Ion implantation method, silicon-on-insulator substrate and method for manufacturing the same

By adjusting the beam current height to control the beam current density in the Smart Cut™ process, the problem of batch-to-batch variation in ion implantation damage state is solved, improving the consistency of silicon layer thickness and surface condition on silicon-on-insulator substrates.

CN122872095BActive Publication Date: 2026-11-24XIAN ESWIN MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611359012.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-24
Estimated Expiration
2046-09-03

AI Technical Summary

Technical Problem

In the Smart Cut™ process, batch variations in ion implantation damage state affect the quality of the silicon layer formed during subsequent dicing and transfer processes. Existing technologies rely solely on beam current tuning, which cannot guarantee consistency.

Method used

The method for preparing a silicon-on-insulator substrate by obtaining the beam current density of an ion beam and adjusting the beam height to make the beam current density fall within a preset density allowable range after the beam current value meets the conditions includes ion implantation of a silicon wafer to form an ion implantation damage layer, and after bonding, cracking the silicon wafer along the damage layer and transferring it to the side of the support substrate.

Benefits of technology

It improves the consistency of ion implantation damage state, reduces the difference in silicon layer thickness and surface roughness between different batches, and improves the surface condition of the silicon layer on the side away from the insulating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122872095B_ABST
    Figure CN122872095B_ABST
Patent Text Reader

Abstract

This application provides an ion implantation method, a silicon-on-insulator substrate, and a method for fabricating the same. The ion implantation method includes: tuning the ion beam used for ion implantation on a wafer to ensure the beam current value meets a preset beam current condition; obtaining the beam current density of the ion beam when the beam current value meets the condition; adjusting the beam current height of the ion beam when the beam current density does not fall within a preset density allowable range; the beam current height adjustment includes determining a target beam current density value within the density allowable range, determining a target beam current height value based on the ion beam current value, beam width, and target beam current density value, and adjusting the beam current height of the ion beam according to the target beam current height value; and performing ion implantation on the wafer using the ion beam when the beam current density falls within the density allowable range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor manufacturing technology, specifically to ion implantation methods, silicon-on-insulator substrates, and methods for their fabrication. Background Technology

[0002] Smart Cut™ technology is currently the mainstream technology for fabricating silicon-on-insulator (SOI) substrates. Its core principle is as follows: hydrogen ions are implanted into the target wafer to form a damage layer at a predetermined depth. After bonding the implanted wafer to the support wafer, appropriate heat treatment is performed to cause bubbling and complete cracking at the ion damage layer, thereby transferring the single-crystal thin film from the implanted wafer to the support substrate.

[0003] In related technologies, beam current tuning of the ion beam is typically required before ion implantation. The ion beam state formed by different beam current tunings may differ, and even if the beam current value meets process requirements, the ion implantation damage state of the wafer may still vary. Differences in the ion implantation damage state can also affect subsequent processing using ion implantation damage. Conventional ion implantation processes are mostly for device doping, and annealing and other processes are usually performed after ion implantation to achieve device performance. In these processes, beam current tuning usually only focuses on the beam current value. In contrast, hydrogen ion implantation in the Smart Cut™ process is used to form the ion implantation damage layer within the wafer upon which subsequent dicing depends. After hydrogen ion implantation, bonding and dicing processes are required; therefore, differences in the ion implantation damage state between different batches can directly affect the quality of the subsequent dicing process and the transferred silicon layer. When using only the beam current value as an evaluation parameter for beam current tuning, even if the beam current values ​​of different batches meet process requirements, the ion implantation damage state of different batches may still differ.

[0004] Therefore, improving the consistency of ion implantation damage state is an issue that needs to be considered in related processes. Summary of the Invention

[0005] This application provides an ion implantation method for a wafer. The ion implantation method includes beam current tuning of an ion beam used for ion implantation on the wafer, such that the beam current value of the ion beam meets a preset beam current value condition. When the beam current value meets the beam current value condition, the beam current density of the ion beam is obtained. When the beam current density does not fall within a preset density allowable range, the beam current height of the ion beam is adjusted to bring the beam current density into the density allowable range. The beam current height adjustment includes determining a target beam current density value within the density allowable range, determining a target beam current height value based on the ion beam current value, beam current width, and target beam current density value, and adjusting the beam current height of the ion beam according to the target beam current height value. When the beam current density falls within the density allowable range, ion implantation is performed on the wafer using the ion beam.

[0006] This application provides, in another aspect, a method for fabricating a silicon-on-insulator (SiI) substrate. The method includes beam tuning of an ion beam used for ion implantation of a silicon wafer to ensure the beam current value meets a preset beam current condition. When the beam current value meets the condition, the beam current density of the ion beam is obtained. When the beam current density does not fall within a preset allowable density range, the beam current height of the ion beam is adjusted to bring the beam current density into the allowable density range. The beam current height adjustment includes determining a target beam current density value within the allowable density range, determining a target beam current height value based on the ion beam current value, beam width, and target beam current density value, and adjusting the beam current height of the ion beam according to the target beam current height value. When the beam current density falls within the allowable density range, ion implantation is performed on the silicon wafer using the ion beam to form an ion implantation damage layer within the silicon wafer. A silicon wafer is bonded to a support substrate, at least one of the bonding surfaces of the silicon wafer and the support substrate having an insulating layer, and the silicon wafer is cracked along the ion implantation damage layer, so that a portion of the silicon wafer is transferred to one side of the support substrate to form a silicon-on-insulator substrate.

[0007] This application provides a silicon-on-insulator (SCI) substrate in another aspect. The SCI substrate includes a supporting substrate, an insulating layer, and a silicon layer. The insulating layer is located on one side of the supporting substrate, and the silicon layer is located on the side of the insulating layer opposite to the supporting substrate. The silicon layer is formed by splitting and transferring a silicon wafer along an ion-implanted damage layer, which is formed by ion implantation of the silicon wafer with an ion beam. The beam current value of the ion beam meets a preset beam current value condition, and the beam current density of the ion beam falls within a preset density allowable range. When the beam current density does not fall within the density allowable range, the beam current density is brought into the density allowable range by adjusting the beam current height. The beam current height adjustment includes determining a target beam current density value within the density allowable range, determining a target beam current height value based on the beam current value, beam width, and target beam current density value of the ion beam, and adjusting the beam current height of the ion beam according to the target beam current height value. For multiple silicon-on-insulator substrates formed from multiple silicon wafers processed by the same continuous ion implantation, the thickness uniformity of the silicon layers between the multiple silicon-on-insulator substrates can be less than 0.8 nm, the surface roughness uniformity between the release surfaces can be less than 1 nm, and the release surface is the side of the silicon layer that faces away from the insulating layer.

[0008] The beam current density of an ion beam is determined by both the beam current value and the cross-sectional area of ​​the ion beam. After the beam current value meets a preset condition, the beam current density is further constrained using a density tolerance range. When the beam current density deviates from the tolerance range, adjusting the beam height to change the cross-sectional area of ​​the ion beam can reduce the difference in ion flux per unit area caused by different beam current tunings, thereby reducing batch-to-batch variations in ion implantation damage distribution. For the fabrication of silicon-on-insulator substrates, improved consistency in ion implantation damage states reduces the differences in subsequent cleavage positions and states, thus improving the consistency of silicon layer thickness across different batches and enhancing the surface condition of the silicon layer on the side facing away from the insulating layer. Attached Figure Description

[0009] Figure 1 A schematic flowchart of an ion implantation method provided in some embodiments of this application is shown.

