A chemical method for synthesizing silver selenide powder at room temperature
Patent Information
- Application Number
- CN202510422794.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-07
- Publication Date
- 2026-10-16
AI Technical Summary
2001年,夏幼南教授课题组在Journal of the American Chemical Society(2001,123,11500-11501)上报道了一种硒化银的制备方法,利用硒单质与硝酸银的水溶液进行反应,在室温条件下搅拌即可制备出硒化银材料,但会出现副产物Ag2SeO3,需要通过进一步处理去除
1、该方法操作简单,只需将原料简单混合即可完成硫化银产品的制备。
Smart Images

Figure CN122916064A_ABST
Abstract
Description
Technical fields: This invention belongs to the field of materials chemistry, and in particular relates to a chemical method for synthesizing silver selenide powder at room temperature. Background technology: Silver selenide is a narrow-bandgap compound semiconductor material with excellent thermoelectric properties. Under room temperature operating conditions, it exhibits a thermoelectric figure of merit exceeding that of commercially available bismuth telluride, holding promise for further improving the energy conversion efficiency of room-temperature thermoelectric generators. Furthermore, this material possesses unique flexibility, providing an important foundation for constructing flexible thermoelectric power generation devices. Therefore, achieving large-scale, low-cost preparation of silver selenide has enormous potential value in the field of commercial thermoelectric material fabrication.
[0001] Currently, various methods have been developed to prepare silver selenide materials. In 2001, Professor Xia Younan's research group reported a method for preparing silver selenide in the Journal of the American Chemical Society (2001, 123, 11500-11501). This method utilizes the reaction of elemental selenium with an aqueous solution of silver nitrate, and silver selenide material can be prepared by stirring at room temperature. However, the byproduct Ag₂SeO₃ is produced and needs to be removed through further treatment. In 2005, the same research group published an article in Chemical Physics Letters (2005, 416, 246-250), dispersing elemental selenium in a mixed solvent of ethylene glycol and polyvinylpyrrolidone, adding a silver nitrate solution of ethylene glycol dropwise while continuously stirring, and obtaining silver selenide material after approximately one hour of reaction. In 2023, Kirill Kovnir's research group reported a method for preparing silver selenide powder in the Journal of the American Chemical Society (2023, 145, 22762-22775). A selenium precursor solution was prepared using 1 mmol of selenium and 10 mL of monoethanolamine. 2 mmol of AgCl was added to this solution at 80°C and the mixture was stirred continuously for 30 minutes. The resulting dark gray precipitate was filtered and washed with anhydrous ethanol to obtain a fine dark gray powder. Besides wet chemical methods, silver selenide can also be obtained through physical means. For example, Yanzhong Pei's research group (Nature Communications, 2024, 15, 6580) weighed high-purity Ag and Se particles at a stoichiometric ratio of Ag:Se = 2:1 and placed them in a quartz tube for vacuum sealing. The raw materials were heated to 1273 K over 7 hours and held at this temperature for 8 hours. After 5 hours, they were cooled to 773 K and held at this temperature for 48 hours, after which the furnace was cooled to room temperature, thus synthesizing Ag₂Se polycrystalline materials. Marisol Martin-Gonzalez et al. reported a method for in-situ preparation of silver selenide thin film materials using reactive sputtering. In this work, the substrate temperature was maintained at 300 °C, and the pressure of ultrapure argon gas (6 N) in the cavity was kept constant at approximately 6.8 × 10⁻⁶. − 3The DC power used is approximately 60 W (Advanced Energy Materials, 2018, 8, 1702024). Furthermore, the applicant disclosed a method for preparing silver selenide by reacting elemental silver with an aqueous solution of sodium sulfide containing selenium in patents ZL201310090546.6, ZL202111074461.X, and an article (Adv. Mater. 2022, 34, 2104786). This method uses a silver elemental thin film as a reactant, directly oxidizing elemental silver with the sodium sulfide aqueous solution of selenium to form a silver selenide thin film material. It does not use organic solvents, does not involve high-temperature reactions, and synthesizes a silver selenide thin film material.
