A large-section i-beam grooveless welding system and method
By generating a gradient composite active film at the intersection of the web and flange of a large-section I-beam, and combining it with plasma arc, magnetic field and ultrasonic vibration, full penetration welding of large-section I-beams was achieved, solving the problems of low welding efficiency and automation in existing thick plate welding technologies, and improving welding quality and production efficiency.
Patent Information
- Application Number
- CN202611434992.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-09-16
AI Technical Summary
Existing technologies make it difficult to achieve full penetration welding of large-section I-beams, especially when the web thickness is ≥30mm. Furthermore, active welding technology cannot achieve automated production, and single physical field-assisted methods have limited effect on improving the penetration depth of thick plates. The flame function has not been fully developed.
A gradient composite active film is generated at the root intersection of the web side end face and the flange plate surface using a dual-channel gradient flame, and then combined with a transfer plasma arc, magnetic field and ultrasonic vibration to achieve full penetration welding.
It enables single-sided or double-sided single-pass full penetration welding of large-section I-beams, reduces beveling steps, improves production efficiency and welding quality, and supports automated production.
Smart Images

Figure CN122938403B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding technology for large steel structures, and in particular to a welding system and method for large-section I-beams that does not require beveling. Background Technology
[0002] Large-section I-beams (web thickness ≥ 16mm) are core load-bearing components in large steel structures and are widely used in bridges, buildings, and marine engineering. To ensure the load-bearing capacity and fatigue resistance of the components, the T-joints between the upper and lower flanges and the web usually require full penetration welding. Currently, the mainstream method in the industry to achieve full penetration welding of T-joints for large-section I-beams is to pre-process K-shaped, double V-shaped, or single V-shaped bevels (bevel angle usually 45°~60°) on the edge of the web to be welded, and then perform multi-pass, multi-layer filler welding using submerged arc welding (SAW) or gas shielded welding.
[0003] In response to the problems of long process, high consumption of welding materials, and low production efficiency in the above-mentioned process, several improvement schemes that eliminate or reduce the need for beveling have emerged in recent years.
[0004] Regarding submerged arc welding without beveling, existing technologies have proposed a beveling-free welding scheme for 16mm thick web-plate fully penetrated steel bridge I-beams, and its feasibility has been verified through process tests. Existing technologies have also verified the feasibility of a double-wire submerged arc welding process without beveling or root cleaning in 20mm thick web-plate T-joints. Chinese patent CN108856969A discloses a submerged arc welding method for medium-thick plate T-joints without beveling, but this method requires adjusting the angle between the flange and the horizontal plane to 50°, making the operation complex. Furthermore, it employs multi-pass, multi-layer submerged arc welding, resulting in a large number of weld passes and high heat input, making it unsuitable for the efficient automated production of large-section I-beams. Chinese patent CN115255574A discloses a submerged arc welding manufacturing method for extra-thick plates without beveling. Although it claims to eliminate the need for beveling, it actually prepares an equivalent beveling structure using spacers, still requiring extensive submerged arc welding filling and back-side root cleaning, along with alternating welding, making the process still cumbersome.
[0005] In the field of activator welding technology, activated tungsten inert gas (A-TIG) welding, by applying a layer of activator to the base material surface, can increase the weld penetration depth by 1 to 3 times compared to conventional TIG welding, achieving single-pass penetration without beveling for butt joints of steel plates up to 12mm thick. Studies on activated plasma arc welding (A-PAW) have shown that activators can reduce arc shrinkage and enhance arc penetration. However, all of the above-mentioned activated welding technologies require pre-prepared activators and manual application, making it difficult to precisely control the coating thickness and uniformity. Furthermore, the application process interrupts the welding flow, preventing integration into automated production lines and limiting their widespread application in the manufacture of large steel structures.
[0006] In the field of physical field-assisted welding, magnetic field-assisted TIG welding increases arc energy density by influencing arc morphology. Ultrasonic-assisted perforation plasma arc welding (U-PAW) applies ultrasonic vibrations to the plasma arc and molten pool through a tungsten electrode, improving molten pool flow and enhancing perforation capability. However, the above technologies are all single-physical-field-assisted methods, and there are no reports of applying active film technology in conjunction with multiple physical fields to the beveling-free full penetration welding of large-section I-beam T-joints.
[0007] In summary, the existing technologies still have the following shortcomings: (1) The applicable plate thickness of the non-grooving welding scheme is limited (usually ≤20mm), which makes it difficult to meet the full penetration requirements of large-section I-beams (web thickness ≥30mm); (2) The active welding technology cannot achieve automated production because it requires pre-coating of activators; (3) In the existing flame heating technology, the flame is only used as a physical heating tool, and its chemical modification function has not been developed; (4) The single physical field auxiliary means has limited effect on improving the penetration depth of thick plates, and there is a lack of deep penetration welding schemes with multi-physical field synergy. Summary of the Invention
[0008] To overcome the shortcomings of the prior art, the present invention adopts the following technical solution:
[0009] A welding method for large-section I-beams without beveling, comprising the following steps:
[0010] Assembly steps: Assemble the flange plate and the web plate at right angles. The side end face of the web plate facing the flange plate is a right-angle cut surface without beveling. Control the assembly gap between the side end face of the web plate and the flange plate surface to be no more than 0.5mm.
