A method of harvesting rubber latex that preserves freshness
Patent Information
- Application Number
- CN202611037934.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-10-09
AI Technical Summary
[0005]2.目前生产上关于胶乳的采收运输方面尚无系统的标准,采收过程中的各因素对胶乳的保鲜均有一定的影响,如采收时间,胶乳保险条件以及胶乳运输温度
[0026]试验数据支撑与生产需求:以我国植胶区常用的割制四天一刀(d4)和六天一刀(d6)为基础,通过检测不同采收条件下胶乳的干胶含量、总固形物含量、非胶固形物含量以及 VFA 值等指标,对比农业行业标准(NY/T 4296),使胶乳达到我国特种胶生产需求。
Smart Images

Figure REF-OBJ-1783931051204-000001 
Figure REF-OBJ-1783931051204-000002 
Figure REF-OBJ-1783931051204-000003
Abstract
Description
Technical Field
[0001] This invention relates to the field of rubber tree latex preservation technology, and in particular to a harvesting method for maintaining the freshness of rubber tree latex through closed harvesting, field preservation, and low-temperature transportation. Background Technology
[0002] Natural rubber, as a globally important industrial raw material, has wide applications in defense, rail transportation, and medical and health fields. More than 99% of the world's natural rubber comes from rubber trees and is processed from the latex discharged after the latex cells of the rubber tree are cut. Its main component is polyisoprene, and it also contains a small amount of non-rubber components.
[0003] Hainan, Yunnan, and Guangdong are my country's three major rubber-growing regions, receiving abundant rainfall annually. Rubber tapping operations are easily affected by rainfall, leading to production losses. On one hand, rainwater entering the latex cups along the trunk and tapping lines dilutes the latex concentration, promotes microbial growth, and accelerates latex coagulation and spoilage. On the other hand, rainwater soaking the tapping surface and tapping lines makes normal tapping impossible or causes tapping surface ulceration. Current latex harvesting techniques in my country are extensive, with latex exposed to open environments for extended periods during harvesting. This makes it susceptible to contamination by insects, soil, sawdust, and other mechanical impurities, as well as bacteria and microorganisms. This results in high impurity content and high volatile fatty acid values in fresh latex, leading to significant quality fluctuations and a short shelf life in the initial production stage, severely impacting the quality and stability of natural rubber.
[0004] This method constructs a four-in-one technology chain of "waterproofing, time control, preservation, and temperature stability" to inhibit rainwater intrusion and biological contamination at the source, significantly improving the quality and stability of latex. It focuses on solving the following technical problems: 1. Currently, several rainproof devices have been developed and applied in the market, mainly falling into three categories: ① A combination of a rain cap and a rubber cup cover. This device fixes the rain cap to the tree trunk to block rainwater flowing down the trunk, while the rubber cup cover covers the rubber cup to prevent rainwater from entering; ② A combination of a rain cap and a rain curtain (or rain skirt). This solution adds a hanging rain curtain below the rain cap to cover the cutting surface and rubber cup; ③ A fixed rainproof device. This device typically uses a fixed structure to completely cover the cutting surface and rubber cup, but the cover has operating windows for tapping and collecting rubber. These rainproof devices differ in their practicality, flexibility, and economy. Therefore, there is an urgent need in production for a rainproof device that can effectively protect the cutting surface and rubber cup, is easy to move, and is also inexpensive.
[0005] 2. Currently, there are no systematic standards for the harvesting and transportation of latex in production. Various factors during the harvesting process have a certain impact on the preservation of latex, such as harvesting time, latex preservation conditions, and latex transportation temperature. Therefore, it is necessary to establish a systematic latex preservation technology chain to ensure the quality and stability of natural rubber. Summary of the Invention
[0006] To address the aforementioned technical problems, the present invention aims to provide a harvesting method for maintaining the freshness of rubber tree latex. Based on four aspects of technology—waterproofing, time control, preservation, and temperature stability—it uses the key indicator of latex preservation status during natural rubber production—volatile fatty acid (VFA) value—and the key indicators of latex quality—dry rubber content, total solids content, and non-rubber solids content—as evaluation standards. This forms a complete and reliable rubber tree latex preservation technology, enabling the latex to meet the production requirements of specialty rubbers.
