Acid-resistant microcrystalline preservative plate, preparation method and application thereof

By using municipal sludge incineration ash as raw material, combined with specific additives and processes, acid-resistant microcrystalline anti-corrosion boards were prepared, solving the problem of utilizing municipal sludge incineration ash, realizing high-performance and low-cost resource utilization, and improving the acid resistance and stability of the boards.

CN122878034BActive Publication Date: 2026-11-24SHANGHAI CEO ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611402695.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-24
Estimated Expiration
2046-09-10

AI Technical Summary

Technical Problem

Existing technologies cannot effectively utilize the bag filter dust generated from municipal sludge incineration, resulting in unstable solidification of heavy metals, phosphorus and sulfur oxides affecting the acid resistance of the boards, and the high addition of sodium fluorosilicate leading to high production costs and environmental pollution.

Method used

Using bag filter dust from municipal wastewater treatment plant sludge incineration as the main raw material, combined with soda ash, sodium sulfide, silicon carbide, semi-coke powder, zirconium corundum brick powder, silica powder, and sodium fluorosilicate, acid-resistant microcrystalline anti-corrosion board is prepared through extrusion granulation, melting, calendering, nucleation, crystallization, and cooling processes. The reducing atmosphere is precisely controlled by the composite reduction system of semi-coke powder and silicon carbide to form a FeS-F-Ti-P multiphase composite crystal nucleus system, which improves the crystallization rate and acid resistance.

Benefits of technology

This technology enables the resource utilization of hazardous waste, reduces landfill pollution and disposal costs, and produces corrosion-resistant boards with excellent acid resistance and low cost. It also solves the problem of high phosphorus and high sulfur properties in traditional microcrystalline boards, and improves the mechanical properties and stability of the boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses an acid-resistant microcrystalline anti-corrosion board, its preparation method, and its application. The acid-resistant microcrystalline anti-corrosion board comprises the following raw materials in parts by weight: 52-57 parts of dust collector ash, 14-15 parts of soda ash, 2-2.5 parts of sodium sulfide, 0.03-0.04 parts of silicon carbide, 0.08-0.1 parts of semi-coke powder, 1-1.5 parts of zirconium corundum brick powder, 16-18 parts of silica powder, 7-9 parts of limestone, and 2.5-3 parts of sodium fluorosilicate; the dust collector ash is baghouse dust generated from sludge incineration at a municipal wastewater treatment plant. This invention also discloses a method for preparing the acid-resistant microcrystalline anti-corrosion board. This invention uses sludge incineration bag filter ash as the main raw material to prepare acid-resistant microcrystalline anti-corrosion board, realizing the high-value utilization of hazardous waste. It also fundamentally solves the dual problems of high land resource consumption and large environmental pollution in traditional landfill and solidification treatment, providing an innovative solution for the resource utilization of municipal sludge incineration bag filter ash.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This specification relates to the field of solid waste resource utilization, and in particular to an acid-resistant microcrystalline anti-corrosion board, its preparation method, and its application. Background Technology

[0002] Baghouse dust generated from sludge incineration at municipal wastewater treatment plants is classified as hazardous waste due to its content of heavy metals (such as Cr2O3, PbO, ZnO, etc.) and phosphorus and sulfur oxides. Traditional treatment methods mainly involve landfilling or simple solidification. However, landfilling requires a large amount of land resources, and heavy metals are easily leached by rainwater, polluting the soil and groundwater. While solidification technology can partially reduce environmental risks, it cannot achieve resource utilization. Although industrial dust (such as steel smelting dust) has been used in the building materials industry to a small extent, the high-value utilization technology of municipal sludge incineration ash has long faced bottlenecks due to its complex composition and poor stability. There is an urgent need to develop resource conversion pathways with strong adaptability.

[0003] Industrial microcrystalline slabs are widely used in chemical equipment linings and in construction and water treatment corrosion protection due to their excellent acid and corrosion resistance. Traditional microcrystalline slab production relies on natural minerals such as quartz sand and feldspar, as well as chemical raw materials such as soda ash and sodium fluorosilicate, resulting in high production costs and resource consumption. In existing processes, 5-8% sodium fluorosilicate is often added to lower the melting temperature and introduce nucleating agents. However, excessive sodium fluorosilicate reacts with kiln refractory materials, leading to lining erosion, shortening kiln life, and generating fluorine-containing waste gas, increasing environmental treatment costs. Furthermore, existing technologies for utilizing hazardous waste are mostly limited to low-end building materials (such as cement admixtures), whose formulations are difficult to adapt to the high phosphorus and high sulfur characteristics of sludge incineration ash, easily causing uneven microcrystalline phase distribution and affecting the mechanical properties and acid resistance stability of the slabs.

