A method for enhancing oxidation rate of sodium thioantimonite

CN122916209APending Publication Date: 2026-10-16SHAOGUAN WEIYING NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611302208.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-10-16

AI Technical Summary

Technical Problem

[0003]目前,针对含硫代亚锑酸钠的碱性浸出液,常采用空气、氧气或其他氧化剂进行氧化处理,使Sb(Ⅲ)逐步转化为Sb(V),并在碱性条件下形成焦锑酸钠沉淀,然而,三价锑硫配合物在液相中的氧化反应速度较慢,氧气传质和界面反应效率不足,导致氧化沉锑时间较长,而且,硫代亚锑酸钠体系不同于普通无机锑盐溶液,其溶液中存在较多硫化物和硫代硫酸盐等还原性硫物种,体系中的硫化钠、硫代硫酸盐等硫物种在氧化条件下容易被过度氧化为,导致氧气利用率降低、母液盐负荷增加,并可能因盐分夹带影响焦锑酸钠产品质量,为了提高反应速率而直接提高通气量时,体系氧化电位容易快速升高,虽然短时间内可增强氧传质,但同时会加剧硫酸盐副产物生成,且后期继续高强度供氧对锑转化贡献有限,反而不利于副反应控制和晶体熟化

Benefits of technology

[0020] 1. This invention utilizes homologous catalytic seed crystals to provide an adsorption, enrichment, and homologous nucleation interface for antimonythionate ions. A sulfur-oxygen buffer solution regulates the redox environment and inhibits sulfate byproducts. A stepped aeration method matches the oxygen supply intensity to the three stages of adsorption, rapid oxidation, and ripening. Subsequent thermal separation, washing, and drying ensure product purity and main component stability, enabling the system to achieve a high degree of reaction and low oxidation rate under normal atmospheric pressure. The amount of antimony produced and the total antimony content of stable sodium pyroantimonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_8
    Figure SMS_8
Patent Text Reader

Abstract

The application discloses a method for strengthening oxidation by improving the oxidation rate of sodium thioantimonite, and belongs to the technical field of sodium pyroantimonate processing. The method is mainly aimed at the technical problem that the oxidation rate of antimony, the inhibition effect of side reactions and the quality stability of sodium pyroantimonate product need to be further improved under the condition of normal-pressure air oxidation. The method specifically comprises the following steps: placing an alkaline leaching solution containing sodium thioantimonite in a reaction kettle with a gas distributor and stirring; and adding a sulfur-oxygen buffer solution and homologous catalytic crystal seeds into the reaction kettle. The method provides a homologous catalytic crystal seed for the adsorption enrichment and homologous nucleation interface of sodium thioantimonite, and the sulfur-oxygen buffer solution regulates the oxidation-reduction environment and inhibits the by-product of sulfate, and the method is combined with step-by-step aeration, so that the oxidation rate and the quality stability of sodium pyroantimonate product are improved, the side reactions are inhibited, and the reaction mother liquor has good reusing adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium pyroantimonate processing technology, and more specifically to an enhanced oxidation method for increasing the oxidation rate of sodium thioantimonite. Background Technology

[0002] Sodium thioantimonite is one of the common antimony-containing forms when antimony ore, antimony-containing dust, antimony smelting intermediates, or antimony-containing secondary resources are leached in an alkaline sulfidation system. In this type of alkaline leachate, antimony usually exists in the form of soluble trivalent antimony-sulfur complexes. The system also contains high concentrations of free sodium hydroxide, sodium sulfide, thiosulfate, and other reducing sulfur species. In order to recover and utilize antimony, it is usually necessary to further oxidize the trivalent antimony in the liquid phase and convert it into pentavalent antimony precipitates, such as sodium pyroantimonite.

[0003] Currently, alkaline leachates containing sodium thiostite are often treated with air, oxygen, or other oxidants to gradually convert Sb(III) to Sb(V), forming sodium pyrostite precipitate under alkaline conditions. However, the oxidation reaction rate of trivalent antimony sulfide complexes in the liquid phase is slow, and the oxygen mass transfer and interfacial reaction efficiency are insufficient, resulting in a long oxidation precipitation time. Moreover, the sodium thiostite system differs from ordinary inorganic antimony salt solutions, containing more reducing sulfur species such as sulfides and thiosulfates. Under oxidizing conditions, these sulfur species are easily over-oxidized to form sodium thiostite. This leads to a decrease in oxygen utilization, an increase in mother liquor salt load, and may affect the quality of sodium pyroantimonate products due to salt entrainment. When the aeration rate is directly increased to improve the reaction rate, the oxidation potential of the system tends to rise rapidly. Although oxygen mass transfer can be enhanced in the short term, it will also exacerbate the formation of sulfate byproducts. Furthermore, the continued high-intensity oxygen supply in the later stage has limited contribution to antimony conversion and is not conducive to the control of side reactions and crystal maturation.