[0011] Pretreatment steps: The root junction area of the web side end face and the flange plate surface is simultaneously chemically modified using a dual-channel gradient flame. The first channel sprays a strong reducing flame to generate a dense underlayer in situ on the metal surface, and the second channel sprays a weak reducing flame to generate a porous surface layer in situ on the outside of the dense underlayer. This forms a gradient composite active film covering a predetermined width in the root junction area of the web side end face and the flange plate surface.
[0012] Welding steps: Ignite the transfer-type plasma arc behind the point where the pretreatment step is completed. The plasma arc acts on the root of the T-shaped joint covered by the gradient composite active film. Utilize the synergistic effect of the arc contraction effect of the gradient composite active film and the pinhole effect of the plasma arc to allow the plasma arc to penetrate the full thickness of the web and form a stable pinhole. Simultaneously fill the hole with filler wire to complete the full penetration welding.
[0013] Post-weld protection steps: Protect the high-temperature weld seam with a protective gas after welding.
[0014] Furthermore, it also includes a monitoring step: real-time monitoring of the surface temperature of the root junction area of the web side end face and the flange plate surface and the thickness of the gradient composite active film, and adjusting the gas combustion ratio and / or flame core distance of the reducing flame in the first channel and / or the second channel according to the monitoring results, so that the temperature and film thickness are stabilized within a preset range.
[0015] Furthermore, a strong reducing flame with an O2 / C3H8 volume ratio of 0.80~0.90:1 is injected into the first channel to generate a dense underlayer with FeO as the main phase and a thickness of 5~8μm.
[0016] The second channel sprays a weakly reducing flame with an O2 / C3H8 volume ratio of 0.90~1.00:1 and CO2 incorporated, generating a porous surface layer containing Fe3C particles with a thickness of 5~10μm.
[0017] The total thickness of the gradient composite active film is 10~18μm.
[0018] Furthermore, the fuel gas in the second channel contains 0.3% to 1.5% by volume of a halogen-containing gas, which is selected from at least one of carbon tetrachloride vapor or trichloroethylene vapor. The halogen atoms produced by the decomposition of the halogen-containing gas at high temperature can further reduce the ionization energy of the arc atmosphere, enhance the arc contraction effect, and its strong electronegativity is conducive to capturing free electrons, further increasing the arc temperature gradient, thereby enhancing the efficiency of the active film.
[0019] Furthermore, in the pretreatment step, the dual-channel gradient flame moves at a speed of 200~250 mm / min;
[0020] The distance between the flame core of the first channel spraying strong reducing flame and the workpiece surface is 5~6mm, the distance between the flame core of the second channel spraying weak reducing flame and the workpiece surface is 7~8mm, and the interval between the first channel and the second channel along the welding direction is 20~30mm.
[0021] Furthermore, when the web thickness is 30~35mm, full penetration welding can be completed by performing a single welding on the front side;
[0022] When the thickness of the web plate is 35~40mm, a magnetic field and an ultrasonic vibration field along the axis of the plasma arc welding gun are applied simultaneously during the welding process, and full penetration welding can be completed by performing a front welding through the plasma arc.
[0023] When the web thickness is 40mm~50mm, a magnetic field and an ultrasonic vibration field along the axial direction of the plasma arc welding gun are applied simultaneously during the welding process. After the welding on the front side is completed, the pretreatment steps and welding steps are repeated on the back side to complete the full penetration welding.
[0024] Furthermore, the welding current of the plasma arc is 280~350A, the voltage is 30~35V, and the welding speed is 200~250mm / min; the magnetic field strength is 10~50mT, and the direction is along the axis of the plasma arc welding gun; the frequency of the ultrasonic vibration is 20~50kHz, and the power is 100~300W.
[0025] This invention also provides a welding system for large-section I-beams without beveling, used to realize the above-mentioned welding method for large-section I-beams without beveling, including:
[0026] Walking mechanism;
[0027] A flame pretreatment unit is installed at the front end of the walking mechanism. It includes a first channel nozzle and a second channel nozzle. Both the first channel nozzle and the second channel nozzle include two nozzles, and the two nozzles are respectively arranged on both sides of the web thickness direction. Their nozzles are both directed to the root intersection area of the web side end face and the flange plate surface, so as to simultaneously perform flame treatment on the root intersection area of the web side end face and the flange plate surface. The flame pretreatment unit is connected to a gas supply system with a flow proportional valve.
[0028] The plasma arc welding unit is installed on the traveling mechanism and located behind the flame pretreatment unit, and includes a welding power source capable of outputting a transfer-type plasma arc and a plasma arc welding torch.
[0029] The tail protective gas cover is installed at the rear of the plasma arc welding unit.
[0030] Furthermore, it also includes:
[0031] A magnetic field generating device is installed outside the plasma arc welding torch to generate a magnetic field along the axial direction of the plasma arc welding torch.
[0032] An ultrasonic vibration device is installed on the outside of the plasma arc welding torch to couple ultrasonic vibration to the molten pool.
