricating phase, wherein the nonionic emulsifier is isomeric tridecyl alcohol polyoxyethylene ether. The lubricating phase is slowly added to the basic anti-collapse dispersion, with the addition time controlled at 5 minutes. After addition, the mixture is stirred at 850 rpm for 30 minutes to obtain a composite lubricating anti-collapse solution.

[0026] S2. Add 14.0g of sulfonated asphalt powder, 6.0g of graphite powder, and 5.0g of flake mica powder sequentially to the composite lubricating anti-collapse fluid obtained in step S1. Stir at 1250rpm for 5min after each addition. After all materials are added, continue stirring at 1250rpm for 48min to obtain the sealing slurry. Slowly add 4.0g of oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium magnesium aluminum silicate composite nanosheets and 3.25g of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres to the sealing slurry. Control the addition time to 8min. After addition, shear disperse at 3250rpm for 30min. Then add 0.3g of polyether-modified organosilicon defoamer and 0.175g of 1,2-benzisothiazolin-3-one. Continue stirring at 500rpm for 20min. Filter through a 100-mesh sieve to obtain the anti-collapse lubricant for drilling fluid.

[0027] Preparation of potassium-magnesium-aluminum silicate composite nanosheets supported on oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase: A1. Add 100.0g of sodium silicate to 650.0g of deionized water in a glass reactor equipped with a mechanical stirrer, thermometer, and dropper. Start stirring and stir at 400rpm for 30min at 25℃ until the sodium silicate is completely dissolved, obtaining a silicate solution. Separately, add 42.0g of aluminum nitrate nonahydrate and 36.0g of magnesium nitrate hexahydrate to 300.0g of deionized water and stir at 400rpm for 30min at 25℃ until the aluminum nitrate nonahydrate and magnesium nitrate hexahydrate are completely dissolved, obtaining a magnesium aluminum salt solution. Adjust the stirring speed of the silicate solution to... Add the magnesium aluminum salt solution to the silicate solution at a constant pressure dropping device at a rate of 3.5 mL / min, maintaining the system temperature at 25°C during the addition process. Control the dropping nozzle to be below the liquid surface and close to the outer edge of the stirrer to ensure rapid dispersion of the magnesium aluminum salt solution upon entering the silicate solution. After the addition is complete, continue stirring for 20 minutes. Slowly adjust the pH to 10.4 with ammonia water, controlling the ammonia water dropping rate at 1.0 mL / min during the adjustment process. After the pH stabilizes for 10 minutes, raise the system temperature to 75°C and age it at 75°C with stirring at 500 rpm for 4 minutes. A magnesium aluminosilicate precursor slurry was obtained by stirring at 500 rpm for 1.5 h at 75 °C. 19.5 g of potassium chloride was added to the magnesium aluminosilicate precursor slurry, and the mixture was stirred at 500 rpm for 1.5 h at 75 °C to obtain a potassium-containing magnesium aluminosilicate precursor slurry. The potassium-containing magnesium aluminosilicate precursor slurry was transferred to a polytetrafluoroethylene-lined hydrothermal reactor, with the liquid volume controlled to 75% of the effective volume of the reactor. After sealing, the reactor was placed in a forced-air drying oven and hydrothermally reacted at 160 °C for 12 h. After the reaction, the reactor was allowed to cool naturally to 25 °C. The hydrothermal reactor was then opened, and the resulting slurry was transferred to a centrifuge tube and centrifuged at 5000 rpm for 1 h. 0 min, collect precipitate A; add precipitate A to 500.0 g deionized water and stir to disperse for 10 min, then centrifuge at 5000 rpm for 10 min, and repeat washing with water until the pH of the washing solution is 7.0; then wash the washed precipitate A twice with 200.0 g anhydrous ethanol, centrifuge at 5000 rpm for 10 min after each wash, and collect the solid; place the obtained solid in a vacuum drying oven and vacuum dry at 80℃ and a vacuum degree of -0.08 MPa for 10 h, grind for 10 min after drying, and pass through a 200 mesh sieve to obtain potassium magnesium aluminum silicate composite nanosheets.

[0028] A2. Add 90.0g of the potassium-magnesium-aluminum silicate composite nanosheets obtained in step A1 to 575.0g of deionized water. First, mechanically stir at 400rpm for 20min, then ultrasonically disperse at 500W power and 40kHz frequency for 40min. During ultrasonication, control the system temperature to not exceed 35℃ to obtain a nanosheet dispersion. Separately, add 12.0g of cerium nitrate hexahydrate, 9.0g of zirconium oxynitrate hydrate, 3.0g of yttrium nitrate hexahydrate, and 55.0g of urea to 300.0g of deionized water and stir at 400rpm at 25℃. For 30 minutes, all components were completely dissolved to obtain a cerium-zirconium-yttrium salt solution. This solution was then added to the nanosheet dispersion in one step, and the mixture was stirred at 500 rpm for 20 minutes. The temperature was then raised to 90°C, and the mixture was stirred at 500 rpm for 5 hours at 90°C to deposit the cerium-zirconium-yttrium precursor onto the surface of the potassium-magnesium-aluminum silicate composite nanosheets. After the reaction, the mixture was cooled to 25°C, and the slurry was centrifuged at 5000 rpm for 10 minutes to collect precipitate B. Precipitate B was added to 500.0 g of deionized water and stirred for 10 minutes, then centrifuged at 5000 rpm for 1 minute. The mixture was washed repeatedly with water until the pH of the washing solution reached 7.0. It was then washed twice with 200.0 g of anhydrous ethanol, centrifuged at 5000 rpm for 10 min after each wash, and the solid was collected. The obtained solid was placed in a vacuum drying oven and vacuum-dried at 80℃ and -0.08 MPa for 10 h to obtain potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors. The potassium magnesium aluminum silicate composite nanosheets supported on the cerium-zirconium-yttrium precursors were ground in an agate mortar for 30 min to ensure uniform powder dispersion. The ground powder was then spread evenly in an alumina crucible. The thickness of the material should not exceed 10 mm. It is placed in an air atmosphere furnace and heated to 550 °C at a rate of 5 °C / min. It is then held at 550 °C for 3 hours. After the holding period, the temperature is lowered to 500 °C, and the atmosphere is switched to a hydrogen-nitrogen mixture. The hydrogen gas fraction in the hydrogen-nitrogen mixture is 5%, and the flow rate of the hydrogen-nitrogen mixture is 200 mL / min. The mixture is held at 500 °C for 3 hours. After the holding period, the hydrogen-nitrogen mixture is continued to be introduced and the furnace is cooled to 25 °C. The powder is then removed, pulverized for 10 minutes, and passed through a 200-mesh sieve to obtain oxygen-vacancy cerium-zirconium yttrium composite oxide solid solution phase supported potassium magnesium aluminum silicate composite nanosheets.