[0004] Current hazardous waste resource utilization technologies have significant shortcomings: First, potential functional components such as Al2O3 and SiO2 in dust collector ash are not effectively activated and are only used as fillers, resulting in low product added value. Second, heavy metal solidification relies on physical coating rather than chemical stabilization, posing a risk of secondary release when exposed to acidic environments for extended periods. Third, phosphorus and sulfur oxides are prone to forming glassy phase defects during sintering, leading to a decrease in the acid resistance of the slabs. Meanwhile, the high addition amount of sodium fluorosilicate has long plagued the industry. While existing technologies attempt to replace some sodium fluorosilicate with borax and lithium carbonate, it is difficult to balance low-temperature sintering with material performance, and costs increase significantly. Summary of the Invention

[0005] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide an acid-resistant microcrystalline anti-corrosion board, its preparation method and application, to solve the problems in the prior art.

[0006] This invention provides an acid-resistant microcrystalline anti-corrosion board, comprising the following raw materials in parts by weight: 52-57 parts of dust collector ash, 14-15 parts of soda ash, 2-2.5 parts of sodium sulfide, 0.03-0.04 parts of silicon carbide, 0.08-0.1 parts of semi-coke powder, 1-1.5 parts of zirconium corundum brick powder, 16-18 parts of silica powder, 7-9 parts of limestone, and 2.5-3 parts of sodium fluorosilicate; wherein the dust collector ash is bag filter dust produced by sludge incineration in municipal sewage treatment plants.

[0007] The present invention also provides a method for preparing the acid-resistant microcrystalline anti-corrosion board as described above, comprising the following steps: mixing each component with hot water, extruding and granulating, melting, calendering, nucleating, crystallizing, and cooling to obtain the acid-resistant microcrystalline anti-corrosion board.

[0008] The present invention also provides the application of the acid-resistant microcrystalline anti-corrosion board described above in the lining of chemical equipment, building anti-corrosion materials and / or water treatment equipment.

[0009] The beneficial effects of the acid-resistant microcrystalline anti-corrosion board, its preparation method, and its application according to the present invention include, but are not limited to:

[0010] This invention replaces traditional mineral raw materials with baghouse dust generated from the incineration of sludge from municipal wastewater treatment plants, achieving resource utilization of hazardous waste and significantly reducing landfill pollution and disposal costs, thus possessing both environmental and economic value. Through the synergistic optimization of briquetting and crystallization annealing processes, the uniform distribution of raw material components and precise control of the microcrystalline structure are ensured, resulting in a corrosion-resistant board with excellent acid resistance. Furthermore, the product cost is significantly lower than that of traditional microcrystalline boards, providing a new material solution for the industrial corrosion protection field that combines the advantages of hazardous waste resource utilization, high performance, and low cost. Detailed Implementation

[0011] In this invention, the term "microcrystalline anti-corrosion board or microcrystalline plate or microcrystalline glass" refers to a high-strength, high-wear-resistant, and corrosion-resistant protective material and building material made by melting, rolling, nucleating, crystallizing, and annealing raw materials.

[0012] This invention provides an acid-resistant microcrystalline anti-corrosion board, comprising the following raw materials in parts by weight: 52-57 parts of dust collector ash, 14-15 parts of soda ash, 2-2.5 parts of sodium sulfide, 0.03-0.04 parts of silicon carbide, 0.08-0.1 parts of semi-coke powder, 1-1.5 parts of zirconium corundum brick powder, 16-18 parts of silica powder, 7-9 parts of limestone, and 2.5-3 parts of sodium fluorosilicate; wherein the dust collector ash is bag filter dust produced by sludge incineration in municipal sewage treatment plants.

[0013] In some embodiments, the dust is obtained by incinerating sludge, recovering it through baghouse dust collection, and then ball milling. The incineration temperature is 450℃-1000℃. More preferably, the ball milling speed is 300 r / min-500 r / min, and the milling time is 10 min-30 min. In this invention, the ash generated from the incineration of sludge from municipal wastewater treatment plants is recovered through electrostatic precipitator and baghouse dust collection. The majority of the ash is collected by electrostatic precipitator and disposed of as general solid waste. A small amount of ash, containing harmful components such as calcium hydroxide and activated carbon from the flue gas, is collected by baghouse dust collection and disposed of as hazardous waste.

[0014] In some embodiments, based on the total mass of the dust, the dust includes the following oxides in the following mass percentages: Na₂O 0.8–1.2 wt%, MgO 2.5–4 wt%, and Al₂O₃ 18–21 wt%. wt%, SiO2 30–40.5 wt%, P2O5 15–18 wt%, SO3 0.8–1.1 wt%, K2O 2.4–2.8 wt%, CaO 5–6.3 wt%, TiO2 0.6–0.8 wt%, Cr2O3 0.01–0.04 wt%, MnO 0.05–0.18 wt%, Fe2O3 5–6.5 wt%, NiO 0.01–0.03 wt%, CuO 0.06–0.10 wt%, ZnO 0.05–0.20 wt%, Rb2O 0.01–0.03 wt%, SrO 0.02–0.05 wt%, ZrO2 0.05–0.15 wt%, BaO 0.05–0.2 wt%, PbO 0.01–0.04 wt%. The content of each oxide in the dust collected in this application refers to the oxide equivalent of the corresponding element. This content was obtained by detecting the content of the corresponding element according to the "General Rules for Wavelength Dispersive X-ray Fluorescence Spectroscopy Method" (JY / T 0569-2020) and then converting it using stoichiometric relationships. It should be noted that wavelength dispersive X-ray fluorescence spectroscopy directly measures the characteristic X-ray intensity of the element. The content of elements other than oxygen is reported in the form of common oxides after conversion. This conversion result does not mean that each element in the dust collected in the dust exists entirely as an independent phase of the listed oxides. The content of each oxide can also be detected using the methods specified in GB / T 176-2025 "Chemical Analysis Methods for Cement" and GB / T4734-2022 "Chemical Analysis Methods for Daily-Use Ceramic Materials and Products". In this application, the element content was determined using the "General Rules for Wavelength Dispersive X-ray Fluorescence Spectroscopy Method" (JY / T0569-2020) and then converted. It should be understood that the above content ranges can be independently selected within their respective ranges, as long as the sum of the selected component contents is 100 wt%. Those skilled in the art can adjust the specific content of each component within the above range according to actual needs, so that the total content meets 100 wt%.

