Rough copper layer based on nanoparticle deposition and removal and preparation method thereof
By using nanoparticle deposition and selective removal to form a uniform pit structure on the copper layer surface, the problem of uncontrollable copper surface roughness in existing technologies is solved, and the bonding strength and production efficiency of multilayer metal coatings are improved.
Patent Information
- Application Number
- CN202611317574.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-08-28
AI Technical Summary
Existing copper surface roughening treatment technologies suffer from problems such as uncontrollable roughness, poor uniformity, and low batch-to-batch consistency, resulting in insufficient adhesion of subsequent plating layers, high production costs, and difficult maintenance.
A method of nanoparticle deposition and selective removal is adopted. Inert nanoparticles are deposited on the surface of a copper layer and then selectively dissolved to form a uniformly distributed pit structure. The roughness is controlled by the particle size of the nanoparticles, thus preparing a rough copper layer based on nanoparticle deposition and removal.
It achieves high-precision roughness control of the copper layer surface, improves the bonding strength of multi-layer metal coatings, reduces production costs, and improves batch reproducibility and in-plane uniformity.
Smart Images

Figure CN122856296B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to surface treatment technology, specifically to a rough copper layer based on nanoparticle deposition and removal and its preparation method. Background Technology
[0002] In multilayer metal composite electroplating processes, the copper layer is the core bottom layer or intermediate transition layer of the precision electronic plating structure. Its surface microstructure, roughness uniformity, and structural stability directly determine the interfacial bonding performance and overall service reliability of subsequent functional plating layers such as nickel, gold, silver, and tin. If the copper layer surface is too smooth, the subsequently deposited metal plating layers can only rely on a single chemical bond for adhesion, without a mechanical anchoring structure to assist in locking. Under conditions such as subsequent packaging, high-temperature heating, mechanical bending, and thermal cycling, stress concentration is prone to occur at the plating interface, leading to failure problems such as peeling, delamination, and flaking, which seriously reduces the conductivity stability, weather resistance, and service life of precision electronic components. Therefore, controlling, uniform, and adaptable roughening treatment of the electroplated copper layer is a core key process for improving the interfacial bonding of multilayer metal plating layers and ensuring the quality of precision electroplated products.
[0003] Currently, the mainstream copper surface roughening technologies in the industry mainly include three types: chemical micro-etching, mechanical grinding / sandblasting, and conventional electroplating. These technologies can achieve copper surface roughening to a certain extent, but they have the following drawbacks: Firstly, there is the chemical micro-etching method. This method uses a persulfate-sulfuric acid or hydrogen peroxide-sulfuric acid etching system. The oxidant oxidizes the copper surface to form copper oxide, which is then dissolved in an acidic medium. Selective etching is achieved by relying on the high chemical activity at the grain boundaries and lattice defects on the copper surface, resulting in a rough surface. However, this etching process is highly random, relying solely on the disordered corrosion caused by microscopic defects in the material. This leads to randomly distributed corrosion pits, grain boundary trenches, and sharp spikes on the copper surface. On the one hand, the roughness varies greatly between different production batches and different areas of the same material, resulting in poor controllability, in-plane uniformity, and batch-to-batch reproducibility, making standardized and precise control impossible. On the other hand, the surface spikes easily cause concentrated current in subsequent electroplating, leading to a loose and highly porosity upper plating layer. Narrow and deep corrosion pits easily retain electroplating solution and bubbles, inducing defects such as pinholes and voids in the plating layer. Furthermore, the micro-etching solution is consumed quickly, has poor stability, and requires frequent replacement, resulting in high overall maintenance costs and production losses.
[0004] Secondly, mechanical grinding / sandblasting. This method uses physical external force to grind and impact the copper surface, creating scratches and pits to achieve a roughening effect. This process is a physical damage-based roughening method, with poor substrate compatibility, easily causing deformation and damage to thin copper foil and precision circuit substrates, making it unsuitable for processing ultra-thin, precision electronic substrates. Furthermore, the rough morphology produced by physical processing is completely random, with no regular adjustable roughness, extremely low precision, and the process easily introduces dust, metal debris, and other foreign matter, causing secondary contamination of the copper surface, affecting the purity of subsequent plating layers and the stability of interface bonding, thus failing to meet the production requirements of high-end precision electroplating.
[0005] Thirdly, the conventional electroplating roughening method. This method promotes rapid, disordered crystallization of the copper layer by controlling high current density and omitting electroplating additives, forming a rough surface with coarse grains. This process has a narrow roughness control range and poor adjustability. Furthermore, the resulting rough structure is merely a disordered accumulation of grain protrusions without regular pit anchoring structures, failing to provide effective mechanical interlocking sites for subsequent plating layers. This results in poor mechanical interlocking performance, weak thermal shock and bending resistance at the plating interface, and a risk of plating delamination and peeling. Therefore, the roughening modification effect is limited.
[0006] Therefore, how to overcome the shortcomings of the existing technology is the subject of this invention. Summary of the Invention
[0007] The purpose of this invention is to provide a rough copper layer based on nanoparticle deposition and removal and its preparation method, so as to solve the above-mentioned technical problems.
[0008] To achieve the above objectives, the first aspect of this application provides a method for preparing a rough copper layer based on nanoparticle deposition and removal, comprising the following steps: S1. Prepare a nano-composite copper plating solution, wherein the nano-composite copper plating solution is an acidic aqueous solution of copper sulfate, comprising, by mass concentration: 50-100 g / L copper ions, 100-200 g / L 98% sulfuric acid, 20-60 μg / L chloride ions, 5-25 g / L inert nanoparticles, 0.05-0.8 g / L cationic dispersant, with the balance being deionized water; S2. Using a copper substrate as the cathode, electroplating is performed using the aforementioned nanocomposite copper plating solution to deposit a composite copper layer with embedded inert nanoparticles on the surface of the copper substrate. S3. Clean the electroplated copper substrate and then use a selective removal solution to selectively dissolve and remove the inert nanoparticles on the surface of the composite copper layer, forming a uniformly distributed pit structure on the surface of the copper layer to obtain a rough copper layer.