[0029] Boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres: B1. Add 100.0g of nano-titanium dioxide, 8.0g of boric acid, and 160.0g of melamine to a planetary ball mill jar. The milling media is zirconia balls, with a ball-to-material mass ratio of 6:1. The milling speed is 350 rpm, and the milling time is 5 hours. The milling method involves pausing for 5 minutes every 30 minutes to prevent the material from overheating. After milling, a boron-nitrogen-titanium composite precursor is obtained. Place the boron-nitrogen-titanium composite precursor in an alumina boat with a thickness not exceeding 8mm. Then place the alumina boat in the constant temperature zone of a tubular furnace. Introduce ammonia gas into the tubular furnace at a flow rate of 300mL / min to first replace the air in the furnace tubes with ammonia gas. After 30 min, the temperature was increased to 780℃ at 5℃ / min under continuous ammonia gas purging, and heat-treated at 780℃ for 2 h. Then, the temperature was increased to 920℃ at 3℃ / min, and reacted at 920℃ for 4 h. After the reaction, the ammonia gas flow rate was maintained at 300 mL / min and the furnace was cooled to 25℃. The product was then removed. The product was ground for 20 min, added to 600.0 g of deionized water and stirred and washed for 10 min. The product was centrifuged at 5000 rpm for 10 min, and the washing was repeated 3 times. The solid was collected. The solid was placed in a forced-air drying oven and dried at 70℃ for 8 h to obtain boron-modified titanium nitride nanocore material.

[0030] B2. Add 90.0g of the boron-modified titanium nitride nanomaterial obtained in step B1 to 500.0g of deionized water. First, mechanically stir at 400rpm for 20min, then ultrasonically disperse at 500W power and 40kHz frequency for 40min, controlling the system temperature not to exceed 35℃ during ultrasonication to obtain a core material dispersion. Add 76.0g of calcium nitrate tetrahydrate to 185.0g of deionized water and stir at 400rpm for 20min at 25℃ to obtain a calcium source solution. Add 22.0g of ammonium dihydrogen phosphate to 150.0g of deionized water... A phosphorus source solution was obtained by stirring at 400 rpm for 20 min at 25℃. 2.45 g of ammonium fluoride was added to 70.0 g of deionized water, and the mixture was stirred at 400 rpm for 20 min at 25℃ to obtain a fluorine source solution. The core material dispersion was placed in a reactor equipped with a pH detection device, a dropping device, and a temperature control jacket. The phosphorus source solution and fluorine source solution were added sequentially while stirring at 500 rpm. After stirring for 20 min, the pH was adjusted to 10.2 with ammonia water, and the system was heated to 45℃. Subsequently, a calcium source solution was added dropwise at a rate of 2 mL / min, with continuous pH monitoring and [further details needed]. The pH of the system was maintained at 10.2 with ammonia solution. After the calcium source solution was added dropwise, the reaction was carried out at 45℃ with stirring at 500 rpm for 4 hours. After the reaction was completed, heating was stopped, and the mixture was aged at 25℃ for 8 hours. After aging, the mixture was centrifuged at 5000 rpm for 10 minutes to collect precipitate C. Precipitate C was added to 500.0 g of deionized water and washed with stirring for 10 minutes, then centrifuged at 5000 rpm for 10 minutes. The washing was repeated until the pH of the washing solution reached 7.0. Subsequently, the mixture was washed twice with 200.0 g of anhydrous ethanol. After each washing, the mixture was centrifuged at 5000 rpm for 10 minutes to collect the solid. The obtained solid was placed in a vacuum drying oven and vacuum dried for 12 h at 70 °C and a vacuum degree of -0.08 MPa. The dried precipitate C was placed in an alumina crucible with a thickness not exceeding 10 mm and placed in a nitrogen atmosphere furnace with a nitrogen flow rate of 200 mL / min. Nitrogen was first introduced for 30 min to replace the air in the furnace, and then the temperature was increased to 480 °C at 5 °C / min. The furnace was heat-treated at 480 °C for 2 h, and then cooled to 25 °C in a nitrogen atmosphere. The solid was then pulverized for 10 min and passed through a 200-mesh sieve to obtain boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres.