[0015] In some embodiments, the dust comprises the following oxides in weight percentages: Na₂O 1.10 wt%, MgO 3.70 wt%, Al₂O₃ 20.52 wt%, SiO₂ 40.10 wt%, P₂O₅ 17.30 wt%, SO₃ 0.96 wt%, K₂O 2.60 wt%, CaO 6.10 wt%, TiO₂ 0.74 wt%, Cr₂O₃ 0.03 wt%, MnO 0.13 wt%, Fe₂O₃ 6.10 wt%, NiO 0.02 wt%, CuO 0.08 wt%, ZnO 0.17 wt%, Rb₂O 0.02 wt%, SrO 0.04 wt%, ZrO₂ 0.10 wt%, BaO 0.16 wt%, and PbO 0.03 wt%.

[0016] In some embodiments, the dust can be in the following weight proportions: 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, or 57 parts.

[0017] In some embodiments, the density of the heavy soda ash is 1000–1200 kg / m³. 3 Soda ash is also known as baking soda, soda ash, sodium carbonate, and soda ash.

[0018] In some embodiments, the mass percentage of the soda ash can be 14 parts or 15 parts.

[0019] In some embodiments, the mass percentage of sodium sulfide can be 2 parts, 2.1 parts, 2.2 parts, 2.3 parts, 2.4 parts, or 2.5 parts. The sulfide ions provided by the sodium sulfide in this invention can also form stable sulfides with some heavy metal ions in the glass or solidify them within the glass network, reducing the risk of heavy metal leaching.

[0020] In some embodiments, the silicon carbide is a one-dimensional linear material with an aspect ratio of 10–50, a Beta (β) crystal form, a diameter of 0.1–1.0 μm, a length of 5–50 μm, and a density of 3.21 g / cm³. 3 It can be obtained through commercial channels, such as purchasing from Nanjing Jicang Nanotechnology Co., Ltd.

[0021] In some embodiments, the mass percentage of silicon carbide may be 0.03 parts or 0.04 parts.

[0022] In some embodiments, the particle size of the semi-coke powder is ≥120 mesh (particle size <0.124 mm). Semi-coke, also known as semi-coke, is a solid carbonaceous product with lower volatile matter content obtained by pyrolyzing high-volatile bituminous coal with non-caking or weak-caking properties under medium and low temperature conditions. The semi-coke powder of the present invention conforms to GB / T 25211-2023 Classification and Quality Requirements of Semi-coke Products.

[0023] In some embodiments, the mass percentage of the semi-coke powder can be 0.08 to 0.1 parts, or 0.08 parts, 0.09 parts, or 0.1 parts. In this invention, the mass percentage of the semi-coke powder cannot be too low or too high. If it is too low, it cannot achieve effective reduction; if it is too high, it will form elemental iron. During the experiment, it was found that when the amount of semi-coke powder added was 1.2 wt% (based on the total mass of all raw materials in the acid-resistant microcrystalline anti-corrosion plate), elemental iron was found at the bottom of the crucible after melting, rolling, nucleation, crystallization, and annealing.

[0024] In some embodiments, the particle size of the zirconia-alumina brick powder is ≥325 mesh (particle size ≤0.045 mm). Zirconia-alumina brick powder, also known as zirconia brick powder, is a eutectic material produced by melting alumina and zirconium oxide as main raw materials in an electric arc furnace at a high temperature above 2000℃. The Al2O3 content in the zirconia-alumina brick powder is not less than 50 wt%, such as 50 wt%, 55 wt%, or 60%, and the ZrO2 content is not less than 38 wt%, such as 38 wt%, 40 wt%, 42 wt%, or 44%, with the remainder being impurities. The zirconia-alumina brick powder is waste scrap material after use. The oxides in the zirconia-alumina brick powder of this application are obtained according to the provisions of GB / T 4734-2022 Chemical Analysis Methods for Daily-Use Ceramic Materials and Products.

[0025] In some embodiments, the mass percentage of the zirconium corundum brick powder can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, or 1.5 parts.

[0026] In some embodiments, the silica powder has a particle size ≥200 mesh (particle size ≤0.074 mm).