[0004] To address this technical deficiency, a solution is proposed. Summary of the Invention

[0005] The purpose of this invention is to provide an enhanced oxidation method to improve the oxidation rate of sodium thioantimonite, mainly addressing the technical problems that need further improvement in the conversion rate of Sb(III) to Sb(V), the side reaction suppression effect, and the quality stability of sodium pyroantimonite products under atmospheric pressure air oxidation conditions.

[0006] The objective of this invention can be achieved through the following technical solution: an enhanced oxidation method for increasing the oxidation rate of sodium thiostite, comprising the following steps:

[0007] S1. Dissolve sodium hydroxide, sodium sulfide and sodium thiosulfate in deionized water to prepare a sulfur-oxygen buffer solution.

[0008] S2. Place the alkaline leachate containing sodium thiostite in a reaction vessel equipped with a gas distributor and stir. Add sulfur-oxygen buffer and homologous catalytic seed crystals to the reaction vessel. Heat the reaction vessel to 80-85℃ to obtain the reaction solution to be oxidized.

[0009] S3. Using a step-by-step oxidation process, air is introduced into the reaction vessel containing the reaction solution to be oxidized to carry out oxidation and ripening, thereby obtaining an oxidation and ripening reaction solution.

[0010] S4. While still hot, perform solid-liquid separation on the oxidative ripening reaction solution. Wash the separated solids with deionized water at 80-85℃ until pH=8-9, then transfer them to a drying oven at 100-110℃ and dry them until the moisture content is below 0.3% to obtain sodium pyroantimonate product. The separation mother liquor is recycled by adding alkali to prepare a sulfur-oxygen buffer mother liquor.

[0011] Furthermore, in step S1, the concentration of sodium hydroxide in the sulfur-oxygen buffer is 60-80 g / L, the concentration of sodium thiosulfate is 20-40 g / L, and the concentration of sodium sulfide is 2-5 g / L.

[0012] Furthermore, in step S2, the ratio of the alkaline leachate containing sodium thiostite, the sulfur-oxygen buffer solution, and the homologous catalytic seed crystals is 1L:1L:1.5-2g, and the stirring speed is 900-1000r / min.

[0013] Furthermore, the total antimony concentration of the alkaline leachate containing sodium thiostite is 28-30 g / L, the free sodium hydroxide concentration is 50-60 g / L, and the sodium sulfide concentration is 10-12 g / L.

[0014] Furthermore, the preparation method of the homologous catalytic seed crystal is as follows: sodium pyroantimonate is ball-milled and sieved to obtain sodium pyroantimonate particles with a particle size of 5-15 μm; under the protection of an inert gas atmosphere, the sodium pyroantimonate particles and the activation solution are mixed and stirred, the reaction system is heated to 80-90℃, stirred for 60-80 min, and then post-treated to obtain the homologous catalytic seed crystal.

[0015] Furthermore, the solid-liquid ratio of the sodium pyroantimonate particles to the activation solution is 1:5-6. The post-treatment includes: after the reaction is completed, the reaction system is naturally cooled to room temperature under stirring, filtered, the filter cake is washed three times with 1mol / L sodium hydroxide aqueous solution and then dried, sealed and kept to obtain homologous catalytic seed crystals.

[0016] Furthermore, the activation solution is obtained by dissolving a mixture of sodium hydroxide, sodium sulfide, sodium thiosulfate, and sodium antimonothioate nonahydrate in a weight ratio of 50:3-4:20:8-9 in deionized water and then bringing the volume to 1L.

[0017] Furthermore, the stepwise oxidation process is as follows: with a volume of 1L of the reaction liquid to be oxidized, air is continuously introduced into the reactor at a flow rate of 0.4-0.5L / min for 20-30 minutes under normal pressure. Then, the flow rate is increased to 0.8-1.0L / min and continued for 100 minutes. Finally, the flow rate is reduced to 0.3-0.4L / min and continued for 30-40 minutes.