[0031] Example 2: The difference between this example and Example 1 is that this example provides a production process for an anti-collapse lubricant for drilling fluids, the steps of which include: S1. Add 18.0g of deionized water to a reactor and stir at 300rpm at 25℃. Add 1.0g of polyanionic cellulose and stir for 30min. Then add 0.8g of polyacrylamide and continue stirring for 30min to obtain a polymer hydration solution. Add 8.0g of potassium humate, 2.0g of potassium chloride, and 0.5g of sodium borate to the polymer hydration solution and stir for 20min to obtain a basic anti-collapse dispersion. Mix 5.0g of polyether polyol, 3.0g of fatty acid soap, and 1.5g of nonionic emulsifier and stir at 45℃ for 20min to obtain a lubricating phase, wherein the nonionic emulsifier is lauryl alcohol polyoxyethylene ether. Add the lubricating phase to the basic anti-collapse dispersion and stir at 700rpm for 20min to obtain a composite lubricating anti-collapse solution.

[0032] S2. Add 10.0g of sulfonated asphalt powder, 4.0g of graphite powder and 3.0g of flake mica powder to the composite lubricating anti-collapse fluid obtained in step S1, and stir and disperse at 1000rpm for 35min to obtain a sealing slurry; add 2.0g of oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase-supported potassium magnesium aluminum silicate composite nanosheets and 1.5g of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres to the sealing slurry, and shear and disperse at 2500rpm for 20min, add 0.1g of dimethyl silicone oil emulsion and 0.05g of 2-methyl-4-isothiazolin-3-one, continue stirring for 20min, filter through an 80-mesh sieve to obtain an anti-collapse lubricant for drilling fluid.

[0033] Preparation of potassium-magnesium-aluminum silicate composite nanosheets supported on oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase: A1. Add 90.0g of sodium silicate to 600.0g of deionized water and stir at 300rpm for 30min at 25℃ to obtain a silicate solution. Add 38.0g of aluminum nitrate nonahydrate and 32.0g of magnesium nitrate hexahydrate to 250.0g of deionized water and stir at 300rpm for 30min at 25℃ to obtain a magnesium aluminum salt solution. While stirring at 400rpm, add the magnesium aluminum salt solution dropwise to the silicate solution at 2mL / min. After the addition is complete, adjust the pH to 10.0 with ammonia water and age at 70℃ for 3h to obtain a magnesium aluminum silicate precursor slurry. Add 16.0 g of potassium chloride to the magnesium aluminum silicate precursor slurry and continue stirring for 1 h to obtain a potassium-containing magnesium aluminum silicate precursor slurry. Transfer the potassium-containing magnesium aluminum silicate precursor slurry to a hydrothermal reactor and hydrothermally react at 150 °C for 10 h. After the hydrothermal reaction is completed, allow it to cool naturally to 25 °C and centrifuge at 5000 rpm for 10 min to collect precipitate A. Wash precipitate A with deionized water until the pH of the washing solution is 7.0, and then wash it twice with anhydrous ethanol, using 200.0 g of anhydrous ethanol each time. Then, vacuum dry it at 70 °C for 8 h to obtain potassium-containing magnesium aluminum silicate composite nanosheets.

[0034] A2. Add 80.0g of the potassium-magnesium-aluminum-silicate composite nanosheets obtained in step A1 to 500.0g of deionized water and ultrasonically disperse for 30min at an ultrasonic power of 500W and a frequency of 40kHz to obtain a nanosheet dispersion. Add 10.0g of cerium nitrate hexahydrate, 7.0g of zirconium oxynitrate hydrate, 2.0g of yttrium nitrate hexahydrate, and 45.0g of urea to 250.0g of deionized water and stir at 300rpm for 30min at 25℃ to obtain a cerium-zirconium-yttrium salt solution. Add the cerium-zirconium-yttrium salt solution to the nanosheet dispersion and stir at 500rpm for 4h at 85℃. After the reaction is complete, cool to 25℃ and centrifuge at 5000rpm for 10min to collect precipitate B. Use deionized water to collect precipitate B. The nanosheets were washed with water until the pH of the washing solution reached 7.0, and then washed twice with anhydrous ethanol, using 200.0 g of anhydrous ethanol each time. They were then vacuum dried at 70 °C for 8 h to obtain potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors. The cerium-zirconium-yttrium precursor-supported potassium magnesium aluminum silicate composite nanosheets were ground for 30 min, placed in an air atmosphere furnace, and heated to 520 °C at 5 °C / min and held for 2 h. After the holding period, the atmosphere was switched to a hydrogen-nitrogen mixture with a hydrogen gas fraction of 4%, and the mixture was introduced at 200 mL / min. The mixture was held at 480 °C for 2 h, cooled to 25 °C, pulverized, and passed through a 200-mesh sieve to obtain oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium magnesium aluminum silicate composite nanosheets.

[0035] Preparation of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres: B1. 90.0g of nano-titanium dioxide, 6.0g of boric acid and 140.0g of melamine were added to a ball mill jar with a ball-to-material mass ratio of 5:1. The mixture was ball-milled at 300rpm for 4h to obtain a boron-nitrogen-titanium composite precursor. The boron-nitrogen-titanium composite precursor was placed in a tube furnace and heat-treated at 760℃ for 1.5h under an ammonia atmosphere by introducing ammonia gas at 200mL / min and raising the temperature at 5℃ / min. Then, the temperature was raised to 900℃ for 3h. After the reaction, the mixture was cooled to 25℃ under an ammonia atmosphere and ground for 20min. It was washed three times with deionized water, using 200.0g of deionized water each time. The mixture was then dried at 60℃ for 6h to obtain boron-modified titanium nitride nanocore material.