[0010] Figure 2 The diagram shows a cross-section and beam current parameters of a ribbon ion beam in some embodiments of this application.

[0011] Figure 3 The flowcharts for beam tuning and release determination in some embodiments of this application are shown.

[0012] Figure 4 A flowchart illustrating a method for determining the allowable density range in some embodiments of this application is shown.

[0013] Figure 5 A schematic flowchart of a method for fabricating a silicon-on-insulator substrate according to some embodiments of this application is shown.

[0014] Figure 6 A schematic diagram of the structure of a silicon-on-insulator substrate provided in some embodiments of this application is shown.

[0015] Figure 7A The changes in thermal wave measurements in the comparative example are shown.

[0016] Figure 7B The variation of thermal wave measurements in the embodiment is shown.

[0017] Figure 8A The changes in beam current values ​​in the comparative example are shown.

[0018] Figure 8B The variation of the beam current value in the embodiment is shown.

[0019] Figure 9A The variation in beam height in the comparative example is shown.

[0020] Figure 9B The variation of beam height in the embodiment is shown.

[0021] Figure 10A The variation in beam density in the comparative example is shown.

[0022] Figure 10B The variation of beam current density in the embodiments is shown. Detailed Implementation

[0023] The technical solutions in this application will now be clearly and completely described with reference to the accompanying drawings.

[0024] Silicon-on-insulator (SiS) substrates can be fabricated using a layer transfer process. In one layer transfer process, hydrogen ion implantation is first performed on a silicon wafer to form an ion-implanted damage layer at a predetermined depth. Subsequently, the hydrogen-implanted silicon wafer is bonded to a support substrate, and heat treatment causes the silicon wafer to cleave along the ion-implanted damage layer, transferring a portion of the silicon wafer to the support substrate side. The state of the ion-implanted damage layer not only affects whether the silicon wafer can cleave along the predetermined region but also influences the cleavage location and the thickness of the transferred silicon layer.

[0025] Thermometry can be used to evaluate the damage state after ion implantation. Thermometry utilizes laser-excited thermal waves on the wafer surface and obtains measurement values ​​based on the reflection or scattering of these waves. The thermometry values ​​are related to the damage depth, implantation dose, and damage distribution caused by ion implantation, and therefore can be used to characterize the ion implantation damage state. For batch-processed wafers, thermometry values ​​from different batches can also be compared to evaluate the consistency of ion implantation damage states across batches.

[0026] Thermometry results can be used to evaluate the uniformity of ion implantation damage and the consistency between different batches. When batches corresponding to different beam current tunings show different values ​​in the thermometry results, it can manifest as stratification or step-like phenomena.

[0027] Thermal wave measurement plays two main roles in this application. Firstly, batches with historically satisfactory thermal wave measurement results can serve as reference batches to establish the allowable beam current density range. Secondly, the thermal wave measurement results in the comparative examples and embodiments can be used to observe the differences in ion implantation damage states corresponding to different beam current control methods. Thermal wave measurement can serve as a detection method for evaluating ion implantation damage states. The ion implantation process can also be performed without thermal wave measurement.

[0028] Compared to conventional ion implantation for doping purposes, in the Smart Cut™ layer transfer process, hydrogen ion implantation is used to form an ion-implanted damage layer at a predetermined depth in the silicon wafer for subsequent dicing. While conventional doping ion implantation typically involves processes such as annealing to adjust the doping and lattice states, in the Smart Cut™ layer transfer process, the ion-implanted damage layer directly participates in subsequent dicing and layer transfer. Therefore, differences in damage states formed during the ion implantation stage can continue to propagate along the state of the ion-implanted damage layer, the dicing location, and the state of the transferred silicon layer.

[0029] The ion beam formed by a low-energy, high-current hydrogen ion implantation device can be ribbon-shaped. After beam tuning, the device can obtain beam parameters such as beam current value, beam height, and beam width. The beam current value represents the total beam current of the ion beam. During beam tuning, ion source parameters, magnet current, and electrical parameters affecting the beam cross-sectional dimensions can be adjusted to ensure that the beam state meets the requirements of the corresponding ion implantation process.

[0030] During batch ion implantation, beam current tuning can be performed separately before each batch begins ion implantation. Even if different beam current tunings achieve the same or similar beam current values, the beam current height of the ribbon ion beam may still differ. When the beam current width is usually kept relatively stable under the same equipment and wafer specifications, changes in beam current height will alter the cross-sectional area of ​​the ion beam, thereby causing variations in the beam current density formed by different beam current tunings.

[0031] Beam tuning can involve adjusting multiple equipment parameters. These parameters may include ion source parameters, magnet current, and focusing lens voltage. When the beam density does not meet the requirements and further fine-tuning of the beam height is needed, parameters affecting the beam cross-sectional dimensions, such as the focusing lens voltage and suppression electrode voltage, can also be adjusted. Different parameters may influence each other; therefore, re-measuring the actual beam parameters after each adjustment provides a more accurate evaluation of the adjusted ion beam state than relying solely on the adjustment instructions.

[0032] The goal of beam tuning is not to fix the beam height at the same value. For different beam tunings, as long as the combination of beam current and beam height ensures that the beam density falls within the allowable range of the current process, the beam density condition is met. Therefore, the beam current and beam height can change according to the current equipment condition, while the beam density is used to constrain the beam state per unit area.

[0033] Beam current density reflects the relationship between beam current value and ion beam cross-sectional area. When beam current density changes, the ion flux per unit area per unit time on the wafer surface also changes. Under the condition that the implanted ion type is the same and the implantation energy and target implantation dose meet the process settings, this change in ion flux per unit area will further affect the damage distribution within the ion implantation damage layer, and can be manifested by thermal wave measurements.

[0034] Under the same target implantation dose, changes in beam current density can alter the ion flux entering a unit area of ​​the wafer per unit time, and affect the formation and accumulation of implantation defects within the ion implantation damage layer. Higher beam current densities may increase the number of vacancy-interstitial atom pairs and other implantation defects formed per unit time, altering the damage accumulation state near the implantation layer. Differences in ion implantation damage distribution further influence the cleavage location and crack propagation state during subsequent wafer cleaving, and may be reflected in differences in the thickness and surface roughness of the transferred silicon layer.

[0035] At lower beam current densities, the implantation time required to reach the target implantation dose may be prolonged, and fluctuations in the beam state during a longer implantation process may also affect the consistency of ion implantation damage state. Therefore, for different implantation energies, target implantation doses, and other process conditions, a beam current density range matching the corresponding process conditions can be determined through Design of Experiments (DOE).

[0036] Therefore, controlling the total beam current within an acceptable range does not guarantee that ion beams formed by different beam tunings will have similar beam current states per unit area. For the same beam current value, when the beam height is different while the beam width is basically stable, the beam current density may still be different. Introducing beam current density into the judgment process before ion implantation can evaluate the ion beam state from the combination of beam current value and cross-sectional area.