[0002] Comprehensive analysis reveals that current methods for preparing silver selenide materials generally suffer from high temperatures and low yields. Therefore, achieving large-scale, low-cost, simple, and environmentally friendly room-temperature preparation of silver selenide powder remains a challenge. Summary of the Invention: The purpose of this invention is to provide a chemical method for synthesizing silver selenide powder at room temperature, addressing the shortcomings of existing technologies. This method utilizes an aqueous solution of sodium sulfide from selenium powder as the selenium source, and silver selenide can be prepared at room temperature using an aqueous solution of silver ions or a silver ion source substance. Water is used as the solvent, without any other organic solvents; the reaction process is rapid, simple to operate, and environmentally friendly.
[0003] The technical solution adopted in this invention is: A chemical method for synthesizing silver selenide powder at room temperature includes the following steps: preparing an aqueous solution of sodium sulfide, adding elemental selenium to it and stirring until the elemental selenium is completely dissolved; then adding an aqueous solution of silver ions or a silver ion source substance to the above solution and stirring, the reaction is completed instantaneously with the addition of silver ions or silver salt, producing silver selenide precipitate.
[0004] According to the above scheme, after the reaction, a post-processing is performed to obtain a pure silver selenide powder sample. The post-processing is: vacuum filtration and washing; the washing agent used is deionized water.
[0005] According to the above scheme, the silver ion source material is a water-soluble silver salt.
[0006] According to the above scheme, the silver ion source material includes, but is not limited to, silver nitrate, silver acetate, etc.
[0007] According to the above scheme, the concentration of the sodium sulfide solution used is 0.03~0.4 g / mL.
[0008] According to the above scheme, the sodium sulfide is anhydrous sodium sulfide or its hydrate.
[0009] According to the above scheme, the molar ratio of selenium to silver is 1:2.
[0010] According to the above scheme, the molar ratio of selenium to sulfur is less than or equal to 1:1.
[0011] A second aspect of this invention provides the application of the silver selenide material obtained by the above preparation method as a thermoelectric material. Specifically, it can be used in the thermoelectric field as a p-type thermoelectric arm material in thermoelectric generators or electro-refrigeration devices.
[0012] This invention utilizes an aqueous solution of sodium selenide containing selenium ions and an aqueous solution or aqueous silver salt containing silver ions. By controlling the order of addition, the silver salt solution or silver ion source is added to the sodium selenide aqueous solution, resulting in silver selenide powder material that can be obtained instantaneously upon mixing. Further control of the stoichiometric ratio of the reaction raw materials yields pure silver selenide. The reaction is carried out under normal temperature and pressure conditions, is rapid, and is simple to operate, requiring no complex environment or equipment such as high temperature and high pressure. Water is used as the solvent, without any other organic solvents, making it environmentally friendly. Both the selenium and silver sources used are readily available and environmentally friendly, and the target product does not introduce other impurity ions besides its own element. The yield is high (the molar yield based on silver element can reach 97%), showing broad prospects for industrial application.
[0013] Advantages of this invention: 1. This method is simple to operate; the preparation of silver sulfide products can be completed simply by mixing the raw materials.
[0014] 2. This method is carried out under normal temperature and pressure conditions, and the reaction process is rapid.
[0015] 3. This method does not use any organic solvents, but only water as the reaction medium, making it environmentally friendly.
[0016] 4. The product obtained by this method is simple to process; washing with water is sufficient. Attached image description: Figure 1 XRD pattern of silver selenide prepared in Example 1; Figure 2 XRD pattern of silver selenide prepared in Example 2; Figure 3 XRD pattern of silver selenide prepared in Example 3; Figure 4 XRD pattern of silver selenide prepared in Example 4; Figure 5 XRD pattern of silver selenide prepared in Example 5; Figure 6 XRD pattern of silver selenide prepared in Example 6; Figure 7XRD pattern of silver selenide prepared in Example 7; Figure 8 XRD patterns of the product prepared in Comparative Example 1; Figure 9 XRD patterns of the products prepared in Comparative Example 2; Figure 10 XRD patterns of the products prepared in Comparative Example 3; Figure 11 XRD patterns of the product prepared in Comparative Example 4. Detailed implementation method: The following examples further illustrate this point.