[0036] B2. Add 80.0g of the boron-modified titanium nitride nanomaterial obtained in step B1 to 450.0g of deionized water and ultrasonically disperse for 30min at an ultrasonic power of 500W and a frequency of 40kHz to obtain a core material dispersion; add 58.0g of calcium nitrate tetrahydrate to 150.0g of deionized water and stir at 300rpm for 20min at 25℃ to obtain a calcium source solution; add 18.0g of ammonium dihydrogen phosphate to 120.0g of deionized water and stir at 300rpm for 20min at 25℃ to obtain a phosphorus source solution; add 1.7g of ammonium fluoride to 50.0g of deionized water and stir at 300rpm for 20min at 25℃ to obtain a fluorine source solution; under stirring at 500rpm, add the phosphorus source solution and fluorine source solution... The pH of the core material dispersion was adjusted to 9.8 with ammonia, and then calcium source solution was added dropwise at 1 mL / min, maintaining the pH at 9.8 with ammonia during the addition. The mixture was stirred at 40 °C for 3 h, then aged for 6 h, and centrifuged at 5000 rpm for 10 min to collect precipitate C. Precipitate C was washed with deionized water until the pH of the washing solution reached 7.0, and then washed twice with anhydrous ethanol, using 200.0 g of anhydrous ethanol each time. The precipitate C was then vacuum dried at 60 °C for 10 h. The dried precipitate C was placed in a nitrogen atmosphere furnace, and nitrogen was introduced at 200 mL / min. The temperature was increased to 460 °C at 5 °C / min for 1.5 h, cooled to 25 °C, pulverized, and passed through a 200-mesh sieve to obtain boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres.

[0037] Example 3: The difference between this example and Example 1 is that this example provides a production process for an anti-collapse lubricant for drilling fluids, the steps of which include: S1. Add 26.0g of deionized water to a reactor and stir at 800rpm at 45℃. Add 3.0g of polyanionic cellulose and stir for 50min. Then add 2.5g of polyacrylamide and continue stirring for 50min to obtain a polymer hydrate. Add 14.0g of potassium humate, 6.0g of potassium chloride, and 2.0g of sodium borate to the polymer hydrate in sequence and stir for 40min to obtain a basic anti-collapse dispersion. Mix 10.0g of polyether polyol, 6.0g of fatty acid soap, and 4.0g of nonionic emulsifier and stir at 55℃ for 40min to obtain a lubricating phase. The nonionic emulsifier is oleyl alcohol polyoxyethylene ether. Add the lubricating phase to the basic anti-collapse dispersion and stir at 1000rpm for 40min to obtain a composite lubricating anti-collapse solution.

[0038] S2. Add 18.0g of sulfonated asphalt powder, 8.0g of graphite powder and 7.0g of flake mica powder to the composite lubricating anti-collapse fluid obtained in step S1, and stir and disperse at 1500rpm for 60min to obtain a sealing slurry; add 6.0g of oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium magnesium aluminum silicate composite nanosheets and 5.0g of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres to the sealing slurry, and shear and disperse at 4000rpm for 40min, add 0.5g of mineral oil defoamer and 0.3g of 1,2-benzisothiazolin-3-one, continue stirring for 20min, and filter through a 120-mesh sieve to obtain an anti-collapse lubricant for drilling fluid.

[0039] Preparation of potassium-magnesium-aluminum silicate composite nanosheets supported on oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase: A1. Add 110.0g of sodium silicate to 700.0g of deionized water and stir at 500rpm for 30min at 25℃ to obtain a silicate solution. Add 46.0g of aluminum nitrate nonahydrate and 40.0g of magnesium nitrate hexahydrate to 350.0g of deionized water and stir at 500rpm for 30min at 25℃ to obtain a magnesium aluminum salt solution. While stirring at 600rpm, add the magnesium aluminum salt solution dropwise to the silicate solution at 5mL / min. After the addition is complete, adjust the pH to 10.8 with ammonia water and age at 80℃ for 5h to obtain a magnesium aluminum silicate precursor slurry. Add 23.0 g of potassium chloride to the magnesium aluminum silicate precursor slurry and continue stirring for 2 h to obtain a potassium-containing magnesium aluminum silicate precursor slurry. Transfer the potassium-containing magnesium aluminum silicate precursor slurry to a hydrothermal reactor and hydrothermally react at 170 °C for 14 h. After the hydrothermal reaction is completed, allow it to cool naturally to 25 °C and centrifuge at 5000 rpm for 10 min to collect precipitate A. Wash precipitate A with deionized water until the pH of the washing solution is 7.0, and then wash it twice with anhydrous ethanol, using 200.0 g of anhydrous ethanol each time. Then, vacuum dry it at 90 °C for 12 h to obtain potassium-containing magnesium aluminum silicate composite nanosheets.

[0040] A2. Add 100.0g of the potassium-magnesium-aluminum-silicate composite nanosheets obtained in step A1 to 650.0g of deionized water and ultrasonically disperse for 50min at an ultrasonic power of 500W and a frequency of 40kHz to obtain a nanosheet dispersion. Add 14.0g of cerium nitrate hexahydrate, 11.0g of zirconium oxynitrate hydrate, 4.0g of yttrium nitrate hexahydrate, and 65.0g of urea to 350.0g of deionized water and stir at 500rpm for 30min at 25℃ to obtain a cerium-zirconium-yttrium salt solution. Add the cerium-zirconium-yttrium salt solution to the nanosheet dispersion and stir at 500rpm for 6h at 95℃. After the reaction is complete, cool to 25℃ and centrifuge at 5000rpm for 10min to collect precipitate B. Use deionized water to collect precipitate B. The nanosheets were washed with water until the pH of the washing solution reached 7.0, and then washed twice with anhydrous ethanol, using 200.0 g of anhydrous ethanol each time. They were then vacuum dried at 90 °C for 12 h to obtain potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors. The cerium-zirconium-yttrium precursor-supported potassium magnesium aluminum silicate composite nanosheets were ground for 30 min, placed in an air atmosphere furnace, and heated to 580 °C at a rate of 5 °C / min and held for 4 h. After the holding period, the atmosphere was switched to a hydrogen-nitrogen mixture with a hydrogen gas fraction of 6%. The hydrogen-nitrogen mixture was introduced at a rate of 200 mL / min and held at 520 °C for 4 h. After cooling to 25 °C, the nanosheets were pulverized and passed through a 200-mesh sieve to obtain oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium magnesium aluminum silicate composite nanosheets.