[0027] In some embodiments, the mass percentage of the silica powder may be 16 parts, 17 parts, or 18 parts.

[0028] In some embodiments, the mass percentage of the limestone can be 7 parts, 7.2 parts, 7.5 parts, 7.8 parts, 8 parts, 8.2 parts, 8.5 parts, 8.8 parts, or 9 parts.

[0029] In some embodiments, the mass percentage of sodium fluorosilicate can be 2.5 parts, 2.6 parts, 2.7 parts, 2.8 parts, 2.9 parts, or 3 parts. In this invention, sodium fluorosilicate introduces fluoride ions. Fluoride ions have extremely strong fluxing and surface tension-reducing effects, which can significantly lower the melting temperature under boron-free conditions and help to remove bubbles and improve the surface finish of the glass.

[0030] In some embodiments, the acid-resistant microcrystalline anti-corrosion board components by mass percentage include: 54 parts dust, 14.6 parts soda ash, 2.2 parts sodium sulfide, 0.03 parts silicon carbide, 0.09 parts semi-coke powder, 1.28 parts zirconium corundum brick powder, 17.2 parts silica powder, 7.9 parts limestone, and 2.7 parts sodium fluorosilicate.

[0031] The second aspect of this invention protects a method for preparing the acid-resistant microcrystalline anti-corrosion board as described above, comprising the following steps:

[0032] The components are mixed with hot water, extruded and granulated, melted, rolled and shaped, nucleated, crystallized and cooled to obtain the acid-resistant microcrystalline anti-corrosion board.

[0033] In some embodiments, the mass ratio of the sum of the total mass of the components to the mass of the hot water is (90-110):8, or it can be 90:8, 92:8, 95:8, 98:8, 100:8, 102:8, 105:8, 108:8, or 110:8.

[0034] In some embodiments, the temperature of the hot water is 60–70°C, or it can be 60°C, 62°C, 64°C, 68°C, or 70°C. Using hot water within the above temperature range for mixing improves the uniformity of the mixture. If cold water is used for mixing, the mixture will be uneven, which will adversely affect the subsequent melting process.

[0035] In some embodiments, the particle size after extrusion granulation is 5-8 mm, or it can be 5 mm, 6 mm, 7 mm, or 8 mm. This invention employs a pelletizing process, which significantly improves the bulk density and flowability of the raw materials, effectively avoiding component segregation and hazardous waste pollution risks caused by dust during the melting process. Simultaneously, the denser spherical structure enhances the contact area between raw material particles, promoting heat transfer efficiency during the melting stage, shortening the glass transition reaction time, and reducing energy consumption. Furthermore, the components within the spherical particles achieve microscopic uniform distribution through mechanical pressure, providing a more stable phase basis for the subsequent crystallization reaction, thereby ensuring the uniformity and reliability of the acid-resistant microcrystalline anti-corrosion performance of the sheet. Without granulation, the microcrystalline anti-corrosion sheet would have poor flowability, high hazardous waste pollution, and high reaction energy consumption.

[0036] In some embodiments, the extrusion granulation pressure is 20-25 MPa, or it can be 20 MPa, 21 MPa, 22 MPa, 23 MPa, 24 MPa, or 25 MPa.

[0037] In some embodiments, the melting temperature is not lower than 1520°C, such as 1530°C, 1540°C, 1560°C, 1580°C, or 1600°C. In this invention, melting refers to melting, decomposing, and reacting the mixed components in a high-temperature electric glass furnace to form a homogeneous, bubble-free glass melt.

[0038] In some embodiments, the melting time is 20 to 24 hours, or it can be 20 hours, 21 hours, 22 hours, 23 hours, or 24 hours.

[0039] In some embodiments, the drawing speed of the calendering process is 25–40 m / s, and the glass is calendered into a continuous glass strip with a thickness of 10–16 mm. The calendering process involves passing molten glass into the gap between one or more pairs of opposing rotating rolls in a calendering mill, where it is subjected to strong extrusion and stretching forces to be pressed into a continuous glass strip. The continuous glass strip continues to be conveyed for nucleation and crystallization.

[0040] In some embodiments, the calendering temperature is 1340–1360°C, or it can be 1340°C, 1350°C, or 1360°C.

[0041] In some embodiments, the nucleation temperature is 770–810°C, but can also be 770°C, 775°C, 780°C, 785°C, 790°C, 800°C, 805°C, or 810°C. At this nucleation temperature, a large number of extremely small crystal nuclei (such as nucleation agents induced by TiO2 or ZrO2) are uniformly precipitated inside the glass, providing growth sites for subsequent crystallization.

[0042] In some implementations, the nucleation time is 90 to 120 minutes, or it can be 90 minutes, 100 minutes, 110 minutes, or 120 minutes.

[0043] In some embodiments, the crystallization temperature is 840–860°C, or it can be 840°C, 845°C, 850°C, 855°C, or 860°C. At the crystallization temperature, the crystal nuclei formed during the nucleation stage grow sufficiently to form a large number of fine crystals. The microcrystals and the residual glass together constitute the multiphase structure of the glass-ceramic.

