Precision casting process for turbine blades

By controlling the silica sol content and adding polyurethane foam and eutectic white cast iron particles, the problems of high turbine blade shell strength and poor yielding were solved, improving the high-temperature creep performance and fatigue performance of turbine blades and preventing cracks.

CN122938239BActive Publication Date: 2026-11-24SHANGHAI WANZE PRECISION CASTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611435423.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-24
Estimated Expiration
2046-09-16

AI Technical Summary

Technical Problem

In the existing precision casting process for turbine blades, the high amount of silica sol added to the mold shell results in high strength and poor yielding after the mold shell is baked. Stress concentration occurs during the solidification process of the turbine blade, affecting its high-temperature creep performance and fatigue performance.

Method used

By controlling the silica sol content, the amount of mullite generated in the shell is reduced, enhancing microelasticity. Polyurethane foam occupiers and eutectic white cast iron particles are placed at the root of the convex side of the shell blade and the root of the rim plate to buffer solidification shrinkage stress and locally accelerate solidification.

Benefits of technology

It effectively reduces the solidification shrinkage stress of turbine blades, reduces residual stress, improves high-temperature creep performance and fatigue performance, and prevents crack formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122938239B_ABST
    Figure CN122938239B_ABST
Patent Text Reader

Abstract

This application relates to a precision casting process for turbine blades, specifically within the field of precision casting technology. The process includes preparing an inner mold shell blank layer on a turbine blade wax model; installing a tooling fixture on the inner mold shell blank layer, with the fixture's recess covering the convex adjustment area; injecting polyurethane foam into the recess, which, after curing, forms a polyurethane block; removing the tooling and applying a low-silica outer layer slurry to the polyurethane block location, followed by baking; the polyurethane block decomposes to form hollows; coating the hollows with eutectic white cast iron particles mixed with an inorganic binder; and casting using a mold shell. The eutectic white cast iron particles, through melting and heat absorption, cool the junction between the blade and the shroud, accelerating solidification. This application utilizes the micro-elasticity of the low-silica mold shell to release shrinkage stress, combined with the melting and heat absorption of the eutectic white cast iron particles at stress concentration points to accelerate local solidification. This reduces the solidification shrinkage stress of the turbine blade at both the overall and local levels, effectively inhibiting recrystallization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of precision casting, and in particular to the precision casting of turbine blades. Background Technology

[0002] Turbine blades are core hot-section components of aero engines and are typically formed using investment casting. In existing technology, the steps for manufacturing turbine blades are as follows: A slurry is applied to the surface of the turbine blade wax mold and then sand-coated to form an inner mold shell blank layer, ensuring the surface quality of the casting. This process is repeated to form a reinforcing layer on the outer side, which is the main source of the shell's strength. The reinforcing layer slurry is typically prepared by mixing silica sol, fused alumina powder, mullite powder, and fused alumina sand in specific proportions. After each layer is applied, the mold is fired to obtain the shell. The turbine blade is then cast using this shell, and after solidification, the turbine blade is obtained. Following the turbine blade, subsequent heat treatment is performed to impart the required high-temperature strength.

[0003] Regarding shell preparation, existing outer layer slurry formulations contain a high amount of silica sol, resulting in high strength but poor resilience after shell firing. During turbine blade solidification, the solidification shrinkage is hindered by the rigidity of the shell, especially in the transition section where the blade body connects to the shroud. This abrupt change in cross-section leads to stress concentration and generates significant residual stress. This residual stress becomes the primary cause of recrystallization during subsequent high-temperature heat treatment, significantly reducing the turbine blade's high-temperature creep resistance and fatigue performance. Summary of the Invention

[0004] The purpose of this invention is to provide a precision casting process for turbine blades to solve at least one of the above-mentioned technical problems.