[0041] Preparation of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres: B1. 110.0g of nano-titanium dioxide, 10.0g of boric acid and 180.0g of melamine were added to a ball mill jar with a ball-to-material mass ratio of 7:1. The mixture was ball-milled at 400rpm for 6h to obtain a boron-nitrogen-titanium composite precursor. The boron-nitrogen-titanium composite precursor was placed in a tube furnace and heat-treated at 800℃ for 2.5h under an ammonia atmosphere by introducing ammonia gas at 400mL / min and raising the temperature at 5℃ / min to 800℃. Then, the temperature was raised to 940℃ for 5h. After the reaction, the mixture was cooled to 25℃ under an ammonia atmosphere and ground for 20min. It was washed three times with deionized water, using 200.0g of deionized water each time. The mixture was then dried at 80℃ for 10h to obtain boron-modified titanium nitride nanocore material.

[0042] B2. Add 100.0g of the boron-modified titanium nitride nanomaterial obtained in step B1 to 550.0g of deionized water and ultrasonically disperse for 50min at an ultrasonic power of 500W and a frequency of 40kHz to obtain a core material dispersion; add 94.0g of calcium nitrate tetrahydrate to 220.0g of deionized water and stir at 500rpm for 20min at 25℃ to obtain a calcium source solution; add 26.0g of ammonium dihydrogen phosphate to 180.0g of deionized water and stir at 500rpm for 20min at 25℃ to obtain a phosphorus source solution; add 3.2g of ammonium fluoride to 90.0g of deionized water and stir at 500rpm for 20min at 25℃ to obtain a fluorine source solution; while stirring at 500rpm, add the phosphorus source solution and fluorine source solution... In the core material dispersion, the pH was adjusted to 10.6 with ammonia, and then a calcium source solution was added dropwise at 3 mL / min, maintaining the pH at 10.6 with ammonia during the addition. The reaction was stirred at 50 °C for 5 h, followed by aging for 10 h. The precipitate C was collected by centrifugation at 5000 rpm for 10 min. The precipitate C was washed with deionized water until the pH of the washing solution reached 7.0, and then washed twice with anhydrous ethanol, using 200.0 g of anhydrous ethanol each time. The precipitate C was then vacuum dried at 80 °C for 14 h. The dried precipitate C was placed in a nitrogen atmosphere furnace, and nitrogen was introduced at 200 mL / min. The temperature was increased to 500 °C at 5 °C / min for 2.5 h. After cooling to 25 °C, the precipitate was pulverized and passed through a 200-mesh sieve to obtain boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres.

[0043] Comparative Example 1 The difference between this comparative example and Example 1 is that, in step S2, the potassium magnesium aluminum silicate composite nanosheets supported by the oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase are not added, and the potassium magnesium aluminum silicate composite nanosheets supported by the oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase are replaced with potassium magnesium aluminum silicate composite nanosheets of equal mass.

[0044] Comparative Example 2 The difference between this comparative example and Example 1 is that boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres are not added in step S2, and boron-modified titanium nitride nanocore material of equal mass is used instead of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres.

[0045] Comparative Example 3 The difference between this comparative example and Example 1 is that, in step S2, the potassium-magnesium-aluminum silicate composite nanosheets supported by the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase and the boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres are not added. Instead, the potassium-magnesium-aluminum silicate composite nanosheets supported by the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase are replaced with potassium-magnesium-aluminum silicate composite nanosheets of equal mass, and the boron-modified titanium nitride nanocore material is replaced with boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres of equal mass.

[0046] The performance of the anti-collapse lubricants for drilling fluids obtained in Examples 1-3 and Comparative Examples 1-3 was tested in accordance with national and industry standard testing specifications.

[0047] The drilling fluid anti-collapse lubricants obtained in Examples 1-3 and Comparative Examples 1-3 were used as test samples. The apparent viscosity, plastic viscosity, medium-pressure filtration loss, high-temperature and high-pressure filtration loss, lubrication coefficient reduction rate, shale rolling recovery rate, plugging rate, and viscosity retention rate were evaluated using the same base slurry system. For base slurry preparation, 400.0 g of deionized water was added to a high-speed mixing cup, stirring was started and the speed was adjusted to 4000 rpm. 16.0 g of sodium-based bentonite was slowly added over a period of 3 minutes. After addition, stirring continued for 20 minutes. The resulting slurry was transferred to a sealed container and allowed to stand at 25°C for 24 hours to hydrate, yielding a pre-hydrated base slurry. For test slurry preparation, 400.0 g of pre-hydrated base slurry was added to a high-speed mixing cup, and 12.0 g of the drilling fluid anti-collapse lubricant to be tested was added at 4000 rpm. Stirring continued for 20 minutes. After stirring, the slurry was allowed to stand in a sealed container at 25°C for 2 hours to obtain the test slurry.