[0009] In a further technical solution, in S1, the inert nanoparticles are any one of silicon dioxide, aluminum oxide, and titanium dioxide.
[0010] In a further technical solution, the inert nanoparticles are nano-silica particles with a particle size of 80nm~100nm.
[0011] In a further technical solution, in S1, the cationic dispersant is at least one of hexadecyltrimethylammonium bromide and polydiallyldimethylammonium chloride.
[0012] In a further technical solution, the cationic dispersant is hexadecyltrimethylammonium bromide.
[0013] In a further technical solution, the preparation process of the nanocomposite copper plating solution described in S1 includes: S11. Dissolve the cationic dispersant in deionized water and stir until completely dissolved to obtain an aqueous solution of the cationic dispersant. S12. Add inert nanoparticles to the cationic dispersant aqueous solution, stir and mix, and then perform ultrasonic dispersion for 20-40 min to obtain a uniform nanoparticle dispersion. S13. Dissolve copper sulfate pentahydrate and sulfuric acid in deionized water and stir until completely dissolved to obtain the basic copper plating solution. S14. Add the nanoparticle dispersion to the base copper plating solution, stir evenly, and then add deionized water to make up the volume to obtain the nanocomposite copper plating solution.
[0014] In a further technical solution, during the S2 electroplating process, mechanical stirring or ultrasonic-assisted dispersion is used to maintain the suspension of inert nanoparticles in the plating solution.
[0015] In a further technical solution, in S3, when the inert nanoparticles are nano-silica, the selective removal solution is a sodium hydroxide solution with a mass fraction of 5% to 10%, the removal temperature is 30 to 50°C, and the removal time is 10 to 20 minutes.
[0016] In a further technical solution, after S3 removal is completed, the process involves sequential rinsing with deionized water, neutralization with dilute sulfuric acid, rinsing again with water, and drying.
[0017] According to a second aspect of this application, a rough copper layer is provided, which is prepared by the preparation method described in the first aspect, wherein the surface of the rough copper layer has a uniformly distributed pit structure that matches the size of the inert nanoparticles.
[0018] The rough copper layer based on nanoparticle deposition and removal and its preparation method provided in this application have the following technical advantages: By selectively removing inert nanoparticles after co-deposition with copper, the process leverages the highly linear relationship between copper surface roughness and nanoparticle size. Target roughness can be preset by selecting nanoparticles of different sizes, resulting in high precision and predictability. The nanoparticles are uniformly dispersed and captured in the plating solution, leading to a uniform roughness distribution within the copper surface and good batch-to-batch reproducibility. This effectively solves the problems of large random fluctuations in roughness, poor in-plane uniformity, and low batch-to-batch consistency associated with traditional chemical micro-etching and mechanical polishing processes.
[0019] Furthermore, by selectively removing nanoparticles to form a uniformly distributed pit structure on the copper layer surface, these pits can provide stable mechanical interlocking anchoring sites for subsequent nickel, gold, silver, tin, and other plating layers, significantly improving the bonding strength between multiple metal plating layers. At the same time, the plating solution system is stable, has a long service life, is easy to operate, and has low production costs, making it suitable for large-area, large-scale precision electronic electroplating production. Attached Figure Description
[0020] Figure 1 This is a roughened copper surface morphology diagram (scale bar 100 μm) of Example 1 of the present invention. Figure 2 This is a roughened copper surface morphology diagram (scale bar 100 μm) of Embodiment 2 of the present invention. Figure 3 This is a roughened copper surface morphology diagram of Comparative Example 1 of the present invention (scale bar 100 μm). Figure 4 This is a two-dimensional height topography image (5μm×5μm scanning area) of AFM in Embodiment 1 of the present invention. Figure 5 This is a histogram of the overall height distribution (all scanned areas) of Embodiment 1 of the present invention. Figure 6 This is the height distribution grayscale histogram of Embodiment 1 of the present invention; Figure 7 This is a table of roughness statistical parameters for Embodiment 1 of the present invention; Figure 8 This is a two-dimensional height topography image (5μm×5μm scanning area) of AFM in Embodiment 2 of the present invention; Figure 9 This is a histogram of the overall height distribution (all scanned areas) of Embodiment 2 of the present invention. Figure 10 This is the height distribution grayscale histogram of Embodiment 2 of the present invention; Figure 11 This is a table of roughness statistical parameters for Embodiment 2 of the present invention; Figure 12 This is a two-dimensional height topography image (5μm×5μm scanning area) of AFM for Comparative Example 1 of the present invention. Figure 13 This is a histogram of the overall height distribution (all scanned areas) of Comparative Example 1 of the present invention. Figure 14 This is the height distribution grayscale histogram of Comparative Example 1 of the present invention; Figure 15 This is a table of roughness statistical parameters for Comparative Example 1 of the present invention; Figure 16 This is an overall flowchart of the rough copper layer preparation method according to an embodiment of the present invention; Figure 17 This is a flow chart illustrating the preparation process of the nanocomposite copper plating solution according to an embodiment of the present invention. Figure 18 This is a roughened copper surface morphology diagram (scale bar 100 μm) of the blank comparative example 1 of the present invention. Figure 19 This is a two-dimensional height topography image (5μm×5μm scanning area) of AFM for the blank comparative example 1 of this invention. Figure 20 This is a histogram of the overall height distribution (all scanned areas) of the blank comparative example 1 of this invention. Figure 21 This is the height distribution grayscale histogram of the blank comparative example 1 of this invention; Figure 22 This is a table of roughness statistical parameters for the blank comparative example 1 of this invention. Detailed Implementation
[0021] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0022] The terms "first," "second," etc., used in this article do not specifically refer to order or sequence, nor are they intended to limit this case; they are merely used to distinguish components or operations described using the same technical terms.