[0037] When analyzing batch processing data, even if the beam current values ​​of different batches are all within the process allowable range, the thermal measurement results may still show batch-to-batch variations. Further comparison of the beam height and the beam density determined based on the beam current value, beam height, and beam width reveals a correlation between the batch-to-batch variations in thermal measurement values ​​and beam density, but not necessarily with the variations in the beam current value itself. Based on this correlation, beam density can be used as a further evaluation parameter after beam tuning and a release condition before ion implantation begins.

[0038] This application embodiment, based on the relationship between beam current value, beam current height, beam current width, and beam current density, acquires the beam current density of the ion beam before ion implantation begins and compares it with a preset density allowable range. If the beam current density does not fall within the density allowable range, the cross-sectional area of ​​the ion beam is changed by adjusting the beam current height to bring the beam current density into the density allowable range. The beam current height adjustment includes determining a target beam current density value within the density allowable range, determining a target beam current height value based on the ion beam current value, beam current width, and target beam current density value, and adjusting the beam current height of the ion beam according to the target beam current height value. After the beam current density meets the density allowable range, ion implantation of the wafer is then performed using the ion beam.

[0039] In the embodiment of silicon-on-insulator substrate fabrication, the silicon wafer can be a single-crystal silicon wafer. The ion implantation surface of the silicon wafer can be exposed or have an oxide layer. When the ion implantation surface has an oxide layer, the ion beam can be implanted into the silicon wafer through the oxide layer. Whether the ion implantation surface of the silicon wafer has an oxide layer or not does not change the control relationship based on beam current density to determine and adjust the beam current height.

[0040] The following description, with reference to the accompanying drawings, illustrates the ion implantation method, the relationship between beam parameters, the beam tuning and release determination process, the establishment of the density allowable range, and its application in the fabrication of silicon substrates on insulators. The detailed implementation methods are further explained at the end. Figure 7A , 7B 8A, 8B, 9A, 9B Figure 10A and 10B Comparative examples and implementation examples are set up to compare the beam current value, beam height, beam density, and thermal wave measurement results.

[0041] See Figure 1 This application provides an ion implantation method. The ion implantation method may include steps S110 to S150. Figure 1 This is used to illustrate the control relationship between beam tuning, beam density acquisition, beam density determination, beam height adjustment, and ion implantation.

[0042] Step S110 involves tuning the ion beam used for ion implantation of the wafer to ensure that the beam current meets a preset beam current condition. The beam current condition can be a target value condition or an allowable range condition corresponding to the relevant process formulation. Figure 1 This illustrates the beam tuning and beam density control process after the beam current value meets the conditions. For details on the beam tuning and release determination process, please refer to [link to relevant documentation]. Figure 3 .

[0043] Step S120: Obtain the beam current density of the ion beam used for ion implantation of the wafer.

[0044] For example, the beam current density can be obtained after the ion beam current value meets the beam current value condition and before the current batch of wafers begins ion implantation. The beam current density can be determined by the ion implantation equipment based on the beam current parameters obtained after beam tuning, or it can be determined by a calculation unit that interacts with the ion implantation equipment based on the beam current value, beam height, and beam width.

[0045] Step S130: Determine whether the beam density obtained in step S120 falls within a preset density allowable range. The density allowable range has a lower density limit and an upper density limit. When the beam density is greater than or equal to the lower density limit and less than or equal to the upper density limit, it can be considered that the beam density falls within the density allowable range. When the beam density is lower than the lower density limit or higher than the upper density limit, it can be considered that the beam density does not fall within the density allowable range.

[0046] If the beam current density falls within the allowable density range, step S150 can be executed. If the beam current density does not fall within the allowable density range, step S140 can be executed. Therefore, after beam tuning is completed, if the beam current density has fallen within the allowable density range, beam height adjustment does not need to be performed. If the beam current density obtained after beam tuning already meets the allowable density range, ion implantation can be performed directly.

[0047] Step S140: Adjust the beam height of the ion beam to change the beam density within the allowable density range. When the beam density is below the lower limit, the beam height can be reduced to decrease the cross-sectional area of ​​the ion beam and increase the beam density; when the beam density is above the upper limit, the beam height can be increased to increase the cross-sectional area of ​​the ion beam and decrease the beam density.

[0048] After completing one beam height adjustment, steps S120 and S130 can be repeated, i.e., the adjusted beam density can be reacquired, and it can be determined whether the reacquired beam density falls within the allowable density range. If the reacquired beam density still does not fall within the allowable density range, the beam height can be adjusted again. By repeatedly acquiring, judging, and adjusting, the beam density can be gradually brought closer to and into the allowable density range.

[0049] In step S150, if the beam current density falls within the allowable density range, ion implantation is performed on the wafer using an ion beam. Therefore, the actual ion beam entering the implantation process is simultaneously constrained by both the beam current value and the allowable density range, rather than solely relying on whether the beam current value meets the set conditions to determine whether ion implantation should begin.

[0050] For different batches, the production process involves separate beam tuning. Figure 1 The control relationships shown can be executed separately before each batch of ion implantation begins. Even if different batches have different beam current heights after beam tuning, controlling the beam current density according to the same allowable density range, or according to the allowable density range corresponding to each process condition, can reduce the difference in ion beam state per unit area between different batches.

[0051] The beam height adjustment and beam density reassessment can be performed automatically by the ion implantation equipment. If automatic adjustment fails to bring the beam density into the allowable range, an anomaly handling procedure can be initiated. Anomaly handling is used to prevent batches with beam densities consistently below the allowable range from directly undergoing ion implantation, and to ensure that the equipment status can be addressed during subsequent manual tuning or maintenance.

[0052] See Figure 2 The ion beam can be a strip ion beam 200. The cross-section of the strip ion beam 200 has a beam current width W along a first direction and a beam current height H along a second direction different from the first direction. The beam current width W can be greater than the beam current height H, making the cross-section of the ion beam appear as a strip extending in one direction. The beam current value of the strip ion beam 200 is denoted as I.

[0053] For a ribbon ion beam 200, the beam current density D can be determined based on the beam current value I, the beam current height H, and the beam current width W. In one specific implementation, the beam current density D satisfies: D = I / (H × W) In the formula, H×W represents the cross-sectional area of ​​the ribbon ion beam 200. The beam current density D is determined by both the beam current value and the cross-sectional area. Therefore, even with the same or similar beam current values, changes in beam height will still cause changes in beam current density.

[0054] For the same equipment and the same wafer specification, the beam width W can be determined by the corresponding beam current setting of the equipment and remains relatively stable between different beam current tunings. In a specific equipment setting, when performing ion implantation on a wafer with a diameter of 300 mm, the beam width W is 300 mm; when performing ion implantation on a wafer with a diameter of 200 mm, the beam width W is 200 mm. The beam width values ​​of 300 mm and 200 mm are used to illustrate the calculation of beam current density under specific equipment conditions. Different equipment can use different beam width setting methods.