[0007] To achieve the above objectives, the present invention employs the following technical measures: a harvesting method for maintaining the freshness of rubber tree latex, comprising the following steps: S1. Rain protection measures for latex: Install rain protection devices in the latex mining area.
[0008] S2. Latex harvesting time: Select different time points for tapping, and harvest the latex 4 hours later.
[0009] S3. Field preservation of latex: Add ammonia water of different concentrations (1% concentration) to the latex cup before tapping.
[0010] S4. Low-temperature transportation of latex: Latex harvested in the field is placed under different temperature conditions and delivered to the latex collection station within 3 hours.
[0011] S5. Latex quality testing: After the latex arrives at the latex receiving station, the VFA value, dry latex content, total solids content, and non-latex solids content of the fresh latex are tested. If the latex meets the standards, it can be used for subsequent production.
[0012] Optionally, in step S1, the rainproof device can be any one of the following: a combination of a felt rain cap and a plastic cup cap, a combination of a felt rain cap and a rain curtain (or rain skirt), or a fixed rain cover. In this device, the rain cap or fixed rain cover is fixed to the tree trunk with staples, and the joint is coated with waterproof material to block rainwater flowing down the tree trunk; the plastic cup cap or rain curtain (or rain skirt) covers the plastic cup to prevent rainwater from entering. The waterproof material can be asphalt waterproof material or polymer waterproof material.
[0013] Preferably, in step S1, the rainproof device is a combination of an tar paper rainproof cap and a shell-shaped rubber cup cap, and the waterproof material is polyurethane waterproof coating.
[0014] Optionally, in step S1, a hydrophobic material, such as fluorocarbon coating PTFE, can be applied to the inside of the plastic cup. Specifically, after cleaning the plastic cup, a brush is used to apply the hydrophobic material evenly to the inner wall of the plastic cup to form a hydrophobic layer.
[0015] Optionally, in step S2, the harvesting time can be selected as 2:30 tapping and 6:30 harvesting, 4:30 tapping and 8:30 harvesting, or 6:30 tapping and 10:30 harvesting.
[0016] Preferably, in step S2, the summer harvesting time is selected as 2:30 tapping and 6:30 harvesting or 4:30 tapping and 8:30 harvesting, and the winter harvesting time is selected as 4:30 tapping and 8:30 harvesting or 6:30 tapping and 10:30 harvesting.
[0017] More preferably, in step S2, the summer harvest time is selected as 2:30 tapping and 6:30 harvesting, and the winter harvest time is selected as 4:30 tapping and 8:30 harvesting.
[0018] Optionally, in step S3, 1% ammonia water can be added to the rubber cup before tapping, with the addition amount being 0 ml, 4 ml, or 8 ml.
[0019] Preferably, in step S3, the amount of 1% ammonia added to the glue cup is 0 ml.
[0020] Optionally, in step S4, the latex is transported on ice or at 4°C.
[0021] Preferably, in step S4, the latex is transported on ice.
[0022] Optionally, in step S5, the dry adhesive content is ≥25%, the total solids content is ≥30%, the non-adhesive solids content is ≤5%, the ammonia content is ≤0.05%, and the VFA value is ≤0.1.
[0023] Preferably, in step S5, the dry adhesive content is ≥30%, the total solids content is ≥33%, and the VFA value is ≤0.05.