[0023] The terms "connection" or "positioning" as used in this article can refer to two or more components or devices making direct physical contact with each other, or making indirect physical contact with each other, or to two or more components or devices operating or moving with each other.
[0024] The terms “include,” “including,” and “have” used in this article are all open-ended, meaning they include but are not limited to.
[0025] Unless otherwise specified, the terms used herein generally have their ordinary meaning in the context of the art, the subject matter, and the specific context. Certain terms used to describe this case will be discussed below or elsewhere in this specification to provide additional guidance to those skilled in the art in describing the case.
[0026] The terms “front,” “back,” “up,” “down,” “left,” and “right” used in this article are directional terms. In this case, they are only used to describe the positional relationship between the structures and are not intended to limit the specific direction of the protection scheme or its actual implementation.
[0027] The main chemical reagents and materials used in the embodiments of this invention are as follows: copper sulfate pentahydrate (CuSO4·5H2O), analytical grade, purity ≥99.0%; concentrated sulfuric acid (H2SO4), analytical grade, 98%; concentrated hydrochloric acid (HCl), analytical grade, 36-38%, used to provide a chloride ion source; nano-silica (SiO2) particles, with particle sizes of 80nm and 100nm, and specific surface areas of approximately 50 m² / g and approximately 35 m² / g, respectively; hexadecyltrimethylammonium bromide (CTAB), analytical grade, purity ≥99.0%; sodium hydroxide (NaOH), analytical grade, purity ≥96.0%; hydrogen peroxide (H2O2), analytical grade, 30%; copper foil substrate, 8-inch circular electrolytic copper foil, thickness 0.3mm, purity ≥99.9%; deionized water, resistivity ≥18.2 MΩ·cm, prepared in the laboratory; nitrogen, high-purity nitrogen, purity ≥99.999%.
[0028] The main experimental equipment used in this invention embodiment is as follows: DC regulated power supply, output current 0-3A, output voltage 0-30V; constant temperature water bath, temperature control range room temperature-100℃, temperature control accuracy ±0.5℃; ultrasonic cleaner, frequency 40kHz, power 500W; mechanical stirring device, speed range 0-2000rpm; atomic force microscope (AFM), used for surface roughness characterization; optical microscope (OM), used for surface morphology observation; thermal shock test chamber, temperature range -70℃~+300℃; bending test machine, used for bending reliability testing; electroplating tank, PP material, effective volume 5L, equipped with anode and cathode clamps; phosphor bronze anode, purity ≥99.9%, size 150mm×100mm×5mm.
[0029] Example 1: In this example, a rough copper layer was prepared by co-deposition of 80nm nano-silica particles, as described below. Figure 16 , 17 As shown, it includes the following steps: S1. Prepare the nano-composite copper plating solution.
[0030] The plating solution used in this embodiment consists of: 80 g / L copper ions (added in the form of copper sulfate pentahydrate), 100 g / L sulfuric acid (98% H2SO4), 40 μg / L chloride ions (added in the form of HCl), 2 g / L nano silica (particle size 80nm), and 0.3 g / L hexadecyltrimethylammonium bromide (CTAB).
[0031] Plating solution preparation method: Prepare the above plating solution according to the following steps.
[0032] S11. Weigh 0.9g of CTAB and add it to 300mL of deionized water. Stir the solution in a 40℃ water bath until completely dissolved to obtain an aqueous solution of CTAB.
[0033] S12. Weigh 6g of 80nm SiO2 nanoparticle powder and slowly add it to the above CTAB aqueous solution while stirring. Place the mixture in an ultrasonic cleaner and ultrasonically disperse it for 30 minutes at a frequency of 40kHz and a power of 500W to obtain a uniform nanoparticle dispersion.
[0034] S13. Weigh 942g of copper sulfate pentahydrate and add it to approximately 2L of deionized water, stirring until completely dissolved. Slowly add 300g of 98% concentrated sulfuric acid while stirring, being careful to avoid exothermic reactions. Add 120μg of concentrated HCl solution and stir until homogeneous.
[0035] S14. Add the above nanoparticle dispersion to the copper sulfate-sulfuric acid mixed solution and stir until homogeneous. Make up to 3L with deionized water and continue stirring for 30 minutes to obtain the final plating solution.
[0036] S2. Using a copper substrate as the cathode, electroplating is performed using the aforementioned nanocomposite copper plating solution to deposit a composite copper layer with embedded inert nanoparticles on the surface of the copper substrate.
[0037] Substrate pretreatment: Use an 8-inch circular copper foil as the substrate with a thickness of 0.3mm, and perform pretreatment according to the following steps.
[0038] Degreasing treatment: Immerse the copper foil in a 5% NaOH solution at 50°C for 5 minutes to remove surface oil.
[0039] Water washing: Rinse the copper foil surface with deionized water 3 times, 30 seconds each time.
[0040] Pickling and activation: Immerse the copper foil in a 10% H2SO4 solution and soak it at room temperature for 1 minute to remove the surface oxide layer.
[0041] Water washing: Rinse the copper foil surface with deionized water 3 times, 30 seconds each time, and set aside.
[0042] The following electroplating process parameters were used for the co-deposition of copper and nanoparticles: current density 3 A / dm² (ASD), plating bath temperature 25℃, mechanical stirring at 400 rpm, plating time 3 minutes, phosphor bronze anode material, and anode-cathode distance 10 cm. The pretreated copper foil was used as the cathode, and the phosphor bronze plate as the anode, both vertically immersed in the plating bath. A DC power supply was connected, and electroplating was performed according to the above parameters. Mechanical stirring was maintained during the electroplating process to ensure uniform suspension of the nanoparticles in the plating bath.