[0005] The technical problem solved by this invention can be achieved by the following technical solutions: The precision casting process for turbine blades includes the following steps: a. Preparing the inner mold shell blank: The turbine blade wax mold is coated with slurry and sand to form an inner mold shell blank layer. The inner mold shell blank layer has an inner mold shell blank transition section at the connection between the blade forming position and the blade forming position. The inner mold shell blank transition section has a convex adjustment area corresponding to the root of the convex side of the blade and the root of the blade. b. Preparation of tooling: The tooling includes a base with a downward-opening receiving cavity that accommodates the inner mold shell blank transition section; The base is equipped with a locking mechanism to lock the inner mold shell blank layer; The base has a recess above the receiving cavity, and the opening edge of the recess covers the convex adjustment area; The base is fitted with a sealing ring surrounding the recessed opening; The base is provided with a filling port, which is connected to the recessed area through the recessed upper bottom; c. Application tooling: A layer of paraffin is sprayed onto the inner wall of the recess, the base is locked to the transition section of the inner mold blank, and the sealing ring seals the recess above the convex adjustment area. Polyurethane foam is injected into the depression through the injection port. The polyurethane foam fills the depression and forms a polyurethane block after curing. Remove the tooling, and the inner wall of the recess is separated from the polyurethane block through the paraffin layer; d. Adhesion of outer slurry and firing of the mold shell: Prepare the outer layer slurry to adhere to the inner mold shell blank layer. The outer layer slurry comprises the following components by mass percentage: Silica sol 15%–16%, fused alumina powder 24%–25%, mullite powder 36%–37%, fused alumina sand 18%–19%, distilled water 3%–5%, wood fiber 1%–2%; Apply the outer layer slurry to the outside of the inner mold shell blank, avoiding the top of the polyurethane block, with a thickness of 3-10 mm to achieve the desired firing thickness. After firing, a shell is obtained, and the polyurethane block decomposes during the firing of the shell to form a hollow structure. e. Casting and solidification: After the shell is fired, eutectic white cast iron particles mixed with inorganic binder are coated on the hollowed-out areas. The casting process using a mold shell allows eutectic white cast iron particles to absorb heat during melting, thereby cooling and accelerating solidification at the junction of the turbine blade and the rim plate.

[0006] When turbine blades shrink during solidification, the turbine shell, due to its high-temperature strength, resists deformation. However, when the shell strength exceeds the turbine blade's shrinkage stress, the shell does not undergo compliant deformation, hindering turbine blade shrinkage and causing stress concentration at abrupt changes in the cross-section. Plastic deformation occurs inside the turbine blade and is retained as residual stress. This residual stress becomes a catalyst for recrystallization during subsequent high-temperature heat treatment, significantly reducing the turbine blade's high-temperature creep and fatigue performance, thereby increasing the risk of cracking during subsequent service.

[0007] This invention controls the content of silica sol, resulting in a reduction in mullite in the overall shell after calcination. This leads to a decrease in high-temperature strength and rigidity, while enhancing microelasticity. Consequently, it provides a slight elasticity relative to the original shell, offering a small amount of variable compensation for cooling and shrinkage. When the turbine blades solidify and shrink, the shell adapts to the deformation through microelasticity to buffer the shrinkage force.

[0008] Stress is more concentrated at the abrupt changes in the cross-section of turbine blades. Polyurethane foam occupies space and acts as a placeholder in the convex adjustment areas at the root of the blade's convex side and the root of the rim plate, preventing the subsequent outer coating from covering these areas. During firing, the polyurethane block decomposes, creating hollow areas. Before casting the turbine blade, eutectic white cast iron particles are placed in these hollow areas. During solidification, these particles undergo a phase transformation near the turbine blade's solidification temperature, absorbing heat and accelerating local solidification. This compresses the time window for stress accumulation, ensuring pre-cooling and support at the abrupt changes in the turbine blade's cross-section. This ensures that the abrupt changes are pre-formed with sufficient molten metal, while also eliminating common cracks in these areas.

[0009] By controlling the content of silica sol to make the shell slightly elastic, and by setting eutectic white cast iron particles at the abrupt change of cross section to accelerate solidification through phase transformation, the solidification shrinkage stress of the turbine blade is reduced at both the overall and local levels. As a result, the recrystallization process is effectively suppressed during subsequent heat treatment, thereby enabling the high-temperature creep performance and fatigue performance of the turbine blade to reach the design expectations.

[0010] Preferably, the base is provided with an exhaust port, which is connected to the recessed upper bottom through the recess, and the injection port and the exhaust port are spaced apart on the upper bottom of the recess.

[0011] During the process of injecting polyurethane foam into the depression, the air inside the depression is compressed by the polyurethane foam. As the amount of polyurethane foam increases, the pressure inside the depression continues to rise, which may result in incomplete filling of the polyurethane foam or the base being pushed apart from the inner mold shell layer during the injection of polyurethane foam.