[0024] In summary, through systematic research and technological optimization, this invention has overcome the barriers outlined in the background one by one: 1. Solving the problem of rainwater damage to latex production – using rainproof devices. Selection of Rain Protection Devices: Three main types of rain protection products currently on the market were used, and their rain protection effect, cost control, and ease of operation were comprehensively evaluated. While fixed rain covers offer good rain protection, they are extremely inconvenient during rubber cutting and collection, cannot be moved according to changes in the cutting surface, and have high manufacturing costs. The combination of a rain cap and rain curtain (or rain skirt) provides good rain protection, but the rain curtain requires heavy support and is prone to displacement in strong winds, causing rainwater to seep into the latex cup and sometimes even touch the latex tongue, resulting in latex leakage. Furthermore, this device is inconvenient to operate during rubber cutting and collection, requiring frequent movement of the rain curtain, increasing labor intensity and time costs. While the combination of a rain cap and latex cup cap offers less rain protection than the other two and cannot prevent lateral wind and rain, its installation is simple, operation is convenient during rubber cutting and collection, and it is inexpensive, effectively reducing the impact of rainwater on the latex.
[0025] 2. Solving the problem of high impurity content and volatile fatty acid value in fresh latex -- Standardized latex preservation technology chain Standardized operation: Precise tapping and collection times are specified (tapping at 2:30 am and collecting at 6:30 am in summer, tapping at 4:30 am and collecting at 8:30 am in winter), ammonia addition amount (1% concentration, 0-8 ml optional, 0 ml preferred), and latex transportation and storage temperature (transporting on ice or at 4 ℃, preferably on ice), ensuring the reproducibility of the operation.
[0026] Experimental data support and production needs: Based on the commonly used tapping schedule of four days per cut (d4) and six days per cut (d6) in rubber-growing areas of my country, the dry rubber content, total solids content, non-rubber solids content, and VFA value of latex under different harvesting conditions were tested and compared with agricultural industry standards (NY / T 4296) to ensure that the latex meets the production needs of special rubber in my country.
[0027] In summary, this invention systematically solves the production problems in rubber tree production in my country, such as high impurity content and high volatile fatty acid value in fresh latex. By constructing a four-in-one technology chain of "waterproofing, time control, freshness preservation, and temperature stability," and through rigorous index testing, a complete and reliable rubber tree latex preservation technology has been formed, enabling the latex to meet the production requirements of specialty rubbers. Attached Figure Description
[0028] Figure 1 shows the rubber tree rain protection device selected in this invention, wherein, a: tar paper rain cap and shell-shaped rubber cup lid; b: normal rubber cup; c: rubber cup with hydrophobic coating.
[0029] Figure 2 shows the effects of different rain protection devices on the indicators of fresh latex. "Closed" indicates a rain protection device using a combination of an tar paper rain cap and a shell-shaped cup lid; "Closed + Hydrophobic" indicates a latex cup using a combination of an tar paper rain cap and a shell-shaped cup lid with a hydrophobic coating; and "Normal" indicates a normal latex cup without any rain protection device or hydrophobic coating. Where: a: Effect of different rain protection devices on the dry latex content at d4 cutting; b: Effect of different rain protection devices on the dry latex content at d6 cutting; c: Effect of different rain protection devices on the total solids content of latex at d4 cutting; d: Effect of different rain protection devices on the total solids content of latex at d6 cutting; e: Effect of different rain protection devices on the VFA value of latex at d4 cutting; f: Effect of different rain protection devices on the VFA value of latex at d6 cutting. Note: Different lowercase letters indicate significant differences between groups, α=0.05.
[0030] Figure 3 shows the effects of different harvesting times on the indicators of fresh latex. a: Effect of different harvesting times on the dry latex content under d4 tapping; b: Effect of different harvesting times on the dry latex content under d6 tapping; c: Effect of different harvesting times on the total latex solids content under d4 tapping; d: Effect of different harvesting times on the total latex solids content under d6 tapping; e: Effect of different harvesting times on the latex VFA value under d4 tapping; f: Effect of different harvesting times on the latex VFA value under d6 tapping. Note: Different lowercase letters indicate significant differences between groups, α=0.05.