[0043] S3. Clean the electroplated copper substrate and then use a selective removal solution to selectively dissolve and remove the inert nanoparticles on the surface of the composite copper layer, forming a uniformly distributed pit structure on the surface of the copper layer to obtain a rough copper layer.
[0044] First, remove the plated part and rinse the surface with deionized water three times for 30 seconds each time to remove any residual plating solution.
[0045] The second step involves immersing the plated part in an 8% NaOH aqueous solution and soaking it in a constant temperature water bath at 45°C for 10 minutes to selectively dissolve and remove SiO2 nanoparticles.
[0046] The third step is to remove the plated part and rinse the surface with deionized water three times, for 30 seconds each time.
[0047] The fourth step is to immerse the plated parts in a 5% H2SO4 solution at room temperature for 30 seconds to neutralize them.
[0048] Step 5: Remove the plated part and rinse the surface with deionized water 3 times, 30 seconds each time.
[0049] The sixth step is to dry the surface with high-purity nitrogen gas to obtain a rough copper layer sample.
[0050] Blank comparison example 1: S1. Prepare a pure acidic copper plating solution (without nano-SiO2 particles). The plating solution used in this comparative example consisted of: 80 g / L copper ions (added in the form of copper sulfate pentahydrate), 100 g / L sulfuric acid (98% H2SO4), 40 μg / L chloride ions (added in the form of HCl), with the balance being deionized water. No nano-silica particles or dispersants were added.
[0051] S11. Measure 300 mL of deionized water for later use.
[0052] S12. Weigh 942g of copper sulfate pentahydrate and add it to about 2L of deionized water. Stir until completely dissolved. Slowly add 300g of 98% concentrated sulfuric acid while stirring to avoid the risk of exothermic reaction. Then add 120μg of concentrated HCl solution and stir until homogeneous to obtain a copper sulfate-sulfuric acid mixed solution.
[0053] S13. Add the reserved deionized water to the copper sulfate-sulfuric acid mixed solution, stir evenly, and make up to 3L with deionized water. Continue stirring for 30 minutes to obtain a pure acidic copper plating solution without nanoparticles.
[0054] S2. Electroplating to prepare a pure copper plating layer This comparative example uses the same substrate and pretreatment process as Example 1: an 8-inch circular copper foil with a thickness of 0.3 mm is selected as the substrate; the complete pretreatment process is carried out in sequence: soaking in 5% NaOH solution at 50°C for 5 minutes to remove oil, rinsing with deionized water 3 times (30 seconds each time), soaking in 10% H2SO4 solution at room temperature for 1 minute for acid washing and activation, and rinsing with deionized water 3 times (30 seconds each time).
[0055] The electroplating process parameters were the same as in Example 1: current density 3 A / dm², plating solution temperature 25℃, mechanical stirring speed 400 rpm, electroplating time 3 minutes, phosphorus copper anode, and cathode-cathode distance 10 cm. The pretreated copper foil was used as the cathode and vertically immersed in the prepared pure acidic copper plating solution along with the phosphorus copper anode. A DC power supply was connected for electroplating, and mechanical stirring at 400 rpm was maintained throughout the process to ensure a uniform and stable plating solution system.
[0056] S3, post-treatment and selective removal process First, after electroplating is completed, remove the plated part and rinse the surface with deionized water 3 times, 30 seconds each time, to remove the residual plating solution on the surface; The second step is to immerse the plated parts in an 8% NaOH aqueous solution and soak them in a constant temperature water bath at 45°C for 10 minutes to complete the alkaline removal treatment exactly the same as in Example 1. Third step, remove the plated part and rinse the surface with deionized water 3 times, 30 seconds each time; The fourth step is to immerse the plated parts in a 5% H2SO4 solution at room temperature for 30 seconds for neutralization. Step 5: Remove the plated part and rinse the surface with deionized water 3 times, 30 seconds each time; Step 6: Dry the surface with high-purity nitrogen to obtain a blank comparative pure copper plating sample.
[0057] Figure 18 The image shown is a roughened copper surface morphology diagram of the blank comparative example 1 of this invention. By comparing it with the corresponding surface morphology of Example 1, it can be seen that: under completely identical electroplating, alkaline removal and acid-base post-treatment processes, the surface of the pure copper plating without the addition of nano-SiO2 is generally smooth and clean, without large-area undulations, irregular holes and discrete pit clusters. Only slight fine textures of copper plating are present. The macroscopic and micron-level morphology is uniform and regular, which forms a significant visual difference from the rough morphology of Example 1 with dense and uniform pits.
[0058] Figure 19 This is a two-dimensional AFM (5μm × 5μm scanning area) morphology image of the blank comparative example 1 of this invention. Compared to the numerous uniformly deep and densely distributed nano-pit structures in the AFM morphology of Example 1 under the same scanning area, the pure copper coating in this comparative example has extremely small height undulations, a smooth surface contour, and no obvious depressions, pits, or other characteristic microstructures. The surface undulations of the coating tend to be uniform, and there are no specific point depressions formed after the removal of nanoparticles as seen in Example 1.
[0059] Figure 20 This is a histogram of the overall height distribution (all scanned areas) of the blank comparative example 1 of this invention. Figure 21 The grayscale histogram of the height distribution of the blank comparative example 1 of this invention further verifies the morphological differences between the two groups of samples from a quantitative perspective: the height distribution range of the copper layer surface in this comparative example is narrow, the peak height is concentrated, the overall surface height difference is minimal, and the surface is uniform; while the height distribution range of the sample in Example 1 is wider and more discrete, with a large number of low-level depressions formed after the removal of surface nano-SiO2 particles. This result indicates that the blank control group did not show a significant improvement in roughness after undergoing the same electroplating and alkali treatment process.
