AI Technical Summary
[0006]本发明提供了一种脱硝催化剂载体钛钼粉的制备方法,旨在解决现有技术中钼含量精确控制困难、高温煅烧过程中钼损失严重、产物孔结构不适合脱硝催化需求以及批次一致性差等关键技术问题
[0032]第一,钼保留率高。由于采用中低温反应和配位锚定技术,钼在煅烧过程中的升华和损失得到有效抑制,钼保留率可达98%以上,远高于现有技术中喷雾干燥高温煅烧工艺的钼保留率。这使得最终产品中MoO3含量能够精确控制在目标范围内,满足脱硝催化剂对活性组分负载量的严格要求。
Smart Images

Figure CN122894977A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst support material preparation technology, specifically a method for preparing titanium-molybdenum powder as a denitrification catalyst support. Background Technology
[0002] SCR (Selective Catalytic Reduction) denitrification technology is currently the mainstream technology for controlling nitrogen oxides in coal-fired power plants. Titanium-molybdenum based catalyst supports are widely used due to their excellent resistance to sulfur poisoning, good catalytic activity, and stability. Titanium-molybdenum powder is a key support material for SCR denitrification catalysts, with molybdenum oxide playing a crucial role in anchoring active components, stabilizing crystal structure, and improving resistance to poisoning. However, existing methods for preparing titanium-molybdenum powder have significant shortcomings, affecting the performance and industrial application of denitrification catalysts.
[0003] A search revealed the patent CN107737588A (published on February 27, 2018) entitled "A Denitrification Catalyst". The patent discloses a denitrification catalyst whose raw materials, by weight, are 35-45 parts titanium dioxide, 2-5 parts antimony oxide, 10-20 parts glass fiber, 1-3 parts vanadium pentoxide, 3-6 parts molybdenum oxide, and 3-6 parts tungsten oxide. However, this technical solution has the following shortcomings: First, the method focuses on the formulation design of the finished catalyst, directly molding the mixture of components such as titanium dioxide and molybdenum oxide without involving the preparation process of a special titanium-molybdenum powder carrier material, thus failing to achieve precise control over the phase structure, particle size distribution, and dispersibility of the titanium-molybdenum powder itself; Second, the method uses a traditional mixed extrusion process, where the molybdenum source is prone to migration and aggregation during high-temperature calcination, resulting in uneven distribution of active components in the catalyst and affecting catalytic efficiency; Third, this patent does not optimize key properties such as the pore structure and specific surface area of the denitrification catalyst carrier, resulting in a low specific surface area of the prepared catalyst carrier, which is not conducive to the full dispersion and loading of active components.
[0004] A search revealed the patent CN103638980A (published on March 19, 2014), entitled "A Denitrification Catalyst." This patent discloses a denitrification catalyst prepared from the following components in the indicated weight fractions: 25-35 parts molybdenum trioxide; 10-18 parts tungsten trioxide; 55-80 parts titanium dioxide; 2-5 parts vanadium pentoxide; 6-17 parts limestone; 2.5-6 parts stearic acid; 2.5-3 parts glass powder; 3.5-5 parts inorganic silica gel; 2.5-3.5 parts polyethylene; and 0.5-1.5 parts paraffin wax. However, this technical solution has the following shortcomings when used as a denitrification catalyst support: First, this method also focuses on the overall formulation design of the finished catalyst, directly mixing molybdenum trioxide as an additive into the catalyst components, rather than specifically preparing high-performance titanium-molybdenum powder support materials, thus lacking precise control over the morphology and dispersion state of molybdenum in the TiO2 support; Second, this method uses a conventional mixed extrusion molding process, during which molybdenum trioxide is prone to sublimation and crystal growth, reducing the thermal stability and service life of the catalyst; Third, this technical solution does not consider the optimization of the pore structure and the distribution of acidic sites required for the denitrification catalyst, and cannot meet the specific requirements of SCR denitrification catalysts for support performance, resulting in limited pore volume and specific surface area of the prepared catalyst support, which affects the further improvement of catalytic activity.
[0005] The aforementioned problems indicate that existing molybdenum-containing denitrification catalyst preparation technologies suffer from shortcomings such as the lack of titanium-molybdenum powder preparation processes, difficulty in precisely controlling molybdenum content, insufficient high-temperature stability, and unsuitable product pore structures for denitrification catalysis requirements. Therefore, this invention provides a method for preparing titanium-molybdenum powder specifically for SCR denitrification catalyst supports, aiming to solve key technical problems such as precise control of molybdenum content, product consistency, and catalytic activity, thereby meeting the urgent demand of the denitrification catalyst industry for high-performance titanium-molybdenum powder support materials. Summary of the Invention
[0006] This invention provides a method for preparing titanium-molybdenum powder as a denitrification catalyst support, aiming to solve key technical problems in existing technologies such as difficulty in accurately controlling molybdenum content, severe molybdenum loss during high-temperature calcination, unsuitable product pore structure for denitrification catalysis requirements, and poor batch-to-batch consistency. This invention utilizes the acidic properties of metatitanic acid and the weakly basic properties of ammonium heptamolybdate to conduct a neutralization and coordination reaction under medium-to-low temperature conditions, allowing molybdenum to be uniformly dispersed in the titanium precursor in a coordinated form. Subsequently, calcination at a suitable temperature chemically anchors molybdenum to the surface or subsurface of the TiO2 lattice in the form of MoO3, forming a stable Ti-O-Mo chemical bond structure, thereby preparing a high-performance titanium-molybdenum powder support material suitable for SCR denitrification catalysts.
[0007] In a first aspect, the present invention provides a method for preparing titanium-molybdenum powder as a denitrification catalyst support, comprising the following steps:
[0008] S10: Raw material preparation steps: Take metatitanic acid slurry or filter cake, wherein the metatitanic acid is calculated as TiO2 and the solid content of TiO2 is 10% to 35% by weight; Separately, take ammonium heptamolybdate and dissolve it in deionized water to prepare a solution with a molybdenum concentration of 5% to 20% by weight.
[0009] S20: Reactive mixing step. Calculate the amount of ammonium heptamolybdate based on the MoO3 content in the final titanium-molybdenum powder being 3% to 12% by weight. Under stirring conditions, slowly add the ammonium heptamolybdate solution to the metatitanic acid slurry. Metatitanic acid is acidic with a pH of 1.0 to 2.5, while the ammonium heptamolybdate solution is weakly alkaline. The two undergo neutralization and coordination reactions to generate a uniform molybdenum-titanium precursor precipitate or gel. Control the reaction temperature to 40°C to 80°C and the reaction time to 0.5 hours to 2 hours.
[0010] S30: Drying step, drying the reaction material at 100℃ to 150℃ until the moisture content is less than 10% by weight, to obtain dry material;
[0011] S40: Calcination step, the dry material is calcined at 350℃ to 550℃ for 2 to 5 hours to convert metatitanic acid into anatase TiO2, while molybdenum is highly dispersed in the form of MoO3 and chemically anchored to the surface or subsurface of the TiO2 lattice to obtain titanium molybdenum powder.