[0018] Furthermore, the method for preparing the sulfur-oxygen buffer mother liquor from the separation mother liquor is as follows: Take the separation mother liquor after antimony precipitation by oxidation of sodium thiostite, and detect the concentrations of sodium thiosulfate, sodium sulfide, and sodium hydroxide in it. Then, add sodium hydroxide and sodium thiosulfate to the mother liquor so that the concentration of sodium hydroxide in the sulfur-oxygen buffer mother liquor reaches 60-80 g / L, the concentration of sodium thiosulfate reaches 20-40 g / L, and the concentration of sodium sulfide reaches 2-5 g / L, thus preparing the sulfur-oxygen buffer solution.

[0019] The present invention has the following beneficial effects:

[0020] 1. This invention utilizes homologous catalytic seed crystals to provide an adsorption, enrichment, and homologous nucleation interface for antimonythionate ions. A sulfur-oxygen buffer solution regulates the redox environment and inhibits sulfate byproducts. A stepped aeration method matches the oxygen supply intensity to the three stages of adsorption, rapid oxidation, and ripening. Subsequent thermal separation, washing, and drying ensure product purity and main component stability, enabling the system to achieve a high degree of reaction and low oxidation rate under normal atmospheric pressure. The amount of antimony produced and the total antimony content of stable sodium pyroantimonate.

[0021] 2. In addition, the present invention further ball-mills and sieves sodium pyroantimonate to obtain sodium pyroantimonate particles with a large effective contact area. Then, it is treated with an activation solution containing sodium hydroxide, sodium sulfide, sodium thiosulfate and sodium thioantimonate nonahydrate to form antimony hydroxylation sites, sulfur coordination sites and antimony-sulfur surface structures compatible with antimony thioantimonate ions on its surface. The homologous catalytic seed crystals serve as nucleation carriers for sodium pyroantimonate products and can also perform interfacial adsorption and enrichment of antimony thioantimonate ions in the liquid phase, promoting preferential oxidation of Sb(III) on the seed crystal surface. The generated Sb(V) is directly deposited and grown on the homologous crystal face, so that the non-solid antimony in the system can be quickly converted into solid-phase sodium pyroantimonate, shortening the antimony oxidation precipitation process and increasing the reaction rate of antimony oxidation precipitation.

[0022] 3. This invention also utilizes a combination of a sulfur-oxygen buffer solution and a stepped aeration method. During the oxidation of sodium thiostite, sodium hydroxide in the sulfur-oxygen buffer solution maintains a strongly alkaline environment, while sodium sulfide and sodium thiosulfate regulate the redox state of the system, ensuring that the oxidation reaction is favorable for the conversion of Sb(III) to Sb(V) but unfavorable for the excessive oxidation of sulfur species. The range of gas flow is as follows: the low gas flow rate in the first section is conducive to the adsorption of seed crystals and the formation of the interfacial reaction layer; the high gas flow rate in the middle section enhances oxygen mass transfer and accelerates antimony oxidation; and the reduced gas flow rate in the last section reduces the continued peroxidation of residual sulfur species and promotes crystal maturation. This allows the oxygen in the air to oxidize the target antimony precipitate while reducing the generation of sulfate byproducts, thereby increasing the oxidation rate while inhibiting the occurrence of side reactions. Detailed Implementation

[0023] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0024] Example 1

[0025] This embodiment provides an enhanced oxidation method to increase the oxidation rate of sodium thiostite, specifically including the following steps:

[0026] Step 1: Preparation of homologous catalytic seed crystals

[0027] Sodium pyroantimonate was ball-milled and sieved to obtain sodium pyroantimonate particles with a particle size of 5-15 μm.

[0028] Weigh out 50g of sodium hydroxide, 3g of sodium sulfide, 20g of sodium thiosulfate, 8g of sodium antimony thiohydrate and 800mL of deionized water, mix and stir to dissolve, then make up to 1L to obtain the activation solution.

[0029] Weigh 100g of sodium pyroantimonate particles and 500mL of activation solution and add them to an argon-protected reaction flask. Stir the mixture at 600r / min and heat it to 80℃. Stir for 60min and allow it to cool naturally to room temperature while stirring. Filter the mixture and wash the filter cake three times with a 1mol / L sodium hydroxide aqueous solution. Dry the cake and seal it to obtain homologous catalytic seed crystals.