[0031] Figure 4 shows the effects of different ammonia addition amounts on the indicators of fresh latex. a: Effect of different ammonia addition amounts on the dry latex content under tapping conditions d4 and d6; b: Effect of different ammonia addition amounts on the total solids content of latex under tapping conditions d4 and d6; c: Effect of different ammonia addition amounts on the VFA value of latex under tapping conditions d4 and d6. Note: Different lowercase letters indicate significant differences between groups, α=0.05.
[0032] Figure 5 shows the effects of different transportation and storage temperatures on the properties of fresh latex. a: Effect of different transportation and storage temperatures on the VFA value of latex under d4 tapping conditions; f: Effect of different transportation and storage temperatures on the VFA value of latex under d6 tapping conditions. Note: Different lowercase letters indicate significant differences between groups, α=0.05. Detailed Implementation
[0033] The embodiments of the present invention are described in detail below. These embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation schemes and specific operation processes. However, the scope of protection of the present invention is not limited to the following embodiments.
[0034] Example 1
[0035] The impact of rubber tree latex harvesting and preservation techniques on latex quality 1. Test Methods 1.1 Detection of Fresh Latex Indicators 1.1.1 Detection of latex dry rubber content After filtering fresh rubber latex through an 80-mesh sieve to remove impurities, 10 g of latex was placed on a glass petri dish for each sample. The bottom of the dish was gently rotated to ensure the latex covered the bottom. 300 μL of 5% acetic acid solution was added to coagulate the latex, and the mixture was left at room temperature for about 10 hours. After the film had solidified, it was rinsed with water, and a large curd was used to collect all the solidified rubber particles. The curd was then soaked in water. The water was changed several times during this process, pressing the curd to remove excess water and soluble components. Finally, the film was rinsed with deionized water and dried in an 80 ℃ oven until constant weight. The weight of the dry film was then measured. The ratio of the dry film weight to the latex weight is the dry rubber content, expressed as a percentage.
[0036] 1.1.2 Detection of total solids content in latex After filtering fresh rubber latex through an 80-mesh sieve to remove impurities, take approximately 50 g of latex from each sample and place it on a glass petri dish. Gently rotate the dish to ensure the latex covers the bottom, and dry it directly at 80 °C until constant weight. Weigh the dry matter. The ratio of the dry matter weight to the total latex weight is the total solids content, expressed as a percentage. The difference between the total solids content and the dry latex content is the non-latex solids content, also expressed as a percentage.
[0037] 1.1.3. VFA value test of latex After filtering fresh rubber latex through an 80-mesh sieve to remove impurities, take approximately 50 g of latex from each sample and place it in a beaker. Add 50 ml of 30% ammonium sulfate solution using a burette. Maintain the beaker in a water bath at 70 °C and continue stirring until the latex solidifies. Cover the beaker with a watch glass and continue in the water bath for a total of 15 minutes. Slowly pour out the whey and filter it through dry filter paper. Transfer the curd to a mortar and pestle to extract more whey, then filter again. Transfer 25 ml of the filtered whey to a dry 50 ml Erlenmeyer flask, add 5 ml of 50% sulfuric acid solution for acidification, and then distill for at least 15 minutes. Add 10 ml of the acidified whey to the inner tube, allowing vapor to enter. Collect 100 ml of the distillate, purge with nitrogen gas, and titrate with 5 mM Ba(OH)₂, recording the titration number. Phenolphthalein or bromothymol blue is used as an indicator. 0.5 g of the indicator is dissolved in 100 ml of 50% ethanol solution (see national standard GB / T 8292 for specific methods).