[0012] According to the present invention, by reacting metatitanic acid (TiO2·nH2O) with ammonium heptamolybdate ((NH4)6Mo7O) 24 Neutralization and coordination reactions between the two: Under acidic conditions (pH = 1.0-2.5), the Ti-OH groups on the surface of metatitanic acid react with the Mo7O groups released from the dissociation of ammonium heptamolybdate. 24 6- The molybdenum oxide anion undergoes a coordination reaction to form a Ti-Mo-O complex intermediate; during subsequent calcination, Ti-OH in this intermediate is converted into anatase TiO2, while Mo7O... 24 6- The molybdenum is oxidized and decomposed into MoO3, which forms Ti-O-Mo coordination bonds with the TiO2 surface, achieving chemical anchoring. During subsequent calcination, the coordinated molybdenum is converted to MoO3 and forms Ti-O-Mo chemical bonds with the TiO2 surface, achieving chemical anchoring of molybdenum on the TiO2 support. This chemical bonding structure effectively inhibits the sublimation and migration of molybdenum during high-temperature calcination, significantly improving molybdenum retention. Simultaneously, it allows MoO3 to exist in a highly dispersed state on or subsurface of TiO2, forming numerous acidic and active sites, thus endowing the titanium-molybdenum powder with excellent catalytic performance.
[0013] Furthermore, in step S20, the Ti-OH groups on the surface of metatitanic acid react with the molybdenum oxide anions (mainly Mo7O) dissociated from ammonium heptamolybdate. 246- (Depending on pH and concentration) the following coordination reaction occurs: Ti-OH + H+ + + [Mo7O 24 ] 6- → Ti-O-Mo (coordination precursor) + H₂O. Under acidic conditions (pH 1.0-2.5), the molybdenum oxide anion is protonated, enhancing its electrophilicity and facilitating condensation coordination with the oxygen atoms of Ti-OH, forming a three-dimensional network structure with Ti-O-Mo bonds. This precursor is an amorphous gel or precipitate, in which Mo and Ti are linked by chemical bonds at the atomic scale.
[0014] Further, in step S40, the final formation of the Ti-O-Mo chemical bond depends on dehydration condensation during drying and calcination. During drying at 100-150℃, coordinated water and physically adsorbed water are gradually removed, and the Ti-O-Mo bond further condenses. During calcination at 350-550℃, residual organic ligands and hydroxyl groups in the precursor undergo oxidative decomposition, and metatitanic acid dehydrates and transforms into anatase TiO2. Simultaneously, Mo species are retained in the form of MoO3 and anchored to the TiO2 surface or subsurface through the original Ti-O-Mo bonds. X-ray photoelectron spectroscopy (XPS) analysis shows that the binding energy of Mo 3d is located at 232.5-233.5 eV, consistent with the standard value of MoO3, and there is no low-valence Mo peak, indicating that Mo exists in the +6 valence state. Raman spectroscopy analysis shows that the binding energy of Mo 3d is located at 950-980 cm⁻¹. -1 Characteristic vibrational peaks attributable to Mo-O-Ti bridging bonds were observed at [location], while only the independent Raman peak of MoO3 (approximately 820 cm⁻¹) was observed in the physically mixed sample. -1 and 994 cm -1 This proves that Mo exists in a chemically bonded rather than physically adsorbed form.
[0015] In some embodiments, the TiO2 solid content of the metatitanic acid slurry or filter cake in step S10 is preferably 15 to 30% by weight, more preferably 20 to 28% by weight. By controlling the solid content of metatitanic acid, the viscosity of the reaction system can be adjusted, which is beneficial to the dispersion and mixing of the ammonium heptamolybdate solution, while ensuring that the reaction system has a suitable solid content, providing a good foundation for subsequent drying and calcination.
[0016] In some embodiments, the molybdenum concentration of the ammonium heptamolybdate solution in step S10 is preferably 8 to 15% by weight, more preferably 10 to 12% by weight. Too low a solution concentration will result in an excessively large reaction volume and reduced production efficiency; too high a solution concentration may lead to insufficient dissolution of ammonium heptamolybdate, affecting the uniformity of the reaction.
[0017] In some embodiments, the MoO3 content in the final titanium-molybdenum powder in step S20 is preferably 5% to 10% by weight, and more preferably 6% to 8% by weight. If the MoO3 content is too low, it cannot provide sufficient acidic sites and active sites, affecting the activity of the denitration catalyst; if the MoO3 content is too high, it is easy for MoO3 to aggregate on the TiO2 surface, reducing the dispersion, and may also block the pores of the support, affecting the mass transfer efficiency.
[0018] In some embodiments, the pH of the metatitanic acid slurry in step S20 is 1.0 to 2.5, preferably 1.2 to 2.0, and more preferably 1.5 to 1.8. The acidic environment of metatitanic acid is conducive to the coordination reaction between the molybdenum oxide anion in ammonium heptamolybdate and titanium species, forming a uniform molybdenum-titanium complex. When the pH is below 1.0, the molybdenum oxide anion is excessively protonated to form molybdate precipitate, losing its coordination activity; when the pH is above 2.5, the degree of polymerization of the molybdenum oxide anion decreases, and its coordination ability with Ti-OH is weakened, resulting in uneven Mo distribution. Therefore, the determination of the pH range is based on the balance between the existing form and coordination activity of the molybdenum oxide anion.
[0019] In some embodiments, the reaction temperature in step S20 is preferably 50°C to 70°C, more preferably 55°C to 65°C. The reaction temperature affects the coordination reaction rate and the formation rate of the precursor network. Below 40°C, the reaction rate is too slow, and Ti-O-Mo bond formation is insufficient; above 80°C, ammonium heptamolybdate may undergo thermal decomposition, and the precursor gel network shrinks too quickly, leading to premature aggregation of Mo species. The preferred temperature range of this invention was determined through kinetic experiments; within this range, the reaction can be completed within 0.5-2 hours, and the product has the highest specific surface area.
[0020] In some embodiments, the reaction time in step S20 is preferably 0.8 hours to 1.5 hours, more preferably 1 hour to 1.2 hours. The choice of reaction time is based on the time required for the precursor gel network to reach a balanced structure. If the reaction time is too short, the coordination will be insufficient, and if it is too long, the network may be over-crosslinked, affecting the subsequent pore structure.
[0021] In some embodiments, the ammonium heptamolybdate solution in step S20 is added slowly, with the addition rate controlled at 0.5 mL to 5 mL per second, preferably 1 mL to 3 mL per second. Slow addition helps maintain the pH stability of the reaction system, allowing the molybdenum oxide anions to fully coordinate with the titanium species, forming a uniform precursor precipitate or gel. If the addition rate is too fast, it may lead to excessively high local pH, causing rapid hydrolysis and aggregation of molybdate ions.
[0022] In some embodiments, the drying temperature in step S30 is preferably 110°C to 140°C, more preferably 120°C to 130°C. The selection of the drying temperature is based on the water removal kinetics in the precursor and the degree of condensation of the Ti-O-Mo bonds: if the temperature is too low (<100°C), dehydration will be incomplete, and the rapid release of water vapor during subsequent calcination will cause the powder to crack; if the temperature is too high (>150°C), the Mo species in the precursor may be prematurely oxidized or migrated, affecting the final dispersion. The moisture content of the dried material is preferably less than 8% by weight, more preferably less than 5% by weight.
[0023] In some embodiments, the calcination temperature in step S40 is preferably 450°C to 500°C, and more preferably 460°C to 480°C. The selection of the calcination temperature is based on the crystallization temperature of anatase TiO2 and the sublimation temperature of MoO3. The anatase phase begins to form above 350°C, and crystallization tends to be complete around 500°C; however, when the temperature exceeds 550°C, anatase begins to transform into the rutile phase, and the chemical anchoring state of MoO3 (sublimation point about 795°C) on the TiO2 surface may be destroyed, leading to Mo migration and volatilization. Therefore, the 350-550°C range ensures both controllable transformation of the TiO2 crystal form and avoids significant loss of Mo, with 450-500°C being the optimal equilibrium range.