[0048] For apparent viscosity and plastic viscosity tests, the test slurry is stirred at 4000 rpm for 5 minutes at 25℃ and immediately poured into the sample cup of the rotary viscometer until the liquid level reaches the scale mark of the sample cup. The test temperature is controlled at 25℃, and stable readings are taken at 600 rpm and 300 rpm in sequence. Each sample is tested in parallel 3 times and the average value is taken. The apparent viscosity is calculated as 1 / 2 of the 600 rpm reading, and the unit is mPa·s. The plastic viscosity is calculated as the 600 rpm reading minus the 300 rpm reading, and the unit is mPa·s.

[0049] During the medium-pressure filtration loss test, the test slurry is stirred evenly at 25℃, poured into a filtration cup, filter paper is placed in the cup and the cup is sealed. The filtration is carried out at 25℃ and 0.69MPa for 30 minutes. The volume of the filtrate is collected and read. Each sample is tested in parallel 3 times and the average value is taken. The result is recorded as the medium-pressure filtration loss, and the unit is mL.

[0050] During the high-temperature and high-pressure filtration loss test, the test slurry was placed in an aging tank, sealed, and then placed in a roller furnace. It was aged at 150°C for 16 hours. After aging, it was cooled to 25°C, and the aged slurry was stirred at 4000 rpm for 10 minutes. Then it was poured into a high-temperature and high-pressure filtration loss cup and filtered at 150°C and 3.5 MPa for 30 minutes. The filtrate volume was collected and read. Each sample was tested in parallel three times and the average value was taken. The result was recorded as the high-temperature and high-pressure filtration loss, in mL.

[0051] During the lubrication coefficient reduction test, pre-hydrated base slurry and test slurry were taken separately, and the lubrication coefficient was tested using an extreme pressure lubrication instrument at 25℃. Before the test, the samples were stirred at 4000 rpm for 5 minutes. Each sample was tested in parallel 3 times and the average value was taken. The lubrication coefficient reduction rate was calculated by dividing the difference between the lubrication coefficient of the pre-hydrated base slurry and the lubrication coefficient of the test slurry by the lubrication coefficient of the pre-hydrated base slurry and then multiplying by 100%.

[0052] For the shale rolling recovery rate test, the same batch of mudstone and shale rock fragments were taken, and the fragments with a particle size of 2.0-5.0 mm were obtained by sieving. The rock fragments were placed in an oven at 105℃ for 4 hours and cooled to 25℃. 50.0 g of dry rock fragments were weighed and added to an aging tank containing 350.0 g of test slurry. After sealing, the tank was rolled at 120℃ for 16 hours. After rolling, the tank was cooled to 25℃ and the rock fragments were recovered through a 40-mesh sieve. The surface of the rock fragments was quickly rinsed with deionized water to remove the slurry. The rinsing time was controlled to be 30 seconds. The recovered rock fragments were placed in an oven at 105℃ for 4 hours and cooled to 25℃. The mass of the recovered dry rock fragments was weighed. Each sample was tested in parallel 3 times and the average value was taken. The shale rolling recovery rate was calculated by dividing the mass of the recovered dry rock fragments by the mass of the initial dry rock fragments and then multiplying by 100%.

[0053] For the plugging rate test, a ceramic sand disc with a pore size of 5.0 μm was selected as the plugging medium. First, the pre-hydrated base slurry was filtered for 30 min at 25℃ and 3.5 MPa, and the filtration loss was recorded as the blank filtration loss. Then, the test slurry was loaded into the plugging evaluation device and filtered for 30 min at 25℃ and 3.5 MPa through the same specification ceramic sand disc. The filtration loss of the test slurry was recorded. Each sample was tested in parallel 3 times and the average value was taken. The plugging rate was calculated by dividing the difference between the blank filtration loss and the test slurry filtration loss by the blank filtration loss and then multiplying by 100%.

[0054] For viscosity retention testing, the test sample was placed in a sealed glass bottle, with the liquid volume being 80% of the effective volume of the glass bottle. The initial apparent viscosity was first measured at 25°C. Then, the sealed glass bottle was placed in a 45°C constant temperature oven and allowed to stand for 30 days. After removal, the temperature was restored to 25°C, and the bottle was stirred at 4000 rpm for 5 minutes. The apparent viscosity after storage was then measured using the same method. Each sample was tested in parallel three times, and the average value was taken. The viscosity retention rate was calculated by dividing the apparent viscosity after storage by the initial apparent viscosity and then multiplying by 100%.

[0055] The performance test data above are shown in Table 1.

[0056] Table 1: Performance Test Results

[0057] The test results in Table 1 clearly show that Examples 1-3 exhibit significant advantages over Comparative Examples 1-3 in terms of anti-collapse, plugging, filtration loss reduction, lubrication drag reduction, and storage stability. This demonstrates that the present invention effectively solves the problems of existing drilling fluid anti-collapse lubricants, such as single plugging scale, insufficient lubricating film strength, limited shale inhibition ability, and unstable filtration loss control effect, by introducing oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase loaded potassium magnesium aluminum silicate composite nanosheets and boron modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres.

[0058] The apparent viscosity of Examples 1-3 was 39.2-46.8 mPa·s, and the plastic viscosity was 25.5-30.2 mPa·s, both higher than those of Comparative Examples 1-3. This indicates that the system of the present invention has better suspension stability and solid phase carrying capacity, which is beneficial for the uniform dispersion of sulfonated asphalt powder, graphite powder, flake mica powder and nano-modified materials in drilling fluid, reducing sedimentation and agglomeration.

