Composite textile material, method for its production and use

CN122876755APending Publication Date: 2026-10-09CENT SOUTH UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611375687.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-10-09

AI Technical Summary

Technical Problem

聚对苯二甲酸乙二醇酯针刺毡凭借优异的力学性能、耐候性与成本优势,是当前汽车地毯的主流基材,但聚酯材料本身为绝缘高分子,存在易滋生细菌、摩擦易积聚静电、导热性差导致乘坐区域热量堆积等固有缺陷,难以满足高端内饰的使用标准

Benefits of technology

1、本发明将经硅烷偶联剂处理的纳米氧化锌与抗静电剂引入聚酯材料中,通过熔融共混、纺丝和针刺形成抗菌层。硅烷偶联剂对纳米氧化锌进行表面处理,有利于改善纳米氧化锌在聚酯基体中的分散性及界面相容性,从而使所得抗菌层兼具抗菌性能和抗静电性能。由实施例测试结果可知,所得复合纺织材料对大肠杆菌和金黄色葡萄球菌的抗菌率均≥99%,同时具有较低的体积电阻率。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application discloses a kind of composite textile materials and preparation method and application thereof, and is related to the field of textile material preparation.The composite textile material is five-layered composite structure in turn, including antibacterial layer, adhesive layer, carbon fiber layer, adhesive layer and bottom layer;The application is prepared by filler surface modification, blending granulation, spinning needle punching forming and matched hot-pressing composite process, the obtained material has antibacterial, antistatic and heat conduction performance, and has good mechanical properties and the ability to maintain mechanical properties after water, and can be used in automotive interior carpet and other scenes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile material preparation, specifically to a composite textile material, its preparation method, and its application. Background Technology

[0002] As demands for a superior driving and riding experience continue to rise, automotive interior carpets have evolved from traditional functions like sound insulation, dust prevention, and decoration to multifunctional integrations such as antibacterial, heat conduction and temperature regulation, and antistatic properties. Polyethylene terephthalate (PET) needle-punched felt, with its excellent mechanical properties, weather resistance, and cost advantages, is currently the mainstream substrate for automotive carpets. However, polyester itself is an insulating polymer, possessing inherent drawbacks such as susceptibility to bacterial growth, static electricity buildup due to friction, and poor thermal conductivity leading to heat accumulation in seating areas, making it difficult to meet the standards for high-end interiors.

[0003] Existing technologies for addressing the aforementioned deficiencies still have several shortcomings: First, conventional small-molecule antibacterial agents are prone to migration and precipitation from fibers, exhibiting poor water resistance and durability, and poor compatibility with the polyester matrix. This can easily lead to filament breakage and decreased fiber strength during spinning, and some antibacterial components can even cause yellowing of the material, making them unsuitable for light-colored interior trims. Second, traditional ionic antistatic agents rely on ambient humidity to function, with their antistatic effect significantly diminishing in dry environments. They are also prone to interacting with antibacterial fillers, simultaneously weakening both antibacterial and antistatic properties. Furthermore, the precipitation of small molecules can lead to increased VOCs in the vehicle interior. Third, carbon-based fillers introduced to improve thermal conductivity tend to agglomerate and stack in the bonding system, failing to form a continuous and effective thermal conduction pathway and damaging the adhesive toughness of the bonding layer, resulting in decreased interlayer peel strength and delamination and powdering during use. Fourth, the multilayer composite process and material system have insufficient compatibility, preventing the binder from fully wetting the fiber interface, resulting in weak interlayer bonding. Mechanical properties degrade significantly in water or humid and hot environments, limiting service life.

[0004] Therefore, developing a composite textile material that combines long-lasting antibacterial properties, stable antistatic properties, high thermal conductivity, strong interlayer bonding, and suitability for industrial mass production is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] To address the above problems, this invention involves blending nano-zinc oxide treated with a silane coupling agent and an antistatic agent with polyester, preparing an antibacterial layer through melt spinning and needle punching, and then using an adhesive containing graphene and a compatibilizer to composite the antibacterial layer, carbon fiber layer, and bottom layer, resulting in a composite textile material with antibacterial, antistatic, and thermal conductivity properties.