[0060] Figure 22 The table of roughness statistical parameters for the blank comparative example 1 of this invention forms a quantitative comparison with the roughness statistical parameters of Example 1: The core roughness parameters such as surface roughness Ra and Rz of the sample in this comparative example are at extremely low levels, which is consistent with the microscopic morphology characteristics of a flat pure copper electroplated layer; while the sample in Example 1 has a significantly improved roughness parameter due to the formation of a uniform pit anchoring structure after the selective removal of nano-SiO2 particles embedded in the surface layer, and the morphology and roughness are highly controllable and stable.
[0061] Based on the above multi-dimensional characterization comparison, in the single-variable experimental system, when only the nano-SiO2 co-deposition process is missing, the final coating cannot form the characteristic uniform pitted rough structure of the present invention, proving that the selective removal mechanism of this application is effective, and that the nano-pits and roughness morphology on the copper layer surface are not caused by process corrosion or other factors.
[0062] Example 2: In this example, a rough copper layer was prepared by co-deposition of 100nm nano-silica particles.
[0063] S1. Prepare the nano-composite copper plating solution.
[0064] Plating solution formulation: The plating solution used in this embodiment consists of: 80 g / L copper ions (added in the form of copper sulfate pentahydrate), 100 g / L sulfuric acid (98% H2SO4), 40 μg / L chloride ions (added in the form of HCl), 5 g / L nano silica (particle size 100nm), and 0.5 g / L hexadecyltrimethylammonium bromide (CTAB).
[0065] Plating solution preparation method: Prepare the above plating solution according to the following steps.
[0066] S11. Weigh 1.5g of CTAB and add it to 300mL of deionized water. Stir in a 40℃ water bath until completely dissolved to obtain an aqueous solution of CTAB.
[0067] S12. Weigh 15g of 100nm nano-SiO2 powder and slowly add it to the above CTAB aqueous solution while stirring. Place the mixture in an ultrasonic cleaner and ultrasonically disperse it for 30 minutes at a frequency of 40kHz and a power of 500W to obtain a uniform nanoparticle dispersion.
[0068] S13. Weigh 942g of copper sulfate pentahydrate and add it to approximately 2L of deionized water, stirring until completely dissolved. Slowly add 300g of 98% concentrated sulfuric acid while stirring, being careful to avoid exothermic reactions. Add 120μg of concentrated HCl solution and stir until homogeneous.
[0069] S14. Add the above nanoparticle dispersion to the copper sulfate-sulfuric acid mixed solution and stir until homogeneous. Make up to 3L with deionized water and continue stirring for 30 minutes to obtain the final plating solution.
[0070] S2. Using a copper substrate as the cathode, electroplating is performed using the aforementioned nanocomposite copper plating solution to deposit a composite copper layer with embedded inert nanoparticles on the surface of the copper substrate. Substrate pretreatment: The substrate pretreatment method is the same as in Example 1, using 8-inch circular copper foil with a thickness of 0.3 mm, and performing degreasing, water washing, acid pickling activation, and water washing in sequence.
[0071] Co-deposition electroplating process: Co-deposition of copper and nanoparticles was performed using the following electroplating process parameters: current density 2A / dm³. 2 (ASD), plating bath temperature 25℃, stirring method: mechanical stirring, stirring speed 400 rpm, electroplating time 5 minutes, anode material: phosphor bronze anode, cathode-cathode distance 10 cm. The pretreated copper foil was used as the cathode, and the phosphor bronze plate as the anode, vertically immersed in the plating bath. A DC power supply was connected, and electroplating was performed according to the above parameters. Mechanical stirring was maintained during the electroplating process to ensure uniform suspension of the nanoparticles in the plating bath.
[0072] S3. Clean the electroplated copper substrate and then use a selective removal solution to selectively dissolve and remove the inert nanoparticles on the surface of the composite copper layer, forming a uniformly distributed pit structure on the surface of the copper layer to obtain a rough copper layer.
[0073] First, remove the plated part and rinse the surface with deionized water three times, 30 seconds each time, to remove any residual plating solution.
[0074] The second step involves immersing the plated part in an 8% NaOH aqueous solution and soaking it in a constant temperature water bath at 45°C for 15 minutes to selectively dissolve and remove SiO2 nanoparticles.
[0075] The third step is to remove the plated part and rinse the surface with deionized water three times, for 30 seconds each time.
[0076] The fourth step is to immerse the plated parts in a 5% H2SO4 solution at room temperature for 30 seconds to neutralize them.
[0077] Step 5: Remove the plated part and rinse the surface with deionized water 3 times, 30 seconds each time.
[0078] The sixth step is to dry the surface with high-purity nitrogen gas to obtain a rough copper layer sample.
[0079] Comparative Example 1: This comparative example uses a traditional chemical micro-etching method to prepare a rough copper layer, for comparison with the method of the present invention.
[0080] Plating solution formulation: The basic plating solution used in this comparative example has the following composition (excluding nanoparticles): copper ions (added in the form of copper sulfate pentahydrate) 80 g / L, sulfuric acid (98% H2SO4) 100 g / L, and chloride ions (added in the form of HCl) 40 μg / L.
[0081] Electroplating process: The following electroplating process parameters were used to prepare the pure copper plating layer: current density 2 A / dm² (ASD), plating solution temperature 25℃, stirring method is mechanical stirring, stirring speed 400 rpm, electroplating time 5 minutes, anode material is phosphor bronze anode, and anode-cathode distance is 10 cm.
[0082] Chemical micro-etching process: After electroplating, the following chemical micro-etching process is used for roughening treatment.
[0083] First, remove the plated part and rinse the surface with deionized water three times, 30 seconds each time.
[0084] The second step is to prepare the micro-etching solution: 20 g / L H2SO4 + 22 g / L H2O.
[0085] The third step is to immerse the plated part in the above-mentioned micro-etching solution and soak it at room temperature for 5 minutes.
[0086] Fourth step, remove the plated part and rinse the surface with deionized water 3 times, 30 seconds each time.