[0059] The medium-pressure filtration loss of Examples 1-3 was 6.2-7.5 mL, significantly lower than that of Comparative Example 1 (9.6 mL), Comparative Example 2 (8.9 mL), and Comparative Example 3 (12.8 mL). The high-temperature and high-pressure filtration loss was 11.8-14.1 mL, also significantly lower than that of Comparative Example 1 (18.7 mL), Comparative Example 2 (17.5 mL), and Comparative Example 3 (24.9 mL). This indicates that the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium-magnesium-aluminum silicate composite nanosheets can enter the microcracks and pore throats of shale through their sheet-like structure. Combined with sulfonated bitumen powder, graphite powder, and sheet-like mica powder, they form a denser sealing layer, thereby improving the problem that conventional sealing agents are difficult to effectively seal micropores.

[0060] The lubrication coefficient reduction rate of Examples 1-3 was 74.6-80.1%, which was significantly higher than that of Comparative Example 1 (66.3%), Comparative Example 2 (58.6%), and Comparative Example 3 (47.2%). This indicates that boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres can play a role in hard bearing, micro-rolling, and inorganic film formation at the friction interface, and form a composite lubrication effect with polyether polyol, fatty acid soap, and graphite powder. This solves the problems of easy damage to the lubrication film and insufficient drag reduction effect of traditional lubricants under high solid phase and complex well wall contact conditions.

[0061] The shale rolling recovery rate of Examples 1-3 was 89.7-94.1%, which was higher than that of Comparative Example 1 (82.5%), Comparative Example 2 (86.1%) and Comparative Example 3 (74.6%). This indicates that potassium magnesium aluminum silicate composite nanosheets, potassium humate, potassium chloride and sodium borate can jointly enhance the shale inhibition and wellbore adsorption protection, and reduce the risk of shale hydration dispersion and spalling.

[0062] The plugging rates of Examples 1-3 were 88.4-93.0%, significantly higher than those of Comparative Example 1 (78.9%), Comparative Example 2 (82.3%), and Comparative Example 3 (66.5%). This indicates that when the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium-magnesium-aluminum silicate composite nanosheets and boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres work together, the sheet-like nanomaterials and the gradient-coated nanospheres can form a micro-nano composite plugging structure, which can make up for the insufficient plugging efficiency of a single sheet-like material or a single core material.

[0063] The viscosity retention rates of Examples 1-3 were 94.8-96.5%, higher than those of Comparative Example 1 (91.2%), Comparative Example 2 (90.6%), and Comparative Example 3 (86.7%), indicating that the system of the present invention has better dispersion stability during storage and can reduce sedimentation, flocculation, and attenuation of effective components. In particular, Comparative Example 3, lacking both the oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase loading structure and the fluorinated calcium phosphate gradient coating structure, showed the most significant decline in various properties, proving that there is a synergistic effect between the two modified materials. Comparative Example 1 mainly showed an increase in filtration loss and a decrease in plugging rate and shale rolling recovery rate, indicating that the oxygen vacancy cerium zirconium yttrium composite oxide solid solution phase loaded potassium magnesium aluminum silicate composite nanosheets mainly contribute to anti-collapse plugging and wellbore stability. Comparative Example 2 mainly showed a significant decrease in the lubrication coefficient reduction rate, indicating that the boron-modified titanium nitride-fluorinated calcium phosphate gradient coated nanospheres mainly contribute to lubrication drag reduction and interfacial film formation.

[0064] Therefore, compared with the prior art, the present invention effectively achieves a comprehensive improvement in shale suppression, microcrack sealing, filtration loss reduction, lubrication and drag reduction, and storage stability.

Claims

1. A production process for an anti-collapse lubricant for drilling fluids, characterized in that the steps include: include: S1. By weight, add 18.0-26.0 parts of deionized water to a reactor and stir at room temperature. Add 1.0-3.0 parts of polyanionic cellulose and stir. Then add 0.8-2.5 parts of polyacrylamide and continue stirring to obtain a polymer hydration solution. Add 8.0-14.0 parts of potassium humate, 2.0-6.0 parts of potassium chloride, and 0.5-2.0 parts of sodium borate to the polymer hydration solution and stir to obtain a basic anti-collapse dispersion. Mix 5.0-10.0 parts of polyether polyol, 3.0-6.0 parts of fatty acid soap, and 1.5-4.0 parts of nonionic emulsifier and stir to obtain a lubricating phase. Add the lubricating phase to the basic anti-collapse dispersion and stir to obtain a composite lubricating anti-collapse solution. S2. Add 10.0-18.0 parts of sulfonated asphalt powder, 4.0-8.0 parts of graphite powder, and 3.0-7.0 parts of flake mica powder to the composite lubricating anti-collapse fluid in sequence, stir and disperse to obtain a sealing slurry; add 2.0-6.0 parts of oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase-supported potassium magnesium aluminum silicate composite nanosheets and 1.5-5.0 parts of boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres to the sealing slurry, shear and disperse, add 0.1-0.5 parts of defoamer and 0.05-0.3 parts of preservative, continue stirring, and filter; The preparation method of the oxygen-vacancy cerium-zirconium-yttrium composite oxide solid solution phase supported potassium-magnesium-aluminum silicate composite nanosheets includes: A1. Dissolve 90.0-110.0 parts by weight of sodium silicate in 600.0-700.0 parts by weight of deionized water and stir at room temperature to obtain a silicate solution; dissolve 38.0-46.0 parts by weight of aluminum nitrate nonahydrate and 32.0-40.0 parts by weight of magnesium nitrate hexahydrate in 250.0-350.0 parts by weight of deionized water to obtain a magnesium aluminum salt solution; while stirring, add the magnesium aluminum salt solution dropwise to the silicate solution, and adjust the pH to 10.0-10 with ammonia.