[0024] In some embodiments, the calcination time in step S40 is preferably 2.5 hours to 4 hours, more preferably 3 hours to 3.5 hours. The calcination time should ensure complete decomposition of the precursor and sufficient crystallization of TiO2, but too long a time will lead to grain growth and a decrease in specific surface area. Therefore, the time range is determined based on thermogravimetric analysis and specific surface area change curves.
[0025] In some embodiments, the calcination process in step S40 is carried out in an air atmosphere, preferably in a tube furnace or box furnace for batch calcination, with a heating rate of 2°C / min to 10°C / min, preferably 3°C / min to 5°C / min. Slow heating is beneficial to the thermal decomposition and phase transformation of the precursor, and reduces powder pulverization and molybdenum loss caused by rapid heating.
[0026] In some preferred embodiments, the present invention further includes step S25, which involves aging the generated molybdenum-titanium precursor precipitate or gel after the reactive mixing step. The aging temperature is 20°C to 40°C, and the aging time is 1 to 4 hours. During this process, residual coordinated water molecules in the precursor network are further removed, and the Ti-O-Mo bonds undergo condensation and ripening, resulting in a denser and more uniform three-dimensional network structure. Compared with the untreated product, the BET specific surface area of the aged sample increases by 5%-15%, and the molybdenum retention rate increases by 1-2 percentage points. The selection of aging temperature and time is based on the following: if the temperature is too low, the ripening rate is slow, and the time needs to be extended; if the temperature is too high, the precursor may dehydrate and crack prematurely, affecting uniformity. The aging treatment can further ripen the molybdenum-titanium complex, forming a more uniform and stable network structure, which is beneficial to the uniform formation of Ti-O-Mo chemical bonds during subsequent calcination.
[0027] In some preferred embodiments, the present invention further includes step S35, which involves pulverizing the dry material after the drying step and before the calcination step to a particle size of less than 100 micrometers, preferably less than 50 micrometers. Pulverization increases the specific surface area of the material, which is beneficial for heat transfer and uniform reaction during subsequent calcination, while also improving the dispersibility of the final titanium-molybdenum powder.
[0028] In some preferred embodiments, the present invention employs a segmented calcination process in the calcination step. The first stage involves holding the calcined product at 200°C to 300°C for 0.5 to 1.5 hours, and the second stage involves holding it at 350°C to 550°C for 2 to 5 hours. The first stage of low-temperature calcination is used to remove residual water of crystallization and organic impurities from the precursor, preventing powder cracking and Mo species migration caused by rapid heating. The second stage of high-temperature calcination is used to achieve the phase transformation from metatitanic acid to anatase TiO2 and the chemical anchoring of MoO3. Compared with direct heating calcination, segmented calcination can increase the specific surface area of the product by 10-20 m². 2 / g, with a more concentrated pore size distribution and an increase in molybdenum retention of approximately 2-3 percentage points. The selection of the two temperature stages is based on the following: the first stage, below 300℃, avoids premature oxidation and migration of Mo species; the second stage is determined according to the TiO2 crystal transformation temperature (anatase formation temperature, approximately 350-550℃). Staged calcination allows the organic components and water of crystallization in the precursor to gradually decompose and release, reducing powder pulverization caused by rapid decomposition, while also promoting uniform dispersion and chemical anchoring of MoO3.
[0029] According to the present invention, the prepared titanium-molybdenum powder has the following characteristics: a MoO3 content of 3% to 12% by weight, a specific surface area of 50 m² / g to 150 m² / g, a pore volume of 0.2 mL / g to 0.6 mL / g, an average pore size of 5 nm to 20 nm, and a molybdenum retention rate of ≥98% by weight. The molybdenum in the titanium-molybdenum powder exists in the form of highly dispersed MoO3 and is anchored to the TiO2 surface or subsurface through Ti-O-Mo chemical bonds, forming a stable chemical bond.
[0030] The core technical mechanism of this invention lies in the fact that: the surface of metatitanic acid (TiO2·nH2O) contains a large number of active Ti-OH groups, which are electropositive in acidic aqueous solutions; ammonium heptamolybdate dissociates into negatively charged molybdenum oxide anions (such as Mo7O) after dissolving in water. 24 6- Mo8O 26 4- (The specific morphology depends on pH and concentration). When the two are mixed, electrostatic attraction and coordination jointly drive the condensation reaction between molybdenum oxide anions and Ti-OH, generating Ti-O-Mo coordination bonds, thus forming a chemically homogeneous molybdenum-titanium precursor gel. During the subsequent drying process, coordination water and physical water are removed, and the Ti-O-Mo bonds further condense; during calcination, the precursor decomposes, metatitanic acid is converted into anatase TiO2, while Mo species are retained in the form of MoO3 and anchored to the TiO2 surface through the original Ti-O-Mo bonds. This chemically anchored structure is quantified by XPS (Mo 3d binding energy 232.5-233.5 eV) and Raman spectroscopy (Mo-O-Ti vibration peak approximately 950-980 cm⁻¹). -1 This was confirmed, in stark contrast to the phase separation characteristics of physically mixed samples.
[0031] Compared with the prior art, the present invention has the following significant advantages:
[0032] First, the molybdenum retention rate is high. Due to the use of medium- and low-temperature reaction and coordination anchoring technology, the sublimation and loss of molybdenum during calcination are effectively suppressed, achieving a molybdenum retention rate of over 98%, far exceeding the molybdenum retention rate of the existing spray drying high-temperature calcination process. This allows the MoO3 content in the final product to be precisely controlled within the target range, meeting the stringent requirements of the denitrification catalyst for the loading of active components.
[0033] Second, the product exhibits good consistency. Through a reactive mixing process, molybdenum achieves uniform molecular-level dispersion in the titanium precursor, and the subsequent drying and calcination process parameters are stable and controllable. Therefore, the consistency between different batches of products is good, which is beneficial for large-scale industrial production.
[0034] Third, it exhibits excellent catalytic activity. Molybdenum is chemically anchored to the surface or subsurface of TiO2 in a highly dispersed state, forming numerous Ti-O-Mo active sites. These active sites provide acidic sites, promoting the adsorption and activation of NH3, while simultaneously enhancing the catalyst's resistance to sulfur poisoning and K2O poisoning. Compared to titanium-molybdenum powder prepared by traditional physical mixing methods, the titanium-molybdenum powder prepared in this invention shows a significant improvement in NOx conversion.
[0035] Fourth, the pore structure is suitable for denitrification catalysis. By controlling the reaction and calcination process parameters, the specific surface area, pore volume, and pore size distribution of titanium-molybdenum powder can be adjusted to suit the pore structure requirements of the support for SCR denitrification catalysts, which is beneficial for the diffusion and mass transfer of reactant gases.
[0036] In a second aspect, the present invention provides a titanium-molybdenum powder as a denitrification catalyst support, which is prepared according to the preparation method described in any embodiment of the first aspect.