[0087] The fifth step is to dry the surface with high-purity nitrogen gas to obtain a chemically micro-etched roughened copper layer sample.
[0088] The samples prepared in Example 1, Example 2, and Comparative Example 1 were subjected to the following performance tests: Surface morphology and roughness testing: The surface morphology of the roughened copper layer was observed using an optical microscope (OM), and the surface roughness Ra value was measured using an atomic force microscope (AFM). The AFM test was conducted in tapping mode, with a scanning range of 5 μm × 5 μm. Five different locations were tested for each sample, and the average value was taken.
[0089] Adhesion thermal shock test: A 10 μm thick nickel layer was electroplated onto the roughened copper layer surface, followed by a thermal shock test. The test conditions were as follows: the sample was placed in a 300℃ oven for 10 minutes, then immediately immersed in room temperature deionized water for rapid cooling, and this cycle was repeated 30 times. The adhesion of the nickel layer was evaluated by observing whether peeling or flaking occurred.
[0090] Bending reliability test: A 10μm thick nickel layer was electroplated on the roughened copper layer surface, and then a bending test was performed. A bending test machine was used, with a bending radius of 1mm and a bending angle of 180°. After 50 bending cycles, the nickel layer was observed for cracking to evaluate the bending reliability of the plating.
[0091] The test results are summarized in the table below:
[0092] The surface morphology of the roughened copper layers prepared in Example 1, Example 2, and Comparative Example 1 was observed using an optical microscope, and the results are as follows: Figure 1 , Figure 2 and Figure 3 As shown: Example 1 uses 80nm nano-silica particles to prepare a roughened copper layer with a uniform and delicate light brownish-red surface. The pit structure is uniform in size and densely and evenly distributed. There are no obvious scratches, grooves or abnormal defects in the entire field of view, and the roughening morphology is excellent.
[0093] Example 2 uses 100nm nano-silica particles to prepare a roughened copper layer with a dark brownish-red surface. The pit size is significantly larger than that of Example 1, and the granular texture is enhanced. However, the pits are still uniformly distributed, with a regular and orderly morphology and no messy structure caused by random corrosion.
[0094] Comparative Example 1 shows a copper layer prepared using traditional chemical micro-etching technology. The surface is light yellowish-brown with a messy morphology, and there are obvious random corrosion grooves, scratches and dot-like deep corrosion pits. Some areas are severely corroded, while others are still close to a smooth substrate, and the surface roughness is uneven. Chemical micro-etching preferentially proceeds along grain boundaries and defects, and cannot form a uniform and regular pit structure.
[0095] The observations above show that the rough copper layers prepared in Examples 1 and 2 of this invention exhibit uniformly distributed pit structures on their surfaces, with pit sizes corresponding to nanoparticle diameters of 80 nm and 100 nm, respectively. Therefore, by adjusting the nanoparticle diameter, the size of the rough structure can be effectively controlled. In contrast, the roughened copper layer prepared using the chemical micro-etching method in Comparative Example 1 has an uneven surface morphology, with a large range of roughness fluctuations, making precise control difficult.
[0096] The rough copper layer prepared in Example 1 was scanned in a 5μm × 5μm area using an atomic force microscope to obtain the three-dimensional height morphology of the surface as shown below. Figure 4 As shown, a large number of uniformly sized and densely distributed microstructures are formed on the surface of the copper layer. The protrusions and depressions are arranged alternately, without large local smooth areas, isolated ultra-large deep etch pits or sharp burrs. The overall micro-undulations are regular and orderly, and the distribution of the protrusions and depressions is highly consistent throughout the entire scanning field of view, proving that the nanoparticle co-deposition-selective removal process of the present invention can achieve uniform and controllable roughening of the copper layer surface.
[0097] Figure 5 A histogram of the surface height distribution corresponding to all pixels in the scanned area is generated. The horizontal axis represents the surface height in nm, and the vertical axis represents the number of pixels at the corresponding height. The height data in this histogram is concentrated in the range of -20nm to +10nm, with the peak center close to the 0nm reference plane. The overall distribution is approximately normal, without obvious bimodal or skewed peaks, and there is no long tail phenomenon at extreme heights.
[0098] Figure 6 A histogram of the contour-based surface height distribution for all pixels in the scanned area is generated. The horizontal axis represents the surface height in nm, and the vertical axis represents the number of pixels at the corresponding height. The distribution curves are concentrated in the range of -20nm to +10nm, with the peak position close to the 0nm reference plane. The curve shape is close to a normal distribution, without bimodal peaks, severe skewness, or extreme height tailing.
[0099] Combination Figure 5 and Figure 6 The statistical results show that the copper layer has small differences in surface unevenness, no areas of excessive corrosion or insufficient roughening, and excellent uniformity in its micro-undulations.
[0100] Figure 7 The roughness statistics for the entire scanned area are presented below, with each parameter analyzed as follows: Extreme values and total fluctuations: The minimum surface height Min is -43.406nm, the maximum height Max is 30.690nm, and the maximum peak-to-valley drop Rpv is 74.097nm. The micro-fluctuation of the copper layer is moderate, which can provide sufficient mechanical interlocking anchoring points. Core roughness indicators: arithmetic mean roughness Ra=4.969nm, root mean square roughness Rq=6.419nm, the micro-roughness values are stable and controllable, and the roughness can be linearly controlled by adjusting the particle size of inert nanoparticles; ten-point average roughness Rz=70.143nm, and the local unevenness is uniform. Height distribution characteristic parameters: Skewness Rsk=-0.140, slightly less than 0, the surface microstructure is mainly composed of regular depressions and pits, with good symmetry in the distribution of concave and convex parts; Kurtosis Rku=4.327, slightly higher than the standard normal distribution benchmark value of 3, with only a few gentle local protrusions, no sharp or abrupt defects, and good micro-surface smoothness.