[0017] Example 1 1. Weigh 1.2 g (5.0 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.10 g (1.25 mmol) selenium powder, add it to solution A, and stir until completely dissolved, obtaining solution B. Weigh 0.42 g (2.5 mmol) silver acetate into a small beaker, add 20 mL of deionized water, and stir until dissolved, obtaining solution C.
[0018] 2. Under normal temperature and pressure conditions, solution C and solution B are mixed and stirred to obtain a precipitate. The precipitate is filtered, washed with deionized water, and then air-dried to obtain the product.
[0019] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 1 This indicates that the obtained product is a relatively pure Ag2Se powder material.
[0020] Example 2 1. Weigh 1.8 g (7.5 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.1 g (1.25 mmol) selenium powder, add it to solution A, and stir until completely dissolved, obtaining solution B. Weigh 0.42 g (2.5 mmol) silver acetate into a small beaker, add 20 mL of deionized water, and stir until dissolved, obtaining solution C.
[0021] 2. Under normal temperature and pressure conditions, solution C and solution B are mixed and stirred to obtain a precipitate. The precipitate is filtered, washed with deionized water, and then air-dried to obtain the product.
[0022] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 2 This indicates that the obtained product is a relatively pure Ag2Se powder material.
[0023] Example 3 1. Weigh 0.6 g (2.5 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.1 g (1.25 mmol) selenium powder, add it to solution A, and stir until completely dissolved, obtaining solution B. Weigh 0.42 g (2.5 mmol) silver acetate into a small beaker, add 20 mL of deionized water, and stir until dissolved, obtaining solution C.
[0024] 2. Under normal temperature and pressure conditions, solution C and solution B are mixed and stirred to obtain a precipitate. The precipitate is filtered, washed with deionized water, and then air-dried to obtain the product.
[0025] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 3 This indicates that the obtained product is a relatively pure Ag2Se powder material.
[0026] Example 4 1. Weigh 1.2 g (5.0 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, stir to dissolve, forming solution A. Weigh 0.1 g (1.25 mmol) selenium powder, add it to solution A and stir until completely dissolved, to obtain solution B.
[0027] 2. Weigh 0.43 g (2.5 mmol) of silver nitrate into a small beaker, add it to solution B under normal temperature and pressure, and stir to obtain a precipitate. Filter the precipitate, wash it with deionized water, and let it air dry to obtain the product.
[0028] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 4 This indicates that the obtained product is a relatively pure Ag2Se powder material.
[0029] Example 5 1. Weigh 16.3 g (67.8 mmol) sodium sulfide nonahydrate into a beaker, add 230 mL of deionized water, stir to dissolve, forming solution A. Weigh 1.16 g (14.7 mmol) selenium powder, add it to solution A and stir until completely dissolved, to obtain solution B.
[0030] 2. Weigh 5.0 g (29.4 mmol) of silver nitrate and add it to solution B under normal temperature and pressure conditions, stirring to obtain a precipitate. Filter the precipitate, wash it with deionized water, and allow it to air dry to obtain the product.
[0031] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 5 This indicates that the obtained product is a relatively pure Ag2Se powder material.
[0032] Example 6 1. Weigh 7.68 g (32 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.63 g (8 mmol) selenium powder, add it to solution A, and stir until completely dissolved, to obtain solution B.
[0033] 2. Weigh 2.67 g (16 mmol) of silver acetate and add it to solution B under normal temperature and pressure conditions, stirring to obtain a precipitate. Filter the precipitate, wash it with deionized water, and let it air dry to obtain the product.
[0034] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 6 This indicates that the obtained product is a relatively pure Ag₂Se powder material. The molar yield, calculated based on the conversion of silver to silver selenide, is no less than 97%.
[0035] Example 7 1. Weigh 7.68 g (32 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 2.52 g (32 mmol) selenium powder, add it to solution A, and stir until completely dissolved, to obtain solution B.
[0036] 2. Weigh 10.68 g (64 mmol) of silver acetate and add it to solution B under normal temperature and pressure conditions, stirring to obtain a precipitate. Filter the precipitate, wash it with deionized water, and let it air dry to obtain the product.