[0033] Furthermore, it also includes:
[0034] The online monitoring unit includes a process infrared thermometer and a spectral reflectance film thickness probe located between the pretreatment unit and the welding unit;
[0035] The central control system is connected to the online monitoring unit, the flow proportional valve of the gas supply system, the welding power supply, the magnetic field generator, and the ultrasonic vibration device.
[0036] Compared with the prior art, the beneficial effects of the present invention are:
[0037] 1. By utilizing CO and H2 in a reducing flame to generate an in-situ FeO / Fe3C gradient composite active film on a metal surface, and through precise control of the oxygen-fuel ratio and flame core distance, online in-situ generation and automated coating of active materials are achieved. Compared with the existing A-TIG and A-PAW technologies, which require pre-preparation of activators and manual application, this method solves the industry problem of the inability to integrate the activator application step into an automated production line for activated welding technology.
[0038] 2. Through the synergistic effect of the arc contraction effect of the gradient composite active film, the pinhole effect of the plasma arc, the magnetic compression effect of the magnetic field, and the acoustic flow / cavitation effect of ultrasonic vibration, the energy density of the plasma arc is dramatically increased. Under this synergistic effect, a single-sided full penetration can be achieved for a 30-40mm thick web, and a double-sided full penetration can be achieved for a 40-50mm thick web.
[0039] 3. This invention completely eliminates the beveling process, reducing the traditional multi-layer, multi-pass welding process of dozens or even hundreds of steps to a single-pass welding or one pass on each side. Simultaneously, post-weld angular deformation is controlled within 0.6°~0.8°, significantly reducing the workload of subsequent corrections.
[0040] 4. The surface temperature and active film thickness after flame treatment are monitored in real time by a process infrared thermometer and a spectral reflectance film thickness probe. Closed-loop regulation is performed through a central control system, which realizes online precise monitoring and real-time control of the active film formation quality, ensuring the stability and consistency of welding quality.
[0041] 5. The function of the flame is expanded from a single physical heating to a dual function of chemical modification and physical heating. That is, the flame not only undertakes the function of preheating before welding, but also generates a gradient composite active film in situ on the metal surface through the chemical reaction of the reducing flame, thus realizing a fundamental expansion of the function of the flame. Attached Figure Description
[0042] Figure 1 This is a schematic diagram of the structure of the present invention;
[0043] Figure 2 This is a schematic diagram of the gantry frame and its components in this invention;
[0044] Figure 3 for Figure 2 A structural diagram from another perspective;
[0045] Figure 4 This is a schematic diagram of another structure of the gantry frame and its components in this invention;
[0046] Figure 5 This is a flowchart of the gas supply system in this invention;
[0047] Figure 6This is a control flow diagram of the present invention.
[0048] In the diagram: 1. Traveling mechanism; 11. Gantry frame; 12. Traveling wheel set; 13. Guide rail; 14. Mounting base; 15. Rotary positioner; 2. Flame pretreatment unit; 21. Support; 22. First channel nozzle; 23. Second channel nozzle; 24. Gas supply system; 241. Oxygen source; 242. Propane source; 243. Carbon dioxide source; 244. Halogen-containing gas source; 245. First mixing chamber; 246. Second mixing chamber; 25. Adjustment mechanism; 3. Plasma arc welding unit; 31. Plasma arc welding torch; 32. Welding power source; 33. Welding torch holder; 4. Tail protective gas cover; 5. Magnetic field generating device; 6. Ultrasonic vibration device; 61. Ultrasonic transducer; 62. Amplitude bar; 63. Ultrasonic generator; 7. Online monitoring unit; 71. Process infrared thermometer; 72. Spectral reflectance film thickness probe; 8. Central control system. Detailed Implementation
[0049] The present invention will be explained in detail through the following embodiments. The purpose of disclosing the present invention is to protect all technical improvements within the scope of the present invention. In the description of the present invention, it should be understood that the terms "upper," "lower," "front," "rear," "left," "right," etc., indicating orientation or positional relationships, are only corresponding to the drawings of this application for the convenience of describing the present invention. The terms "end," "side," "end portion," "lateral portion," "longitudinal portion," etc., indicating orientation or positional relationships, are only descriptions of the orientation in the length and width directions of the corresponding components. That is, "end portion" indicates the head and tail areas in the length direction of the corresponding component, and "side portion" indicates the two sides in the width direction of the corresponding component. The term "provided with" should be understood in the art as "provided with" or "assembled with," and does not limit the specific connection method. The term "corresponding" should be understood in the art as used to describe the relative positional relationship, functional cooperation relationship, or spatial alignment relationship between two components. For the convenience of describing the present invention, it is not intended to indicate or imply that the device or element referred to must have a specific orientation.
[0050] Example 1, as Figure 1-3 As shown, a welding system for large-section I-beams without beveling includes a traveling mechanism 1, a flame pretreatment unit 2, a plasma arc welding unit 3, a filler wire feeding system (not shown in the figure), and a tail protective gas cover 4.