[0101] The rough copper layer prepared in Example 2 was scanned in a 5μm × 5μm area using an atomic force microscope to obtain the three-dimensional height morphology of the surface as shown below. Figure 8 As shown, a large number of uniformly sized and densely distributed microstructures are formed on the surface of the copper layer. The protrusions and depressions are arranged alternately, and the overall microscopic undulations are regular and orderly. Compared with Example 1, this example uses 100nm nano-silica particles with larger particle size. The size of the surface uneven structure is increased simultaneously, the undulation amplitude is more obvious, and the distribution is uniform throughout the entire scanning field of view. There are no large local smooth areas, no isolated ultra-large deep etch pits or sharp burrs. This proves that the present invention can controllably adjust the surface roughness of the copper layer by adjusting the particle size of the nanoparticles.
[0102] Figure 9 , Figure 10 The figures show a statistical histogram and a contour histogram of the surface height distribution corresponding to all pixels in the scanned area, respectively. The horizontal axis represents the surface height (in nm), and the vertical axis corresponds to the number of pixels. The distribution curves show that the height data is concentrated in the range of -25 nm to +25 nm, with the peak center close to the 0 nm reference plane. The overall height distribution exhibits a symmetrical single-peak normal distribution, without obvious double peaks, off-peaks, or extreme height tails, indicating that the copper layer surface has small differences in unevenness and height, and there are no areas of local over-corrosion or insufficient roughening, resulting in excellent uniformity of surface micro-undulations. Compared to Example 1, this example has a wider height distribution range, corresponding to a synchronous increase in roughness, consistent with the trend of increasing nanoparticle size.
[0103] Figure 11 The roughness statistics for the entire scanned area are presented, and the key parameters are analyzed as follows: Extreme values and total fluctuations: The lowest surface height Min is -56.489nm, the highest height Max is 58.741nm, and the maximum peak-to-valley drop Rpv is 115.230nm. The micro-fluctuation amplitude of the copper layer is moderate and significantly increased compared to Example 1, which can provide more mechanical interlocking anchoring points. Core roughness indicators: arithmetic mean roughness Ra = 5.321 nm, root mean square roughness Rq = 7.105 nm. The micro-roughness values are improved in tandem with Example 1, confirming that the roughness increases regularly with the increase of the particle size of inert nanoparticles and has linear control characteristics; ten-point average roughness Rz = 109.287 nm, and the local unevenness is uniform. The height distribution characteristic parameters are: skewness Rsk=0.029, which is close to 0, indicating that the surface microstructure has good symmetry in its uneven distribution and no obvious structural imbalance with a bias towards depressions or protrusions; kurtosis Rku=7.190, which is higher than the standard normal distribution benchmark value of 3, indicating that there are a few local sharp protrusions and depressions on the surface, but the overall distribution still maintains a uniform distribution characteristic and there are no extreme abrupt defects.
[0104] Figure 12 This is an AFM three-dimensional height topography image of the rough copper layer in Comparative Example 1, with a scanning range of 5 μm × 5 μm. The copper layer surface exhibits numerous irregular protrusions and pits of varying depths, lacking a uniform and regular distribution of the surface texture. Isolated, abnormally large protruding particles are present in some areas. The surface is disordered in its undulations, with significant variations in pit depth, and no uniform, controllable micro-roughness structure. This topographic feature indicates that the process in Comparative Example 1 cannot achieve uniform control of the micro-morphology of the copper layer surface, resulting in a highly random surface texture.
[0105] Figure 13 , Figure 14 These are, respectively, the pixel distribution histogram of the copper layer surface height and the contour-based surface height distribution histogram. From... Figure 13 , 14 It can be seen that the overall height distribution range is large, covering the vertical height range from -200nm to 200nm; the pixel height distribution peak is wide and diffuse, with no concentrated or narrow height distribution range, and a large number of pixels are distributed in high and low regions far from the mean. This distribution result proves that the copper layer surface obtained in Comparative Example 1 has a high degree of dispersion in height difference, and the depth of micro protrusions and pits has no uniform scale, making it impossible to accurately and stably control the roughness.
[0106] Figure 15 The surface roughness statistics for the entire scanned area are as follows: Arithmetic mean roughness Ra = 29.9552 nm; root mean square roughness Rq = 41.2553 nm; maximum peak-to-valley height difference Rpv = 428.9778 nm; ten-point mean roughness Rz = 417.2335 nm.
[0107] The surface has a large vertical extreme value difference, with the lowest valley depth reaching -217.8887nm and the highest protrusion peak value reaching 211.091nm. The peak-valley difference exceeds 420nm, indicating that the copper layer has a severe local unevenness.
[0108] Skewness Rsk=-0.2955, slightly less than 0, indicating that the proportion of surface pits is slightly higher than that of convexity; Kurtosis Rku=6.0553, indicating that the kurtosis value is relatively high, and the proportion of pixels at both ends of the height distribution is relatively high, further confirming that the surface convexity scale is discrete and the uniformity is poor.
[0109] By comparing the AFM characterization results of Examples 1 and 2 with those of Comparative Example 1, the following conclusions can be drawn: (1) Regarding the uniformity of morphology: The pit structures on the surface of the roughened copper layer prepared in Examples 1 and 2 of this invention have uniform size and distribution, and the height distribution histogram shows symmetrical narrow peaks; the morphology of the copper surface obtained by chemical micro-etching in Comparative Example 1 is disordered and irregular, with a wide and asymmetrical height distribution and local abnormal defects. The method of this invention significantly improves the uniformity and consistency of the roughened morphology of the copper layer surface.
[0110] (2) Regarding the controllability of roughness: Example 1 uses 80nm nano-silica particles, and Example 2 uses 100nm nano-silica particles. The roughness of both increases synchronously with the increase of particle size, showing a stable linear correspondence. In contrast, the roughness of chemical micro-etching in Comparative Example 1 fluctuates randomly, and it is impossible to accurately preset the target roughness through process parameters. This invention achieves linear and controllable adjustment of roughness.