[0012] An vent is installed on the base and connected to the recess, allowing the injection of polyurethane foam and the expulsion of air to occur simultaneously. This ensures that the pressure inside the recess is always balanced with the external atmospheric pressure, guaranteeing full filling of the polyurethane foam and a stable filling process. Furthermore, the spacing between the injection port and the vent ensures that the polyurethane foam fills the entire recess before reaching the vent.

[0013] Preferably, the exhaust port is conical, and the inner diameter of the end of the exhaust port facing the recess is greater than the inner diameter of the end of the exhaust port away from the recess.

[0014] When gas flows from inside the depression through the conical exhaust port, the cross-sectional area of ​​the flow channel gradually narrows along the flow direction, and the airflow velocity gradually increases along the flow direction. The increased flow velocity creates a larger pressure difference between the inlet and outlet of the exhaust port. This pressure difference drives the gas inside the depression to be discharged from the exhaust port more quickly. In conjunction with the expansion of polyurethane foam inside the depression, the gas inside the depression can be further discharged.

[0015] Meanwhile, the vent is designed with a larger diameter at the end facing the recess and a smaller diameter at the end away from the recess. When separating the base from the inner mold shell blank, the polyurethane block that has solidified and remains in the vent can be smoothly separated in the formed conical channel without damaging the shape of the polyurethane block.

[0016] Preferably, the locking mechanism includes a tension spring and two pins connected to both ends of the tension spring; The base has two pin holes spaced apart at the edge of its receiving cavity; these pin holes are called locking pin holes. The two pins are respectively inserted into the two locking pin holes; This results in a locking mechanism in which the tension spring locks the inner mold shell blank layer to the base.

[0017] The inner mold shell blank layer is formed layer by layer on the surface of the turbine blade wax mold by applying slurry and sand. This process determines that the surface of the inner mold shell blank layer will inevitably have microscopic unevenness, and the dimensions of the inner mold shell blank layer will have certain manufacturing tolerances between different batches and between different individuals in the same batch.

[0018] A tension spring connects two pins, which engage with pin holes at the edge of the base cavity to achieve locking. The tension spring applies a continuous elastic force between the two pins. This elastic force establishes a flexible force transmission path between the locking surfaces. When the dimensions of the inner mold shell blank fluctuate within the tolerance range, the tension spring adapts to the dimensional changes of the inner mold shell blank by slightly altering its own elongation, thereby ensuring that the inner mold shell blank can be stably locked onto the base.

[0019] Preferably, the surface of the receiving cavity of the base is provided with an elastic rubber layer, the thickness of which is 0.3~0.6 mm.

[0020] During the fabrication process, the inner mold shell blank inevitably develops microscopic unevenness on its surface. When the base cavity surface is in direct rigid contact with the inner mold shell blank, the locking force only acts on the protruding points on the surface of the inner mold shell blank. As the base and the inner mold shell blank tighten, cracks will appear in the inner mold shell blank. However, by setting an elastic rubber layer on the cavity surface and adjusting the thickness of the elastic rubber layer, the elastic rubber layer is compressed and deformed when the base and the inner mold shell blank are locked, embedding itself in the microscopic pits of the inner mold shell blank and simultaneously wrapping the protruding points. This allows the locking force to be evenly distributed, thereby reducing the occurrence of indentations and cracks on the surface of the inner mold shell blank.

[0021] Preferably, in step d, after the firing thickness is reached, the shell is first maintained at a temperature of 400-600 degrees Celsius for 60-90 minutes to thermally decompose the polyurethane block, and then the temperature is raised to 1000-1100 degrees Celsius for high-temperature firing of the shell.

[0022] This technical solution involves maintaining the polyurethane block at 400-600 degrees Celsius for 60-90 minutes to ensure complete decomposition without the appearance of carbon impurities. Subsequently, the temperature is raised to 1000-1100 degrees Celsius for high-temperature firing of the shell, which provides sufficient firing strength.