8. Stir and age at 70-80℃ to obtain magnesium aluminum silicate precursor slurry. Add 16.0-23.0 parts of potassium chloride and continue stirring to obtain potassium-containing magnesium aluminum silicate precursor slurry. Transfer the potassium-containing magnesium aluminum silicate precursor slurry to a hydrothermal reactor and hydrothermally react at 150-170℃. Cool to room temperature, centrifuge, and collect precipitate A. Wash precipitate A with deionized water, then wash with anhydrous ethanol, and vacuum dry to obtain potassium-containing magnesium aluminum silicate composite nanosheets. A2. Add 80.0-100.0 parts of potassium magnesium aluminum silicate composite nanosheets to 500.0-650.0 parts of deionized water and disperse ultrasonically to obtain a nanosheet dispersion; dissolve 10.0-14.0 parts of cerium nitrate hexahydrate, 7.0-11.0 parts of zirconium oxynitrate hydrate, 2.0-4.0 parts of yttrium nitrate hexahydrate, and 45.0-65.0 parts of urea in 250.0-350.0 parts of deionized water to obtain a cerium-zirconium-yttrium salt solution; add the cerium-zirconium-yttrium salt solution to the nanosheets. The reaction was carried out in the dispersion of the cerium-zirconium-yttrium nanosheets at 85-95℃, centrifuged, and precipitate B was collected. Precipitate B was washed with deionized water and then with anhydrous ethanol, and dried under vacuum at 70-90℃ to obtain potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors. The potassium magnesium aluminum silicate composite nanosheets supported on cerium-zirconium-yttrium precursors were ground, placed in an air atmosphere, heated to 520-580℃ and held at that temperature, then switched to a hydrogen-nitrogen mixed atmosphere and held at 480-520℃. After cooling to room temperature, the nanosheets were pulverized and sieved. The preparation method of the boron-modified titanium nitride-fluorinated calcium phosphate gradient-coated nanospheres includes: B1. By weight, 90.0-110.0 parts of nano-titanium dioxide, 6.0-10.0 parts of boric acid and 140.0-180.0 parts of melamine are added to a ball mill jar and ball milled to obtain a boron-nitrogen-titanium composite precursor. Under an ammonia atmosphere, the boron-nitrogen-titanium composite precursor is heated to 760-800℃ for heat treatment, then heated to 900-940℃ for reaction, cooled to room temperature, ground, washed with deionized water, and dried to obtain boron-modified titanium nitride nanocore material. B2. Add 80.0-100.0 parts of boron-modified titanium nitride nanomaterial to 450.0-550.0 parts of deionized water and disperse ultrasonically to obtain a core material dispersion; dissolve 58.0-94.0 parts of calcium nitrate tetrahydrate in 150.0-220.0 parts of deionized water to obtain a calcium source solution; dissolve 18.0-26.0 parts of ammonium dihydrogen phosphate in 120.0-180.0 parts of deionized water to obtain a phosphorus source solution; dissolve 1.7-3.2 parts of ammonium fluoride in 50... A fluorine source solution was obtained by adding 0-90.0 parts of deionized water; under stirring, the phosphorus source solution and fluorine source solution were added to the core material dispersion, the pH was adjusted to 9.8-10.6 with ammonia, and then the calcium source solution was added dropwise to maintain the pH at 9.8-10.

6. The reaction was stirred, aged, centrifuged, and precipitate C was collected; precipitate C was washed with deionized water and then with anhydrous ethanol, and dried under vacuum at 60-80℃; under a nitrogen atmosphere, it was heat-treated at 460-500℃, pulverized, and sieved.

2. The production process of the anti-collapse lubricant for drilling fluid according to claim 1, characterized in that, In step S1, the nonionic emulsifier is selected from at least one of lauryl alcohol polyoxyethylene ether, isotridecyl alcohol polyoxyethylene ether, and oleyl alcohol polyoxyethylene ether.

3. The production process of the anti-collapse lubricant for drilling fluid according to claim 1, characterized in that, In step S2, the defoamer is selected from at least one of polyether-modified silicone defoamer, dimethyl silicone oil emulsion, and mineral oil defoamer; the preservative is selected from at least one of 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, 1,2-benzisothiazolin-3-one, and 2-bromo-2-nitro-1,3-propanediol.

4. The production process of the anti-collapse lubricant for drilling fluid according to claim 1, characterized in that, In step A1, the vacuum drying temperature is 70-90℃.

5. The production process of the anti-collapse lubricant for drilling fluid according to claim 1, characterized in that, In step A2, the temperature is raised to 520-580℃ and held for 2-4 hours, and the temperature is held at 480-520℃ for 2-4 hours.

6. The production process of the anti-collapse lubricant for drilling fluid according to claim 1, characterized in that, In step B1, the heat treatment time at 760-800℃ is 1.5-2.5 hours, and the reaction time at 900-940℃ is 3-5 hours.

7. The production process of the anti-collapse lubricant for drilling fluid according to claim 1, characterized in that, In step B2, the heat treatment time at 460-500℃ is 1.5-2.5 hours.

8. A drilling fluid anti-collapse lubricant, characterized in that, The drilling fluid anti-collapse lubricant is prepared according to the production process of the drilling fluid anti-collapse lubricant according to any one of claims 1-7.

Citation Information

Patent Citations

  • Preparation and application for green, environmentally-friendly and highly-efficient water-based drilling fluid lubricant

    CN111117577A

  • Titanium oxide modified graphite phase carbon nitride nano-composite plugging agent and oil-based drilling fluid

    CN119912912A