[0051] The traveling mechanism 1 is a gantry-type traveling mechanism, including a gantry frame 11 spanning above the workpiece, traveling wheel sets 12 disposed at the bottom of the columns on both sides of the gantry frame 11, and a drive device (not shown in the figure) that drives the traveling wheel sets 12 to reciprocate along the guide rails 13 laid on the ground. The crossbeam of the gantry frame 11 is provided with a mounting base 14 extending along the welding direction (i.e., the front-to-back direction). The flame pretreatment unit 2, the plasma arc welding unit 3, and the tail protective gas hood 4 are fixedly mounted on the mounting base 14. The mounting base 14 can move as a whole with the gantry frame 11.
[0052] The flame pretreatment unit 2 includes a support 21, a first channel nozzle 22, a second channel nozzle 23, and a gas supply system 24.
[0053] The bracket 21 is installed below the mounting base 14. The first channel nozzle 22 and the second channel nozzle 23 are arranged at intervals along the welding direction on the bracket 21, with the second channel nozzle 23 located 20-30 mm behind the first channel nozzle 22. Both the first channel nozzle 22 and the second channel nozzle 23 include two nozzles, which are located on the left and right sides of the web respectively (i.e., the two nozzles of the first channel nozzle 22 are located on the left and right sides of the web respectively, and the two nozzles of the second channel nozzle 23 are also located on the left and right sides of the web respectively). The nozzle orifice of each nozzle points to the root intersection area of the side end face of the web and the surface of the flange plate, so as to synchronously spray a reducing flame from both sides into the root intersection area of the side end face of the web and the surface of the flange plate for flame treatment.
[0054] The bracket 21 is also equipped with an adjustment mechanism 25 for adjusting the distance between each nozzle and the workpiece surface. The adjustment mechanism 25 is a manual screw adjustment assembly or an electric push rod assembly, used to adjust the corresponding nozzle to move forward (closer to the root intersection area of the web side end face and the flange plate surface) or backward (away from the root intersection area of the web side end face and the flange plate surface) in the nozzle direction.
[0055] The distance between the flame core of the first channel nozzle 22 and the workpiece surface is 5-6 mm, and the distance between the flame core of the second channel nozzle 23 and the workpiece surface is 7-8 mm.
[0056] The gas supply system 24 includes an oxygen source 241, a propane source 242, a carbon dioxide source 243, and a halogen-containing gas source 244. The oxygen source 241 and propane source 242 are connected to the first channel nozzle 22 via independent supply lines. The oxygen source 241, propane source 242, carbon dioxide source 243, and halogen-containing gas source 244 are connected to the second channel nozzle 23 via independent supply lines. Each supply line is equipped with a mass flow controller or a flow proportional valve (not shown in the figure). The supply line to the first channel nozzle 22 is connected to a first mixing chamber 245, used to mix oxygen and propane at a volume ratio of 0.80~0.90:1 before supplying the mixture to the first channel nozzle 22. The supply line to the second channel nozzle 23 is connected to a second mixing chamber 246, used to mix oxygen and propane at a volume ratio of 0.90~1.00:1, and then incorporate carbon dioxide before supplying the mixture to the second channel nozzle 23.
[0057] The plasma arc welding unit 3 includes a plasma arc welding torch 31, a welding power source 32, an ion gas supply system, and a shielding gas supply system.
[0058] The plasma arc welding torch 31 is fixedly installed on the mounting base 14 by the welding torch holder 33, located behind the flame pretreatment unit 2, and the distance between it and the flame pretreatment unit 2 along the welding direction is 40~80mm, that is, it is located 40~80mm behind the second channel nozzle 23. The axial direction of the plasma arc welding torch 31 can be perpendicular to the flange plate surface, or it can be at an angle of 0°~15° with the normal of the flange plate surface.
[0059] The welding power source 32 is installed in a control cabinet next to one of the columns of the gantry 11. It is a variable polarity welding power source, capable of outputting DC positive polarity mode and pulse mode. The ion gas channel of the plasma arc welding torch 31 is connected to an external ion gas supply system, which provides a mixture of argon and hydrogen gas at a flow rate of 2.8~3.5 L / min. The shielding gas channel of the plasma arc welding torch 31 is connected to an external shielding gas supply system, which provides argon-rich shielding gas at a flow rate of 18~22 L / min.
[0060] The filler wire feeding system provides the plasma arc welding torch 31 with a filler wire of 1.2 mm in diameter and feeds it into the molten pool.
[0061] The tail gas shield 4 is installed behind the plasma arc welding torch 31 and fixed to the mounting base 14. The lower end of the tail gas shield 4 is provided with an air outlet, which is a narrow slit structure extending along the welding direction. It is connected to the protective gas supply system through a gas supply pipeline and continuously outputs protective gas to the high-temperature weld after welding.
[0062] Example 2, as Figure 1-3 As shown, in this embodiment, based on embodiment one, a magnetic field generating device 5 is added to the outside of the plasma arc welding gun 31, and an ultrasonic vibration device 6 is added to the outside or inside of the plasma arc welding gun 31.