[0023] In summary, this application includes at least one of the following beneficial technical effects: 1. This invention controls the content of silica sol, resulting in a reduction of mullite in the overall shell after calcination, leading to decreased high-temperature strength, weakened rigidity, and enhanced micro-elasticity. This provides a slight elasticity relative to the original shell, offering a small amount of variable compensation for cooling and shrinkage. When the turbine blades solidify and shrink, the shell adapts to deformation through micro-elasticity to buffer the shrinkage force. 2. Turbine blades exhibit greater stress concentration at abrupt changes in cross-section. Polyurethane foam occupies space and acts as a placeholder in the convex adjustment areas at the root of the blade's convex side and the root of the rim plate, preventing subsequent outer coating slurry from covering these areas. During firing, the polyurethane block decomposes, creating hollow areas. Before turbine blade casting, eutectic white cast iron particles are placed in these hollow areas. During solidification, these particles undergo a phase transformation near the turbine blade's solidification temperature, absorbing heat and accelerating local solidification. This compresses the stress accumulation time window, ensuring pre-cooling and support at abrupt changes in cross-section, guaranteeing pre-forming of these areas with sufficient molten metal and eliminating common cracks in these locations. 3. By controlling the content of silica sol to make the shell slightly elastic, and by setting eutectic white cast iron particles at the abrupt change of cross section to accelerate solidification through phase transformation, the solidification shrinkage stress of the turbine blade is reduced at both the overall and local levels. As a result, the recrystallization process is effectively suppressed during subsequent heat treatment, thereby enabling the high-temperature creep performance and fatigue performance of the turbine blade to reach the design expectations. Attached Figure Description

[0024] Figure 1 This application is a structural schematic diagram illustrating the assembly relationship between the tooling and the inner mold shell blank layer; Figure 2 for Figure 1 The cross-sectional view along AA shows the assembly relationship between the tooling and the inner mold shell blank layer; Figure 3 This is a structural schematic diagram of the tooling used in this application.

[0025] Reference numerals in the attached drawings: 1. Inner mold shell blank layer; 2. Base; 3. Locking mechanism; 4. Recess; 5. Sealing ring; 6. Injection port; 7. Vent. Detailed Implementation

[0026] The following is in conjunction with the appendix Figure 1 - Appendix Figure 3 This application will be described in further detail.

[0027] Reference Figure 1 , Figure 2 and Figure 3 The precision casting process for turbine blades includes the following steps: a. Preparation of inner mold shell blank layer 1: The turbine blade wax mold is coated with slurry and sand to form an inner mold shell blank layer 1. The inner mold shell blank layer 1 has an inner mold shell blank transition section at the connection between the blade forming position and the blade forming position. The inner mold shell blank transition section has a convex adjustment area corresponding to the root of the convex side of the blade and the root of the blade.

[0028] b. Preparation of tooling: The fixture includes a base 2 with a downward-facing receiving cavity that accommodates the inner mold shell blank transition section. A locking mechanism 3 is provided on the base 2 to lock the inner mold shell blank layer 1. A recess 4 is provided above the receiving cavity on the base 2, and the opening edge of the recess 4 covers the convex adjustment area. A sealing ring 5 is fitted around the opening of the recess 4 on the base 2. A filling port 6 is provided on the base 2, and the filling port 6 connects to the recess 4 through the upper bottom of the recess 4.

[0029] c. Application tooling: A paraffin wax layer is sprayed onto the inner wall of the recess 4. The base 2 is locked to the transition section of the inner mold blank, and the sealing ring 5 seals the recess 4 above the convex adjustment area. Polyurethane foam is injected into the recess 4 through the injection port 6. The polyurethane foam fills the recess 4 and forms a polyurethane block after curing. The tooling is removed, and the inner wall of the recess 4 separates from the polyurethane block through the paraffin wax layer.

[0030] d. Adhesion of outer slurry and firing of the mold shell: Prepare the outer layer slurry to adhere to the inner mold shell blank layer 1. The outer layer slurry comprises the following components by mass percentage: 15%–16% silica sol, 24%–25% fused alumina powder, 36%–37% mullite powder, 18%–19% fused alumina sand, 0.5%–1% reinforcing agent, 3%–5% distilled water, and 1%–2% wood fiber.

[0031] The outer layer of slurry is applied to the outside of the inner mold shell blank layer 1, avoiding the top of the polyurethane block. The thickness of the slurry is 3-10 mm to achieve the desired firing thickness. After firing, the mold shell is obtained. The polyurethane block decomposes during the firing of the mold shell, forming hollows.

[0032] e. Casting and solidification: After the mold shell is fired, eutectic white cast iron particles mixed with an inorganic binder are coated onto the hollow areas. Using the mold shell for casting, the eutectic white cast iron particles absorb heat through melting, which cools the junction between the turbine blade and the rim and accelerates solidification.