[0038] The VFA value is defined as the number of grams of KOH required to neutralize the VFA in a latex containing 100 g of total solids. The calculation formula is as follows:
[0039] Where 134.64 is a proportionality coefficient, calculated from the relative molecular weight of KOH, the valence ratio of KOH to Ba(OH)2, and the mass ratio of acidified whey to distilled whey; c is the actual concentration of Ba(OH)2 in mol / L; V is the actual titration volume of Ba(OH)2 in ml; m is the mass of latex in g; TSC is the total solids content of latex in %; DRC is the dry glue content of latex in %; and ρ is the density of whey in Mg / m³. 3 .
[0040] 1.2 Effects of different harvesting techniques on fresh latex indicators 1.2.1 The impact of rainproof devices on the properties of fresh latex The installation of rainproof devices and rubber cups with hydrophobic coatings (Figure 1) defines "sealed" as the area created by moving the movable rubber cup lid above the cup after tapping; "hydrophobic" refers to using rubber cups with hydrophobic coatings; and "conventional" refers to using normal rubber cups without hydrophobic coatings and without any rainproof devices. Multiple batches of experiments were conducted to compare the dry latex content, total solids content, non-rubber solids content, and VFA value of fresh latex harvested using different rainproof devices with those harvested using conventional methods.
[0041] 1.2.2 Effect of latex harvesting time on fresh latex indicators Three harvesting time treatments were set up: 2:30 tapping and 6:30 collection, 4:30 tapping and 8:30 collection, and 6:30 tapping and 10:30 collection. The effects of different harvesting times on indicators such as dry latex content, total solids content, non-rubber solids content, and VFA value were compared.
[0042] 1.2.3 Effects of ammonia addition in the field on the indicators of fresh latex Four treatments were set up, namely adding 0 ml, 2 ml, 4 ml, and 8 ml of ammonia water (w / v=1%) to the rubber cup before tapping. The effects of ammonia addition on the dry latex content, total solids content, non-rubber solids content, and VFA value of fresh latex were compared.
[0043] 1.2.4 Effects of Transportation and Storage Temperature on the Indicators of Fresh Latex Field-collected latex was mixed and divided into four equal portions. These portions were then placed on ice, at 4 ℃, at room temperature (25 ℃), and at 35 ℃ for 3 h, respectively. The effects of different storage and transportation conditions on the VFA value were analyzed. 1.3 Data Analysis Linear regression analysis was performed using SPSS software, and graphs were generated using Origin software. All data are expressed as mean ± standard deviation.
[0044] Test results 2.1 The impact of rainproof devices on the properties of fresh latex Figure 2 shows the indicators of fresh latex under rainproof devices and conventional harvesting conditions. All harvests showed a dry latex content >25%, total solids content >30%, non-latex solids content <5%, and VFA value <0.1, meeting the requirements for specialty latex production in my country. Regarding dry latex content, there was no significant difference between the latex harvested in July and September. However, in November, the dry latex content under closed harvesting conditions was slightly higher than under the other two conditions, especially in the second harvest of day 6, where the dry latex content under closed harvesting conditions was significantly higher than under the other two conditions. Figure 2 ab); The trend of total solids content is similar to that of dry adhesive content, with no significant difference in the early stage. After entering November, the total solids content under closed conditions was higher than that under the other two conditions. Figure 2 cd).
[0045] Regarding volatile fatty acids, the VFA values in September were higher than those in July and November under both tapping conditions. This is because Hainan Island experiences more rainfall from August to November that year, and the increased precipitation combined with higher temperatures in September leads to higher VFA values. In the first cut of September tapped on days 4 and 6, the VFA values of latex under closed and closed+hydrophobic conditions were significantly lower than those under conventional open conditions. Meanwhile, the VFA value of latex under closed conditions tapped on day 6 was significantly lower than that under closed+hydrophobic conditions. Entering November, although temperatures decreased, rainfall remained high. In the second and third cuts tapped on day 4, the VFA values of latex under closed conditions were significantly lower than those under closed+hydrophobic conditions and conventional open conditions. Figure 2 The above results indicate that both high temperature and rainfall increase the VFA value of latex and reduce its stability. Adding a sealed rainproof device and adding a hydrophobic coating can effectively reduce the VFA value of latex. Latex with only a sealed rainproof device and no hydrophobic coating has better stability.