[0006] This invention provides a composite textile material, which has 5 layers, including an antibacterial layer, an adhesive layer, a carbon fiber layer, an adhesive layer, and a bottom layer in sequence; The antibacterial layer comprises polyester, and a silane coupling agent, nano zinc oxide, and an antistatic agent mixed in the polyester; The adhesive layer includes an adhesive, and a silane coupling agent, graphene, and a compatibilizer mixed in the adhesive; The carbon fiber layer is a 3-4 mm thick carbon fiber felt; The bottom layer is a 2-3mm thick polyethylene terephthalate base felt; The composite textile material exhibits an antibacterial rate of ≥99% against both Escherichia coli and Staphylococcus aureus, an odor rating of 4-4.5, a thermal conductivity of 0.837-0.995 W / (m·K), and a volume resistivity of (3-4)×10⁻⁶. 11 Ω·cm, tensile breaking strength is 1200-1300N / 5cm, and the tensile breaking strength decreases by 12-19% after contact with water.

[0007] The present invention also provides a method for preparing the composite textile material, comprising the following steps: Step 1: Spray the silane coupling agent onto the nano zinc oxide, dry it, and then mix it with polyester to obtain the nano polyester material. Step 2: After mixing the nano-polyester material and antistatic agent evenly, melt extrude the mixture using a twin-screw extruder to obtain nano-polyester masterbatch; Step 3: Place the nano-polyester masterbatch in a spinning machine for melt spinning, and cut it after air cooling to obtain antibacterial short fibers; open, comb and lay the antibacterial short fibers in sequence to form a fiber web, and needle punch the fiber web to obtain an antibacterial layer; Step 4: Spray the silane coupling agent onto the graphene, dry it, then mix it with the binder and compatibilizer. After mixing evenly, place it in a twin-screw extruder and melt-extrude it to obtain a molten thermally conductive adhesive. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer, then laminate a carbon fiber layer, continue to apply the thermally conductive adhesive to the back of the carbon fiber felt, and finally laminate a bottom layer. After hot pressing, the composite textile material is obtained.

[0008] Further, in step 1, the mass ratio of the nano zinc oxide to the polyester is (1-1.5):(94-95).

[0009] Furthermore, the particle size of the nano zinc oxide in step 1 is 50 nm.

[0010] Furthermore, in step 1, the silane coupling agent is sprayed onto the nano zinc oxide at a mass fraction of 1 wt%, and the solvent is ethanol and deionized water in a volume ratio of 1:1.

[0011] Furthermore, the polyester in step 1 is polyethylene terephthalate.

[0012] Furthermore, the silane coupling agent in step 1 is γ-glycidoxypropyltrimethoxysilane.

[0013] Furthermore, the mass of the silane coupling agent in step 1 is 0.5-2% of the mass of the nano zinc oxide.

[0014] Furthermore, the drying temperature in step 1 is 80-100℃, and the drying time is 1-2 hours.

[0015] Further, in step 2, the mass ratio of the antistatic agent to the polyester is (4-5):(94-95).

[0016] Furthermore, the antistatic agent in step 2 is a polyether-polyamide block copolymer antistatic agent, brand name Irgastat P18.

[0017] Furthermore, the processing temperature of the twin-screw extruder in step 2 is 240-260℃.

[0018] Furthermore, the processing temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃.

[0019] Furthermore, the spinning temperature in step 3 is 250-260℃.

[0020] Furthermore, the temperature of the air cooling in step 3 is 20-40℃.

[0021] Furthermore, the thickness of the fiber web in step 3 is 2 mm.

[0022] Furthermore, in step 3, the pre-needling density is set to 20-30 needles / cm². 2 The density of acupuncture needles on the front is 40-50 needles / cm². 2 The density of needles on the reverse side is 35-50 needles / cm². 2 .

[0023] Further, in step 4, the mass ratio of graphene, binder and compatibilizer is (0.8-1.5):(94-95):(4-5).