[0030] Step 2: Prepare sulfur-oxygen buffer solution

[0031] Sodium hydroxide, sodium sulfide, and sodium thiosulfate were dissolved in deionized water to prepare a sulfur-oxygen buffer solution with a sodium hydroxide concentration of 60 g / L, a sodium thiosulfate concentration of 20 g / L, and a sodium sulfide concentration of 2 g / L.

[0032] Step 3: Prepare the reaction solution to be oxidized

[0033] Weigh out 1L of alkaline leachate containing sodium thiostite and place it in a reaction vessel equipped with a gas distributor. Stir the vessel at a stirring speed of 900 r / min. Add 1L of sulfur-oxygen buffer solution and 1.5g of homologous catalytic seed crystals to the reaction vessel. Heat the reaction vessel to 80℃ to obtain the reaction solution to be oxidized.

[0034] The total antimony concentration of the alkaline leachate containing sodium thiostite was 28 g / L, the free sodium hydroxide concentration was 50 g / L, and the sodium sulfide concentration was 10 g / L.

[0035] Step 4: Oxidative ripening

[0036] At atmospheric pressure, air is introduced into a reactor containing 2L of oxidizing reaction solution. Air is continuously introduced into the reactor at a flow rate of 0.8L / min for 20min. Then the flow rate is increased to 1.6L / min and continued for 100min. The flow rate is then reduced to 0.6L / min and continued for 30min to obtain the oxidizing and ripening reaction solution.

[0037] Step 5: Preparation of sodium pyroantimonate product

[0038] While the oxidative ripening reaction solution is still hot, solid-liquid separation is performed. The separated solids are washed with deionized water at 80°C until pH=8, and then transferred to a drying oven at 100°C to dry until the moisture content is below 0.3%, thus obtaining sodium pyroantimonate product.

[0039] Example 2

[0040] This embodiment provides an enhanced oxidation method to increase the oxidation rate of sodium thiostite, specifically including the following steps:

[0041] Step 1: Preparation of homologous catalytic seed crystals

[0042] Sodium pyroantimonate was ball-milled and sieved to obtain sodium pyroantimonate particles with a particle size of 5-15 μm.

[0043] Weigh out 50g of sodium hydroxide, 3.5g of sodium sulfide, 20g of sodium thiosulfate, 8.5g of sodium antimony thiohydrate, and 800mL of deionized water. Mix and stir to dissolve, then bring the volume to 1L to obtain the activation solution.

[0044] Weigh 100g of sodium pyroantimonate particles and 550mL of activation solution and add them to an argon-protected reaction flask. Stir the mixture at 700r / min and heat it to 85℃. Stir for 70min and allow it to cool naturally to room temperature while stirring. Filter the mixture and wash the filter cake three times with 1mol / L sodium hydroxide aqueous solution. Dry the cake and seal it to obtain homologous catalytic seed crystals.

[0045] Step 2: Prepare sulfur-oxygen buffer solution

[0046] Sodium hydroxide, sodium sulfide, and sodium thiosulfate were dissolved in deionized water to prepare a sulfur-oxygen buffer solution with a sodium hydroxide concentration of 70 g / L, a sodium thiosulfate concentration of 30 g / L, and a sodium sulfide concentration of 3.5 g / L.

[0047] Step 3: Prepare the reaction solution to be oxidized

[0048] Weigh out 1L of alkaline leachate containing sodium thiostite and place it in a reaction vessel equipped with a gas distributor. Stir the vessel at a stirring speed of 950 r / min. Add 1L of sulfur-oxygen buffer solution and 1.7g of homologous catalytic seed crystals to the reaction vessel. Heat the reaction vessel to 83℃ to obtain the reaction solution to be oxidized.

[0049] The total antimony concentration of the alkaline leachate containing sodium thiostite was 29 g / L, the free sodium hydroxide concentration was 55 g / L, and the sodium sulfide concentration was 11 g / L.

[0050] Step 4: Oxidative ripening

[0051] At atmospheric pressure, air is introduced into a reactor containing 2L of reaction solution to be oxidized. Air is continuously introduced into the reactor at a flow rate of 0.9L / min for 25min. Then the flow rate is increased to 1.8L / min and continued for 100min. The flow rate is then reduced to 0.7L / min and continued for 35min to obtain the oxidative ripening reaction solution.