[0046] 2.2 Effect of latex harvesting time on fresh latex indicators Figure 3 shows the indicators of fresh latex under different harvesting times. For all tapping times, the dry latex content was >30%, the total solids content was >33%, the non-latex solids content was <5%, and the VFA value was <0.1, meeting the requirements for special rubber production in my country. In the third tapping in November (d4), the dry latex content and total solids content under the conditions of tapping at 2:30 and collecting at 4:30 were significantly lower than those under the conditions of tapping at 6:30 and collecting at 8:30. For the remaining tapping times, there were no significant differences in the dry latex content and total solids content under different tapping times. Figure 3 ad).
[0047] Regarding volatile fatty acids, in summer (July and September), there was an overall trend that the earlier the tapping time, the lower the VFA value of the latex. Particularly in the first tapping in July and the second tapping in September (d4), the VFA value of latex tapped at 2:30 and collected at 4:30 was significantly lower than that of latex tapped at 6:30 and collected at 8:30. In winter (November), the opposite occurred: the earlier the tapping time, the higher the VFA value of the latex. Especially in the third tapping in November (d4), the VFA value of latex tapped at 2:30 and collected at 4:30 was significantly higher than that of latex tapped at 6:30 and collected at 8:30. Figure 3 Based on the production requirements of rubber trees and local conditions, it is recommended to tap rubber at 2:30 in summer and at 4:30 in winter. This helps to reduce the VFA value of the latex and increase its quality and stability.
[0048] 2.3 Effects of ammonia addition in the field on the indicators of fresh latex Figure 4 shows the indicators of fresh latex under different ammonia addition levels. For all cuts, the dry latex content was >30%, the total solids content was >33%, the non-latex solids content was <5%, and the VFA value was <0.1, meeting the requirements for specialty rubber production in my country. There were no significant differences in the dry latex content and total solids content under different ammonia addition levels. Figure 4 ab). Regarding volatile fatty acids, the VFA value initially increased and then decreased with increasing ammonia concentration. In all cuts in July, the VFA value of latex with 2 ml of 1% ammonia added was significantly higher than that of latex with 0 ml, 4 ml, and 8 ml of 1% ammonia added in the field. In the d6 cut in September, the VFA value of latex with 8 ml of 1% ammonia added was significantly lower than that of latex with 0 ml and 2 ml of 1% ammonia added. Figure 4 c).
[0049] Ammonia, as a mainstream latex preservative, can indeed reduce the VFA value of latex, improve its stability, and inhibit coagulation. However, high concentrations of ammonia can darken the color of natural rubber, reduce its plasticity retention, and react chemically with aldehyde and carboxyl groups on the side chains of natural rubber molecules, causing protein denaturation or degradation of non-rubber components, thus altering the molecular structure. Furthermore, ammonia has a strong volatile and irritating odor, polluting the environment and harming rubber workers and manufacturers. Therefore, the natural rubber processing industry is actively exploring low-ammonia or ammonia-free latex preservation methods. Considering that the VFA value of latex is below 0.06 without ammonia, meeting the requirements for specialty rubber production in my country, in high-quality latex production, 4ml or 8ml of 1% ammonia can be added only during the first five taps each year or when the latex dry content is extremely high to prevent premature coagulation. From the sixth tap onwards, ammonia can be discontinued.