[0037] According to the present invention, this titanium-molybdenum powder, when used as a support material for SCR denitrification catalysts, provides excellent catalytic performance. Because molybdenum is highly dispersed on the TiO2 support surface in a chemically anchored form, it forms numerous acidic and active sites. These sites effectively promote the adsorption and activation of NH3 on the catalyst surface, improving NOx conversion efficiency. Simultaneously, the presence of Ti-O-Mo chemical bonds enhances the catalyst's thermal stability and resistance to poisoning, extending its service life.
[0038] In some embodiments, the NOx conversion rate of the titanium-molybdenum powder is greater than or equal to 85% in the range of 350°C to 450°C, preferably greater than or equal to 90%. In some preferred embodiments, the activity retention rate of the titanium-molybdenum powder after K2O poisoning test is greater than or equal to 70%, preferably greater than or equal to 75%. This indicates that the titanium-molybdenum powder prepared by the present invention has good resistance to alkali metal poisoning and can maintain stable catalytic performance in the complex flue gas environment of coal-fired power plants.
[0039] In some embodiments, the titanium-molybdenum powder has a BET specific surface area of 80 m² / g to 120 m² / g, a pore volume of 0.3 mL / g to 0.5 mL / g, and an average pore size of 8 nm to 15 nm. This pore structure facilitates the diffusion and mass transfer of reactant gases within the catalyst support, while providing a sufficiently large specific surface area for the dispersion and loading of the active components.
[0040] In some embodiments, the particle size distribution of the titanium-molybdenum powder is D50 = 1 micrometer to 10 micrometers, and D90 ≤ 30 micrometers. A suitable particle size distribution ensures the molding performance and packing density of the titanium-molybdenum powder in subsequent catalyst preparation processes, while also facilitating the uniform loading of the active component on the support surface.
[0041] Thirdly, the present invention provides the application of the above-mentioned titanium-molybdenum powder in the preparation of SCR denitration catalyst, including mixing titanium-molybdenum powder with active components, molding and calcining to obtain SCR denitration catalyst.
[0042] According to the present invention, the titanium-molybdenum powder prepared by the present invention is used as a carrier material and mixed with active components such as vanadium pentoxide. A catalyst carrier is prepared by extrusion molding or coating process, followed by low-temperature drying and high-temperature calcination to obtain a complete SCR denitrification catalyst. This catalyst has the characteristics of high activity, good selectivity, excellent thermal stability, and strong resistance to poisoning, and is suitable for flue gas denitrification in coal-fired power plants, industrial boilers, and other fields.
[0043] In some embodiments, the method for preparing SCR denitration catalyst using the titanium-molybdenum powder includes the following steps: mixing titanium-molybdenum powder with active components such as vanadium pentoxide source and tungsten source, adding binder and pore-forming agent, mixing evenly and then extruding to obtain catalyst support; drying the catalyst support at 100°C to 150°C for 2 to 4 hours, and then calcining it at 400°C to 500°C for 3 to 5 hours to obtain SCR denitration catalyst.
[0044] In some embodiments, the loading of vanadium pentoxide, the active component of the SCR denitrification catalyst, is from 1 wt% to 5 wt%, preferably from 2 wt% to 4 wt%. The loading of the tungsten source, calculated as WO3, is from 3 wt% to 10 wt%, preferably from 5 wt% to 8 wt%. The loading of the active component should be optimized and adjusted according to specific operating conditions and denitrification requirements.
[0045] Compared with the prior art, the present invention has outstanding substantive features and significant progress, specifically reflected in:
[0046] First, this invention achieves molecular-level mixing and chemical bonding of molybdenum and titanium through a reactive mixing process, which is fundamentally different from existing technologies. Existing technologies, such as CN108910951B, employ a spray drying high-temperature thermal decomposition process, where the molybdenum source is prone to sublimation and decomposition at high temperatures, resulting in a high molybdenum loss rate and failing to achieve chemical bonding. In contrast, this invention utilizes the neutralization and coordination reaction between metatitanic acid and ammonium heptamolybdate to form Ti-O-Mo chemical bonds under medium- and low-temperature conditions, achieving a molybdenum retention rate of over 98%.
[0047] Secondly, this invention optimizes the pore structure of the denitration catalyst support. By controlling the reaction and calcination process parameters, a titanium-molybdenum powder support with suitable specific surface area, pore volume, and pore size distribution can be prepared, meeting the specific requirements of SCR denitration catalysts for the support pore structure and facilitating the diffusion and mass transfer of reactant gases.
[0048] Furthermore, this invention improves product consistency. Due to the use of a reactive mixing process, molybdenum is uniformly dispersed in the titanium precursor, and subsequent process parameters are stable and controllable. Therefore, the consistency between different batches of products is good, which is beneficial for large-scale industrial production.
[0049] Finally, the titanium-molybdenum powder prepared by this invention exhibits excellent catalytic performance. Molybdenum is highly dispersed on the TiO2 surface in a chemically anchored form, forming a large number of active sites, which endows the catalyst with high activity, good selectivity, and excellent resistance to poisoning, enabling it to maintain stable denitrification performance in complex flue gas environments. Attached Figure Description
[0050] Figure 1 This is a flowchart of the preparation method of the present invention. Detailed Implementation
[0051] The various embodiments or implementation schemes in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments.
[0052] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with an embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0053] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0054] As described in the background section, the preparation of titanium-molybdenum powder as a carrier for SCR denitration catalysts currently mainly adopts a spray drying high-temperature thermal decomposition process. This process has the following technical problems: it is difficult to accurately control the molybdenum content; during the spray drying process, the molybdenum source and the titanium source can only achieve physical mixing and cannot form chemical bonds; the sublimation and migration of molybdenum during high-temperature calcination leads to a high molybdenum loss rate, usually between 15% and 25%; the pore structure of the product is not suitable for denitration catalysis requirements, with low specific surface area and pore volume; and the consistency between different batches of products is poor, which is not conducive to large-scale industrial production.
[0055] Based on this, the present invention provides a method for preparing titanium-molybdenum powder as a denitrification catalyst support. By utilizing the acidic properties of metatitanic acid and the weakly basic properties of ammonium heptamolybdate, a neutralization and coordination reaction is carried out under medium and low temperature conditions, so that molybdenum is uniformly dispersed in the titanium precursor in a coordinated form. Subsequently, calcination is carried out at a moderate temperature, so that molybdenum is chemically anchored to the surface or subsurface of TiO2 in the form of MoO3, forming a stable Ti-O-Mo chemical bond structure.
[0056] In a first aspect, the present invention provides a method for preparing titanium-molybdenum powder as a denitrification catalyst support, comprising the following steps:
[0057] S10: Raw material preparation steps: Take metatitanic acid slurry or filter cake, wherein the metatitanic acid is calculated as TiO2 and the solid content of TiO2 is 10% to 35% by weight; Separately, take ammonium heptamolybdate and dissolve it in deionized water to prepare a solution with a molybdenum concentration of 5% to 20% by weight.
[0058] S20: Reactive mixing step. Calculate the amount of ammonium heptamolybdate based on the MoO3 content in the final titanium-molybdenum powder being 3% to 12% by weight. Under stirring conditions, slowly add the ammonium heptamolybdate solution to the metatitanic acid slurry. Metatitanic acid is acidic with a pH of 1.0 to 2.5, while the ammonium heptamolybdate solution is weakly alkaline. The two undergo neutralization and coordination reactions to generate a uniform molybdenum-titanium precursor precipitate or gel. Control the reaction temperature to 40°C to 80°C and the reaction time to 0.5 hours to 2 hours.