[0052] Step 5: Preparation of sodium pyroantimonate product

[0053] While the oxidative ripening reaction solution is still hot, solid-liquid separation is performed. The separated solids are washed with deionized water at 83°C until pH=8.5, and then transferred to a drying oven at 105°C to dry until the moisture content is below 0.3%, thus obtaining sodium pyroantimonate product.

[0054] Example 3

[0055] This embodiment provides an enhanced oxidation method to increase the oxidation rate of sodium thiostite, specifically including the following steps:

[0056] Step 1: Preparation of homologous catalytic seed crystals

[0057] Sodium pyroantimonate was ball-milled and sieved to obtain sodium pyroantimonate particles with a particle size of 5-15 μm.

[0058] Weigh out 50g of sodium hydroxide, 4g of sodium sulfide, 20g of sodium thiosulfate, 9g of sodium antimony thiohydrate and 800mL of deionized water, mix and stir to dissolve, then make up to 1L to obtain the activation solution;

[0059] Weigh 100g of sodium pyroantimonate particles and 600mL of activation solution and add them to an argon-protected reaction flask. Stir the mixture at 800r / min and heat it to 90℃. Stir for 80min and allow it to cool naturally to room temperature while stirring. Filter the mixture and wash the filter cake three times with a 1mol / L sodium hydroxide aqueous solution. Dry the cake and seal it to obtain homologous catalytic seed crystals.

[0060] Step 2: Prepare sulfur-oxygen buffer solution

[0061] Sodium hydroxide, sodium sulfide, and sodium thiosulfate were dissolved in deionized water to prepare a sulfur-oxygen buffer solution with a sodium hydroxide concentration of 80 g / L, a sodium thiosulfate concentration of 40 g / L, and a sodium sulfide concentration of 5 g / L.

[0062] Step 3: Prepare the reaction solution to be oxidized

[0063] Weigh out 1L of alkaline leachate containing sodium thiostite and place it in a reaction vessel equipped with a gas distributor. Stir the vessel and set the stirring speed to 1000r / min. Add 1L of sulfur-oxygen buffer and 2g of homologous catalytic seed crystals to the reaction vessel. Heat the reaction vessel to 85℃ to obtain the reaction solution to be oxidized.

[0064] The alkaline leachate containing sodium thiostite has a total antimony concentration of 30 g / L, a free sodium hydroxide concentration of 60 g / L, and a sodium sulfide concentration of 12 g / L.

[0065] Step 4: Oxidative ripening

[0066] At atmospheric pressure, air is introduced into a reactor containing 2L of reaction solution to be oxidized. Air is continuously introduced into the reactor at a flow rate of 1.0L / min for 30min. Then the flow rate is increased to 2.0L / min and continued for 100min. The flow rate is then reduced to 0.8L / min and continued for 40min to obtain the oxidative ripening reaction solution.

[0067] Step 5: Preparation of sodium pyroantimonate product

[0068] While the oxidative ripening reaction solution is still hot, solid-liquid separation is performed. The separated solids are washed with deionized water at 85°C until pH=9, and then transferred to a drying oven at 110°C to dry until the moisture content is below 0.3%, thus obtaining sodium pyroantimonate product.

[0069] Example 4

[0070] This embodiment provides an enhanced oxidation method to increase the oxidation rate of sodium thiostite, specifically including the following steps:

[0071] Step 1: Preparation of homologous catalytic seed crystals

[0072] Sodium pyroantimonate was ball-milled and sieved to obtain sodium pyroantimonate particles with a particle size of 5-15 μm.

[0073] Weigh out 50g of sodium hydroxide, 4g of sodium sulfide, 20g of sodium thiosulfate, 9g of sodium antimony thiohydrate and 800mL of deionized water, mix and stir to dissolve, then make up to 1L to obtain the activation solution;

[0074] Weigh 100g of sodium pyroantimonate particles and 600mL of activation solution and add them to an argon-protected reaction flask. Stir the mixture at 800r / min and heat it to 90℃. Stir for 80min and allow it to cool naturally to room temperature while stirring. Filter the mixture and wash the filter cake three times with a 1mol / L sodium hydroxide aqueous solution. Dry the cake and seal it to obtain homologous catalytic seed crystals.