[0044] In some embodiments, the crystallization time is 150–180 min, or it can be 150 min, 160 min, 170 min, or 180 min. In this invention, crystallization and annealing are performed sequentially in a crystallization annealing furnace. After crystallization is completed, natural annealing is performed directly in the crystallization annealing furnace.

[0045] In some implementations, the temperature is cooled to ≤75°C.

[0046] This invention employs a semi-coke powder-silicon carbide composite reduction system, precisely suppressing SO2 generation through staged reduction control. Due to its high reactivity, semi-coke powder rapidly releases reducing gases such as CO in the early stages of melting, preferentially reacting with Fe2O3 and SO3 in the dust collector ash, promoting the reduction of Fe... 3+ Reduced to Fe 2+ It combines with S to form a stable FeS phase, suppressing the escape of S as SO2 from the source. In the later stages of melting, the semi-coke powder is almost completely consumed. At this point, silicon carbide, with its high melting point and slow oxidation characteristics, continuously releases CO gas, maintaining a weakly reducing atmosphere in the melt. This atmosphere prevents Fe from escaping. 2+ Further reduction to metallic iron can also suppress the secondary oxidation of residual sulfur. The linear structure of silicon carbide forms a spatial barrier network in the melt, slowing down the diffusion rate of reducing gases and ensuring controllable reduction intensity, thereby avoiding the risk of iron seepage caused by the accumulation of elemental iron at the bottom of the kiln. This precise atmosphere control breaks through the bottleneck of traditional technologies where it is difficult to simultaneously control sulfur to prevent the formation of sulfur dioxide gas and suppress iron to prevent the formation of elemental iron. It achieves the triple goals of environmental friendliness, production safety, and efficient resource utilization, providing a new solution for the development of high-performance building materials based on hazardous waste. In addition, silicon carbide has persistent and stable reducing properties (weak reducing properties). If coal powder is used, the reducing properties are not persistent; if graphite powder is used, the reducing properties are too strong, and the price is moderate.

[0047] The nucleating agent of this invention forms a FeS-F-Ti-P multiphase composite nucleus system through the in-situ reaction of sodium sulfide with Fe2O3, P2O5, and TiO2 in dust collector ash. During the melting stage, FeS serves as the primary nucleus substrate, and its surface adsorbs F2O3 produced by the decomposition of sodium fluorosilicate. - The ions form a fluorine-rich interface layer, significantly reducing the nucleation activation energy of silicate melts. Simultaneously, P2O5 in the dust combines with TiO2 to form a titanium phosphate microcrystalline phase, which, together with FeS, constitutes a multi-level heterogeneous nucleation network, significantly improving the crystallization rate of the microcrystalline plate and ensuring uniform grain size, thus avoiding the decline in mechanical properties caused by localized coarsening. The core elements (Fe, P, Ti) of the FeS-F-Ti-P composite nucleating agent all originate from the dust itself, solving the problem of high-phosphorus dust and enabling the full utilization of valuable elements in hazardous waste, truly achieving "waste treatment with waste."

[0048] The acid resistance of this invention stems from a multi-level synergistic mechanism of "physical densification - chemical passivation - structural stabilization": ① Physical level: A highly oriented β-wollastonite main crystalline phase and a titanium phosphate secondary crystalline phase are interwoven in the microcrystalline plate. The β-wollastonite grains are columnar, forming a through-type framework, while the titanium phosphate grains fill the gaps in the framework, together with the residual glass phase, forming a "crystal-crystal-glass" three-phase composite structure. This dense structure significantly hinders H2O. + SO4 2- This reduces the penetration path of corrosive media and decreases the diffusion rate of acid. ② Chemical level: FeS preferentially interacts with H₂. + Selective corrosion occurs, forming a dense FeSO4 passivation film whose ion-selective permeability can block H. + Further infiltration. Simultaneously, the oxidation products of FeS (Fe3O4, FeO, Fe2O3) react with PO4 in the solution. 3- (Derived from dust collector ash) combines to form an FePO4 deposit layer, repairing local micro-cracks and achieving dynamic self-healing protection, thereby improving acid corrosion resistance. ③ Composition level: F produced during the melting process of sodium fluorosilicate decomposes... - Ions partially replace the O in the silicon-oxygen network (introduced into the glass body from the dust of the raw material). 2- This forms [SiO3F]. 3- Tetrahedral structural unit. The strong electronegativity of fluorine makes the Si-F bond energy higher than that of the Si-O bond, resulting in a more compact network structure and reduced free volume. In acidic media, H... + It is difficult to attack strongly bonded fluorine-silicon networks, and F - With H + Combine to generate HF2 - Alternatively, HF can escape into the gas phase rather than remain inside the material, thus avoiding structural collapse caused by acid etching and providing sustained-release protection.

[0049] The present invention also provides the application of the acid-resistant microcrystalline anti-corrosion board described above in the lining of chemical equipment, building anti-corrosion materials and / or water treatment equipment.