[0059] S30: Drying step, drying the reaction material at 100℃ to 150℃ until the moisture content is less than 10% by weight, to obtain dry material;
[0060] S40: Calcination step, the dry material is calcined at 350℃ to 550℃ for 2 to 5 hours to convert metatitanic acid into anatase TiO2, while molybdenum is highly dispersed in the form of MoO3 and chemically anchored to the surface or subsurface of the TiO2 lattice to obtain titanium molybdenum powder.
[0061] The technical solution of the present invention will be described in detail below through specific embodiments. It should be noted that the process parameters in Embodiments 1-7 are systematically selected within the scope of the claims, in order to demonstrate the influence of different parameter combinations on product performance and to provide experimental basis for determining the optimal parameters.
[0062] Example 1
[0063] This embodiment provides a method for preparing titanium-molybdenum powder as a denitrification catalyst support, specifically including the following steps:
[0064] Step S10: Raw material preparation. Take metatitanic acid slurry, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 20% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 10% by weight.
[0065] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 6% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 2 ml per second. The initial pH of the metatitanic acid slurry is 1.5, and the ammonium heptamolybdate solution is weakly alkaline, resulting in neutralization and coordination reactions between the two. Control the reaction temperature at 60°C and the reaction time at 1 hour to generate a uniform molybdenum-titanium precursor precipitate or gel.
[0066] Step S30: Drying. The reacted material is dried at 120°C until the moisture content is less than 8% by weight to obtain dry material.
[0067] Step S40: Calcination. The dry material is calcined at 470°C for 3 hours to convert metatitanic acid into anatase TiO2. At the same time, molybdenum is highly dispersed in the form of MoO3 and chemically anchored to the surface or subsurface of the TiO2 lattice to obtain titanium molybdenum powder.
[0068] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content is 6.1% by weight, BET specific surface area is 95 square meters per gram, pore volume is 0.38 ml per gram, average pore size is 12 nanometers, and molybdenum retention rate is 98.5% by weight.
[0069] Example 2
[0070] The difference between this embodiment and Embodiment 1 is that the specific process parameters have been optimized and adjusted.
[0071] Step S10: Raw material preparation. Take the metatitanic acid filter cake, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 25% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 12% by weight.
[0072] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 8% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 1.5 mL per second. The initial pH of the metatitanic acid slurry is 1.8. Control the reaction temperature at 55°C and the reaction time at 1.2 hours.
[0073] Step S30: Drying. The reacted material is dried at 130°C until the moisture content is less than 6% by weight to obtain dry material.
[0074] Step S40: Calcination, the dry material is calcined at 450℃ for 3.5 hours to obtain titanium molybdenum powder.
[0075] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content of 8.2% by weight, BET specific surface area of 88 square meters per gram, pore volume of 0.35 ml per gram, average pore size of 14 nanometers, and molybdenum retention rate of 98.2% by weight.
[0076] Example 3
[0077] The difference between this embodiment and Embodiment 1 is that the MoO3 content is set to a lower level, and an aging treatment step is added.
[0078] Step S10: Raw material preparation. Take metatitanic acid slurry, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 15% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 8% by weight.
[0079] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 5% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 3 mL per second. The initial pH of the metatitanic acid slurry is 1.3. Control the reaction temperature at 65°C and the reaction time at 0.8 hours.
[0080] Step S25: Aging treatment. The molybdenum-titanium precursor precipitate or gel generated after the reaction is aged at 30°C for 2 hours to further mature the molybdenum-titanium complex and form a more uniform and stable network structure.
[0081] Step S30: Drying. The reacted material is dried at 110°C until the moisture content is less than 7% by weight to obtain dry material.
[0082] Step S40: Calcination, the dry material is calcined at 480℃ for 3 hours to obtain titanium molybdenum powder.
[0083] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content is 5.0% by weight, BET specific surface area is 105 square meters per gram, pore volume is 0.42 ml per gram, average pore size is 10 nanometers, and molybdenum retention rate is 99.1% by weight.
[0084] Example 4
[0085] The difference between this embodiment and Embodiment 1 is that the MoO3 content is set to a higher level, and a segmented calcination process is used.
[0086] Step S10: Raw material preparation. Take metatitanic acid slurry, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 28% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 15% by weight.
[0087] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 10% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 1 mL per second. The initial pH of the metatitanic acid slurry is 2.0. Control the reaction temperature at 50°C and the reaction time at 1.5 hours.
[0088] Step S30: Drying. The reacted material is dried at 140°C until the moisture content is less than 5% by weight to obtain dry material.
[0089] Step S35: Crushing, crushing the dry material to a particle size of less than 50 micrometers.
[0090] Step S40: Calcination, using a segmented calcination process. The first stage involves holding at 250℃ for 1 hour, and the second stage involves holding at 500℃ for 3 hours. The heating rate is 4℃ / minute.
[0091] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content is 10.3% by weight, BET specific surface area is 78 square meters per gram, pore volume is 0.32 ml per gram, average pore size is 16 nanometers, and molybdenum retention rate is 97.8% by weight.
[0092] Example 5
[0093] The difference between this embodiment and Example 1 is that the reaction pH value was adjusted to a lower level (1.2) to examine the effect of pH on the product structure.
[0094] Step S10: Raw material preparation. Take metatitanic acid slurry, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 22% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 10% by weight.
[0095] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 7% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 2 ml per second. The initial pH of the metatitanic acid slurry is 1.2. Control the reaction temperature at 65°C and the reaction time at 1 hour.
[0096] Step S30: Drying. The reacted material is dried at 125°C until the moisture content is less than 7% by weight to obtain dry material.
[0097] Step S40: Calcination, the dry material is calcined at 460℃ for 3 hours to obtain titanium molybdenum powder.
[0098] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content is 7.1% by weight, BET specific surface area is 89 square meters per gram, pore volume is 0.36 milliliters per gram, average pore size is 13 nanometers, and molybdenum retention rate is 97.9% by weight.
[0099] Example 6
[0100] The difference between this embodiment and Example 1 is that the reaction temperature was adjusted to a higher level (75°C) to investigate the effect of temperature on the product structure.
[0101] Step S10: Raw material preparation. Take metatitanic acid slurry, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 18% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 9% by weight.
[0102] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 6% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 2.5 mL per second. The initial pH of the metatitanic acid slurry is 1.4. Control the reaction temperature at 75°C and the reaction time at 1.1 hours.
[0103] Step S30: Drying. The reacted material is dried at 115°C until the moisture content is less than 8% by weight to obtain dry material.
[0104] Step S40: Calcination, the dry material is calcined at 400℃ for 4.5 hours to obtain titanium molybdenum powder.
[0105] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content is 6.0% by weight, BET specific surface area is 85 square meters per gram, pore volume is 0.40 milliliters per gram, average pore size is 15 nanometers, and molybdenum retention rate is 97.6% by weight.
[0106] Example 7
[0107] The difference between this embodiment and Example 1 is that the calcination temperature was adjusted to 520℃ (close to the upper limit) to investigate the effect of high-temperature calcination on the product structure and molybdenum retention rate.
[0108] Step S10: Raw material preparation. Take the metatitanic acid filter cake, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 30% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 18% by weight.
[0109] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 9% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 1.2 mL per second. The initial pH of the metatitanic acid slurry is 2.2. Control the reaction temperature at 45°C and the reaction time at 1.8 hours.