[0033] When turbine blades shrink during solidification, the turbine shell, due to its high-temperature strength, resists deformation. However, when the shell strength exceeds the turbine blade's shrinkage stress, the shell does not undergo compliant deformation, hindering turbine blade shrinkage and causing stress concentration at abrupt changes in the cross-section. Plastic deformation occurs inside the turbine blade and is retained as residual stress. This residual stress becomes a catalyst for recrystallization during subsequent high-temperature heat treatment, significantly reducing the turbine blade's high-temperature creep and fatigue performance, thereby increasing the risk of cracking during subsequent service.

[0034] This invention controls the content of silica sol, resulting in a reduction in mullite in the overall shell after calcination. This leads to a decrease in high-temperature strength and rigidity, while enhancing microelasticity. Consequently, it provides a slight elasticity relative to the original shell, offering a small amount of variable compensation for cooling and shrinkage. When the turbine blades solidify and shrink, the shell adapts to the deformation through microelasticity to buffer the shrinkage force.

[0035] Stress is more concentrated at the abrupt changes in the cross-section of turbine blades. Polyurethane foam occupies space and acts as a placeholder in the convex adjustment areas at the root of the blade's convex side and the root of the rim plate, preventing the subsequent outer coating from covering these areas. During firing, the polyurethane block decomposes, creating hollow areas. Before casting the turbine blade, eutectic white cast iron particles are placed in these hollow areas. During solidification, these particles undergo a phase transformation near the turbine blade's solidification temperature, absorbing heat and accelerating local solidification. This compresses the time window for stress accumulation, ensuring pre-cooling and support at the abrupt changes in the turbine blade's cross-section. This ensures that the abrupt changes are pre-formed with sufficient molten metal, while also eliminating common cracks in these areas.

[0036] By controlling the content of silica sol to make the shell slightly elastic, and by setting eutectic white cast iron particles at the abrupt change of cross section to accelerate solidification through phase transformation, the solidification shrinkage stress of the turbine blade is reduced at both the overall and local levels. As a result, the recrystallization process is effectively suppressed during subsequent heat treatment, thereby enabling the high-temperature creep performance and fatigue performance of the turbine blade to reach the design expectations.

[0037] Example 1

[0038] Reference Figure 1 , Figure 2 and Figure 3In this embodiment, the base 2 can use simulation software to perform numerical simulation calculations on the solidification and cooling process of the turbine blade, obtain the stress change distribution map of the turbine blade, lock the stress concentration area of ​​the turbine blade, and obtain the shape parameters according to the required thickness of the inner mold shell blank layer 1. Based on the three-dimensional contour data of the transition section of the inner mold shell blank, the base 2 with a receiving cavity is made by 3D printing, and the inner wall surface of the receiving cavity is basically consistent with the outer surface shape of the transition section of the inner mold shell blank layer 1.

[0039] In this embodiment, the base 2 is provided with an exhaust port 7, which is connected to the recess 4 through the upper bottom of the recess 4, and the injection port 6 and the exhaust port 7 are spaced apart on the upper bottom of the recess 4.

[0040] During the process of injecting polyurethane foam into the depression 4, the original air in the depression 4 is compressed by the polyurethane foam. As the amount of polyurethane foam increases, the pressure in the depression 4 continues to rise, which may result in the polyurethane foam not being filled properly, or the base 2 being pushed apart from the inner mold shell layer 1 during the injection of polyurethane foam.

[0041] An exhaust port 7 is provided on the base 2 and is connected to the recess 4, so that the injection of polyurethane foam and the expulsion of air are synchronized. The pressure inside the recess 4 is always balanced with the external atmospheric pressure, ensuring that the polyurethane foam is fully filled and the filling process is stable. At the same time, the interval between the injection port 6 and the exhaust port 7 ensures that the polyurethane foam fills the entire recess 4 before reaching the exhaust port 7.

[0042] The exhaust port 7 is conical, with the inner diameter of the end facing the recess 4 being larger than the inner diameter of the end away from the recess 4. When gas flows from inside the recess 4 through the conical exhaust port 7, the cross-sectional area of ​​the flow channel gradually narrows along the flow direction, and the airflow velocity gradually increases along the flow direction. The increased velocity creates a larger pressure difference between the inlet and outlet of the exhaust port 7. This pressure difference drives the gas inside the recess 4 to be discharged more quickly from the exhaust port 7. Combined with the expansion of polyurethane foam inside the recess 4, the gas inside the recess 4 can be further discharged. At the same time, the exhaust port 7 is designed with a larger diameter at the end facing the recess 4 and a smaller diameter at the end away from the recess 4. When separating the base 2 from the inner mold shell blank layer 1, the solidified polyurethane block remaining in the exhaust port 7 can be smoothly separated within the formed conical channel without damaging the shape of the polyurethane block.