[0063] The magnetic field generating device 5 is an excitation coil assembly, sleeved on the outside of the plasma arc welding torch 31 and coaxially arranged with the plasma arc welding torch 31. Specifically, the magnetic field generating device 5 includes a ring-shaped magnetic core and an excitation winding wound on the ring-shaped magnetic core. The excitation winding is connected to an adjustable excitation power supply, which outputs DC current. By adjusting the DC excitation current, the magnetic field generating device 5 generates a magnetic field along the axial direction of the plasma arc welding torch 31. The magnetic field strength is 10~50mT, and the excitation current is adjustable from 0~5A.
[0064] The ultrasonic vibration device 6 includes an ultrasonic transducer 61, an amplitude transformer 62, and an ultrasonic generator 63. The ultrasonic transducer 61 is fixedly mounted on the mounting base 14. One end of the amplitude transformer 62 is connected to the ultrasonic transducer 61, and the other end is connected to the plasma arc welding torch 31. The welding torch holder 33 is connected to the mounting base 14 via an elastic connector, allowing the plasma arc welding torch 31 to vibrate slightly along its axial direction. This transmits the ultrasonic vibration generated by the ultrasonic transducer 61 through the amplitude transformer 62 to the torch body and nozzle of the plasma arc welding torch 31, and couples it to the molten pool. The ultrasonic generator 63 is installed in a control cabinet next to a column on one side of the gantry crane. It is electrically connected to the ultrasonic transducer 61 via a high-frequency cable and can output a high-frequency electrical signal with a frequency of 20~50kHz and a power of 100~300W.
[0065] Example 3, as Figure 1-3 and Figure 6 As shown, this embodiment, based on embodiment two, further adds an online monitoring unit 7 and a central control system 8.
[0066] The online monitoring unit 7 includes a process infrared thermometer 71 and a spectral reflectance film thickness probe 72. The process infrared thermometer 71 is installed between the flame pretreatment unit 2 and the plasma arc welding unit 3, with its probe facing the root intersection area of the web side end face and the flange plate surface, for real-time monitoring of the surface temperature after flame treatment. The spectral reflectance film thickness probe 72 is installed beside the process infrared thermometer 71. Its emitting end emits a detection beam towards the surface of the gradient composite active film, and its receiving end receives the reflected spectral signal. By analyzing the interference characteristics of the reflected spectrum, the thickness of the gradient composite active film is calculated in real time.
[0067] The central control system 8, an industrial computer or programmable logic controller, is located on one side of the gantry 11. The central control system 8 is connected via signal cables or a wireless communication module to the process infrared thermometer 71, the spectral reflectance film thickness probe 72, the flow proportional valve, the welding power supply 32, the adjustable excitation power supply, and the ultrasonic generator 63. The central control system 8 has a built-in control program that can receive detection signals from each sensor and send control commands to each actuator.
[0068] Example 4, as Figure 4 As shown, in this embodiment, based on any one of embodiments one to three, a rotary positioner 15 is also installed on the crossbeam of the gantry frame 11. The mounting base 14 is fixedly installed on the rotating part of the rotary positioner 15. The rotary positioner 15 is signal-connected to the central control system 8, and the central control system 8 controls the rotary positioner 15 to drive the mounting base 14 to rotate 180° around the vertical axis, thereby causing the flame pretreatment unit 2, the plasma arc welding unit 3, the magnetic field generating device 5, the ultrasonic vibration device 6, and the tail protective gas cover 4 to rotate as a whole 180°, so as to weld the back side of the web plate.
[0069] When the front welding is completed and the back welding is required, the central control system 8 controls the rotary positioner 15 to drive the mounting base 14 to rotate 180° around the vertical axis, so that the flame pretreatment unit 2, the plasma arc welding unit 3, the magnetic field generating device 5, the ultrasonic vibration device 6, the online monitoring unit 7 and the tail protective gas cover 4 rotate as a whole 180°. Then the walking mechanism 1 moves in the opposite direction along the welding direction and repeats the pretreatment and welding steps on the back of the web.
[0070] Example 5: A welding method for large-section I-beams without beveling. This example uses a large-section I-beam made of Q355B material, with a web thickness of 30mm and a flange thickness of 40mm as the welding object.
[0071] The welding system described in Embodiment 1 is used. The distance between the flame core of the first channel nozzle 22 and the workpiece surface is set to 5 mm, the distance between the flame core of the second channel nozzle 23 and the workpiece surface is set to 7 mm, and the interval between the first channel nozzle 22 and the second channel nozzle 23 along the welding direction is set to 20 mm.
[0072] The welding current of the plasma arc welding unit 3 is set to 310A, the voltage to 32V, and the welding speed to 220mm / min. The ionizing gas is a mixture of argon and hydrogen (Ar+5%H2) with a flow rate of 3.0L / min; the shielding gas is an argon-rich shielding gas (Ar+8%CO2) with a flow rate of 20L / min.
[0073] The operation steps are as follows:
[0074] Assembly steps: Assemble the flange plate and web plate at right angles. The side end face of the web plate facing the flange plate is a right-angle cut surface without any beveling. Control the assembly gap between the side end face of the web plate and the flange plate surface to be no greater than 0.5mm; in this embodiment, the assembly gap is controlled within 0.3mm.