[0055] When the beam current value I and beam width W are in the corresponding process conditions, decreasing the beam current height H can decrease the cross-sectional area of ​​the ion beam, thus increasing the beam current density D; conversely, increasing the beam current height H can increase the cross-sectional area of ​​the ion beam, thus decreasing the beam current density D. Therefore, the beam current height can be used as an adjustment factor for the beam current density.

[0056] When the current beam density is below the lower limit, it needs to be increased, which can be achieved by adjusting the beam height in the direction of decreasing the beam density. When the current beam density is above the upper limit, it needs to be decreased, which can be achieved by adjusting the beam height in the direction of increasing the beam density. Therefore, both situations of low and high beam density can be corrected by adjusting the beam height in opposite directions.

[0057] If the beam density is not within the allowable density range, a target beam density value within the allowable range can be determined first, and then a target beam height value can be determined based on the current beam value, beam width, and target beam density value. The target beam density value D0 can be any target value within the allowable density range. When the current beam value is I0, the target beam height value H0 can satisfy: The target beam density value does not necessarily have to be randomly selected within the allowable density range. The target beam density value can be determined based on the beam densities of multiple reference batches used when establishing the allowable density range. For example, when determining the allowable density range using the average and standard deviation of the beam densities from multiple reference batches, the average beam density of these batches can be used as the target beam density value. In other implementations, the target beam density value can also be preset within the allowable density range based on the control strategy of the corresponding process formulation.

[0058] H0 = I0 / (D0 × W) Adjusting the ion beam according to the target beam height value H0 can cause the beam height to change towards the value corresponding to the target beam density value D0. After adjustment, the beam current value and beam height can be remeasured, and the beam density can be recalculated to confirm whether the actual beam density has fallen within the allowable density range.

[0059] The completion of a beam height adjustment as described in this application refers to the ion implantation equipment performing an adjustment action on the beam height. It does not require the actual adjusted beam height to be exactly equal to the calculated target beam height value. After completing an adjustment action, the actual beam value and actual beam height are reacquired, and the beam density is re-determined. If the re-determined beam density falls within the allowable density range, the current beam state is considered to meet the ion implantation conditions; if the re-determined beam density still does not fall within the allowable density range, the next beam height adjustment can be performed.

[0060] The beam current height can be changed by adjusting beam tuning parameters that affect the cross-sectional dimensions of the ion beam. For example, at least one of the focusing lens voltage and the suppression electrode voltage can be adjusted.

[0061] During beam height adjustment, the beam current value may change due to variations in equipment status or tuning parameters. Therefore, the target beam height value can be calculated using the beam current value obtained in the current measurement, and the beam current value and beam height can be reacquired after adjustment. After reacquiring the beam current value and beam height, the beam density can be re-evaluated using the actual beam current parameters, without requiring the beam current value to remain strictly constant throughout the adjustment process.

[0062] When the corresponding process allows, the beam current value can be kept within a preset allowable range, and the beam height can be adjusted within this range. The allowable beam current value range is used to limit the overall beam current state, and the allowable density range is used to limit the beam current state per unit area formed by the combination of beam current value and cross-sectional area. Both can be used together as judgment conditions after beam tuning.

[0063] The beam current, beam height, and beam width can be obtained using existing measurable parameters of the ion implantation equipment. Therefore, when determining the beam density based on the beam current I, beam height H, and beam width W, calculations can be performed based on existing beam parameters from the beam tuning process, without requiring additional beam profile measurement equipment to obtain the beam density. Compared to measuring local distributions at multiple locations on the cross-section, establishing the beam density using I, H, and W reduces the reliance on additional beam profile measurement hardware.

[0064] See Figure 3 In one specific implementation method, the beam current value condition and the beam current density condition can be combined into the same beam tuning and release determination process. Figure 3 The flowchart shown is for further explanation. Figure 1 Lower-level implementation of beam density determination and beam height adjustment.

[0065] Step S310: Perform beam current tuning to bring the ion beam current value into a preset allowable range. Beam current tuning can be performed by adjusting ion source parameters, magnet current, and beam shaping-related electrical parameters. After the beam current value reaches the corresponding process-allowed state, ion implantation does not begin directly; instead, the beam current density is evaluated further.

[0066] Step S320: Obtain the current beam current value and beam height of the current ion beam, and determine the current beam density based on the current beam current value, beam height, and beam width. Since the beam current value may change when the beam shaping parameters are changed, after the beam height adjustment is completed, the actual beam current value and beam height can be obtained again, and the beam density can be re-determined.

[0067] Step S330: Determine whether the current beam current density falls within the allowable density range. If the current beam current density falls within the allowable density range, step S380 can be executed to perform ion implantation on the wafer; if the current beam current density does not fall within the allowable density range, proceed to the beam height adjustment and anomaly handling process.

[0068] Step S340: Determine whether the current number of automatic adjustments has reached the preset upper limit. If the number of adjustments has not reached the upper limit, proceed to step S350. Step S350: Adjust the beam height according to the position of the current beam density relative to the allowable density range. The beam height can be decreased when the beam density is too low and increased when the beam density is too high. Specifically, a target beam density value within the allowable density range can be determined. A target beam height value is determined based on the current beam value, beam width, and target beam density value. The beam height is then adjusted according to the target beam height value by changing at least one of the focusing lens voltage and the suppression electrode voltage.

[0069] After step S350 is completed, return to step S320 to remeasure the beam parameters and determine the beam density, so that the beam height can be corrected by combining the actual beam state of the adjusted equipment.

[0070] When step S340 determines that the number of adjustment attempts has reached the upper limit and the beam density has not yet fallen within the allowable density range, step S360 can be executed.

[0071] Step S360: Output an alarm and switch to manual beam optimization. Manual beam optimization allows for readjustment of ion source parameters, magnet current, and electrical parameters affecting beam height.

[0072] Step S370: Determine whether the manually tuned beam density falls within the allowable density range. If the manually tuned beam density falls within the allowable density range, proceed to step S380; if the manually tuned beam density still does not fall within the allowable density range, proceed to step S390.

[0073] Step S380: Ion implantation is performed on the wafer using an ion beam.

[0074] Step S390: Stop the current batch of ion implantation and perform equipment maintenance.

[0075] In one specific example, the maximum number of automatic retry cycles can be set to 10. This 10-cycle limit illustrates that the automatic recovery process can have a limited number of retries. The actual maximum number can be set according to the device tuning strategy. Limited retries, alarms, and implantation stoppages prevent batches with beam densities consistently below the allowable density range from entering the ion implantation process.

[0076] See Figure 4The allowable density range can be determined based on multiple reference batches where the ion implantation damage state has historically met the requirements. The allowable density range is used to provide a quantitative judgment boundary for beam current density, so that subsequent beam current tuning can be judged according to the same statistical benchmark, or according to the statistical benchmark corresponding to each process condition, to determine whether the beam current density meets the ion implantation conditions.

[0077] Step S410: Determine multiple reference batches. Reference batches can be selected from batches that have undergone ion implantation and have corresponding beam tuning data and thermal measurement results. The thermal measurement results corresponding to the reference batches meet preset requirements. For example, batches whose thermal measurement results meet the homogeneity requirements and do not exhibit batch-to-batch stratification can be selected as reference batches.