[0043] The locking mechanism 3 includes a tension spring and two pins connected to both ends of the tension spring. Two pin holes, called locking pin holes, are spaced apart at the edge of the receiving cavity of the base 2. The two pins are respectively inserted into the two locking pin holes. This forms the locking mechanism 3, whereby the tension spring locks the inner mold shell blank layer 1 to the base 2.

[0044] The inner mold shell blank layer 1 is formed layer by layer on the surface of the turbine blade wax mold by applying slurry and sand. This process determines that the surface of the inner mold shell blank layer 1 will inevitably have microscopic unevenness, and the dimensions of the inner mold shell blank layer 1 have certain manufacturing tolerances between different batches and between different individuals in the same batch.

[0045] A tension spring connects two pins, which are engaged with pin holes at the edge of the base 2's receiving cavity to achieve locking. The tension spring applies a continuous elastic force between the two pins. This elastic force establishes a flexible force transmission path between the locking mating surfaces. When the dimensions of the inner mold shell blank 1 fluctuate within the tolerance range, the tension spring adapts to the dimensional changes of the inner mold shell blank 1 through a slight change in its own elongation, thereby ensuring that the inner mold shell blank 1 can be stably locked onto the base 2.

[0046] When the inner mold shell layer 1 is too thick, the tension spring extends appropriately to generate a slightly larger elastic force, but it is still within the range that the inner mold shell layer 1 can withstand. When the inner mold shell layer 1 is too thin, the tension spring shortens appropriately to generate a slightly smaller elastic force, but it is still sufficient to maintain the locking state between the base 2 and the inner mold shell layer 1. The locking force of the tension spring is always controlled within the strength range allowed by the inner mold shell layer 1, and no local stress exceeding the bearing capacity of the inner mold shell layer 1 will be generated. At the same time, the locking force is always kept above the threshold required for sealing, and the locking function will not be lost due to slight fluctuations in the size of the inner mold shell layer 1.

[0047] The receiving cavity surface of the base 2 is provided with an elastic rubber layer, the thickness of which is 0.3~0.6 mm. During the manufacturing process, the inner mold shell blank layer 1 inevitably develops microscopic unevenness on its surface. When the receiving cavity surface of the base 2 is in direct rigid contact with the inner mold shell blank layer 1, the locking force only acts on the protruding points on the surface of the inner mold shell blank layer 1. As the base 2 and the inner mold shell blank layer 1 are locked together, cracks will appear in the inner mold shell blank layer 1. However, by providing an elastic rubber layer on the receiving cavity surface and adjusting the thickness of the elastic rubber layer, when the base 2 and the inner mold shell blank layer 1 are locked together, the elastic rubber layer undergoes compression deformation and embeds itself in the microscopic pits of the inner mold shell blank layer 1, while simultaneously wrapping around the protruding points. This allows the locking force to be evenly distributed, thereby reducing the occurrence of indentations and cracks on the surface of the inner mold shell blank layer 1.

[0048] Example 2

[0049] This embodiment mainly focuses on the low-pressure turbine blades of aero-turbofan engines. When using the shell-making process, the first layer is the surface corundum layer, the second and third layers are transition layers, and the fourth to seventh layers are reinforcing corundum layers. In this embodiment, the first and third layers are the inner mold shell blank layer 1, and the fourth to seventh layers are formed by applying the outer slurry, that is, the reinforcing layers formed on the outside.

[0050] In this embodiment, the specific components of the outer slurry are as follows: The composition includes 15.96% silica sol, 24.16% fused alumina powder, 36.27% mullite powder, 18.04% fused alumina sand, 0.58% reinforcing agent, 3.91% distilled water, and 1.08% wood fiber.

[0051] The advantage of this formulation lies in its ability to enhance the overall micro-elasticity of the shell while ensuring its basic strength by controlling the silica sol content, thereby effectively suppressing recrystallization defects in turbine blades during solidification and subsequent heat treatment.