[0050] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0051] Before further describing specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terminology used in the embodiments of the present invention is for describing specific embodiments and not for limiting the scope of protection of the present invention; in the specification and claims of the present invention, unless otherwise expressly stated in the text, the singular forms "a", "an" and "this" include the plural forms.

[0052] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. In addition to the specific methods, apparatus, and materials used in the embodiments, based on the knowledge of the prior art possessed by one of ordinary skill in the art and the description of this invention, any prior art methods, apparatus, and materials similar to or equivalent to those described, apparatus, and materials in the embodiments of this invention may be used to implement the present invention.

[0053] The dust used in the following examples was obtained from bag filter dust produced by incinerating sludge from a sewage treatment plant in a town in Shanghai. The dust included the following oxides by mass percentage: Na2O 1.10%, MgO 3.70%, Al2O3 20.52%, SiO2 40.10%, P2O5 17.30%, SO3 0.96%, K2O 2.60%, CaO 6.10%, TiO2 0.74%, Cr2O3 0.03%, MnO 0.13%, Fe2O3 6.10%, NiO 0.02%, CuO 0.08%, ZnO 0.17%, Rb2O 0.02%, SrO 0.04%, ZrO2 0.10%, BaO 0.16%, and PbO 0.03%. Semi-coke powder, zirconium corundum brick powder, and silicon carbide microwires were all obtained through commercial channels. The silicon carbide was purchased from Nanjing Jicang Nanotechnology Co., Ltd. The SiC nanowires (SiC short fibers or SiC whiskers) are one-dimensional wires with an aspect ratio of 10–50, a Beta (β) crystal form, a diameter of 0.1–1.0 μm, a length of 5–50 μm, and a density of 3.21 g / cm³. 3 Zirconium corundum brick powder contains the following oxides by mass percentage: Al2O3 55%, ZrO2 40%, with the balance being other unavoidable impurities.

[0054] Examples 1-6

[0055] The mass percentage (wt%) of the raw material components of the acid-resistant microcrystalline anti-corrosion boards of Examples 1-6 are shown in Table 1.

[0056] Table 1

[0057]

[0058] A method for preparing an acid-resistant microcrystalline anti-corrosion board includes the following steps:

[0059] 1) Preparation of raw materials: Weigh each raw material according to the formula by mass percentage, put them into a three-dimensional motion mixer (model CMPS-1000, purchased from Shandong KoniLer Machinery Equipment Co., Ltd.) and dry mix for 5 minutes until uniform. Then spray hot water with 8% of the total weight of the raw materials and stir continuously for 10 minutes until uniform.

[0060] 2) Pelletizing: The mixed batch material is transferred to a double roller extrusion granulator (model ZKDG-1, purchased from Henan Zhengkuang Machinery Co., Ltd.) and pressed into dense pellets with a diameter of 6mm under a pressure of 22MPa. After natural stacking and drying, the granulated material is obtained.

[0061] 3) Melting: The granulated material is evenly added to the electric glass furnace and vitrified at a temperature above 1520°C. The residence time of the raw material in the furnace is 21 hours. The qualified glass melt flows out through the outlet.

[0062] 4) Calendering: The molten glass flowing out of the outlet passes through the lip brick (a key refractory material component connecting the outlet of the melting furnace and the roll gap of the calender) and enters the calender (model YD-1400, purchased from Qingdao Yuanding Special Machinery Manufacturing Co., Ltd.), where it is calendered into a continuous glass strip with a thickness of 15mm; the temperature during calendering is 1360℃ and the drawing speed during calendering is 35m / s.

[0063] 5) Nucleation, crystallization and annealing: The rolled glass ribbon is introduced into the crystallization annealing furnace, nucleated at 770℃ for 90 min, and then crystallized at 850℃ for 160 min. After crystallization, it is annealed and cooled to ≤75℃ before exiting the crystallization annealing furnace.

[0064] 6) Cutting and Packaging: After cooling, the microcrystalline plates are cut to obtain finished products, which are then packaged and transferred to the warehouse.

[0065] Comparative Example 1

[0066] Sodium sulfide is not added. The specific formula is shown in Table 1. The preparation method is the same as in Example 1.

[0067] Comparative Example 2

[0068] Without adding silicon carbide, the specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0069] Comparative Example 3

[0070] No semi-coke powder was added. The specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0071] Comparative Example 4

[0072] Without adding zirconium corundum brick powder, the specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0073] Comparative Example 5

[0074] Sodium fluorosilicate is not added. The specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0075] Comparative Example 6

[0076] Without adding sodium sulfide and silicon carbide, the specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0077] Comparative Example 7

[0078] Without adding silicon carbide and semi-coke powder, the specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0079] Comparative Example 8

[0080] Sodium sulfide and semi-coke powder are not added. The specific formula is shown in Table 1, and the preparation method is the same as in Example 1.

[0081] Physical performance testing:

[0082] 1) Bulk density: As specified in JC / T 2097-2011 Industrial Microcrystalline Sheets.

[0083] 2) Water absorption rate: as specified in JC / T 2097-2011 Industrial Microcrystalline Sheets.