[0050] 2.4 Effect of transportation and storage temperature on VFA value Figure 5 shows the indicators of fresh latex under different transportation and storage temperatures. The VFA values of latex under both tapping conditions increased with increasing transportation and storage temperatures, especially in September (high temperature). Under d4 tapping conditions, the VFA values of latex stored on ice after the third cut in July and the first and third cuts in September were significantly lower than those stored at 35℃. The VFA values of latex stored on ice and at 4℃ after the second cut in September and the second cut in November were significantly lower than those stored at room temperature and 35℃. The VFA value of latex stored at 35℃ after the third cut in November was significantly higher than the VFA values of latex stored under the other three storage conditions. Figure 5 a). Of the two cuts made on September d6, the VFA values of latex stored on ice and at 4°C were significantly lower than those stored at room temperature and 35°C. Figure 5 (b) In actual production, latex should be transported under ice or 4°C conditions to prevent an increase in the VFA value and maintain latex stability. If ice storage and transportation are not possible, transport should be carried out in the dark as much as possible, and the latex should be delivered to the receiving station as soon as possible to avoid an increase in the VFA value due to temperature rise, which would reduce the stability of the latex.
[0051] The above description is merely a specific embodiment of the present invention, and the scope of protection of the present invention is not limited thereto. Any transformations or substitutions that can be conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A harvesting method for maintaining the freshness of rubber tree latex, characterized in that, Includes the following steps: S1. Rain protection measures for latex: Install rain protection devices in the latex mining area; S2. Latex harvesting time: Select tapping at 2:30 and harvesting at 6:30, tapping at 4:30 and harvesting at 8:30, and tapping at 6:30 and harvesting at 10:
30. S3. Field preservation of latex: Add 1% ammonia water to the latex cup before tapping; S4. Low-temperature transportation of latex: Latex harvested in the field is placed on ice or transported at 4 ℃ and delivered to the latex collection station within 3 hours. S5. Latex quality testing: After the latex arrives at the latex receiving station, the VFA value, dry latex content, total solids content, and non-latex solids content of the fresh latex are tested. Once the latex meets the standards, it can be used for subsequent production.
2. The harvesting method according to claim 1, characterized in that, In step S1, the rainproof device can be any one of the following: a combination of tarpaulin rainproof cap and rubber cup cap, a combination of tarpaulin rainproof cap and rainproof curtain / rainproof skirt, or a fixed rainproof cover. The rain cap / fixed rain cover is fixed to the tree trunk with staples, and the joint is coated with waterproof material; the glue cup cap / rain curtain / rain skirt covers the glue cup; the waterproof material is selected from asphalt waterproof material or polymer waterproof material.
3. The harvesting method according to claim 2, characterized in that, In step S1, the rainproof device is a combination of an tar paper rainproof cap and a shell-shaped rubber cup cap, and the waterproof material is polyurethane waterproof coating.
4. The harvesting method according to claim 1, characterized in that, In step S1, applying a hydrophobic material to the inside of the cup involves cleaning the cup, then using a brush to apply the hydrophobic material evenly to the inner wall of the cup to form a hydrophobic layer.
5. The harvesting method according to claim 1, characterized in that, In step S2, the summer harvesting time is selected as 2:30 tapping and 6:30 harvesting or 4:30 tapping and 8:30 harvesting, and the winter harvesting time is selected as 4:30 tapping and 8:30 harvesting or 6:30 tapping and 10:30 harvesting.
6. The harvesting method according to claim 5, characterized in that, In step S2, the summer harvest time is selected as 2:30 tapping and 6:30 harvesting, and the winter harvest time is selected as 4:30 tapping and 8:30 harvesting.
7. The harvesting method according to claim 1, characterized in that, In step S3, the amount of ammonia water with a concentration of 1% added is 0 ml, 4 ml or 8 ml, preferably 0 ml.
8. The harvesting method according to claim 1, characterized in that, In step S4, the latex is transported on ice.
9. The harvesting method according to claim 1, characterized in that, In step S5, the dry adhesive content is ≥25%, the total solids content is ≥30%, the non-adhesive solids content is ≤5%, the ammonia content is ≤0.05%, and the VFA value is ≤0.
1.
10. The harvesting method according to claim 9, characterized in that, In step S5, the dry adhesive content is ≥30%, the total solids content is ≥33%, and the VFA value is ≤0.05.