[0078] Step S420: Obtain beam parameters corresponding to multiple reference batches. For each reference batch, the beam current value, beam height, and beam width after beam tuning can be obtained, and the reference beam current density of each reference batch can be obtained according to D=I / (H×W). Multiple reference batches thus form a set of beam current density data corresponding to the required ion implantation damage state.

[0079] Step S430 involves statistically analyzing the beam densities corresponding to multiple reference batches. This statistical analysis reveals the concentration and dispersion of the beam densities across the multiple reference batches. Specifically, the average and standard deviation of the beam densities for the multiple reference batches can be calculated.

[0080] Step S440: Determine the allowable density range based on statistical results. In one specific implementation, the lower density limit can be obtained by subtracting three times the standard deviation from the average beam current density of multiple reference batches, and the upper density limit can be obtained by adding three times the standard deviation to the average. Subsequent batches can proceed to the subsequent ion implantation process when their beam current density falls between the lower and upper density limits.

[0081] The allowable density range can be determined based on the statistical results of a reference batch. For example, in one instance, the allowable density range could be 8.5 × 10⁻⁶. -4 mA / mm² up to 9.5 × 10 -4 mA / mm². In the specific tests described later, the permissible density range was 9.5 × 10⁻⁶. -4 mA / mm² to 10.5 × 10 -4 mA / mm².

[0082] In addition to the examples above, the target injection dose is 6.0 × 10¹ 6 In the case of ions / cm², different injection energies can correspond to different allowable ranges of beam current and density. Several exemplary process formulations are given below for different injection energies.

[0083] Table 1 Examples of beam parameters for different injection energies

[0084] As shown in the table examples, with the same target injection dose, different injection energies correspond to different allowable beam current and density ranges. Specifically, when the target injection dose is 6.0 × 10¹ 6 When the beam current is measured in ions / cm², the allowable ranges for both beam current and density can be set separately as the injection energy varies. For different process formulations, the corresponding allowable density range can be determined based on the statistical results of relevant reference batches.

[0085] A reference batch is used to determine the allowable density range, establishing a link between the allowable density range and the beam state of the reference batch whose thermal wave measurement results meet preset requirements. Subsequent batches no longer judge whether the beam tuning meets the requirements based on the total beam current value, but rather compare the actual beam current density with the upper and lower limits formed based on the reference data.

[0086] The number of reference batches can be determined based on existing production data. In one specific embodiment, the beam current density data corresponding to the first 25 wafers can be used as a benchmark for establishing the density tolerance range. The sample size corresponding to 25 wafers is used as an example to illustrate how existing batch data can be used to form the density tolerance range.

[0087] The mean and standard deviation provide a specific statistical representation of the allowable density range. When using the mean ± 3σ, the allowable density range takes into account both the center location and the dispersion of the reference beam density.

[0088] The allowable density range has upper and lower limits, which can simultaneously constrain both excessively high and excessively low beam densities. When the beam density is too high, it can be reduced by increasing the beam height; when the beam density is too low, it can be increased by decreasing the beam height. Thus, a corresponding relationship can be formed between the allowable density range and the two-way adjustment of the beam height.

[0089] The density allowable range can also provide a unified quantitative judgment condition for different operators or different automatic tunings. By using the same statistical rules and density boundaries, the differences in beam state judgment caused by different operating experiences can be reduced, and the consistency and repeatability of beam tuning results from different times can be improved.

[0090] Beam tuning involves first bringing the beam current to the target state set by the corresponding process, and then calculating the beam current density based on the measured beam current value and beam height. When the beam current density falls within the allowable density range, ion implantation of that batch of wafers can begin; if the beam current density does not fall within the allowable density range, the parameters affecting the beam height can be adjusted further.

[0091] If the beam density is outside the allowable range, first determine the target beam density value D0 within the allowable range. Then, calculate the target beam height value H0 based on the current beam value I0, beam width W, and the target beam density value D0, and adjust the beam height towards the target value. Adjusting based on the target beam height provides a quantitative target for beam height adjustment. After adjustment, recalculate the beam density based on the actual measured beam value and beam height.

[0092] The number of repetitions can be recorded. If the number of repetitions has not reached the preset upper limit, beam height adjustment and beam density determination can continue. If the repetition limit is reached but the beam density still falls below the allowable range, the automatic repetition process can be stopped and an alarm message output.

[0093] In one specific example, the maximum number of automatic retry attempts can be set to 10. The 10 attempts dictate that exception handling can be configured with a limited number of retries. Different ion implantation devices can have their own maximum number of retries set according to their device tuning strategies and process control methods.

[0094] After an alarm is issued, manual beam optimization can be performed. Manual beam optimization involves readjusting ion source parameters, magnet current, and electrical parameters affecting beam height to attempt to bring the beam density within the allowable range. If the beam density still does not fall within the allowable range after manual tuning, ion implantation for the current batch can be stopped, and the equipment can be maintained.

[0095] By setting a limited number of retries, alarms, and implantation stop mechanisms, batches with beam current densities consistently below the allowable range can be prevented from directly undergoing ion implantation. This also prevents the automatic recovery process from repeatedly consuming excessive equipment time. The handling of anomalies related to limited retries, alarms, and implantation stop mechanisms can be integrated with… Figure 1 The beam density control process shown is used in conjunction with this.

[0096] The beam current density is determined by both the beam current value and the cross-sectional area of ​​the ion beam. When the beam heights formed by different beam tunings differ, the beam current densities may still differ even if the beam current values ​​meet the same or similar conditions. Figure 1 The method shown compares the beam density with the allowable density range before ion implantation begins, and adjusts the beam height based on the comparison results, so that the beam density during actual ion implantation is constrained by the quantization range.

[0097] By constraining the beam current density of different batches to the same allowable range, or to the allowable range corresponding to each process condition, the difference in ion flux per unit area per unit time on the wafer surface of different batches can be reduced. When the difference in ion flux per unit area is reduced, the batch-to-batch difference in damage distribution within the ion implantation damage layer can also be reduced. Thermometry measurements, as a characterization of the ion implantation damage state, can also show small batch-to-batch differences.

[0098] This application uses existing beam parameters such as beam current value, beam height, and beam width to determine beam density, thus establishing quantitative judgment conditions for beam density without adding a dedicated beam profile measurement device. The allowable density range also provides a consistent evaluation benchmark for different beam tuning operations, resulting in better repeatability of beam tuning results.

[0099] The control relationship of adjusting the beam height based on the beam current density before ion implantation can also be used to prepare silicon substrates on insulators. The ion beam used to form an ion-implanted damaged layer within a silicon wafer can be determined according to the corresponding layer transfer process; the following description uses a hydrogen ion beam as a specific implementation. The ion implantation damage state affects the subsequent wafer dicing quality and the thickness of the transferred silicon layer. The following... Figure 5 and Figure 6 This section describes the application of this ion implantation method in the fabrication of silicon-on-insulator substrates and related products. Comparative examples and embodiments with specific process parameters are provided at the end of the detailed implementation instructions.

[0100] See Figure 5 This application also provides a method for fabricating a silicon-on-insulator substrate. This fabrication method may include steps S510 to S550. Figure 5 This is used to illustrate the relationship between hydrogen ion implantation constrained by beam current density and subsequent layer transfer processes.