[0084] 3) Wear amount: in accordance with the provisions of "JC / T 2097-2011 Industrial Microcrystalline Sheets".

[0085] 4) Acid (alkali) resistance: in accordance with the provisions of "JC / T 2097-2011 Industrial Microcrystalline Sheets".

[0086] 5) Impact toughness: As specified in JC / T 2097-2011 Industrial Microcrystalline Sheets.

[0087] 6) Resistance to rapid cooling and heating: As specified in JC / T 2097-2011 Industrial Microcrystalline Sheets.

[0088] 7) Bending strength: As specified in JC / T 2097-2011 Industrial Microcrystalline Sheets.

[0089] The results are shown in Table 2.

[0090] Table 2

[0091]

[0092] Table 2 shows that a density of 1.84 g / cm³ was used. 3 After testing with concentrated sulfuric acid (approximately 98%), the mass loss of the microcrystalline anti-corrosion board did not exceed 1.0%; and after testing with 20% dilute sulfuric acid, the mass loss of the microcrystalline anti-corrosion board did not exceed 4.0%. This demonstrates that the microcrystalline anti-corrosion boards obtained in Examples 1-6 possess acid resistance. In contrast, Comparative Example 5 (without sodium fluorosilicate), Comparative Example 6 (without sodium sulfide and silicon carbide), Comparative Example 7 (without silicon carbide and semi-coke powder), and Comparative Example 8 (without sodium sulfide and semi-coke powder) exhibited poor acid resistance. Furthermore, the impact toughness, resistance to rapid cooling and heating, and flexural strength of the acid-resistant microcrystalline anti-corrosion boards in Examples 1-6 were significantly higher than those in Comparative Examples 1-8.

[0093] As shown in Table 2, Comparative Example 1, which does not contain sodium sulfide, suffers from a significantly reduced crystallization ability due to the excessively low sulfur content in the glass matrix. Some crystals fail to fully crystallize, resulting in substandard product quality. Comparative Example 2, which does not contain silicon carbide, exhibits a significantly decreased crystallization ability due to the difficulty in maintaining a reducing atmosphere during the later stages of glass melting. Only some crystals crystallize after initial crystallization, and a large number of sulfur bubbles appear in the acid-resistant microcrystalline anti-corrosion board, leading to substandard product quality. Furthermore, Comparative Example 6, which does not contain sodium sulfide or silicon carbide, shows decreased acid resistance, increased abrasion, reduced impact toughness, and significant declines in resistance to rapid heating and cooling, as well as flexural strength. In summary, Na₂S and SiC play irreplaceable roles in the process: Na₂S introduces an appropriate amount of sulfur into the glass and reacts in situ with Fe₂O₃, P₂O₅, and TiO₂ in the dust to form a FeS-F-Ti-P multiphase composite nucleus system, thus ensuring full crystallization of the product; SiC, on the other hand, maintains a weakly reducing atmosphere in the melt by continuously releasing CO gas in the later stages of melting; simultaneously, its linear structure forms a spatial barrier network in the glass melt, slowing down the diffusion rate of reducing gases, controlling the reduction intensity, and preventing Fe… 2+ It is further reduced to elemental iron. Furthermore, SiC inhibits the secondary oxidation of residual sulfur, ensuring the homogenization of the glass melt and the stability of its crystallization properties. Both are indispensable; the absence of either will lead to incomplete crystallization or product defects, preventing the product from meeting quality standards.

[0094] Table 2 shows that Comparative Example 3, which did not contain semi-coke powder, suffered from insufficient reducing atmosphere during the early stages of glass melting, resulting in a significant decrease in the glass's crystallization ability. Only a portion of the glass crystallized after melting, indicating that the product quality was substandard. Compared to Comparative Example 3, Comparative Example 7, which did not contain either silicon carbide or semi-coke powder, showed a wear rate of 0.275 g / cm³. 2 Significantly increased to 0.748 g / cm³ 2 Impact toughness from 1.73 kJ / m 2 Reduced to 1.35 kJ / m2 The resistance to rapid heating and cooling decreased from 82% to 62%, and the flexural strength decreased from 64.4 MPa to 53 MPa. Compared with Comparative Example 3, the abrasion loss of Comparative Example 8, which did not contain sodium sulfide and semi-coke powder, decreased from 0.275 g / cm³. 2 Significantly increased to 0.324 g / cm³ 2 Impact toughness from 1.73 kJ / m 2 Reduced to 1.56 kJ / m 2 The resistance to rapid heating and cooling decreased from 82% to 68%, and the flexural strength decreased from 64.4 MPa to 57 MPa. The results indicate that semi-coke powder is a fundamental condition for ensuring a reducing atmosphere in the early stages of melting, and its absence directly leads to insufficient crystallization ability. Based on this, SiC and Na2S further optimized product performance from two dimensions: maintaining the reducing atmosphere in the later stages and introducing sulfur to promote crystallization, respectively. These three elements work together and are indispensable; the absence of any one element will lead to a decline in product performance—the performance loss was most severe when both semi-coke powder and silicon carbide (Comparative Example 7) were simultaneously absent, indicating that they have a synergistic effect in ensuring sufficient crystallization and product densification.