[0075] Step 2: Prepare sulfur-oxygen buffer solution

[0076] Take the separation mother liquor after antimony precipitation by sodium thiostite oxidation, and test the concentrations of sodium thiosulfate, sodium sulfide, and sodium hydroxide. Then, add sodium hydroxide and sodium thiosulfate to the mother liquor to make the concentration of sodium hydroxide in the sulfur-oxygen buffer mother liquor reach 80 g / L, the concentration of sodium thiosulfate reach 40 g / L, and the concentration of sodium sulfide reach 5 g / L, thus preparing the sulfur-oxygen buffer solution.

[0077] Step 3: Prepare the reaction solution to be oxidized

[0078] Weigh out 1L of alkaline leachate containing sodium thiostite and place it in a reaction vessel equipped with a gas distributor. Stir the vessel and set the stirring speed to 1000r / min. Add 1L of sulfur-oxygen buffer and 2g of homologous catalytic seed crystals to the reaction vessel. Heat the reaction vessel to 85℃ to obtain the reaction solution to be oxidized.

[0079] The alkaline leachate containing sodium thiostite has a total antimony concentration of 30 g / L, a free sodium hydroxide concentration of 60 g / L, and a sodium sulfide concentration of 12 g / L.

[0080] Step 4: Oxidative ripening

[0081] At atmospheric pressure, air is introduced into a reactor containing 2L of reaction solution to be oxidized. Air is continuously introduced into the reactor at a flow rate of 1.0L / min for 30min. Then the flow rate is increased to 2.0L / min and continued for 100min. The flow rate is then reduced to 0.8L / min and continued for 40min to obtain the oxidative ripening reaction solution.

[0082] Step 5: Preparation of sodium pyroantimonate product

[0083] While the oxidative ripening reaction solution is still hot, solid-liquid separation is performed. The separated solids are washed with deionized water at 85°C until pH=9, and then transferred to a drying oven at 110°C to dry until the moisture content is below 0.3%, thus obtaining sodium pyroantimonate product.

[0084] Comparative Example 1

[0085] The difference between this comparative example and Example 3 is that step 1 is omitted, and the sodium pyroantimonate particles in step 1 are used instead of the homologous catalytic seed crystals in step 3.

[0086] Comparative Example 2

[0087] The difference between this comparative example and Example 3 is that no homologous catalytic seed crystals were added in step 3.

[0088] Comparative Example 3

[0089] The difference between this comparative example and Example 3 is that sodium sulfide and sodium thiosulfate were not added to the sulfur-oxygen buffer solution in step 2.

[0090] Comparative Example 4

[0091] The difference between this comparative example and Example 3 is that the oxidation and ripening operation in step 4 is adjusted as follows: under normal pressure, air is introduced into the reactor containing 2L of reaction solution to be oxidized, and air is continuously introduced into the reactor for 170 minutes at a flow rate of 2.0L / min to obtain the oxidation and ripening reaction solution.

[0092] Performance testing:

[0093] In the oxidation ripening reaction stage of Examples 1-4 and Comparative Examples 1-4, the content of non-solid antimony in the oxidation ripening reaction solution was measured at 30, 50, 70, 90, and 120 min of oxidation ripening reaction, and the content was determined according to the formula. The degree of reaction is calculated at different reaction time points, where w0 is the total antimony content in the alkaline leachate containing sodium thiostite, and w t The content of non-solid antimony in the oxidative ripening reaction solution is measured at 30, 50, 70, 90, and 120 min. The antimony content in the liquid can be determined with reference to standard HJ 1046-2019.

[0094] The determination of the oxidizing reaction solution and oxidative ripening reaction solution in Examples 1-4 and Comparative Examples 1-4 The content in the oxidative ripening reaction solution and the reaction solution to be oxidized was calculated. The difference in content in the reaction solution The content can be determined according to standard GB / T 23844-2019;

[0095] The total antimony content in the sodium pyroantimonate products prepared in Examples 1-4 and Comparative Examples 1-4 was determined according to standard HG / T 3254-2010.

[0096] The above performance test data consisted of at least five sets, and then the arithmetic mean was taken. The specific test data is shown in Table 1 below.

[0097] Table 1 - Performance Measurement Data of Samples

[0098]

[0099] Data Analysis:

[0100] Comparative analysis of the data in Table 1 above shows that in Examples 1-3, with appropriate increases in the activation intensity of homologous catalytic seed crystals, concentration of sulfur-oxygen buffer solution, amount of seed crystals added, reaction temperature, and aeration intensity, the degree of reaction and the total antimony content of the product all showed a gradual increasing trend. The content difference gradually decreases, indicating that by enhancing the activation of the seed crystal surface, improving the sulfur-oxygen buffering capacity, and matching an appropriate oxygen supply intensity, the conversion of thioantimonite to sodium pyroantimonite can be promoted, while reducing the side reaction of excessive oxidation of sulfur species to sulfate.