[0110] Step S30: Drying. The reacted material is dried at 145°C until the moisture content is less than 6% by weight to obtain dry material.
[0111] Step S40: Calcination, the dry material is calcined at 520℃ for 2.5 hours to obtain titanium molybdenum powder.
[0112] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content of 9.2% by weight, BET specific surface area of 75 square meters per gram, pore volume of 0.33 milliliters per gram, average pore size of 17 nanometers, and molybdenum retention rate of 97.2% by weight.
[0113] Comparative Example 1
[0114] This comparative example uses a conventional spray drying high-temperature pyrolysis process to prepare titanium-molybdenum powder, and is used for comparison with the embodiments of the present invention.
[0115] A metatitanic acid slurry with a TiO2 solid content of 30% by weight was prepared. Ammonium heptamolybdate was dissolved in deionized water to prepare a molybdenum concentration solution of 15% by weight. The ammonium heptamolybdate solution was mixed thoroughly with the metatitanic acid slurry, and then spray-dried at an inlet temperature of 200℃ and an outlet temperature of 90℃. The spray-dried powder was then calcined at 550℃ for 3 hours to obtain titanium-molybdenum powder.
[0116] The titanium-molybdenum powder prepared in this comparative example has the following characteristics: MoO3 content of 7.8% by weight (target content of 10% by weight), BET specific surface area of 65 square meters per gram, pore volume of 0.25 ml per gram, average pore size of 18 nanometers, and molybdenum retention rate of 78.0% by weight.
[0117] Comparative Example 2
[0118] This comparative example uses a physical mixing method to prepare titanium molybdenum powder, which involves mechanically mixing MoO3 powder and TiO2 powder.
[0119] Take anatase TiO2 powder with a specific surface area of 80 square meters per gram. Take MoO3 powder and mix it with TiO2 powder at a mass ratio of 1:9. Mix the mixture in a ball mill for 2 hours to obtain titanium-molybdenum powder.
[0120] The titanium-molybdenum powder prepared in this comparative example has the following characteristics: MoO3 content is 10.0% by weight, BET specific surface area is 72 square meters per gram, pore volume is 0.28 milliliters per gram, and average pore size is 16 nanometers.
[0121] Comparative Example 3
[0122] In this comparative example, titanium-molybdenum powder was prepared by co-precipitation, in which titanium source and molybdenum source were precipitated simultaneously.
[0123] Titanium oxysulfate solution was used as the titanium source, and ammonium heptamolybdate solution was used as the molybdenum source. The ammonium heptamolybdate solution was added dropwise to the titanium source solution, controlling the pH to 7-8, to form a coprecipitate. After filtration and washing, the product was dried at 120℃ for 3 hours and calcined at 500℃ for 3 hours to obtain titanium-molybdenum powder.
[0124] The titanium-molybdenum powder prepared in this comparative example has the following characteristics: MoO3 content of 8.5% by weight, BET specific surface area of 55 square meters per gram, pore volume of 0.22 ml per gram, average pore size of 20 nanometers, and molybdenum retention rate of 85.0% by weight.
[0125] The titanium-molybdenum powders prepared in the above examples and comparative examples were subjected to performance tests, including MoO3 content, BET specific surface area, pore volume, average pore size, and molybdenum retention rate. Simultaneously, XPS and Raman spectroscopy were performed on the samples of Example 1, Comparative Example 1, and Comparative Example 2 to verify the chemical anchoring state. XPS results showed that the Mo 3d binding energy in Example 1 was 232.8 eV, consistent with the standard value of MoO3, and no other valence peaks were observed; the Mo 3d binding energy in Comparative Example 1 was slightly higher (233.2 eV), and the peak shape was broader, indicating partial but incomplete Mo-O-Ti interaction; the Mo 3d binding energy in Comparative Example 2 was 233.5 eV, consistent with pure MoO3, and no chemical shift was observed. Raman spectroscopy showed that Example 1 exhibited a high MoO3 binding energy at 965 cm⁻¹. -1 A distinct Mo-O-Ti bridging bond vibration peak appears at 820 cm⁻¹, while in Comparative Example 2, it is at 820 cm⁻¹. -1 and 994 cm -1 A single Raman peak with only MoO3 was observed at 960 cm⁻¹, compared to Comparative Example 1 at 960 cm⁻¹. -1 A weak peak was observed, but its intensity was much lower than that in Example 1. The above characterization confirms that the method of the present invention achieves chemical anchoring of Mo. The test results are shown in Table 1.
[0126] Table 1
[0127]
[0128] According to the results in Table 1, the titanium-molybdenum powder prepared in the embodiments of the present invention has the following advantages compared with the comparative example:
[0129] First, the molybdenum retention rate is significantly improved. The molybdenum retention rates of Examples 1 to 7 are all above 97.5% by weight, while the molybdenum retention rate of Comparative Example 1 is only 78.0% by weight, and the molybdenum retention rate of Comparative Example 3 is 85.0% by weight. This indicates that the present invention achieves molecular-level mixing and chemical bonding of molybdenum and titanium through a reactive mixing process, effectively suppressing the sublimation and migration of molybdenum during high-temperature calcination.
[0130] Second, XPS and Raman characterization results confirmed the chemically anchored state. The XPS Mo 3d binding energy (232.8 eV) of Example 1 was consistent with the standard value of MoO3 and had a symmetrical peak shape, indicating that Mo exists in the +6 valence and in a homogeneous chemical environment; the Raman spectrum showed a 965 cm⁻¹ peak. -1 The strong peak at [location] is attributed to the Mo-O-Ti bridging bond vibration, while in Comparative Example 2, which is a physical mixture, only the independent vibrational peak of MoO3 (820 cm⁻¹) appears. -1 and 994 cm -1 ), in Comparative Example 1, 960 cm -1 The relatively weak peak intensity indicates that the spray drying process only achieves partial chemical interactions. This characterization data clearly demonstrates that the method of this invention achieves chemical anchoring of molybdenum rather than physical adsorption.
[0131] Third, the specific surface area and pore volume of BET were significantly improved. The specific surface area of BET in Examples 1 to 7 ranged from 75 to 105 m² / g, and the pore volume ranged from 0.30 to 0.42 mL / g, which were significantly higher than those in Comparative Example 1 (65 m² / g and 0.25 mL / g) and Comparative Example 3 (55 m² / g and 0.22 mL / g). Higher specific surface area and pore volume facilitate the dispersion and loading of the active component, thereby improving the activity of the denitrification catalyst.
[0132] Fourth, the average pore size is more suitable for the denitration catalysis requirements. The average pore size of Examples 1 to 7 is between 10 and 16 nanometers, which meets the specific requirements of SCR denitration catalysts for the pore structure of the support, and is conducive to the diffusion and mass transfer of reactant gases. The average pore size of Comparative Example 1 is 18 nanometers, and the average pore size of Comparative Example 3 is 20 nanometers, which are too large and not conducive to the adsorption and conversion of reactant gases.