[0101] In step S510, using Figures 1 to 3 The ion implantation method shown utilizes a hydrogen ion beam to implant hydrogen ions into a silicon wafer. First, the hydrogen ion beam is tuned to meet a preset current value condition; then, the current density of the hydrogen ion beam is obtained. If the current density is not within the allowable range, the beam height is adjusted to bring it within the allowable range. Beam height adjustment includes determining a target current density value within the allowable range, determining a target beam height value based on the current value, beam width, and target current density value, and adjusting the beam height accordingly. After the current density falls within the allowable range, hydrogen ion implantation is performed on the silicon wafer.

[0102] Hydrogen ion implantation can be performed using a low-energy, high-current ribbon ion beam. The energy and dose of hydrogen ion implantation can be set according to the target transfer layer thickness and process conditions corresponding to the silicon substrate on the insulator. The beam current density during actual hydrogen ion implantation is constrained by the allowable density range.

[0103] In step S520, an ion-implanted damage layer is formed at a predetermined depth on the silicon wafer by hydrogen ion implantation. A portion of silicon material to be transferred is formed between the ion-implanted damage layer and one surface of the silicon wafer. The ion implantation energy is related to the depth of the damage layer, and the state of the ion-implanted damage layer is also related to the damage distribution during the implantation process.

[0104] In step S530, the silicon wafer is bonded to the support substrate to form a bonding structure. At least one of the silicon wafer and the support substrate has an insulating layer on its bonding surface. After bonding, the insulating layer is located between the silicon wafer and the support substrate. The specific bonding method can be selected based on the fabrication process of the silicon-on-insulator substrate.

[0105] In step S540, the bonding structure is heat-treated to allow the silicon wafer to cleave along the ion-implanted damage layer. The damage region formed by hydrogen ion implantation participates in the cleaving process during heat treatment, and the damage distribution within the ion-implanted damage layer affects the cleaving state and location at different positions on the silicon wafer.

[0106] After the silicon wafer is cracked along the ion implantation damage layer, a portion of the silicon wafer is transferred to the support substrate side and forms a silicon layer. The remaining silicon material separates from the transferred silicon layer. Step S550: Forming a silicon-on-insulator substrate.

[0107] When fabricating silicon-on-insulator substrates in different batches, if the hydrogen ion beams formed by different beam tunings have significant differences in beam current density, the damage state of the ion implantation damage layer may also differ. By controlling the beam current density before hydrogen ion implantation begins, ensuring that the actual beam current density during hydrogen ion implantation falls within the allowable range, the differences in ion implantation damage states between different batches can be reduced.

[0108] When the differences in ion implantation damage state are reduced, the differences in cleavage position and crack propagation state formed during subsequent heat treatment and cleaving processes can be reduced. This is beneficial for improving the thickness uniformity of the transferred silicon layer and reducing the surface roughness of the silicon layer on the side away from the insulating layer. The effect of controlling beam current density on improving silicon layer thickness and surface condition stems from the influence of beam current density on ion implantation damage state and subsequent cleaving process. The comparative examples and embodiments below compare thermal wave measurements, beam current values, beam current height, and beam current density, and evaluate the product condition in conjunction with the thickness uniformity between silicon layers on the silicon substrate over the insulator and the surface roughness uniformity between the peeled surfaces.

[0109] For monolithic silicon-on-insulator (SiS) substrates, the state of the ion-implanted damaged layer at different locations on the wafer affects the cleaving process at those locations. When the difference in cleaving location within the wafer plane is small, the thickness difference of the transferred silicon layer at different locations can be reduced. Therefore, the uniformity of the silicon layer thickness within the wafer is a performance aspect that the ion implantation control method of this application may reflect in the final SiS product.

[0110] For multiple silicon-on-insulator (SiS) substrates formed from multiple silicon wafers processed in the same continuous ion implantation, the silicon layer thicknesses of the multiple SiS substrates can be compared to evaluate the inter-wafer thickness uniformity. Inter-wafer thickness uniformity can be characterized by the inter-wafer thickness range, which is the difference between the maximum and minimum silicon layer thicknesses of the multiple SiS substrates. In one specific evaluation, 100 SiS substrates formed from 100 silicon wafers processed in the same continuous ion implantation can be selected for evaluation. The inter-wafer thickness range is used to characterize the consistency of silicon layer thickness among the multiple SiS substrates; the smaller the inter-wafer thickness range, the better the inter-wafer thickness uniformity.

[0111] The target silicon layer thickness on a silicon-on-insulator substrate can be determined according to product design requirements; this application does not limit the target silicon layer thickness. For silicon-on-insulator substrates with different target thicknesses, the beam current density control relationship before ion implantation can be used as a beam current state control method during the hydrogen ion implantation stage.

[0112] See Figure 6 This application also provides a silicon-on-insulator substrate 650. The silicon-on-insulator substrate 650 includes a supporting substrate 620, an insulating layer 630 located on one side of the supporting substrate 620, and a silicon layer 640 located on the side of the insulating layer 630 facing away from the supporting substrate 620. The silicon layer 640 can be... Figure 5 The fabrication method shown involves transferring a portion of a silicon wafer.

[0113] The silicon layer 640 has a corresponding thickness at different locations on the silicon substrate 650 over the insulator. Figure 6 T1, T2, and T3 represent the silicon layer thickness at different locations. The dispersion of silicon layer thickness at different locations can be used to evaluate the uniformity of silicon layer thickness on a silicon substrate 650 on the same insulator. Specific products can determine the thickness measurement locations and thickness uniformity evaluation methods according to product specifications.

[0114] The target silicon layer thickness for the silicon-on-insulator substrate 650 can be determined according to product specifications. The beam current density control relationship before ion implantation can be used for hydrogen ion implantation processes corresponding to different target silicon layer thicknesses.

[0115] The silicon layer 640 is formed by splitting and transferring silicon wafers along the ion-implanted damage layer. The ion-implanted damage layer is formed by hydrogen ion implantation into the silicon wafer using a hydrogen ion beam. The beam current value of the hydrogen ion beam used to form the ion-implanted damage layer meets a preset beam current value condition, and the beam current density of the hydrogen ion beam falls within a preset density allowable range. If the beam current density does not fall within the density allowable range, the beam current height of the hydrogen ion beam is adjusted to bring the beam current density into the density allowable range before hydrogen ion implantation is performed. The beam current height adjustment includes determining a target beam current density value within the density allowable range, determining a target beam current height value based on the hydrogen ion beam current value, beam width, and target beam current density value, and adjusting the beam current height of the hydrogen ion beam according to the target beam current height value.

[0116] Therefore, silicon-on-insulator substrate 650 and Figure 1 The ion implantation control relationship shown is as follows: Figure 5 The fabrication process shown forms a technical connection. The intra-wafer thickness uniformity of silicon layer 640 can be used as one of the parameters for evaluating the silicon layer formation state; the thickness measurement location and evaluation method can be determined according to product specifications.