[0075] Pretreatment step: Start the walking mechanism 1, and the flame pretreatment unit 2 moves along the welding direction with the walking mechanism 1 at a moving speed of 220 mm / min.
[0076] The first channel sprays a strong reducing flame with an O2 / C3H8 volume ratio of 0.85:1, with the flame core 5 mm from the workpiece surface, to flame-treat the root junction area of the web side end face and the flange surface. The carbon monoxide and hydrogen in the strong reducing flame reduce the original oxide scale on the metal surface and react with the iron matrix at high temperature, generating a dense underlayer of approximately 5 μm thickness, primarily composed of FeO. The chemical reaction is as follows:
[0077] Fe₂O₃ + CO → 2FeO + CO₂
[0078] Fe3O4 + CO → 3FeO + CO2
[0079] After a 20mm interval, a weakly reducing flame with an O2 / C3H8 volume ratio of 0.95:1 and CO2 incorporation is injected into the second channel. The distance between the flame core and the workpiece surface is 7mm. In the weakly reducing flame, propane undergoes incomplete combustion to produce a large amount of CO (approximately 8%~12%). CO undergoes a disproportionation reaction on the hot metal surface (approximately 600~850℃): 2CO→C (active) + CO2. The generated active carbon atoms undergo a carburizing reaction with the previously generated FeO: 3FeO+5CO→Fe3C+4CO2. The incorporation of CO2 is used to adjust the CO / CO2 volume ratio (controlled at 3:1~6:1), thereby stabilizing the local carbon potential and avoiding excessive carburizing. Finally, a porous surface layer containing Fe3C particles with a thickness of approximately 5μm is generated on the outside of the dense bottom layer. The porosity of the porous surface layer is approximately 20%~30%, and the average particle size of the Fe3C particles is approximately 0.5~2μm.
[0080] Finally, a gradient composite active film with a total thickness of approximately 10 μm is formed at the root intersection of the web side end face and the flange plate surface. The bottom layer is dense (FeO as the main phase), and the surface layer is porous (FeO + Fe3C particles), with a coverage width of 12-20 mm on both sides of the weld. The instantaneous temperature of the surface thin layer directly affected by the reducing flame reaches 600-850℃. This temperature is used to meet the kinetic requirements of the in-situ formation reaction of FeO and Fe3C, ensuring that the above chemical reaction proceeds fully. At the same time, the heat is conducted through the workpiece to maintain the overall temperature of the welding area and surrounding area (within 50-100 mm on both sides of the weld) at 280-320℃. This temperature is used to meet the preheating requirements of subsequent plasma arc welding and prevent cold cracking.
[0081] Welding Procedure: Immediately ignite the transfer-type plasma arc approximately 50 mm behind the point where the pretreatment step is completed. The plasma arc welding current is 310A, the voltage is 32V, and the welding speed is 220 mm / min. The ionizing gas is a mixture of argon and hydrogen (Ar + 5% H2) at a flow rate of 3.0 L / min; the shielding gas is an argon-rich shielding gas (Ar + 8% CO2) at a flow rate of 20 L / min.
[0082] The plasma arc acts on the root of the T-shaped connector covered by the gradient composite active film. The arc contraction effect of the gradient composite active film (its mechanism is: under the high temperature of the plasma arc, FeO and Fe3C particles in the porous surface structure rapidly decompose and evaporate, generating O atoms and O2) 2- Ions and carbon-containing vapors; of which O 2- With strong electronegativity, it adsorbs free electrons in the outer region of the arc, reducing the conductivity and narrowing the current channel at the arc periphery. This forces the arc current to concentrate towards the center, resulting in arc anode spot shrinkage and increased arc energy density. Simultaneously, the oxygen produced by FeO decomposition alters the oxygen content on the molten pool surface, causing the surface tension temperature gradient to change from negative to positive. The molten pool flow changes from outward dispersion to inward convergence, carrying arc heat to the bottom of the molten pool and further increasing the penetration depth. The porous structure of the porous surface layer facilitates the rapid and uniform release of active materials at the high arc temperature, enhancing the aforementioned arc shrinkage effect. Under the synergistic effect of the plasma arc orifice effect, the plasma arc penetrates the full thickness of the web and forms a stable orifice. A 1.2mm diameter filler wire is simultaneously inserted, completing a single-pass full penetration weld in one pass.
[0083] Post-weld protection steps: The tail protective gas hood 4 behind the plasma arc welding unit 3 continuously outputs protective gas (argon-rich protective gas, Ar+8%CO2, flow rate 20L / min) to protect the high-temperature weld until it cools down and prevents oxidation.
[0084] After welding, the weld was subjected to 100% ultrasonic testing, and the results showed that it was completely penetrated and had no defects such as incomplete welding, cracks, or porosity.
[0085] Macroscopic metallographic dissection of the welded joint showed that the weld throat thickness was equal to the full thickness of the web plate (30 mm), the weld metal was well fused with the base metal, and there were no areas of incomplete penetration.
[0086] The angular deformation of the welded joint was measured to be approximately 0.8°.
[0087] The porosity of the weld is less than 0.2%.