[0024] Furthermore, the adhesive used in step 4 is polyester hot melt adhesive (PES).

[0025] Furthermore, the compatibilizer in step 4 is maleic anhydride-grafted polyester (MAH-g-PET).

[0026] Furthermore, in step 4, the silane coupling agent is sprayed onto the graphene at a mass fraction of 1 wt%, and the solvent is ethanol and deionized water in a volume ratio of 1:1.

[0027] Furthermore, in step 4, the mass of the silane coupling agent is 0.5-2% of the mass of the graphene.

[0028] Furthermore, the drying temperature in step 4 is 80-100℃, and the drying time is 1-2 hours.

[0029] Furthermore, the processing temperature of the twin-screw extruder in step 4 is 130-150℃.

[0030] Furthermore, the processing temperature of the twin-screw extruder is divided into four temperature zones: 130℃, 140℃, 150℃, and 140℃.

[0031] Furthermore, the coating thickness in step 5 is 100-120 μm.

[0032] Furthermore, the thickness of the carbon fiber layer in step 5 is 3-4 mm.

[0033] Furthermore, the carbon fiber layer in step 5 is a carbon fiber felt.

[0034] Furthermore, the thickness of the bottom layer in step 5 is 2-3 mm.

[0035] Furthermore, in step 5, the bottom layer is a polyethylene terephthalate (PET) substrate.

[0036] Furthermore, the temperature of hot pressing in step 5 is 140-150℃.

[0037] Furthermore, the pressure of hot pressing in step 5 is 0.2-0.3 MPa, and the hot pressing time is 120-130 s.

[0038] The present invention also provides an application of the composite textile material as an automotive carpet, wherein the automotive carpet is obtained by cutting the composite textile material.

[0039] The beneficial effects of this invention are: 1. This invention introduces nano-zinc oxide treated with a silane coupling agent and an antistatic agent into a polyester material, forming an antibacterial layer through melt blending, spinning, and needle punching. The silane coupling agent surface-treats the nano-zinc oxide, which improves its dispersibility and interfacial compatibility in the polyester matrix, thus giving the resulting antibacterial layer both antibacterial and antistatic properties. Test results from the examples show that the resulting composite textile material exhibits an antibacterial rate of ≥99% against both *Escherichia coli* and *Staphylococcus aureus*, while also possessing a low volume resistivity.

[0040] 2. This invention uses a polyester hot melt adhesive containing graphene treated with a silane coupling agent and a compatibilizer as the adhesive layer, and a carbon fiber felt is placed between the two adhesive layers. The addition of graphene helps to improve the thermal conductivity of the adhesive layer, and the compatibilizer helps to improve the compatibility between graphene and the polyester hot melt adhesive; at the same time, the carbon fiber felt can provide thermally conductive support, thereby improving the overall thermal conductivity of the composite textile material. The thermal conductivity of the composite textile material obtained in the examples is 0.837~0.995 W / (m·K), indicating that the composite structure has good thermal conductivity.

[0041] 3. This invention employs a five-layer structure formed by sequentially composited antibacterial layer, adhesive layer, carbon fiber layer, adhesive layer, and bottom layer, and bonds each layer together through a hot-pressing process. The polyester hot-melt adhesive melts and impregnates adjacent layers during hot pressing, which improves the bonding stability between layers. The carbon fiber felt and polyethylene terephthalate bottom felt also provide structural support for the composite material. The resulting composite textile material shows no significant color, appearance changes, delamination, or deformation after high-temperature treatment, and exhibits good tensile properties and retention of mechanical properties after contact with water, meeting the comprehensive requirements of antibacterial, antistatic, thermal conductivity, and structural stability for applications such as automotive interior carpets. Detailed Implementation

[0042] The present invention will be further described in detail below with reference to the embodiments.

[0043] This invention prepares nano-polyester masterbatch by blending nano-zinc oxide treated with silane coupling agent and antistatic agent with polyester, and obtains an antibacterial layer by melt spinning, air cooling, cutting, opening, carding, web laying and needle punching; then, the antibacterial layer, carbon fiber layer and bottom layer are sequentially compounded by polyester hot melt adhesive containing graphene and compatibilizer to obtain the composite textile material.