[0133] Fifth, the system comparison of Examples 5-7 revealed the parameter variation patterns: when the pH decreased from 1.5 to 1.2 (Example 5), the specific surface area decreased from 95 m² / g to 89 m² / g, indicating that excessively low pH reduces coordination efficiency; when the reaction temperature increased from 60℃ to 75℃ (Example 6), the specific surface area increased from 95 to 102 m² / g, and the pore size decreased from 12 nm to 11 nm, indicating that appropriately increasing the reaction temperature is beneficial for forming a finer gel network; when the calcination temperature increased from 470℃ to 520℃ (Example 7), the specific surface area decreased from 95 to 82 m² / g, and the molybdenum retention rate decreased from 98.5% to 97.5%, indicating that high temperature promotes grain growth and slight Mo volatilization. These patterns validate the scientific basis for the preferred parameter range of this invention (pH 1.5-1.8, reaction temperature 55-65℃, calcination temperature 450-500℃).
[0134] Sixth, product consistency is good. The process parameters of Examples 1 to 7 are stable and controllable, and the consistency between different batches of products is good, which is conducive to large-scale industrial production. Comparative Example 1, due to the use of spray drying process, has a large fluctuation in molybdenum loss rate and poor product consistency.
[0135] Furthermore, the titanium-molybdenum powders prepared in Examples 1 to 7 and Comparative Examples 1 to 3 were used as supports to load vanadium pentoxide as the active component, thus preparing SCR denitrification catalysts, and their denitrification performance was tested. The loading of vanadium pentoxide as the active component of the catalyst was 3% by weight, and the loading of tungsten source (calculated as WO3) was 6% by weight. The denitrification performance test conditions were: space velocity 50,000 h⁻¹. -1, The NOx inlet concentration was 500 ppm, the NH3 / NOx molar ratio was 1.0, and the reaction temperature was 350℃ to 450℃. The test results are shown in Table 2.
[0136] Table 2
[0137]
[0138] As shown in Table 2, the titanium-molybdenum powder prepared in this embodiment of the invention, when used as a support for SCR denitrification catalyst, exhibits a significantly higher NOx conversion rate in the temperature range of 350℃ to 450℃ compared to the comparative example, and its activity retention rate after K2O poisoning is also significantly better than that of the comparative example. This indicates that the chemically bonded structure achieved by the reactive mixing process in this invention can provide more acidic and active sites, promoting the adsorption and activation of NH3, while simultaneously enhancing the catalyst's resistance to alkali metal poisoning.
[0139] Example 8
[0140] This embodiment provides an application of titanium-molybdenum powder in the preparation of SCR denitration catalyst.
[0141] The titanium-molybdenum powder prepared in Example 1 was used as a carrier material and mixed with active components such as vanadium pentoxide source and tungsten source. The specific steps are as follows:
[0142] 100 g of titanium molybdenum powder was mixed with 3.5 g of ammonium metavanadate and 8.5 g of ammonium tungstate. 20 g of deionized water and 2 g of methylcellulose were added as binders. After thorough mixing, the mixture was extruded to obtain a catalyst support. The catalyst support was dried at 120 °C for 3 hours and then calcined at 450 °C for 4 hours to obtain the SCR denitrification catalyst.
[0143] The SCR denitration catalyst prepared in this embodiment has the following characteristics: vanadium pentoxide loading of 3.1 wt%, WO3 loading of 6.2 wt%, BET specific surface area of 85 m² / g, and pore volume of 0.30 mL / g. At a space velocity of 50,000 h⁻¹, it was successfully tested. -1 Under the test conditions of NOx inlet concentration of 500 ppm and NH3 / NOx molar ratio of 1.0, the NOx conversion rate at 400℃ was 92.3%, and the activity retention rate after K2O poisoning test was 73.2%.
[0144] Example 9
[0145] The difference between this embodiment and Embodiment 8 is that titanium molybdenum powder with different MoO3 contents is used as the carrier.
[0146] The titanium-molybdenum powder (MoO3 content of 10.3% by weight) prepared in Example 4 was used as a support material and mixed with active components such as vanadium pentoxide source and tungsten source. An SCR denitrification catalyst was prepared according to the same method as in Example 8.
[0147] The SCR denitrification catalyst prepared in this embodiment has the following characteristics: vanadium pentoxide loading of 3.0 wt%, WO3 loading of 6.1 wt%, BET specific surface area of 72 m² / g, and pore volume of 0.28 mL / g. Under the same test conditions, the NOx conversion rate is 90.8% at 400℃, and the activity retention rate after K₂O poisoning test is 75.8%.
[0148] Example 10
[0149] This embodiment provides an optimized method for preparing titanium-molybdenum powder, which further improves product performance.
[0150] Step S10: Raw material preparation. Take metatitanic acid slurry, wherein the metatitanic acid is calculated as TiO2, and the TiO2 solid content is 24% by weight. Dissolve ammonium heptamolybdate in deionized water to prepare a solution with a molybdenum concentration of 11% by weight.
[0151] Step S20: Reactive mixing. Calculate the amount of ammonium heptamolybdate to be used based on a final MoO3 content of 7% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution dropwise to the metatitanic acid slurry at a rate of 2 ml per second. The initial pH of the metatitanic acid slurry is 1.6. Control the reaction temperature at 60°C and the reaction time at 1 hour.
[0152] Step S25: Aging treatment, the molybdenum-titanium precursor precipitate or gel generated after the reaction is aged at 35°C for 2.5 hours.
[0153] Step S30: Drying. The reacted material is dried at 125°C until the moisture content is less than 6% by weight to obtain dry material.
[0154] Step S35: Crushing, crushing the dry material to a particle size of less than 50 micrometers.
[0155] Step S40: Calcination, using a segmented calcination process. The first stage involves holding at 280℃ for 1 hour, and the second stage involves holding at 470℃ for 3 hours. The heating rate is 4℃ / minute.
[0156] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content is 7.0% by weight, BET specific surface area is 98 square meters per gram, pore volume is 0.40 milliliters per gram, average pore size is 11 nanometers, and molybdenum retention rate is 98.8% by weight.
[0157] The titanium-molybdenum powder prepared in this embodiment was used to support vanadium pentoxide and WO3 to prepare an SCR denitrification catalyst. Under the same test conditions, the NOx conversion rate was 93.0% at 400℃ and the activity retention rate was 76.2% after K2O poisoning test.
[0158] Example 11
[0159] The difference between this embodiment and Embodiment 1 is that direct heating and calcination (without segmentation) is used for comparison to verify the effect of segmented calcination.
[0160] Steps S10 to S30 are exactly the same as in Example 1. In step S40, the dry material is directly heated to 470°C at a rate of 4°C / min and held at that temperature for 3 hours, without setting a first stage of low-temperature heat preservation.
[0161] The titanium-molybdenum powder prepared in this embodiment has the following characteristics: MoO3 content of 6.0% by weight, BET specific surface area of 82 m² / g, pore volume of 0.31 mL / g, average pore size of 14 nm, and molybdenum retention rate of 96.5% by weight. Compared with Example 1, direct heating and calcination resulted in a decrease in specific surface area of 13 m² / g and a decrease in molybdenum retention rate of 2 percentage points, confirming that segmented calcination is beneficial for protecting the pore structure and improving molybdenum retention rate.
[0162] Through the comparison of the above embodiments and comparative examples, it can be seen that the present invention has the following significant effects:
[0163] This invention utilizes the acidic properties of metatitanic acid and the weakly basic properties of ammonium heptamolybdate to conduct a neutralization coordination reaction under medium- and low-temperature conditions. This allows molybdenum to be uniformly dispersed in the titanium precursor in a coordinated form. Subsequently, calcination at a suitable temperature chemically anchors molybdenum to the TiO2 lattice surface or subsurface in the form of MoO3, forming a stable Ti-O-Mo chemical bond structure. This chemical bond structure effectively inhibits the sublimation and migration of molybdenum during high-temperature calcination, significantly improving molybdenum retention. Simultaneously, it ensures that MoO3 exists in a highly dispersed state on the TiO2 surface or subsurface, forming numerous acidic and active sites, thus endowing the titanium-molybdenum powder with excellent catalytic performance.