[0088] Under identical conditions (same pairing gap, same plasma arc parameters, same welding speed), but without the formation of an active film (i.e., using a neutral flame instead of a reducing flame), a comparative welding experiment was conducted. The results showed that without the active film, the penetration depth was only 19 mm, with an unpenetrated area of 11 mm, making full penetration impossible. This comparative experiment demonstrates that the gradient composite active film described in this invention is one of the key factors for achieving full penetration welding of thick plate T-joints without beveling.
[0089] Example 6: This example uses a large-section I-beam made of Q355B material, with a web thickness of 38mm and a flange thickness of 50mm as the welding object.
[0090] The welding system described in Example 2 (including magnetic field generator 5 and ultrasonic vibration device 6) is used. Based on all the conditions in Example 5, the magnetic field generator 5 and ultrasonic vibration device 6 are activated during the welding process.
[0091] The magnetic field generating device 5 is set to a magnetic field strength of 30 mT, with the magnetic field direction aligned with the axis of the plasma arc welding torch 31, and an excitation current of 3 A. The ultrasonic vibration device 6 is set to an ultrasonic frequency of 35 kHz and a power of 200 W.
[0092] The operation steps are as follows:
[0093] The assembly steps, pretreatment steps, and post-weld protection steps are the same as in Example 5.
[0094] During the welding process, the transfer-type plasma arc is ignited simultaneously with the activation of the magnetic field generator 5 and the ultrasonic vibration device 6. The plasma arc acts on the root of the T-joint covered by the gradient composite active film. The arc contraction effect of the gradient composite active film causes the arc to contract, the pinhole effect of the plasma arc creates penetrating penetration, the magnetic compression effect of the magnetic field further contracts the arc diameter, and the acoustic flow and cavitation effects of the ultrasonic vibration improve the flow of the molten pool and promote bubble escape. The four effects work synergistically to allow the plasma arc to penetrate the full thickness of the 38mm web and form a stable pinhole. Simultaneously, filler wire is inserted, completing a single-pass full penetration weld in one pass.
[0095] After welding, the weld was subjected to 100% ultrasonic testing, and the results showed that it was completely penetrated and had no defects such as incomplete welding, cracks, or porosity.
[0096] Macroscopic metallographic dissection of the welded joint was performed, and the thickness of the weld throat was equal to the total thickness of the web, 38 mm.
[0097] The angular deformation of the welded joint was measured to be approximately 0.6°.
[0098] The porosity of the weld is less than 0.2%.
[0099] Example 7: This example uses a large-section I-beam made of Q355B material and with a web thickness of 45mm as the welding object.
[0100] The welding system described in Example 4 (including a magnetic field generator 5, an ultrasonic vibration device 6, an online monitoring unit 7, a central control system 8, and a rotary positioner 15) is used. The welding system setup is the same as in Example 6.
[0101] The operation steps are as follows:
[0102] Front welding: Following the steps in Example 6, the assembly, pretreatment, four-effect synergistic welding, and post-weld protection are completed on the front side of the workpiece.
[0103] Rotary welding system: After the front welding is completed and confirmed to be qualified by flaw detection, the central control system 8 sends a rotation command to the rotary positioner 15. The rotary positioner 15 drives the mounting base 14 to rotate 180° around the vertical axis, so that the flame pretreatment unit 2, the plasma arc welding unit 3, the magnetic field generating device 5, the ultrasonic vibration device 6 and the tail protective gas cover 4 rotate as a whole 180°.
[0104] Backside welding: Repeat the pretreatment and welding steps on the back side of the web, and perform post-weld protection after the backside welding is completed.
[0105] After welding, the weld was subjected to 100% ultrasonic testing. The results showed that the front and back welds overlapped in the central area of the web thickness, forming a continuous full penetration connection.
[0106] Macroscopic metallographic dissection of the welded joint showed that the total penetration thickness reached more than 60mm (the sum of the front weld depth and the back weld depth, covering the entire 45mm web thickness with overlap), and the full penetration area was continuous and uninterrupted.
[0107] Structures, components, and connection methods not described in detail in this invention are all prior art known to those skilled in the art unless otherwise specified. It is obvious to those skilled in the art that this invention is not limited to the details of the above exemplary embodiments, and that the invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the invention. Therefore, the above embodiments should be regarded as exemplary and non-limiting in all respects. The scope of this invention is defined by the appended claims rather than the foregoing description, and therefore all changes falling within the meaning and scope of the equivalents of the claims are intended to be included within this invention.