[0044] Example 1 This embodiment provides a method for preparing a composite textile material, including the following steps: Step 1: 0.015 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94.5 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin at 260°C. After air cooling at 30°C, cut the masterbatch to obtain antibacterial short fibers. Sequentially open, card, and lay the antibacterial short fibers to form a fiber web with a thickness of 2 mm. Perform pre-needling, front-side needle punching, and back-side needle punching on the fiber web, wherein the pre-needling density is 25 needles / cm². 2 An antibacterial layer is obtained by a needle-punching density of 50 needles / cm² on the front and 40 needles / cm² on the back. Step 4: 0.012 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester were mixed. After being mixed evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0045] In Example 1, the composite textile material was placed at 80±2℃ for 168 hours and then at 23±2℃ and 50±5%RH for 3 hours. The surface of the composite textile material showed no color or appearance change and no degradation. The specific test standard is Section 6.1.4 of Q / BAICC220001-2022.

[0046] The composite textile material was placed at 80±2℃ for 24 hours, and then at 23±2℃ and 50±5%RH for 3 hours. The composite textile material showed no delamination or deformation. The specific test standards are Section 5.10 of Q / BAICC335090-2022 and Section 6.1.1 of Q / BAICC220001-2022. RH stands for Relative Humidity, which is the percentage of water vapor content in the air relative to the saturated water vapor content at the same temperature.

[0047] Example 2 This embodiment provides a method for preparing a composite textile material, including the following steps: Step 1: 0.01 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 95 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 4 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. The antibacterial short fibers are then opened, combed, and laid into a web to form a fiber web with a thickness of 2 mm. The fiber web is then pre-needled, front-side needle-punched, and back-side needle-punched in sequence, with a pre-needling density of 25 needles / cm², a front-side needle-punching density of 40 needles / cm², and a back-side needle-punching density of 35 needles / cm² to obtain an antibacterial layer. Step 4: 0.012 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester were mixed. After being mixed evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0048] Example 3 This embodiment provides a method for preparing a composite textile material, including the following steps: Step 1: 0.015 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94.5 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. Sequentially open, comb, and lay the antibacterial short fibers to form a fiber web with a thickness of 2 mm. Sequentially pre-needle-punch, front needle-punch, and back needle-punch the fiber web, wherein the pre-needle-punch density is 25 needles / cm², the front needle-punch density is 45 needles / cm², and the back needle-punch density is 40 needles / cm², to obtain an antibacterial layer. Step 4: 0.015 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester were mixed. After being mixed evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 145°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0049] Example 4 This embodiment provides a method for preparing a composite textile material, including the following steps: Step 1: 0.02 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. The antibacterial short fibers are then opened, combed, and laid into a web to form a fiber web with a thickness of 2 mm. The fiber web is then pre-needled, front-side needle-punched, and back-side needle-punched in sequence, with a pre-needling density of 25 needles / cm², a front-side needle-punching density of 40 needles / cm², and a back-side needle-punching density of 35 needles / cm² to obtain an antibacterial layer. Step 4: 0.01 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane is uniformly sprayed onto 0.8 parts by weight of graphene at a mass fraction of 1 wt% (solvent is ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester are mixed and placed in a twin-screw extruder. The mixture is then melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder is divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0050] Comparative Example 1 This comparative example provides a method for preparing a composite textile material, including the following steps: Step 1: Mix 95 parts by weight of polyethylene terephthalate and 5 parts by weight of polyether-polyamide block copolymer antistatic agent evenly, and then melt-extrude the mixture using a twin-screw extruder at 240-260℃ to obtain polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 2: Place the polyester masterbatch in a spinning machine and melt spin it at 260°C. After air cooling at 30°C, cut it to obtain polyester staple fibers. Sequentially open, comb, and lay the polyester staple fibers to form a fiber web with a thickness of 2 mm. Sequentially pre-needle-punch, front needle-punch, and back needle-punch the fiber web, wherein the pre-needle-punch density is 25 needles / cm², the front needle-punch density is 50 needles / cm², and the back needle-punch density is 40 needles / cm², to obtain a polyester layer. Step 3: 0.012 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester were mixed. After being mixed evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 4: Apply the thermally conductive adhesive to the back of the polyester layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0051] Comparative Example 2 This comparative example provides a method for preparing a composite textile material, including the following steps: Step 1: 0.015 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94.5 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, the mixture is melt-extruded using a twin-screw extruder at 240-260°C to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240°C, 250°C, 260°C, and 240°C. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. Sequentially open, comb, and lay the antibacterial short fibers to form a fiber web with a thickness of 2 mm. Sequentially pre-needle-punch, front-side needle-punch, and back-side needle-punch the fiber web, wherein the pre-needle-punch density is 25 needles / cm², the front-side needle-punch density is 50 needles / cm², and the back-side needle-punch density is 40 needles / cm², to obtain an antibacterial layer. Step 4: 0.012 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester were mixed. After being mixed evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0052] Comparative Example 3 This comparative example provides a method for preparing a composite textile material, including the following steps: Step 1: 0.015 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94.5 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. Sequentially open, comb, and lay the antibacterial short fibers to form a fiber web with a thickness of 2 mm. Sequentially pre-needle-punch, front-side needle-punch, and back-side needle-punch the fiber web, wherein the pre-needle-punch density is 25 needles / cm², the front-side needle-punch density is 50 needles / cm², and the back-side needle-punch density is 40 needles / cm², to obtain an antibacterial layer. Step 4: Apply molten polyester hot melt adhesive (PES) to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm layer of carbon fiber felt. Continue to apply the polyester hot melt adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm layer of polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0053] Comparative Example 4 This comparative example provides a method for preparing a composite textile material, including the following steps: Step 1: 0.015 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94.5 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. Sequentially open, comb, and lay the antibacterial short fibers to form a fiber web with a thickness of 2 mm. Sequentially pre-needle-punch, front-side needle-punch, and back-side needle-punch the fiber web, wherein the pre-needle-punch density is 25 needles / cm², the front-side needle-punch density is 50 needles / cm², and the back-side needle-punch density is 40 needles / cm², to obtain an antibacterial layer. Step 4: 0.012 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 99 parts by weight of polyester hot melt adhesive (PES) were mixed in. After mixing evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 140°C and 0.3 MPa for 120 s, the composite textile material is obtained.