[0117] In addition to the uniformity of silicon layer thickness of a single silicon-on-insulator (SiS) substrate 650, the silicon layer thickness of 100 SiS substrates 650 from the same production batch can also be compared to evaluate the consistency of silicon layer thickness among different SiS substrates 650. In some embodiments, the inter-wafer thickness difference of the silicon layer of the 100 SiS substrates 650 can be less than 0.8 nm. The side of the silicon layer 640 facing away from the insulating layer 630 is the release surface 642. In some embodiments, the inter-wafer surface roughness difference of the release surfaces of the 100 SiS substrates 650 can be less than 1 nm. For multiple SiS substrates 650 formed from multiple silicon wafers in the same continuous ion implantation process, the surface roughness of the release surface 642 of each SiS substrate 650 can be measured separately. The uniformity of surface roughness between release surfaces can be characterized by the inter-wafer surface roughness difference, which is the difference between the maximum and minimum surface roughness values ​​of the multiple release surfaces 642. The smaller the surface roughness difference between the release surfaces, the better the uniformity of surface roughness among multiple silicon-on-insulator substrates. In one specific evaluation, 100 silicon-on-insulator substrates 650 can be selected, and the surface roughness Ra of each release surface 642 can be measured using an atomic force microscope (AFM), with a test area of ​​10 μm × 10 μm.

[0118] In one product evaluation, 100 silicon-on-insulator (SiI) substrates 650, each formed from 100 silicon wafers processed in the same continuous ion implantation, are evaluated. The inter-wafer thickness range of the silicon layers is determined by the difference between the maximum and minimum silicon layer thicknesses; in this embodiment, the inter-wafer thickness range is 0.67 nm. Following the aforementioned surface evaluation parameters and test conditions, the surface roughness Ra of the release surface 642 is measured using AFM, and the inter-wafer surface roughness range of the release surface is determined by the difference between the maximum and minimum values; in this embodiment, the inter-wafer surface roughness range of the release surface is 0.87 nm.

[0119] In contrast, during the fabrication process where beam current value was primarily used as the beam current tuning and release condition, the thickness difference between silicon layers on the silicon substrate on the insulator varied from 2 nm to 4 nm across different production batches. In this comparative example, the thickness difference between silicon layers was 3.7 nm, measured at 49 points using an ellipsometer. Following the same surface evaluation parameters and testing conditions as the examples, AFM (atomic force microscopy) was used for testing. The surface roughness difference between the peeled surfaces in the comparative example ranged from 1.5 nm to 3 nm, while in this comparative example, it was 1.7 nm. The product evaluation results and the thermal wave measurement results before and after beam current density control corroborate each other, further illustrating the correlation between beam current density control and the stability of the layer-transfer product.

[0120] Comparative Examples and Implementation Examples The following comparative examples and embodiments are placed at the end of the detailed implementation to compare beam current, beam height, beam density, and thermal wave measurement results under the same wafer type, implantation energy, and target implantation dose conditions. The comparative examples illustrate parameter changes when beam tuning is controlled primarily based on beam current, while the embodiments illustrate parameter changes when beam density is used as a release condition and beam height is adjusted according to the beam density state.

[0121] Comparative Example A low-energy, high-current hydrogen ion implantation device was used to implant hydrogen ions into a 300mm diameter P-type single-crystal silicon wafer using a ribbon ion beam. The implantation energy was 42keV, and the target implantation dose was 6.0×10¹. 6 ions / cm². The target value of the beam current is set to 15mA, and it is controlled at 15±1mA during beam tuning. The beam height is not constrained, and the beam density is not used as a release condition before ion implantation.

[0122] Multiple batches of hydrogen ion implantation were performed consecutively, with beam tuning re-tuned before each batch began implantation. After ion implantation was completed, thermal measurements were performed on each wafer, and the corresponding beam current value, beam height, and beam current density calculated based on the beam parameters were recorded.

[0123] See Figure 7A Different batches of thermal wave measurements resulted in different value levels, exhibiting a step-like variation between batches. See also Figure 8A Multiple batches showed beam current values ​​within the permissible range of 15 ± 1 mA, and their variations did not exhibit the same inter-batch steps as the thermal wave measurements. See [link to relevant documentation]. Figure 9A The beam height varies across different batches, exhibiting a trend opposite to that shown by thermal wave measurements. See also Figure 10A The beam current density also varies across different batches, exhibiting the same trend as the thermal wave measurements. Therefore, even with a narrow permissible range for the beam current value, different beam tunings can still produce different beam heights and densities, corresponding to different ion implantation damage states.

[0124] Example The embodiment uses the same low-energy, high-current hydrogen ion implantation equipment, the same 300mm P-type single-crystal silicon wafer, the same 42keV implantation energy, and 6.0×10¹ as the comparative example. 6 Target implantation dose per ions / cm². The difference is that this example uses beam current density as one of the release conditions before ion implantation begins. The permissible density range is set to 9.5 × 10⁻⁶. -4 mA / mm² to 10.5 × 10 -4 mA / mm², the allowable range of beam current is widened to 15±5mA, that is, from 10mA to 20mA.

[0125] Beam tuning was performed separately for each batch before hydrogen ion implantation. After beam tuning, the beam density was calculated based on the current beam current value, beam height, and beam width. The beam density did not fall within 9.5 × 10⁻⁶. -4 mA / mm² to 10.5 × 10 - 4 Continue adjusting the beam height when the beam density is within the mA / mm² range. Once the beam density enters the allowable density range, proceed with hydrogen ion implantation.

[0126] In one specific batch, the tuned beam current was 11.7 mA, and the beam height was 45.7 mm. With a beam width W of 300 mm, the beam density, calculated using D = I / (H × W), was approximately 8.53 × 10⁻⁶. -4 mA / mm², below the lower limit of density. By adjusting parameters such as the focusing lens voltage, the beam height was reduced from 45.7 mm to 39.4 mm, and the calculated beam density was approximately 9.9 × 10⁻⁶. -4 mA / mm², entering the density allowable range, followed by hydrogen ion implantation.

[0127] In another specific batch, the tuned beam current was 13.2 mA, the beam height was 40.8 mm, and the beam density, calculated using the same relationships, was approximately 10.8 × 10⁻⁶. -4 mA / mm², exceeding the upper limit of density. By adjusting the parameters affecting beam height, the beam height was increased from 40.8 mm to 43.5 mm, and the calculated beam density was approximately 10.1 × 10⁻⁶. -4 mA / mm², entering the density allowable range, followed by hydrogen ion implantation.

[0128] The specific batches with low beam density and the specific batches with high beam density demonstrate beam height adjustments in opposite directions. When the beam density is low, the beam height is decreased; when the beam density is high, the beam height is increased. These two adjustment directions are used to bring the beam density into the same allowable range. Therefore, this embodiment does not fix the beam height to a certain absolute value, but rather determines the adjustment direction and target state of the beam height by combining the current beam value and the target beam density value.

[0129] See Figure 7B In the examples, the thermal wave measurements from different batches no longer exhibited the batch-to-batch step changes seen in the comparative example. See also Figure 8B The beam current values ​​in the embodiments can vary over a wider range compared to the comparative examples. See also Figure 9B The beam height can still vary between different batches. See also Figure 10B In practice, the beam density during ion implantation is constrained to a relatively concentrated range.