[0101] Example 4 uses the mother liquor after antimony oxidation and precipitation, which, after replenishment and adjustment, serves as a sulfur-oxygen buffer solution, and its performance is similar to that of Example 3. This indicates that even after testing and replenishment of components such as sodium hydroxide and sodium thiosulfate, the mother liquor can still maintain a good sulfur-oxygen buffering effect and will not significantly weaken the interfacial catalysis and nucleation induction effect of homologous catalytic seeds. The mother liquor in the method of this invention has good reusability.

[0102] In Comparative Example 1, unactivated sodium pyroantimonate particles were used instead of homologous catalytic seeds. Compared with Example 3, the degree of reaction at each stage in Comparative Example 1 decreased. The concentration difference increased to 535 mg / L. This indicates that although the addition of sodium pyroantimonate particles can provide a certain homologous nucleation interface, the lack of hydroxylated antimony sites, sulfur coordination sites, and antimony-sulfur compatible structures constructed by the activation solution on its surface results in insufficient adsorption and enrichment capacity for thioantimonite and interfacial oxidation-promoting capacity, leading to a decrease in both the degree of reaction and the side reaction inhibition effect.

[0103] Comparative Example 2 did not include homologous catalytic seeds. Compared to Example 3, the degree of reaction in Comparative Example 2 decreased significantly at each stage, and the total antimony content of the product also decreased to 63.3%. The concentration difference increased to 660 mg / L. This indicates that, without homologous catalytic seeds, the antimony thioate in the system mainly relies on liquid-phase oxidation and spontaneous nucleation, lacking effective interfacial enrichment sites and homologous deposition supports. This leads to a significant slowdown in the conversion of non-solid antimony to solid-phase sodium pyroantimonate. In the reaction, more oxygen participates in the by-oxidation of sulfur species, proving that homologous catalytic seeds can guide oxygen to preferentially oxidize and precipitate the target antimony species.

[0104] In Comparative Example 3, no sodium sulfide or sodium thiosulfate was added to the sulfur-oxygen buffer solution. Compared to Example 3, the degree of reaction at each stage was reduced, but still higher than that in Comparative Example 1 and Comparative Example 2. This indicates that the homologous catalytic seed crystals can still play a certain role in promoting oxidation and nucleation. In contrast, in Comparative Example 3... The concentration difference increased to 920 mg / L, significantly higher than the 410 mg / L in Example 3. This indicates that if the system relies solely on sodium hydroxide to maintain strong alkalinity, lacking the sulfur-oxygen buffer system composed of sodium sulfide and sodium thiosulfate, sulfur species are easily over-oxidized during air oxidation. This leads to a significant enhancement of side reactions, proving that the key role of the sulfur-oxygen buffer is not just to provide an alkaline environment, but to regulate the redox state of the system, placing it in a reaction range that is conducive to the oxidation of Sb(III) to antimony precipitation, but unfavorable to the peroxidation of sulfur species.

[0105] Comparative Example 4 changed the stepwise ventilation to a constant high-flow-rate ventilation of 2.0 L / min throughout. Compared with Example 3, the reaction rate of Comparative Example 4 at 30 min was 38.6%, slightly higher than that of Example 3 (38.1%), indicating that the high flow rate can enhance oxygen mass transfer and bring a certain instantaneous promoting effect in the initial stage. However, as the reaction progressed, the reaction rate of Comparative Example 4 at 50 min, 70 min, 90 min, and 120 min was significantly lower than that of Example 3. Meanwhile, the reaction rate of Comparative Example 4... The content difference increased to 625 mg / L, while the total antimony content of the product decreased to 64.1%. This indicates that excessively high oxygen supply in the early stage is not conducive to the stable formation of the adsorption layer and interface reaction layer on the seed crystal surface, while continuous high gas volume in the middle and later stages easily promotes the excessive oxidation of sulfur species and affects the maturation of sodium pyroantimonate crystals.

[0106] As can be seen from the comprehensive examples and comparative data, the present invention provides an adsorption enrichment and homologous nucleation interface for antimony thiosulfinate ions by using homologous catalytic seed crystals, regulates the redox environment of the system with sulfur-oxygen buffer solution and inhibits sulfate by-products, and, in conjunction with stepwise aeration, improves the oxidation rate and the quality stability of sodium pyroantimonate product while suppressing side reactions, and has good adaptability to the reuse of the reaction mother liquor.