[0054] Comparative Example 5 This comparative example provides a method for preparing a composite textile material, including the following steps: Step 1: 0.015 parts by weight of γ-glycidyl oxypropyltrimethoxysilane were uniformly sprayed onto 1.5 parts by weight of nano zinc oxide (50 nm) at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 h, 94.5 parts by weight of polyethylene terephthalate were mixed to obtain nano polyester material. Step 2: After uniformly mixing the nano-polyester material and 5 parts by weight of polyether-polyamide block copolymer antistatic agent, melt extrusion is performed using a twin-screw extruder at 240-260℃ to obtain nano-polyester masterbatch. The temperature of the twin-screw extruder is divided into four temperature zones: 240℃, 250℃, 260℃, and 240℃. Step 3: Place the nano-polyester masterbatch in a spinning machine and melt-spin it at 260°C. After air cooling at 30°C, cut it to obtain antibacterial short fibers. Sequentially open, comb, and lay the antibacterial short fibers to form a fiber web with a thickness of 2 mm. Sequentially pre-needle-punch, front-side needle-punch, and back-side needle-punch the fiber web, wherein the pre-needle-punch density is 25 needles / cm², the front-side needle-punch density is 50 needles / cm², and the back-side needle-punch density is 40 needles / cm², to obtain an antibacterial layer. Step 4: 0.012 parts by weight of γ-glycidyl etheroxypropyltrimethoxysilane were uniformly sprayed onto 1 part by weight of graphene at a mass fraction of 1 wt% (the solvent was ethanol and deionized water in a volume ratio of 1:1). After drying at 80°C for 1 hour, 95 parts by weight of polyester hot melt adhesive (PES) and 4 parts by weight of maleic anhydride grafted polyester were mixed. After being mixed evenly, the mixture was placed in a twin-screw extruder and melt-extruded at 130-150°C to obtain a molten thermally conductive adhesive. The temperature of the twin-screw extruder was divided into four temperature zones: 130°C, 140°C, 150°C, and 140°C. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer with a coating thickness of 100 μm. After coating, laminate a 3 mm thick layer of carbon fiber felt. Continue to apply the thermally conductive adhesive with a thickness of 100 μm to the back of the carbon fiber felt. Finally, laminate a 2 mm thick layer of polyethylene terephthalate base felt. After hot pressing all layers at 100°C and 0.3 MPa for 60 s, the composite textile material is obtained.