[0095] As shown in Table 2, the acid (alkali) resistance of the acid-resistant microcrystalline anti-corrosion board in Comparative Example 4, which does not contain zirconium corundum brick powder, is significantly reduced, indicating that the product quality is unqualified.

[0096] As shown in Table 2, in Comparative Example 5, which does not contain sodium fluorosilicate, the absence of F element in the glass matrix significantly reduces the crystallization ability of the acid-resistant microcrystalline anti-corrosion board. The fact that only a portion of the crystals crystallizes after crystallization indicates that the product quality is substandard.

[0097] Furthermore, the acid-resistant microcrystalline anti-corrosion plate of the present invention meets the requirements of 5.1.2 acid loss rate in GB 41015-2021 Technical Requirements for Vitrification Products of Solid Waste, which is no more than 3%; and the requirements of "Table 1 Limits on the Content of Hazardous Substances in Water Leaching and Acid Leaching of Vitrified Products" in 5.3.2, which meet the requirements of Table 1.

[0098] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. An acid-resistant microcrystalline anti-corrosion board, characterized in that, It comprises the following raw materials in parts by weight: 52-57 parts dust collector ash, 14-15 parts soda ash, 2-2.5 parts sodium sulfide, 0.03-0.04 parts silicon carbide, 0.08-0.1 parts semi-coke powder, 1-1.5 parts zirconium corundum brick powder, 16-18 parts silica powder, 7-9 parts limestone, and 2.5-3 parts sodium fluorosilicate; wherein the dust collector ash is bag filter dust produced by sludge incineration in municipal sewage treatment plants; Based on the total mass of the dust collector, the dust collector comprises the following oxides in the following mass percentages: Na₂O 0.8–1.2 wt%, MgO 2.5–4 wt%, Al₂O₃ 18–21 wt%, SiO₂ 30–40.5 wt%, P₂O₅ 15–18 wt%, SO₃ 0.8–1.1 wt%, K₂O 2.4–2.8 wt%, CaO 5–6.3 wt%, TiO₂ 0.6–0.8 wt%, Cr₂O₃ 0.01–0.04 wt%, MnO The total mass percentages of the oxides are 0.05–0.18 wt%, Fe2O3 is 5–6.5 wt%, NiO is 0.01–0.03 wt%, CuO is 0.06–0.10 wt%, ZnO is 0.05–0.20 wt%, Rb2O is 0.01–0.03 wt%, SrO is 0.02–0.05 wt%, ZrO2 is 0.05–0.15 wt%, BaO is 0.05–0.2 wt%, and PbO is 0.01–0.04 wt%, with the sum of the mass percentages of each oxide being 100 wt%.

2. The acid-resistant microcrystalline anti-corrosion board as described in claim 1, characterized in that, The silicon carbide is a one-dimensional linear material with an aspect ratio of 10 to 50 and a β-crystal form.

3. The acid-resistant microcrystalline anti-corrosion board as described in claim 1, characterized in that, The zirconium corundum brick powder contains no less than 50 wt% Al2O3 and no less than 38 wt% ZrO2. And / or, the soda ash is heavy soda ash.

4. The acid-resistant microcrystalline anti-corrosion board as described in claim 1, characterized in that, The particle size of the semi-coke powder is ≥120 mesh; And / or, the particle size of the zirconium corundum brick powder is ≥325 mesh; And / or, the particle size of the silica powder is ≥200 mesh.

5. The method for preparing the acid-resistant microcrystalline anti-corrosion board according to any one of claims 1-4, characterized in that, Includes the following steps: The components are mixed with hot water, extruded and granulated, melted, rolled and shaped, nucleated, crystallized and cooled to obtain the acid-resistant microcrystalline anti-corrosion board.

6. The preparation method according to claim 5, characterized in that, The ratio of the total mass of the components to the mass of the hot water is (90-110):8; And / or, the temperature of the hot water is 60–70°C; And / or, the particle size after extrusion granulation is 5-8 mm; And / or, the pressure of extrusion granulation is 20-25 MPa.

7. The preparation method according to claim 5, characterized in that, The melting temperature shall not be lower than 1520℃; And / or, the melting time is 20–24 hours; And / or, the drawing speed for calendering is 25–40 m / s; And / or, the calendering temperature is 1340~1360℃.

8. The preparation method according to claim 5, characterized in that, The nucleation temperature is 770–810℃; And / or, the nucleation time is 90–120 min; And / or, the crystallization temperature is 840–860℃; And / or, the crystallization time is 150–180 min; And / or, cool to a temperature ≤75°C.

9. The application of the acid-resistant microcrystalline anti-corrosion board as described in any one of claims 1-4 in the lining of chemical equipment, building anti-corrosion materials and / or water treatment equipment.

Citation Information

Patent Citations

  • Microcrystal plate produced based on hazardous waste incineration ash and melting process thereof

    CN119912161A

  • High-gloss black decorative glass prepared from sludge incineration ash through all-electric melting method and method

    CN120483523A