[0107] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for enhancing the oxidation rate of sodium thiostite, characterized in that, Includes the following steps: S1. Dissolve sodium hydroxide, sodium sulfide and sodium thiosulfate in deionized water to prepare a sulfur-oxygen buffer solution. S2. Place the alkaline leachate containing sodium thiostite in a reaction vessel equipped with a gas distributor and stir. Add sulfur-oxygen buffer and homologous catalytic seed crystals to the reaction vessel. Heat the reaction vessel to 80-85℃ to obtain the reaction solution to be oxidized. S3. Using a step-by-step oxidation process, air is introduced into the reaction vessel containing the reaction solution to be oxidized to carry out oxidation and ripening, thereby obtaining an oxidation and ripening reaction solution. S4. While still hot, perform solid-liquid separation on the oxidative ripening reaction solution. Wash the separated solids with deionized water at 80-85℃ until pH=8-9, then transfer them to a drying oven at 100-110℃ and dry them until the moisture content is below 0.3% to obtain sodium pyroantimonate product. The separation mother liquor is recycled by adding alkali to prepare a sulfur-oxygen buffer mother liquor.

2. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 1, characterized in that, In step S1, the concentration of sodium hydroxide in the sulfur-oxygen buffer is 60-80 g / L, the concentration of sodium thiosulfate is 20-40 g / L, and the concentration of sodium sulfide is 2-5 g / L.

3. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 1, characterized in that, In step S2, the ratio of the alkaline leachate containing sodium thiostite, the sulfur-oxygen buffer solution, and the homologous catalytic seed crystals is 1L:1L:1.5-2g, and the stirring speed is 900-1000r / min.

4. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 3, characterized in that, The alkaline leachate containing sodium thiostite has a total antimony concentration of 28-30 g / L, a free sodium hydroxide concentration of 50-60 g / L, and a sodium sulfide concentration of 10-12 g / L.

5. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 1, characterized in that, The preparation method of homologous catalytic seed crystals is as follows: sodium pyroantimonate is ball-milled and sieved to obtain sodium pyroantimonate particles with a particle size of 5-15 μm; under the protection of an inert gas atmosphere, the sodium pyroantimonate particles and the activation solution are mixed and stirred, the reaction system is heated to 80-90℃ and stirred for 60-80 min, and then post-treated to obtain homologous catalytic seed crystals.

6. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 5, characterized in that, The solid-liquid ratio of the sodium pyroantimonate particles and the activation solution is 1:5-6. The post-treatment includes: after the reaction is completed, the reaction system is naturally cooled to room temperature under stirring, filtered, the filter cake is washed three times with 1mol / L sodium hydroxide aqueous solution and then dried, sealed and kept to obtain homologous catalytic seed crystals.

7. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 5, characterized in that, The activation solution is obtained by dissolving a mixture of sodium hydroxide, sodium sulfide, sodium thiosulfate, and sodium antimonothiohydrate in a weight ratio of 50:3-4:20:8-9 in deionized water and then bringing the volume to 1L.

8. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 1, characterized in that, The stepwise oxidation process is as follows: with a volume of 1L of reaction liquid to be oxidized, air is continuously introduced into the reactor at a flow rate of 0.4-0.5L / min for 20-30 minutes under normal pressure. Then, the flow rate is increased to 0.8-1.0L / min and continued for 100 minutes. Finally, the flow rate is reduced to 0.3-0.4L / min and continued for 30-40 minutes.

9. The enhanced oxidation method for increasing the oxidation rate of sodium thiostite according to claim 1, characterized in that, The method for preparing sulfur-oxygen buffer mother liquor from the separation mother liquor is as follows: Take the separation mother liquor after antimony precipitation by oxidation of sodium thiostite, and detect the concentrations of sodium thiosulfate, sodium sulfide, and sodium hydroxide in it. Then, add sodium hydroxide and sodium thiosulfate to the mother liquor so that the concentration of sodium hydroxide in the sulfur-oxygen buffer mother liquor reaches 60-80 g / L, the concentration of sodium thiosulfate reaches 20-40 g / L, and the concentration of sodium sulfide reaches 2-5 g / L, thus preparing the sulfur-oxygen buffer solution.