[0055] Table 1 shows the properties of the composite textile materials obtained in each embodiment and comparative example.

[0056]

[0057] The composite textile materials obtained in Examples 1-4 of this invention all achieved an antibacterial rate of 99% against Escherichia coli and Staphylococcus aureus, a thermal conductivity of 0.837-0.995 W / (m·K), an odor rating maintained at 4-4.5, a tensile breaking strength of 1200-1300 N / 5 cm, and a tensile breaking strength attenuation rate of 12%-19% after contact with water. This indicates that the composite textile materials obtained in this invention can take into account antibacterial, antistatic, thermal conductivity and mechanical properties, and have a good ability to retain mechanical properties after contact with water.

[0058] In Comparative Example 1, without the addition of nano-zinc oxide to the polyester, the antibacterial rates against Escherichia coli and Staphylococcus aureus decreased to 5% and 7%, respectively, showing almost no antibacterial activity. This demonstrates that the introduction of nano-zinc oxide plays an important role in improving the antibacterial properties of composite textile materials.

[0059] In Comparative Example 2, the antistatic agent of the polyether-polyamide block copolymer was replaced with octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, which reduced the antibacterial rates against Escherichia coli and Staphylococcus aureus to 83% and 88%, respectively, while increasing the decrease in tensile strength at break after contact with water to 24%. This invention uses a polyether-polyamide block copolymer antistatic agent, which is beneficial for achieving both antistatic properties and the retention of mechanical properties after contact with water.

[0060] In Comparative Example 3, the adhesive layer without the addition of graphene treated with silane coupling agent and compatibilizer had a thermal conductivity reduced to 0.162 W / (m·K). This indicates that introducing graphene and compatibilizer into the adhesive layer is beneficial to improving the thermal conductivity of the adhesive layer and to forming an effective interlayer thermal conduction path between the antibacterial layer and the carbon fiber layer, thereby improving the overall thermal conductivity of the composite textile material.

[0061] In Comparative Example 4, the addition of graphene to the adhesive layer without a compatibilizer resulted in a thermal conductivity of 0.577 W / (m·K), a tensile breaking strength reduced to 1150 N / 5 cm, and an odor level increased to level 5. This indicates that the absence of a compatibilizer is detrimental to the formation of good interfacial compatibility between graphene and polyester hot melt adhesive, and may affect the uniform dispersion of graphene in the adhesive system, thereby reducing the thermal conductivity and mechanical properties of the resulting composite textile material.

[0062] In Comparative Example 5, each layer was hot-pressed at 100°C and 0.3MPa for 60s, resulting in a decrease in tensile breaking strength to 950N / 5cm and thermal conductivity to 0.619W / (m·K). Compared to the hot-pressing conditions in the examples, the lower hot-pressing temperature and shorter hot-pressing time are not conducive to the full melting and wetting of the polyester hot melt adhesive with adjacent layers, thereby affecting the bonding between layers and interlayer heat transfer, and causing a decrease in the mechanical and thermal properties of the resulting composite textile material.

[0063] In summary, this invention, through the combination of nano-zinc oxide, polyether-polyamide block copolymer antistatic agent, graphene-containing compatibilizer adhesive system, and corresponding hot-pressing composite process, enables the resulting composite textile material to take into account antibacterial, antistatic, thermal conductivity, and mechanical properties.