[0052] The high-temperature strength of the shell is mainly determined by the needle-like mullite three-dimensional network skeleton formed by the reaction of fused corundum powder and SiO2 in silica sol during the calcination process. The high silica sol content in traditional formulations leads to excessive mullite formation, resulting in excessively high high-temperature shell strength and poor resilience. During turbine blade solidification and shrinkage, the shell cannot undergo compliant deformation; rigidity hinders stress concentration and the formation of residual stress, which becomes a trigger for recrystallization during subsequent high-temperature heat treatment.

[0053] This formulation reduces the amount of mullite phase formed during the calcination stage by lowering the silica sol content, resulting in a moderate decrease in high-temperature strength and rigidity, while enhancing microelasticity. This microelasticity allows the shell to buffer shrinkage force through slight adaptive deformation during blade solidification and release stress concentration, effectively inhibiting recrystallization. Distilled water in the formulation ensures the fluidity of the slurry, guaranteeing even application. Wood fibers burn off during shell calcination, forming micropores that improve the shell's permeability and resilience. A reinforcing agent is used to improve the shell's strength during the shell-making stage and burns off during calcination to form micropores, further improving permeability and resilience. The reinforcing agent is a redispersible latex powder (vinyl acetate / ethylene tert-carbonate copolymer, acrylic acid copolymer). Fused corundum powder, mullite powder, and fused corundum sand are used as aggregates to construct the shell skeleton, ensuring sufficient strength.

[0054] In this embodiment, in step d, after the firing thickness is reached, the shell is first maintained at a temperature of 400~600 degrees Celsius for 60~90 minutes to thermally decompose the polyurethane block, and then the temperature is raised to 1000~1100 degrees Celsius for high-temperature firing of the shell.

[0055] This technical solution involves maintaining the polyurethane block at 400-600 degrees Celsius for 60-90 minutes to ensure complete decomposition without the appearance of carbon impurities. Subsequently, the temperature is raised to 1000-1100 degrees Celsius for high-temperature firing of the shell, which provides sufficient firing strength.

[0056] After the turbine blade wax model is prepared, the inner mold shell blank layer 1 is prepared. The turbine blade wax model is treated with a slurry and sandblasting process, and after drying, the inner mold shell blank layer 1 is formed.

[0057] After the inner mold shell blank layer 1 is formed, the tooling is installed on the inner mold shell blank layer 1, so that the base 2 covers the outside of the transition section of the inner mold shell blank. The opening edge of the recess 4 is aligned with and covers the convex adjustment area. The base 2 is locked to the transition section of the inner mold shell blank by the locking mechanism 3. The sealing ring 5 on the base 2 seals the recess 4 above the convex adjustment area. The recess 4 and the outer surface of the convex adjustment area together form a sealed cavity.

[0058] After the base 2 is locked, polyurethane foam is injected into the recess 4 through the injection port 6. The polyurethane foam fills the entire space of the recess 4 and cures to form a polyurethane block. After the polyurethane foam has completely cured, the tooling is removed, and the polyurethane block separates from the inner wall of the recess 4.

[0059] After the tooling is removed, prepare the outer layer slurry according to the aforementioned proportions: 15.96% silica sol, 24.16% fused alumina powder, 36.27% mullite powder, 18.04% fused alumina sand, 0.58% reinforcing agent, 3.91% distilled water, and 1.08% wood fiber. Apply the outer layer slurry to the outside of the inner mold shell blank layer 1, avoiding the top of the polyurethane block, leaving the top of the polyurethane block exposed, until the predetermined firing thickness is achieved, i.e., 5-6 mm.

[0060] After the outer layer of slurry is coated and dried, the shell is fired. In the first stage, the shell is maintained at 400-600 degrees Celsius for 60-90 minutes to allow the polyurethane block to fully decompose into gaseous products and escape completely, thus giving the shell sufficient firing strength. After firing, hollow areas are formed where the polyurethane block decomposed.

[0061] After firing, eutectic white cast iron particles mixed with an inorganic binder are coated onto the hollow areas of the mold shell. The eutectic white cast iron particles adhere to the mold shell through the inorganic binder, and the particles form a stacked layer of eutectic white cast iron particles of a certain thickness through the action of the binder.

[0062] Then, casting is performed, pouring molten metal into the mold shell, and allowing it to stand after casting. The molten metal gradually solidifies within a temperature range of 1250~1350 degrees Celsius, while the eutectic white cast iron particles undergo a phase transformation within a temperature range of 1100~1200 degrees Celsius, melting and absorbing heat. This accelerates the local solidification at the junction of the blade and the ferrule, compressing the time window for stress accumulation. Simultaneously, the outer slurry with low silica sol content gives the mold shell a slight elasticity, buffering the shrinkage force and releasing stress during the solidification and shrinkage of the turbine blade through a small amount of adaptive deformation.