Claims
1. A welding method for large-section I-beams without beveling, characterized in that, Includes the following steps: Assembly steps: Assemble the flange plate and the web plate at right angles. The side end face of the web plate facing the flange plate is a right-angle cut surface without beveling. Control the assembly gap between the side end face of the web plate and the flange plate surface to be no more than 0.5mm. Pretreatment step: A dual-channel gradient flame is used to simultaneously chemically modify the root junction area of the web side end face and the flange plate surface. The first channel sprays a strong reducing flame with an O2 / C3H8 volume ratio of 0.80~0.90:1 to generate a dense underlayer with a thickness of 5~8μm mainly composed of FeO on the metal surface in situ. The second channel sprays a weak reducing flame with an O2 / C3H8 volume ratio of 0.90~1.00:1 and incorporating CO2 to generate a porous surface layer containing Fe3C particles with a thickness of 5~10μm on the outside of the dense underlayer. Thus, a gradient composite active film covering a predetermined width is formed in the root junction area of the web side end face and the flange plate surface. The total thickness of the gradient composite active film is 10~18μm. Welding steps: Ignite the transfer-type plasma arc behind the point where the pretreatment step is completed. The plasma arc acts on the root of the T-shaped joint covered by the gradient composite active film. Utilize the synergistic effect of the arc contraction effect of the gradient composite active film and the pinhole effect of the plasma arc to allow the plasma arc to penetrate the full thickness of the web and form a stable pinhole. Simultaneously fill the hole with filler wire to complete the full penetration welding. Post-weld protection steps: Protect the high-temperature weld seam with a protective gas after welding.
2. The welding method for large-section I-beams without beveling according to claim 1, characterized in that, It also includes a monitoring step: real-time monitoring of the surface temperature of the root junction area of the web side end face and the flange plate surface and the thickness of the gradient composite active film, and adjusting the gas combustion ratio and / or flame core distance of the reducing flame in the first channel and / or the second channel according to the monitoring results, so that the temperature and film thickness are stabilized within a preset range.
3. The welding method for large-section I-beams without beveling according to claim 1, characterized in that, The fuel gas in the second channel contains 0.3% to 1.5% by volume of a halogen-containing gas, wherein the halogen-containing gas is selected from at least one of carbon tetrachloride vapor or trichloroethylene vapor.
4. The welding method for large-section I-beams without beveling according to claim 1, characterized in that, In the pretreatment step, the dual-channel gradient flame moves at a speed of 200~250mm / min; The distance between the flame core of the first channel spraying strong reducing flame and the workpiece surface is 5~6mm, the distance between the flame core of the second channel spraying weak reducing flame and the workpiece surface is 7~8mm, and the interval between the first channel and the second channel along the welding direction is 20~30mm.
5. The welding method for large-section I-beams without beveling according to claim 1, characterized in that, When the thickness of the web plate is 30~35mm, full penetration welding can be completed by performing a single welding on the front side. When the thickness of the web plate is 35~40mm, a magnetic field and an ultrasonic vibration field along the axis of the plasma arc welding gun are applied simultaneously during the welding process, and full penetration welding can be completed by performing a front welding through the plasma arc. When the web thickness is 40mm~50mm, a magnetic field and an ultrasonic vibration field along the axial direction of the plasma arc welding gun are applied simultaneously during the welding process. After the welding on the front side is completed, the pretreatment steps and welding steps are repeated on the back side to complete the full penetration welding.
6. The welding method for large-section I-beams without beveling according to claim 5, characterized in that, The plasma arc welding current is 280~350A, the voltage is 30~35V, and the welding speed is 200~250mm / min; the magnetic field strength is 10~50mT, and the direction is along the axis of the plasma arc welding torch; the ultrasonic vibration frequency is 20~50kHz, and the power is 100~300W.
7. A welding system for large-section I-beams without beveling, used to implement the welding method for large-section I-beams without beveling as described in any one of claims 1-6, characterized in that, include: Walking mechanism; A flame pretreatment unit is installed at the front end of the walking mechanism. It includes a first channel nozzle and a second channel nozzle. Both the first channel nozzle and the second channel nozzle include two nozzles, and the two nozzles are respectively arranged on both sides of the web thickness direction. Their nozzles are both directed to the root intersection area of the web side end face and the flange plate surface, so as to simultaneously perform flame treatment on the root intersection area of the web side end face and the flange plate surface. The flame pretreatment unit is connected to a gas supply system with a flow proportional valve. The plasma arc welding unit is installed on the traveling mechanism and located behind the flame pretreatment unit, and includes a welding power source capable of outputting a transfer-type plasma arc and a plasma arc welding torch. The tail protective gas cover is installed at the rear of the plasma arc welding unit.
8. The welding system for large-section I-beams without beveling according to claim 7, characterized in that, Also includes: A magnetic field generating device is installed outside the plasma arc welding torch to generate a magnetic field along the axial direction of the plasma arc welding torch. An ultrasonic vibration device is installed on the outside of the plasma arc welding torch to couple ultrasonic vibration to the molten pool.
9. The welding system for large-section I-beams without beveling according to claim 8, characterized in that, Also includes: The online monitoring unit includes a process infrared thermometer and a spectral reflectance film thickness probe located between the pretreatment unit and the welding unit; The central control system is connected to the online monitoring unit, the flow proportional valve of the gas supply system, the welding power supply, the magnetic field generator, and the ultrasonic vibration device.
Citation Information
Patent Citations
Moderately thick plate T-shaped joint full-submerged-arc welding beveling-free welding method
CN108856969A
Submerged-arc welding manufacturing method for extra-thick plate without beveling
CN115255574A
H-shaped steel double-wire submerged arc welding I-shaped groove back-chipping-free full penetration welding method
CN116038079A
Plasma welding method of aluminum alloy plate
JP2012061481A