[0064] The antibacterial test standard described in this invention is GB / T 21510-2024, the odor level test standard is Q / JQ 11052-2021, the tensile breaking strength test standard is ISO 13934-1, the test equipment is a tensile testing machine, the thermal conductivity test standard is GB / T 10294-2008, and the volume resistivity test standard is ASTM D257. The test method for the decrease rate of tensile breaking strength after water exposure is as follows: Immerse the composite textile material in water at 25℃ for 10 hours, and then determine the tensile breaking strength according to "ISO 13934-1"; The decrease rate of tensile breaking strength after water exposure = [(tensile breaking strength before water exposure - tensile breaking strength after water exposure) / tensile breaking strength before water exposure] × 100%.

[0065] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any other way. Any modifications or equivalent changes made based on the technical essence of the present invention shall still fall within the scope of protection claimed by the present invention.

Claims

1. A composite textile material, characterized in that, The composite textile material has 5 layers, which include, in sequence, an antibacterial layer, an adhesive layer, a carbon fiber layer, an adhesive layer, and a bottom layer; The antibacterial layer comprises polyester, and a silane coupling agent, nano zinc oxide, and an antistatic agent mixed in the polyester; The adhesive layer includes an adhesive, and a silane coupling agent, graphene, and a compatibilizer mixed in the adhesive; The carbon fiber layer is a 3-4 mm thick carbon fiber felt; The bottom layer is a 2-3mm thick polyethylene terephthalate base felt; The composite textile material exhibits an antibacterial rate of ≥99% against both Escherichia coli and Staphylococcus aureus, an odor rating of 4-4.5, a thermal conductivity of 0.837-0.995 W / (m·K), and a volume resistivity of (3-4)×10⁻⁶. 11 Ω·cm, tensile breaking strength is 1200-1300N / 5cm, and the tensile breaking strength decreases by 12-19% after contact with water.

2. A method for preparing the composite textile material according to claim 1, characterized in that, Includes the following steps: Step 1: Spray the silane coupling agent onto the nano zinc oxide, dry it, and then mix it with polyester to obtain the nano polyester material; Step 2: After mixing the nano-polyester material and antistatic agent evenly, melt extrude the mixture using a twin-screw extruder to obtain nano-polyester masterbatch; Step 3: Place the nano-polyester masterbatch in a spinning machine for melt spinning, and cut it after air cooling to obtain antibacterial short fibers; open, comb and lay the antibacterial short fibers in sequence to form a fiber web, and needle punch the fiber web to obtain an antibacterial layer; Step 4: Spray the silane coupling agent onto the graphene, dry it, then mix it with the binder and compatibilizer. After mixing evenly, place it in a twin-screw extruder and melt-extrude it to obtain a molten thermally conductive adhesive. Step 5: Apply the thermally conductive adhesive to the back of the antibacterial layer, then laminate a carbon fiber layer, continue to apply the thermally conductive adhesive to the back of the carbon fiber felt, and finally laminate a bottom layer. After hot pressing, the composite textile material is obtained.

3. The preparation method according to claim 2, characterized in that, The particle size of the nano zinc oxide in step 1 is 50 nm.

4. The preparation method according to claim 2, characterized in that, The silane coupling agent in step 1 is γ-glycidoxypropyltrimethoxysilane.

5. The preparation method according to claim 2, characterized in that, The antistatic agent in step 2 is a polyether-polyamide block copolymer antistatic agent.

6. The preparation method according to claim 2, characterized in that, The adhesive used in step 4 is a polyester hot melt adhesive.

7. The preparation method according to claim 2, characterized in that, The coating thickness in step 5 is 100-120 μm.

8. The preparation method according to claim 2, characterized in that, The temperature for hot pressing in step 5 is 140-150℃.

9. The preparation method according to claim 2, characterized in that, The pressure for hot pressing in step 5 is 0.2-0.3 MPa, and the hot pressing time is 120-130 s.

10. An application of the composite textile material of claim 1 as an automotive carpet, characterized in that, The car carpet is made by cutting the composite textile material.