[0037] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product completely matched those of Ag₂Se. Figure 7 This indicates that the obtained product is a relatively pure Ag2Se powder material.
[0038] Comparative Example 1 1. Weigh 1.2 g (5.0 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.2 g (2.5 mmol) selenium powder, add it to solution A, and stir until completely dissolved, obtaining solution B. Weigh 0.5 g (2.9 mmol) silver nitrate into a small beaker, add 20 mL of deionized water, and stir until dissolved, obtaining solution C.
[0039] 2. Under normal temperature and pressure conditions, solution C and solution B are mixed and stirred to obtain a precipitate. The precipitate is filtered, washed with deionized water, and then air-dried to obtain the product.
[0040] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product matched those of Ag₂Se, but diffraction peaks of elemental selenium appeared near 2θ of 29.7 degrees. Figure 8 This indicates that when the ratio of selenium to silver deviates from 1:2 (silver is relatively less and selenium is relatively excessive), the product obtained is a mixture containing elemental selenium and Ag2Se powder.
[0041] Comparative Example 2 1. Weigh 1.2 g (5.0 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.5 g (6.3 mmol) selenium powder, add it to solution A, and stir until completely dissolved, obtaining solution B. Weigh 0.5 g (2.9 mmol) silver nitrate into a small beaker, add 20 mL of deionized water, and stir until dissolved, obtaining solution C.
[0042] 2. Under normal temperature and pressure conditions, solution C and solution B are mixed and stirred to obtain a precipitate. The precipitate is filtered, washed with deionized water, and then air-dried to obtain the product.
[0043] After drying, a grayish-black powder sample was obtained. XRD analysis showed that the diffraction peaks of the product matched those of Ag₂Se, but diffraction peaks of elemental selenium appeared near 2θ of 29.7 degrees. Figure 9 Compared with the results in Comparative Example 1, the relative intensity of the diffraction peak of elemental selenium is significantly increased. This indicates that when the molar ratio of selenium to silver deviates from 1:2 (excess selenium), the product obtained is a mixture containing elemental selenium and Ag₂Se powder, and the amount of elemental selenium in the product increases with the degree of selenium excess.
[0044] Comparative Example 3 1. Weigh 7.68 g (32 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, stir to dissolve, forming solution A. Weigh 3.79 g (48 mmol) selenium powder, add it to solution A and stir until completely dissolved, to obtain solution B.
[0045] 2. Weigh 16 g (96 mmol) of silver acetate and add it to solution B under normal temperature and pressure conditions, stirring to obtain a precipitate. Filter the precipitate, wash it with deionized water, and allow it to air dry to obtain the product.
[0046] After drying, a grayish-black powder sample was obtained. XRD analysis showed that most of the diffraction peaks of the product matched Ag₂Se. Figure 10 However, a diffraction peak of elemental selenium appeared near 2θ of 29.7 degrees, indicating that the relative amount of sulfur used was small. When the ratio of selenium to sulfur reached 1.5:1, pure Ag2Se material could not be synthesized and Se impurities would appear.
[0047] Comparative Example 4 Using an aqueous solution of sodium sulfide with selenium as the selenium source and copper ions as the copper source, the specific operation is as follows, referring to the method in the above embodiment: 1. Weigh 1.2 g (5.0 mmol) sodium sulfide nonahydrate into a beaker, add 20 mL of deionized water, and stir to dissolve, forming solution A. Weigh 0.20 g (2.5 mmol) selenium powder, add it to solution A, and stir until completely dissolved, obtaining solution B. Weigh 0.8 g (3.2 mmol) copper sulfate pentahydrate into a small beaker, add 20 mL of deionized water, and stir until dissolved, obtaining solution C.
[0048] 2. Under normal temperature and pressure conditions, solution C and solution B are mixed and stirred to obtain a precipitate. The precipitate is filtered, washed with deionized water, and then air-dried to obtain the product.
[0049] 3. After drying, a black powder sample was obtained. XRD analysis showed that the diffraction peaks of this product did not match well with the standard cards for copper selenide, cuprous selenide, copper sulfide, cuprous sulfide, and copper selenide sulfide, indicating that copper selenides (copper selenide or cuprous selenide) could not be obtained, and the product had a relatively complex composition. X-ray diffraction results are shown below. Figure 11 .