[0130] The comparative example maintains the same main process conditions as the embodiment, but the release conditions after beam tuning differ. The comparative example controls the beam current value within a narrow range of 15±1mA, but batch-to-batch variations still occur in beam height and beam density; the embodiment expands the allowable beam current value range to 10mA to 20mA, while constraining the beam density to 9.5×10⁻⁶. -4 mA / mm² to 10.5 × 10 -4 mA / mm², and adjusts the beam height when the beam density does not meet the requirements. Therefore, the embodiment does not improve the thermal wave measurement results by further tightening the total beam current value, but rather by adjusting the beam height to constrain the beam state per unit area within the allowable density range.

[0131] The results from the comparative examples and embodiments show that using beam current density as a quantitative judgment condition before ion implantation, and adjusting the beam height according to the beam current density relative to the allowable density range, can reduce the beam current density differences corresponding to different beam tunings and reduce the differences in thermal wave measurement values ​​between different batches of wafers. The comparison results of the comparative examples and embodiments correspond to the technical relationship between beam current density, ion flux per unit area, and ion implantation damage distribution.

[0132] In some embodiments, the silicon-on-insulator (SiI) substrate formed using the fabrication method provided in this application can be used as a substrate for subsequent device fabrication. Corresponding functional structures can be formed on or within the silicon layer to manufacture semiconductor devices, photonic devices, or other devices employing SiI structures. Improving the consistency of ion implantation damage states across different batches is beneficial for enhancing the stability of the subsequent SiI substrate fabrication process and device manufacturing process. This application does not limit the specific downstream device types of the SiI substrate.

Claims

1. An ion implantation method, characterized in that, include: The ion beam used for ion implantation of wafers is tuned so that the beam current value of the ion beam meets the preset beam current value conditions. If the beam current value of the ion beam meets the beam current value condition, the beam current density of the ion beam is obtained. If the beam current density does not fall within the preset allowable density range, the beam height of the ion beam is adjusted to bring the beam current density within the allowable density range; and If the beam current density falls within the allowable density range, the wafer is ion implanted using the ion beam. Wherein, the ion beam is a strip-shaped ion beam, and the beam current density of the ion beam is determined by the beam current value, beam current height, and beam current width of the ion beam. The beam current height adjustment includes: Determine the target beam density value within the allowable density range; The target value of beam height is determined based on the beam current value, beam width, and target value of beam current density of the ion beam; The beam height of the ion beam is adjusted according to the target beam height value.

2. The ion implantation method according to claim 1, characterized in that, The ion beam is a ribbon-shaped hydrogen ion beam.

3. The ion implantation method according to claim 1, characterized in that, The beam current density of the ion beam satisfies D = I / (H × W), where D is the beam current density, I is the beam current value, H is the beam current height, and W is the beam current width.

4. The ion implantation method according to claim 1, characterized in that, During the adjustment of the beam height, the beam value remains within a preset allowable range.

5. The ion implantation method according to claim 4, characterized in that, The allowable beam current range is 10 mA to 20 mA, and the allowable density range is 9.5 × 10⁻⁶. -4 mA / mm² to 10.5 × 10 -4 mA / mm².

6. The ion implantation method according to claim 1, characterized in that, The allowable density range is determined based on the beam current density corresponding to multiple reference batches; The reference batch refers to the batch whose thermal wave measurement results meet the preset requirements after ion implantation.

7. The ion implantation method according to claim 6, characterized in that, The allowable density range is determined based on the average and standard deviation of the beam current density corresponding to the multiple reference batches.

8. The ion implantation method according to claim 7, characterized in that, The lower limit of the allowable density range is the average value minus three times the standard deviation, and the upper limit of the allowable density range is the average value plus three times the standard deviation.

9. The ion implantation method according to claim 1, characterized in that, The beam height of the ion beam is adjusted by regulating at least one of the focusing lens voltage and the suppression electrode voltage.

10. The ion implantation method according to claim 1, characterized in that, After adjusting the beam height of the ion beam according to the target beam height value, the beam density of the ion beam is reacquired, and the beam height of the ion beam is adjusted again if the reacquired beam density does not fall within the allowable density range.

11. A method for preparing a silicon-on-insulator substrate, characterized in that, include: The ion beam used for ion implantation of silicon wafers is tuned so that the beam current value of the ion beam meets the preset beam current value conditions. If the beam current value of the ion beam meets the beam current value condition, the beam current density of the ion beam is obtained. If the beam current density does not fall within the preset density allowable range, the beam current height of the ion beam is adjusted so that the beam current density falls within the density allowable range; When the beam current density falls within the density allowable range, the silicon wafer is ion implanted using the ion beam to form an ion implantation damage layer within the silicon wafer. The silicon wafer is bonded to a support substrate, wherein at least one of the silicon wafer and the support substrate has an insulating layer on its bonding surface; and The silicon wafer is cleaved along the ion implantation damage layer, and a portion of the silicon wafer is transferred to one side of the support substrate to form a silicon layer, thereby forming a silicon-on-insulator substrate. Wherein, the ion beam is a strip-shaped ion beam, and the beam current density of the ion beam is determined by the beam current value, beam current height, and beam current width of the ion beam. The beam current height adjustment includes: Determine the target beam density value within the allowable density range; The target value of beam height is determined based on the beam current value, beam width, and target value of beam current density of the ion beam; The beam height of the ion beam is adjusted according to the target beam height value.

12. A silicon-on-insulator substrate, characterized in that, include: Support substrate; An insulating layer is disposed on the supporting substrate; as well as A silicon layer is disposed on the insulating layer and is located on both sides of the insulating layer with the supporting substrate; The silicon layer is formed from the portion of the silicon wafer that is transferred after being split along the ion implantation damage layer. The ion implantation damage layer is formed by ion implantation of the silicon wafer with an ion beam. The beam current value of the ion beam meets a preset beam current value condition. If the beam current density of the ion beam does not fall within a preset density allowable range, the beam current density of the ion beam is adjusted to the preset density allowable range by adjusting the beam current height of the ion beam. Wherein, for multiple silicon-on-insulator (SiS) substrates formed from multiple silicon wafers processed in the same continuous ion implantation, the inter-layer thickness uniformity of the silicon layers among the multiple SiS substrates is less than 0.8 nm, and the inter-layer thickness uniformity is the difference between the maximum and minimum silicon layer thicknesses of the multiple SiS substrates. The surface roughness uniformity between the release facets of the plurality of silicon-on-insulator substrates is less than 1 nm. The surface roughness uniformity between the release facets is the difference between the maximum and minimum surface roughness values ​​of the release facets of the plurality of silicon-on-insulator substrates. The release facet is the side of the silicon layer facing away from the insulating layer. Wherein, the ion beam is a strip-shaped ion beam, and the beam current density of the ion beam is determined by the beam current value, beam current height, and beam current width of the ion beam. The beam current height adjustment includes: Determine the target beam density value within the allowable density range; The target value of beam height is determined based on the beam current value, beam width, and target value of beam current density of the ion beam; The beam height of the ion beam is adjusted according to the target beam height value.

Citation Information

Patent Citations

  • Ion implantation device and adjustment method of beam current density distribution

    CN102237245A

  • Apparatus and techniques for controlling ion implantation uniformity

    CN105264634A