[0111] (3) In terms of structural adaptability: The uniform pit structure formed in the embodiments of the present invention can provide a stable mechanical interlocking anchoring point for subsequent nickel, gold and other coatings; the spikes and deep grooves formed by random corrosion in Comparative Example 1 are prone to current concentration and stress concentration, resulting in poor coating adhesion and low reliability.
[0112] Thermal shock test results showed that after 30 cycles of thermal shock at 300°C, the nickel layer of the samples in Examples 1 and 2 did not exhibit peeling, indicating excellent adhesion between the plating layer and the copper substrate. This is because the rough copper layer surface prepared by the method of the present invention forms a uniform three-dimensional pit structure, allowing the nickel layer to embed into these pits during subsequent nickel plating, forming a mechanical interlocking effect, thereby significantly improving the adhesion of the plating layer.
[0113] In contrast, the sample in Comparative Example 1 showed slight localized peeling after the thermal shock test, indicating insufficient adhesion of the roughened surface prepared by the chemical micro-etching method. This is because the rough structure formed by chemical micro-etching is uneven and mostly consists of open corrosion morphologies, making it difficult to form effective mechanical interlocking.
[0114] Bending test results showed that after 50 cycles of 180° bending, the nickel layer of the samples in Examples 1 and 2 did not crack, indicating that the coating has good bending reliability. This is due to the fact that the uniformly distributed pit structure can effectively release stress during the bending process and avoid coating cracking caused by stress concentration.
[0115] In contrast, the sample in Comparative Example 1 cracked after the bending test, indicating that the roughened surface prepared by the chemical micro-etching method has poor bending reliability. This is because the corrosion pits formed by chemical micro-etching vary in depth, and stress concentration points are easily formed at the deep corrosion pits, leading to cracking of the coating during bending.
[0116] In summary, the method for preparing a rough copper layer based on nanoparticle co-deposition and selective removal provided by this invention has the following advantages compared to traditional chemical micro-etching methods: better controllability of roughness; by adjusting the particle size and concentration of nanoparticles, the roughness and pit size of the copper surface can be precisely controlled. The prepared rough copper layer has a uniform pit distribution, small roughness fluctuation, and high process stability. The formed three-dimensional pit structure provides effective mechanical interlocking, significantly improving the adhesion of subsequent plating layers. Furthermore, the uniform rough structure effectively releases stress, improving the bending reliability of the plating layer. It avoids the large-scale use of oxidants in chemical micro-etching processes, reducing the difficulty of wastewater treatment.
[0117] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a rough copper layer based on nanoparticle deposition and removal, characterized in that, Includes the following steps: S1. Prepare a nano-composite copper plating solution, wherein the nano-composite copper plating solution is an acidic aqueous solution of copper sulfate, comprising, by mass concentration: 50-100 g / L copper ions, 100-200 g / L 98% sulfuric acid, 20-60 μg / L chloride ions, 5-25 g / L inert nanoparticles, 0.05-0.8 g / L cationic dispersant, with the balance being deionized water; wherein the inert nanoparticles are nano-silica particles with a particle size of 80 nm-100 nm; wherein the cationic dispersant is at least one of hexadecyltrimethylammonium bromide and polydiallyldimethylammonium chloride; S2. Using a copper substrate as the cathode, electroplating is performed using the aforementioned nanocomposite copper plating solution to deposit a composite copper layer with embedded inert nanoparticles on the surface of the copper substrate. S3. Clean the electroplated copper substrate and then treat it with a selective removal solution. The selective removal solution is a sodium hydroxide solution with a mass fraction of 5% to 10%, the removal temperature is 30 to 50°C, and the removal time is 10 to 20 minutes. The solution selectively dissolves and removes the inert nanoparticles on the surface of the composite copper layer, forming a uniformly distributed pit structure on the surface of the copper layer, thus obtaining a rough copper layer.
2. The method for preparing a rough copper layer based on nanoparticle deposition and removal according to claim 1, characterized in that: The cationic dispersant is hexadecyltrimethylammonium bromide.
3. The method for preparing a rough copper layer based on nanoparticle deposition and removal according to claim 1, characterized in that, The preparation process of the nanocomposite copper plating solution described in S1 includes: S11. Dissolve the cationic dispersant in deionized water and stir until completely dissolved to obtain an aqueous solution of the cationic dispersant. S12. Add inert nanoparticles to the cationic dispersant aqueous solution, stir and mix, and then perform ultrasonic dispersion for 20-40 min to obtain a uniform nanoparticle dispersion. S13. Dissolve copper sulfate pentahydrate and sulfuric acid in deionized water and stir until completely dissolved to obtain the basic copper plating solution. S14. Add the nanoparticle dispersion to the base copper plating solution, stir evenly, and then add deionized water to make up the volume to obtain the nanocomposite copper plating solution.
4. The method for preparing a rough copper layer based on nanoparticle deposition and removal according to claim 1, characterized in that: During the S2 electroplating process, mechanical stirring or ultrasonic-assisted dispersion is used to maintain the suspension of inert nanoparticles in the plating solution.
5. The method for preparing a rough copper layer based on nanoparticle deposition and removal according to claim 1, characterized in that: After S3 removal, the process involves sequential rinsing with deionized water, neutralization with dilute sulfuric acid, rinsing again with water, and drying.
6. A rough copper layer, characterized in that, The rough copper layer is prepared by any one of the preparation methods described in claims 1 to 5, wherein the surface of the rough copper layer is uniformly distributed with pit structures matching the size of the inert nanoparticles.
Citation Information
Patent Citations
Electrolytic codeposition of polyvinylidene and copolymer particles with copper
US3676308A