[0063] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A precision casting process for turbine blades, characterized in that, Includes the following steps: a. Preparation of the inner mold shell blank layer (1): The turbine blade wax mold is coated with slurry and sand to form an inner mold shell blank layer (1). The inner mold shell blank layer (1) has an inner mold shell blank transition section at the connection between the flange forming position and the blade forming position. The inner mold shell blank transition section has a convex adjustment area corresponding to the root of the convex side of the blade and the root of the flange. b. Preparation of tooling: The tooling includes a base (2), which has a downward-facing receiving cavity that accommodates the inner mold shell blank transition section; The base (2) is provided with a locking mechanism (3) for locking the inner mold shell blank layer (1); The base (2) has a recess (4) above the receiving cavity, and the opening edge of the recess (4) covers the convex adjustment area; The base (2) is fitted with a sealing ring (5) surrounding the opening of the recess (4); The base (2) is provided with a filling port (6), which is connected to the recess (4) through the upper bottom of the recess (4); c. Application tooling: The inner wall of the recess (4) is sprayed with a layer of paraffin wax, the base (2) is locked to the transition section of the inner mold blank, and the sealing ring (5) seals the recess (4) above the convex adjustment area. Polyurethane foam is injected into the depression (4) through the injection port (6), the polyurethane foam fills the depression (4), and forms a polyurethane block after curing; Remove the tooling, and the inner wall of the recess (4) is separated from the polyurethane block through the paraffin layer; d. Adhesion of outer slurry and firing of the mold shell: Prepare the outer layer slurry that adheres to the inner mold shell blank layer (1). The outer layer slurry comprises the following components by mass percentage: Silica sol 15%–16%, fused alumina powder 24%–25%, mullite powder 36%–37%, fused alumina sand 18%–19%, distilled water 3%–5%, wood fiber 1%–2%; Apply the outer layer slurry to the outside of the inner mold shell blank layer (1), avoiding the top of the polyurethane block, with a thickness of 3~10 mm to achieve the firing thickness; After firing, a shell is obtained, and the polyurethane block decomposes during the firing of the shell to form a hollow structure. e. Casting and solidification: After the shell is fired, eutectic white cast iron particles mixed with inorganic binder are coated on the hollowed-out areas. The casting process using a mold shell allows eutectic white cast iron particles to absorb heat during melting, thereby cooling and accelerating solidification at the junction of the turbine blade and the rim plate.

2. The precision casting process of a turbine blade according to claim 1, characterized in that, The base (2) is provided with an exhaust port (7), which is connected to the recess (4) through the upper bottom of the recess (4), and the injection port (6) and the exhaust port (7) are spaced apart on the upper bottom of the recess (4).

3. The precision casting process of a turbine blade according to claim 2, wherein, The exhaust port (7) is conical, and the inner diameter of the end of the exhaust port (7) facing the recess (4) is greater than the inner diameter of the end of the exhaust port (7) away from the recess (4).

4. The investment casting process of a turbine blade according to claim 1, wherein, The locking mechanism (3) includes a tension spring and two pins connected to both ends of the tension spring; The base (2) has two pin holes spaced apart at the edge of the receiving cavity. These pin holes are called locking pin holes. The two pins are respectively inserted into the two locking pin holes; This results in a locking mechanism (3) in which the tension spring locks the inner mold shell blank layer (1) to the base (2).

5. The precision casting process for turbine blades according to claim 1, characterized in that, The surface of the receiving cavity of the base (2) is provided with an elastic rubber layer, the thickness of which is 0.3~0.6 mm.

6. The precision casting process for turbine blades according to claim 1, characterized in that, In step d, after the firing thickness is reached, the shell is first maintained at a temperature of 400-600 degrees Celsius for 60-90 minutes to thermally decompose the polyurethane block, and then the temperature is raised to 1000-1100 degrees Celsius for high-temperature firing of the shell.

Citation Information

Patent Citations

  • Casting method of large allowance-free pressure expander precise casting piece

    CN104999034A

  • Manufacturing device and manufacturing method for single-crystal turbine blade of aero-engine

    CN121042487A