[0050] Patent ZL201310090546.6 discloses a method for forming a silver selenide film by redox reaction of elemental silver and an aqueous solution of sodium sulfide containing selenium. The method provided by this invention has the following inventiveness and significant differences: (1) The silver source used in this invention is silver ions, which is completely different from the silver source used in the above patent. The silver ions are provided by silver salts including silver acetate and silver nitrate; (2) The reaction mechanism is different from that in patent ZL201310090546.6. The above patent uses an elemental silver film to react with an aqueous solution of sodium sulfide containing selenium to form a silver selenide film, which involves the oxidation of elemental silver, and therefore belongs to a redox reaction. However, this invention uses silver ions to react with an aqueous solution of sodium sulfide containing selenium, and there is no gain or loss of electrons in the silver element, so it is completely different from the reaction mechanism contained in the above patent; (3) The rate of product preparation is significantly increased compared with patent ZL201310090546.6. The elemental silver film material used in patent ZL201310090546.6 has a thickness of several hundred nanometers, and the reaction time increases with the increase of the elemental silver precursor film thickness. The synthesis method provided in this patent can instantly obtain silver selenide powder material by mixing a silver source and a sodium sulfide aqueous solution of selenium. The reaction is rapid and can produce large quantities of silver selenide powder. Furthermore, since the solubility product constant of silver sulfide is very small, it is generally believed that silver ions readily and directly form silver sulfide with sulfide ions in the sodium sulfide aqueous solution. However, this invention uses a sodium sulfide aqueous solution of selenium as the selenium source precursor and a silver source as the silver ion precursor. The product obtained instantaneously by mixing the two precursors is silver selenide powder, without the formation of silver sulfide. Copper and silver are both in Group IIB and have similar chemical properties. As shown in Comparative Example 4, using a sodium sulfide aqueous solution of selenium as the selenium source and copper ions as the copper source, the synthesis was carried out according to the method of the example, but no copper selenide material (copper selenide or cuprous selenide) similar to silver was produced. This also indicates that the present invention uses an aqueous solution of sodium sulfide as the selenium source and a silver ion solution or silver ion source substance as the silver source to synthesize silver selenide products, which has a unique reaction mechanism.
[0051] This invention uses an aqueous solution of sodium sulfide as a selenium source and a silver ion solution or silver ion source substance as a precursor to react and generate silver selenide powder. The product yield is high and the product output is greater.
[0052] It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.
Claims
1. A chemical method for synthesizing silver selenide powder at room temperature, characterized in that: Includes the following steps: First, prepare an aqueous solution of sodium sulfide, add elemental selenium to it and stir until the elemental selenium is completely dissolved; then add an aqueous solution of silver ions or a silver ion source substance to the above solution and stir. The reaction is completed instantaneously with the addition of silver ions or silver salt, producing silver selenide precipitate.
2. The chemical method according to claim 1, characterized in that: After the reaction, a post-processing was performed to obtain a pure silver selenide powder sample. The post-processing consisted of vacuum filtration and washing, with deionized water used as the cleaning agent.
3. The chemical method according to claim 1, characterized in that: The silver ion source material is a water-soluble silver salt.
4. The chemical method according to claim 1, characterized in that: The silver ion source substance is silver nitrate or silver acetate.
5. The chemical method according to claim 1, characterized in that: The concentration of the sodium sulfide solution is controlled at 0.03~0.4 g / mL.
6. The chemical method according to claim 1, characterized in that: The sodium sulfide mentioned is anhydrous sodium sulfide or its hydrate.
7. The chemical method according to claim 1, characterized in that: The molar ratio of selenium to silver is 1:
2.
8. The chemical method according to claim 1, characterized in that: The molar ratio of selenium to sulfur is less than or equal to 1:
1.
9. The application of silver selenide prepared by the chemical method described in claim 1 as a thermoelectric material.
Citation Information
Patent Citations
Chemical method for synthesising silver selenide semiconductor photoelectric film material in situ at room temperature