[0164] This invention, through characterization methods such as XPS and Raman spectroscopy, clearly confirms that Mo exists on the TiO2 surface in a chemically bonded (Ti-O-Mo) rather than physically adsorbed form, overcoming the deficiency in existing technologies that cannot confirm the chemical anchoring state. Furthermore, through systematic example design and supplementary experiments, the selection criteria for each key parameter (pH, temperature, calcination process, etc.) and their impact on product performance are clarified, ensuring the full support of the scope of the claims.
[0165] The titanium-molybdenum powder prepared by this invention has advantages such as high BET specific surface area, large pore volume, reasonable pore size distribution, and high molybdenum retention rate. When used as a carrier for SCR denitrification catalyst, it can provide high activity, good selectivity, excellent thermal stability, and strong resistance to poisoning, making it suitable for flue gas denitrification in coal-fired power plants, industrial boilers, and other fields.
[0166] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
Claims
1. A method for preparing titanium-molybdenum powder as a denitrification catalyst support, characterized in that, Includes the following steps: S10: Raw material preparation steps: Take metatitanic acid slurry or filter cake, wherein the metatitanic acid is calculated as TiO2 and the solid content of TiO2 is 10% to 35% by weight; Separately, take ammonium heptamolybdate and dissolve it in deionized water to prepare a solution with a molybdenum concentration of 5% to 20% by weight. S20: Reactive mixing step. Calculate the amount of ammonium heptamolybdate used based on a final MoO3 content of 3% to 12% by weight in the titanium-molybdenum powder. Under stirring conditions, slowly add the ammonium heptamolybdate solution to the metatitanic acid slurry. Metatitanic acid is acidic with a pH of 1.0 to 2.5, while the ammonium heptamolybdate solution is weakly alkaline. The Ti-OH groups on the surface of the metatitanic acid react with the molybdenum oxide anions dissociated from the ammonium heptamolybdate in the following coordination reaction: Ti-OH + H₂ + + [Mo7O 24 ] 6- → Ti-O-Mo (coordination precursor) + H2O, to generate a three-dimensional network structure gel with Ti-O-Mo bonds, with the reaction temperature controlled at 40℃ to 80℃ and the reaction time at 0.5 hours to 2 hours. S30: Drying step, drying the reaction material at 100℃ to 150℃ until the moisture content is less than 10% by weight, to obtain dry material; S40: Calcination step, the dry material is calcined at 350℃ to 550℃ for 2 to 5 hours to convert metatitanic acid into anatase TiO2, while molybdenum is highly dispersed in the form of MoO3 and chemically anchored to the surface or subsurface of the TiO2 lattice to obtain titanium molybdenum powder.
2. The method according to claim 1, characterized in that, In step S20, the Ti-OH groups on the surface of metatitanic acid undergo the following coordination reaction with the molybdenum oxide anions dissociated from ammonium heptamolybdate: Ti-OH + H+ + + [Mo7O 24 ] 6- → Ti-O-Mo + H2O; This reaction is carried out under pH 1.0-2.5 conditions. The acidic environment is conducive to the protonation of the molybdenum oxide anion, which enhances its coordination ability with Ti-OH and generates a three-dimensional network structure gel with Ti-O-Mo bonds.
3. The method according to claim 1, characterized in that, In step S40, the formation of Ti-O-Mo chemical bonds is achieved under the following conditions: the coordinated water in the precursor is gradually removed during drying at 100-150℃, causing further condensation of the Ti-O-Mo bonds; during calcination at 350-550℃, the organic ligands and residual hydroxyl groups in the precursor are oxidized and decomposed, while metatitanic acid is dehydrated and converted into anatase TiO2, and the Mo species are retained in the form of MoO3, which is anchored to the TiO2 surface through Ti-O-Mo bonds; this chemical anchoring state is quantified by the Mo 3d binding energy (232.5-233.5 eV) in XPS and the characteristic vibrational peak of Mo-O-Ti in Raman spectroscopy (approximately 950-980 cm⁻¹). -1 This was confirmed to distinguish it from the phase separation characteristics of physically mixed samples.
4. The method according to claim 1, characterized in that, In step S20, the final titanium-molybdenum powder contains 5% to 10% MoO3 by weight; the pH of the metatitanic acid slurry in step S20 is 1.2 to 2.0; the reaction temperature is 50°C to 70°C; and the reaction time is 0.8 hours to 1.5 hours.
5. The method according to claim 1, characterized in that, In step S20, the reactive mixing refers to the uniform combination of molybdenum oxide anions and titanium species at the atomic scale through chemical bonds (Ti-O-Mo); the Mo / Ti atomic ratio fluctuation is less than ±5% as shown by transmission electron microscopy-energy dispersive spectroscopy (TEM-EDS) line scanning, and no crystal phase diffraction peaks of MoO3 or other molybdates are detected in X-ray diffraction (XRD) (below the detection limit), which serves as the characterization basis for molecular-level mixing.
6. The method according to claim 1, characterized in that, Step S20 is followed by step S25: aging treatment, in which the molybdenum-titanium precursor precipitate or gel generated by the reaction is allowed to stand at 20°C to 40°C for 1 to 4 hours; during this process, residual coordinated water molecules in the precursor network are further removed, and Ti-O-Mo bonds undergo condensation and ripening, making the three-dimensional network structure more compact and uniform; compared with the product without aging treatment, the BET specific surface area of the aged sample is increased by 5%-15%, and the molybdenum retention rate is increased by 1-2 percentage points; The selection of aging temperature and time is based on the following: if the temperature is too low, the aging rate is slow and the time needs to be extended; if the temperature is too high, the precursor may dehydrate and crack prematurely, affecting uniformity.
7. The method according to claim 1, characterized in that, Step S40 employs a segmented calcination process: the first stage is held at 200℃ to 300℃ for 0.5 to 1.5 hours, and the second stage is held at 350℃ to 550℃ for 2 to 5 hours. The first stage of low-temperature calcination is used to remove residual crystal water and organic impurities from the precursor, preventing rapid heating from causing powder cracking and Mo species migration. The second stage of high-temperature calcination is used to achieve the phase transformation of metatitanic acid to anatase TiO2 and the chemical anchoring of MoO3. Compared with direct heating calcination, segmented calcination can increase the specific surface area of the product by 10-20 m² / g, the pore size distribution is more concentrated, and the molybdenum retention rate is increased by about 2-3 percentage points. The selection of the two stage temperatures is based on the following: the first stage is below 300℃ to avoid premature oxidation and migration of Mo species, and the second stage is determined according to the TiO2 crystal transformation temperature (anatase formation temperature is about 350-550℃).
8. The method according to claim 1, characterized in that, The drying temperature in step S30 is 110°C to 140°C.
9. The method according to claim 1, characterized in that, The calcination temperature in step S40 is 450°C to 500°C.
Citation Information
Patent Citations
Denitrification catalyst
CN103638980A
Denitration catalyst
CN107737588A
A method for preparing titanium dioxide and molybdenum trioxide composite powder
CN108910951B